CN107936818A - A kind of ultraviolet light cures solvent-free coated matte finishing coat and preparation method thereof - Google Patents

A kind of ultraviolet light cures solvent-free coated matte finishing coat and preparation method thereof Download PDF

Info

Publication number
CN107936818A
CN107936818A CN201711290907.6A CN201711290907A CN107936818A CN 107936818 A CN107936818 A CN 107936818A CN 201711290907 A CN201711290907 A CN 201711290907A CN 107936818 A CN107936818 A CN 107936818A
Authority
CN
China
Prior art keywords
solvent
ultraviolet light
cures
finishing coat
free coated
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201711290907.6A
Other languages
Chinese (zh)
Inventor
陈日云
林艳斌
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
AODA KOALA PAINT (HUIZHOU) Co Ltd
Original Assignee
AODA KOALA PAINT (HUIZHOU) Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by AODA KOALA PAINT (HUIZHOU) Co Ltd filed Critical AODA KOALA PAINT (HUIZHOU) Co Ltd
Priority to CN201711290907.6A priority Critical patent/CN107936818A/en
Publication of CN107936818A publication Critical patent/CN107936818A/en
Pending legal-status Critical Current

Abstract

The present invention relates to polymeric material field, specifically discloses a kind of ultraviolet light and cures solvent-free coated matte finishing coat, including following weight percent composition:Nine functional group's ultra-branched polyurethane acrylate resins 5% 25%, modified epoxy acrylic ester resin 5% 20%, auxiliary agent 10.8% 26%, photoinitiator 3% 6%, UV reactive diluents 30% 60%.The invention also discloses its preparation method.The ultraviolet light cures specious, excellent performance after solvent-free coated matte topcoating cures, and VOC free discharges in work progress, to human body and environmental-friendly.

Description

A kind of ultraviolet light cures solvent-free coated matte finishing coat and preparation method thereof
Technical field
The present invention relates to polymeric material field, and in particular to a kind of ultraviolet light cure solvent-free coated matte finishing coat and its Preparation method.
Background technology
UV paints are the english abbreviations of Ultraviolet Curing Paint, i.e. ultraviolet-curing paint, its principle of solidification It is coating under ultraviolet light, photoinitiator absorbs ultraviolet light and then decomposition, generates free radicals and light-cured resin and work Property diluent crosslinks, in moment, that is, curable film-forming.There is environmental protection, efficient, low cost.Spraying is photo-curing paint A kind of conventional construction technology, conventional ultraviolet light cure coated matte finishing coat need add 30%-50% organic solvent it is dilute Construction is released, since VOC volatilizees so that the coating of original environmental protection loses an advantage of maximum.How to solve the problems, such as this, subtract It is small extremely urgent to large natural environment pollution.
The content of the invention
, also can be normal in the case of organic solvent-free it is an object of the present invention to provide a kind of UV-curable finish coat Construct and obtain preferable lacquer painting effect.
Technical solution provided by the invention is as follows:
A kind of ultraviolet light cures solvent-free coated matte finishing coat, including following weight percent composition:
Nine functional group ultra-branched polyurethane acrylate resin 5%-25%,
Modified epoxy acrylic ester resin 5%-20%,
Auxiliary agent 10.8%-26%,
Photoinitiator 3%-6%,
UV reactive diluents 30%-60%.The UR2044 of the preferred blue card of the nine functional groups ultra-branched polyurethane acrylate resin; The 6210G in described preferred Changxing of modified epoxy acrylic ester resin.
Further, it is described account for percentage by weight 10.8%-26% auxiliary agent be:
Dispersant 0.3%-3%,
Defoamer 0.1%-0.5%,
Flatting silica 10%-20%,
Polyethylene wax powder 0.1%-1%,
Levelling agent A0.2%-1%,
Levelling agent B0.1%-0.5%.The Luwax A of the preferably German BASF of the Tissuemat E or the 3620 of Clariant.
Further, the dispersant is for the high-molecular block copolymer of the affinity groups containing pigment or containing acidic-group Copolymer solution.It is preferred that BYK-163, BYK-110, BYK-2009 etc..
Further, the defoamer is modified polyorganosiloxane defoamer.The modified polyorganosiloxane defoamer is excellent Select 5300 or 5400 or BYK-141 that moral is modest etc..
Further, the flatting silica is aerosil flatting silica.The preferred Gray of aerosil flatting silica This RAD2105, the flatting silica oil absorption are 120g/100m, are much smaller than most of flatting silica, such as Degussa OK500 oil absorptions are 260g/100m;Therefore viscosity increase to system is minimum, is conducive to be not added with organic solvent directly to spray Apply construction.
Further, the levelling agent A is fluorine-carbon modified polyacrylate high polymer.It is preferred that BYK358N, excellent card 376S。
Further, the levelling agent B is the polyether-modified dimethyl silicone polymer of finger.It is preferred that TEGO245, BYK333.
Further, the photoinitiator for 2- hydroxyls -4 ' -(2- hydroxy ethoxies)- 2- methyl phenyl ketones.It is preferred that Bath The 2959 of husband.
Further, the UV reactive diluents for tripropylene glycol diacrylate, two contracting propane diols double methacrylates, One or both of hydroxyethyl methacrylate.It is preferred that the HEMA in Changxing, DPGDA, TPGDA etc..
A kind of ultraviolet light cures the preparation method of solvent-free coated matte finishing coat, includes the following steps:
Step A. first puts into resin and UV reactive diluents, dispersant to reaction kettle in formula, with 1000-1200 rpms Rotating speed disperses 20-30 minutes;
Step B. is disperseed 20-30 minutes according to formula input defoamer, levelling agent with 800-1200 rpms of rotating speed;
Step C. puts into photoinitiator, is disperseed 20-30 minutes with 1000-1200 rpms of rotating speed;
Step D. disperses 30-40 points according to formula input flatting silica and polyethylene wax powder with 1200-1800 rpms of rotating speed Clock;
Step E. puts into all remaining UV reactive diluents, is disperseed 15-20 minutes with 600-800 rpms of rotating speed, after Filtered and packaged with 300 mesh filter screens.
Compared with prior art, innovative point of the invention is:
Introduce nine functional group's super branched polyurethanes and high reaction rate is provided, it is with extremely low viscosity(600-1200mpa•s), So that in the case where curing rate is exceedingly fast, it can not construct without because of the excessive viscosity of resin, avoid organic volatile The generation of thing.Also arrange in pairs or groups modified epoxy acrylic ester resin, while low viscosity is kept, gloss protrudes after curing, has reason The appearance thought, hardness, wear-resisting property, weatherability, chemical-resistant, resistance tocrocking etc. is good.
UV reactive diluents select low-shrinkage, monomer HEMA, DPGDA of highly diluted, so as to reduce the receipts of system Shrinkage, greatly reduces the viscosity of spraying paint, makes the solvent-free spraying paint more convenient in construction.
Embodiment
The present invention is described in further detail below in conjunction with specific embodiment.
It is as shown in the table for the formula of embodiment 1~6:
Table 1:
The preparation method of above example is:
Step A. first puts into resin and UV reactive diluents, dispersant to reaction kettle in formula, with 1000-1200 rpms Rotating speed disperses 20 minutes;
Step B. is disperseed 20 minutes according to formula input defoamer, levelling agent with 800-1200 rpms of rotating speed;
Step C. puts into photoinitiator, is disperseed 20 minutes with 1000-1200 rpms of rotating speed;
Step D. is disperseed 30 minutes according to formula input flatting silica and polyethylene wax powder with 1200-1800 rpms of rotating speed;
Step E. puts into all remaining UV reactive diluents, is disperseed 15 minutes with 600-800 rpms of rotating speed, rear to use 300 mesh filter screens filter and package.
In order to further illustrate the present invention, by solvent-free coated matte finishing coat made from above method in reciprocating spraying machine Upper construction, does performance test.
The inspection of its performance the results are shown in Table 2:
Table 2:
Result above shows that the present invention, which meets HG/T 3655-2012 standards and solves Conventional UV photocureable coating and do, sprays During painting must using organic solvent to dilute the problem of, entirely without VOC volatilization there is no any destruction to environment, to construction personnel's Health, which also has, to be ensured.
Although description of this invention combination embodiments above carries out, those skilled in the art Member can carry out many replacements, modifications and variations according to above-mentioned content, be obvious.Therefore, it is all it is such substitute, Improve and change is included in the spirit and scope of appended claims.

Claims (10)

1. a kind of ultraviolet light cures solvent-free coated matte finishing coat, it is characterised in that including following weight percent composition:
Nine functional group ultra-branched polyurethane acrylate resin 5%-25%,
Modified epoxy acrylic ester resin 5%-20%,
Auxiliary agent 10.8%-26%,
Photoinitiator 3%-6%,
UV reactive diluents 30%-60%.
2. ultraviolet light according to claim 1 cures solvent-free coated matte finishing coat, it is characterised in that described to account for weight hundred Auxiliary agent point than 10.8%-26% is:
Dispersant 0.3%-3%,
Defoamer 0.1%-0.5%,
Flatting silica 10%-20%,
Polyethylene wax powder 0.1%-1%,
Levelling agent A0.2%-1%,
Levelling agent B0.1%-0.5%.
3. ultraviolet light according to claim 2 cures solvent-free coated matte finishing coat, it is characterised in that the dispersant For the high-molecular block copolymer of the affinity groups containing pigment or the copolymer solution containing acidic-group.
4. ultraviolet light according to claim 2 cures solvent-free coated matte finishing coat, it is characterised in that the defoamer For modified polyorganosiloxane defoamer.
5. ultraviolet light according to claim 2 cures solvent-free coated matte finishing coat, it is characterised in that the flatting silica For aerosil flatting silica.
6. ultraviolet light according to claim 2 cures solvent-free coated matte finishing coat, it is characterised in that the levelling agent A is fluorine-carbon modified polyacrylate high polymer.
7. ultraviolet light according to claim 2 cures solvent-free coated matte finishing coat, it is characterised in that the levelling agent B is the polyether-modified dimethyl silicone polymer of finger.
8. ultraviolet light according to claim 1 or 2 cures solvent-free coated matte finishing coat, it is characterised in that the light Initiator for 2- hydroxyls -4 ' -(2- hydroxy ethoxies)- 2- methyl phenyl ketones.
9. ultraviolet light according to claim 1 or 2 cures solvent-free coated matte finishing coat, it is characterised in that the UV Reactive diluent is tripropylene glycol diacrylate, one kind in two contracting propane diols double methacrylates, hydroxyethyl methacrylate Or two kinds.
10. the ultraviolet light described in a kind of claim 2-7 cures the preparation method of solvent-free coated matte finishing coat, its feature exists In including the following steps:
Step A. first puts into resin and UV reactive diluents, dispersant to reaction kettle in formula, with 1000-1200 rpms Rotating speed disperse 20-30 minutes;
Step B. is disperseed 20-30 minutes according to formula input defoamer, levelling agent with 800-1200 rpms of rotating speed;
Step C. puts into photoinitiator, is disperseed 20-30 minutes with 1000-1200 rpms of rotating speed;
Step D. disperses 30-40 points according to formula input flatting silica and polyethylene wax powder with 1200-1800 rpms of rotating speed Clock;
Step E. puts into all remaining UV reactive diluents, is disperseed 15-20 minutes with 600-800 rpms of rotating speed, after Filtered and packaged with 300 mesh filter screens.
CN201711290907.6A 2017-12-08 2017-12-08 A kind of ultraviolet light cures solvent-free coated matte finishing coat and preparation method thereof Pending CN107936818A (en)