CN107127857A - A kind of solid wood door and window timber preparation technology - Google Patents
A kind of solid wood door and window timber preparation technology Download PDFInfo
- Publication number
- CN107127857A CN107127857A CN201710528651.1A CN201710528651A CN107127857A CN 107127857 A CN107127857 A CN 107127857A CN 201710528651 A CN201710528651 A CN 201710528651A CN 107127857 A CN107127857 A CN 107127857A
- Authority
- CN
- China
- Prior art keywords
- timber
- window
- preparation technology
- solid wood
- carpenter
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses a kind of solid wood door and window timber preparation technology, comprise the following steps:The selection of timber, the preprocessing processing of timber, the preparation of timber, being processed further of timber, the cleaning of timber, the preservation of timber.Processing is dried when early stage is handled the preprocessing of timber with timber preparation technology in the solid wood door and window, so reduce the quality of timber, the hardness of timber can be improved simultaneously, so that more laborsaving during people's taking and placing timber during timber preparation, and it is more accurate when carrying out size sawing and punchinging, prevent because being shunk when the excessive water later stage is dried, cause size and punching larger error occur, and can prevent from damaging by worms when preserving in the later stage, and can prevent timber from contacting water swelling with external environment, timber is caused to damage.
Description
Technical field
The invention belongs to solid wood door and window manufacturing technology field, and in particular to a kind of solid wood door and window timber preparation technology.
Background technology
Door and window is the essential part in house, by door and window can with outside world exchange and conmmunication, while door and window
Sunlight is brought to us and warm, resists the wind and rain and noise in the external world.Solid wood door and window is with simple and unsophisticated, environmentally friendly, elegant and poised for spy
Point, it is deep to be liked by common people.The outward appearance of door and window also embodies a kind of taste of life.Accuracy influence prepared by early stage timber
The preparation of later stage solid wood door and window, if the gap that precision not enough may result between Solid Door window assembly is excessive, so as to influence
Attractive in appearance and quality, and timber not necessarily can timely be processed into door and window after production, so we need to preserve, but
Existing timber preparation technology is simply to be placed on timber one time, and so long-term placement can cause timber absorbs extraneous
Water, cause it to expand, and long-term placement can damage by worms, so we need a new solid wood door and window timber
Preparation technology solves the above problems, and meets the demand of people.
The content of the invention
It is an object of the invention to provide a kind of solid wood door and window timber preparation technology, to solve to carry in above-mentioned background technology
The problem of going out.
To achieve the above object, the present invention provides following technical scheme:A kind of solid wood door and window timber preparation technology, including
Following steps:
A, timber selection:There are certain intensity and toughness, rigidity and hardness, material-structure should be careful;There is the natural line of beauty
Reason, material sense is pleasing;Drying shrinkage, dilatancy and buckling deformation are small;Easy processing, cutting ability is good;
B, timber preprocessing processing:Simple sawing is carried out to timber first, then polished using polishing paper, it is most laggard
Row drying process, makes its moisture content in 8%-14%;
C, timber preparation:According to the size of solid wood door and window, width, length and the thickness of each component are calculated, then to timber
Preliminary sawing is carried out, accurate finishing then is carried out to the timber of sawing using carpenter's plane or carpenter's planing lathe, used
Polishing paper is polished Wood surface, is then blown the wood chip of Wood surface off using air gun, is finally wiped using wet towel;
D, timber are processed further:Chisel is carried out to the timber prepared to cut and milling;It is exactly to be transported using the impact of chisel that chisel, which is cut,
It is dynamic, sharp cutting edge is vertically cut off lumber fibre and enter in it, and wood chip is constantly discharged, gradually process required side
Shape, rectangle or circle are punchinged, and chisel, which is cut, is divided into carpenter's flat chisel and carpenter's flat chisel hole machine tool;Milling:Wood-milling machine is mainly used in curved profile
Such as concavo-convex platform of processing, cambered surface and sphere;
E, timber cleaning:The wood chip of Wood surface to processing is cleared up, and is blown off wood chip using air gun, is then used
Wet towel is wiped, and waits moisture to spontaneously dry;
F, timber preservation:The complete timber of above-mentioned cleaning is subjected to mopping, simple varnish work prevents from placing generation for a long time
Water swelling and situation about damaging by worms occur.
It is preferred that, the carpenter's plane in the step C is divided into planer, plow, rabbet plane, iron plane and special-shaped plane etc..
It is preferred that, carpenter's planing lathe is to drive planing tool to rotate at a high speed to process by cutter shaft, is generally divided into planer
Bed and the major class of press wood planer two.
It is preferred that, the drying of middle timber is divided into natural drying and artificial drying in the step B, when timber is suddenly needed to use
When use artificial drying, faster, but cost is high for such speed;Using natural drying when not being badly in need of using.
It is preferred that, the instrument that the brushing of varnish is used in the step F is hairbrush or spray gun, when workload is small
Using hairbrush;Spray gun is used when workload is big.
The technique effect and advantage of the present invention:The solid wood door and window is with timber preparation technology at preprocessing of the early stage to timber
Processing is dried when reason, the quality of timber is so reduced, while the hardness of timber can be improved so that be prepared by timber
When people's taking and placing timber when it is more laborsaving, and carry out size sawing and when punching it is more accurate, prevent because of water
Point excessive later stage shrinks when drying, causes size and punching larger error occur, and later stage preservation when
Time can prevent from damaging by worms, and can prevent timber from contacting water swelling with external environment, cause timber to damage.
Embodiment
It is clearly and completely described below in conjunction with the technical scheme in the embodiment of the present invention, it is clear that described reality
It is only a part of embodiment of the invention to apply example, rather than whole embodiments.Based on the embodiment in the present invention, this area is general
The every other embodiment that logical technical staff is obtained under the premise of creative work is not made, belongs to what the present invention was protected
Scope.
Embodiment 1
A kind of solid wood door and window timber preparation technology, comprises the following steps:
A, timber selection:There are certain intensity and toughness, rigidity and hardness, material-structure should be careful;There is the natural line of beauty
Reason, material sense is pleasing;Drying shrinkage, dilatancy and buckling deformation are small;Easy processing, cutting ability is good;
B, timber preprocessing processing:Simple sawing is carried out to timber first, then polished using polishing paper, it is most laggard
Row drying process, makes its moisture content 8%;
C, timber preparation:According to the size of solid wood door and window, width, length and the thickness of each component are calculated, then to timber
Preliminary sawing is carried out, accurate finishing then is carried out to the timber of sawing using carpenter's plane or carpenter's planing lathe, used
Polishing paper is polished Wood surface, is then blown the wood chip of Wood surface off using air gun, is finally wiped using wet towel;
D, timber are processed further:Chisel is carried out to the timber prepared to cut and milling;It is exactly to be transported using the impact of chisel that chisel, which is cut,
It is dynamic, sharp cutting edge is vertically cut off lumber fibre and enter in it, and wood chip is constantly discharged, gradually process required side
Shape, rectangle or circle are punchinged, and chisel, which is cut, is divided into carpenter's flat chisel and carpenter's flat chisel hole machine tool;Milling:Wood-milling machine is mainly used in curved profile
Such as concavo-convex platform of processing, cambered surface and sphere;
E, timber cleaning:The wood chip of Wood surface to processing is cleared up, and is blown off wood chip using air gun, is then used
Wet towel is wiped, and waits moisture to spontaneously dry;
F, timber preservation:The complete timber of above-mentioned cleaning is subjected to mopping, simple varnish work prevents from placing generation for a long time
Water swelling and situation about damaging by worms occur.
A kind of above-mentioned solid wood door and window timber preparation technology, wherein, the carpenter's plane in the step C be divided into planer, plow,
Rabbet plane, iron plane and special-shaped plane etc..
A kind of above-mentioned solid wood door and window timber preparation technology, wherein, carpenter's planing lathe is to drive to dig by cutter shaft
Knife up speed rotates to process, and is generally divided into flat planing machine and the major class of press wood planer two.
A kind of above-mentioned solid wood door and window timber preparation technology, wherein, the drying of middle timber is divided into nature and done in the step B
Dry and artificial drying, uses artificial drying when timber is suddenly needed to use, and faster, but cost is high for such speed;When not anxious
Using natural drying when need to using.
A kind of above-mentioned solid wood door and window timber preparation technology, wherein, the instrument that the brushing of varnish is used in the step F is
Hairbrush or spray gun, use hairbrush when workload is small;Spray gun is used when workload is big.
Embodiment 2
A kind of solid wood door and window timber preparation technology, comprises the following steps:
A, timber selection:There are certain intensity and toughness, rigidity and hardness, material-structure should be careful;There is the natural line of beauty
Reason, material sense is pleasing;Drying shrinkage, dilatancy and buckling deformation are small;Easy processing, cutting ability is good;
B, timber preprocessing processing:Simple sawing is carried out to timber first, then polished using polishing paper, it is most laggard
Row drying process, makes its moisture content 11%;
C, timber preparation:According to the size of solid wood door and window, width, length and the thickness of each component are calculated, then to timber
Preliminary sawing is carried out, accurate finishing then is carried out to the timber of sawing using carpenter's plane or carpenter's planing lathe, used
Polishing paper is polished Wood surface, is then blown the wood chip of Wood surface off using air gun, is finally wiped using wet towel;
D, timber are processed further:Chisel is carried out to the timber prepared to cut and milling;It is exactly to be transported using the impact of chisel that chisel, which is cut,
It is dynamic, sharp cutting edge is vertically cut off lumber fibre and enter in it, and wood chip is constantly discharged, gradually process required side
Shape, rectangle or circle are punchinged, and chisel, which is cut, is divided into carpenter's flat chisel and carpenter's flat chisel hole machine tool;Milling:Wood-milling machine is mainly used in curved profile
Such as concavo-convex platform of processing, cambered surface and sphere;
E, timber cleaning:The wood chip of Wood surface to processing is cleared up, and is blown off wood chip using air gun, is then used
Wet towel is wiped, and waits moisture to spontaneously dry;
F, timber preservation:The complete timber of above-mentioned cleaning is subjected to mopping, simple varnish work prevents from placing generation for a long time
Water swelling and situation about damaging by worms occur.
A kind of above-mentioned solid wood door and window timber preparation technology, wherein, the carpenter's plane in the step C be divided into planer, plow,
Rabbet plane, iron plane and special-shaped plane etc..
A kind of above-mentioned solid wood door and window timber preparation technology, wherein, carpenter's planing lathe is to drive to dig by cutter shaft
Knife up speed rotates to process, and is generally divided into flat planing machine and the major class of press wood planer two.
A kind of above-mentioned solid wood door and window timber preparation technology, wherein, the drying of middle timber is divided into nature and done in the step B
Dry and artificial drying, uses artificial drying when timber is suddenly needed to use, and faster, but cost is high for such speed;When not anxious
Using natural drying when need to using.
A kind of above-mentioned solid wood door and window timber preparation technology, wherein, the instrument that the brushing of varnish is used in the step F is
Hairbrush or spray gun, use hairbrush when workload is small;Spray gun is used when workload is big.
Embodiment 3
A kind of solid wood door and window timber preparation technology, comprises the following steps:
A, timber selection:There are certain intensity and toughness, rigidity and hardness, material-structure should be careful;There is the natural line of beauty
Reason, material sense is pleasing;Drying shrinkage, dilatancy and buckling deformation are small;Easy processing, cutting ability is good;
B, timber preprocessing processing:Simple sawing is carried out to timber first, then polished using polishing paper, it is most laggard
Row drying process, makes its moisture content 14%;
C, timber preparation:According to the size of solid wood door and window, width, length and the thickness of each component are calculated, then to timber
Preliminary sawing is carried out, accurate finishing then is carried out to the timber of sawing using carpenter's plane or carpenter's planing lathe, used
Polishing paper is polished Wood surface, is then blown the wood chip of Wood surface off using air gun, is finally wiped using wet towel;
D, timber are processed further:Chisel is carried out to the timber prepared to cut and milling;It is exactly to be transported using the impact of chisel that chisel, which is cut,
It is dynamic, sharp cutting edge is vertically cut off lumber fibre and enter in it, and wood chip is constantly discharged, gradually process required side
Shape, rectangle or circle are punchinged, and chisel, which is cut, is divided into carpenter's flat chisel and carpenter's flat chisel hole machine tool;Milling:Wood-milling machine is mainly used in curved profile
Such as concavo-convex platform of processing, cambered surface and sphere;
E, timber cleaning:The wood chip of Wood surface to processing is cleared up, and is blown off wood chip using air gun, is then used
Wet towel is wiped, and waits moisture to spontaneously dry;
F, timber preservation:The complete timber of above-mentioned cleaning is subjected to mopping, simple varnish work prevents from placing generation for a long time
Water swelling and situation about damaging by worms occur.
A kind of above-mentioned solid wood door and window timber preparation technology, wherein, the carpenter's plane in the step C be divided into planer, plow,
Rabbet plane, iron plane and special-shaped plane etc..
A kind of above-mentioned solid wood door and window timber preparation technology, wherein, carpenter's planing lathe is to drive to dig by cutter shaft
Knife up speed rotates to process, and is generally divided into flat planing machine and the major class of press wood planer two.
A kind of above-mentioned solid wood door and window timber preparation technology, wherein, the drying of middle timber is divided into nature and done in the step B
Dry and artificial drying, uses artificial drying when timber is suddenly needed to use, and faster, but cost is high for such speed;When not anxious
Using natural drying when need to using.
A kind of above-mentioned solid wood door and window timber preparation technology, wherein, the instrument that the brushing of varnish is used in the step F is
Hairbrush or spray gun, use hairbrush when workload is small;Spray gun is used when workload is big.
Finally it should be noted that:The preferred embodiments of the present invention are the foregoing is only, are not intended to limit the invention,
Although the present invention is described in detail with reference to the foregoing embodiments, for those skilled in the art, it still may be used
To be modified to the technical scheme described in foregoing embodiments, or equivalent substitution is carried out to which part technical characteristic,
Within the spirit and principles of the invention, any modification, equivalent substitution and improvements made etc., should be included in the present invention's
Within protection domain.
Claims (5)
1. a kind of solid wood door and window timber preparation technology, it is characterised in that:Comprise the following steps:
A, timber selection:There are certain intensity and toughness, rigidity and hardness, material-structure should be careful;There is the natural line of beauty
Reason, material sense is pleasing;Drying shrinkage, dilatancy and buckling deformation are small;Easy processing, cutting ability is good;
B, timber preprocessing processing:Simple sawing is carried out to timber first, then polished using polishing paper, it is most laggard
Row drying process, makes its moisture content in 8%-14%;
C, timber preparation:According to the size of solid wood door and window, width, length and the thickness of each component are calculated, then to timber
Preliminary sawing is carried out, accurate finishing then is carried out to the timber of sawing using carpenter's plane or carpenter's planing lathe, used
Polishing paper is polished Wood surface, is then blown the wood chip of Wood surface off using air gun, is finally wiped using wet towel;
D, timber are processed further:Chisel is carried out to the timber prepared to cut and milling;It is exactly to be transported using the impact of chisel that chisel, which is cut,
It is dynamic, sharp cutting edge is vertically cut off lumber fibre and enter in it, and wood chip is constantly discharged, gradually process required side
Shape, rectangle or circle are punchinged, and chisel, which is cut, is divided into carpenter's flat chisel and carpenter's flat chisel hole machine tool;Milling:Wood-milling machine is mainly used in curved profile
Such as concavo-convex platform of processing, cambered surface and sphere;
E, timber cleaning:The wood chip of Wood surface to processing is cleared up, and is blown off wood chip using air gun, is then used
Wet towel is wiped, and waits moisture to spontaneously dry;
F, timber preservation:The complete timber of above-mentioned cleaning is subjected to mopping, simple varnish work prevents from placing generation for a long time
Water swelling and situation about damaging by worms occur.
2. a kind of solid wood door and window timber preparation technology according to claim 1, it is characterised in that:In the step C
Carpenter's plane is divided into planer, plow, rabbet plane, iron plane and special-shaped plane etc..
3. a kind of solid wood door and window timber preparation technology according to claim 1, it is characterised in that:Carpenter's planer
Bed is to drive planing tool to rotate at a high speed to process by cutter shaft, is generally divided into flat planing machine and the major class of press wood planer two.
4. a kind of solid wood door and window timber preparation technology according to claim 1, it is characterised in that:In in the step B
The drying of timber is divided into natural drying and artificial drying, and artificial drying, such speed are used when timber is suddenly needed to use
Faster, but cost is high;Using natural drying when not being badly in need of using.
5. a kind of solid wood door and window timber preparation technology according to claim 1, it is characterised in that:It is clear in the step F
The instrument that the brushing of paint is used is hairbrush or spray gun, and hairbrush is used when workload is small;Adopted when workload is big
Use spray gun.