CN106784419A - A kind of corrosion-resistant dynamic lithium battery aluminum hull and preparation method thereof - Google Patents

A kind of corrosion-resistant dynamic lithium battery aluminum hull and preparation method thereof Download PDF

Info

Publication number
CN106784419A
CN106784419A CN201611191166.1A CN201611191166A CN106784419A CN 106784419 A CN106784419 A CN 106784419A CN 201611191166 A CN201611191166 A CN 201611191166A CN 106784419 A CN106784419 A CN 106784419A
Authority
CN
China
Prior art keywords
aluminum hull
aluminum
corrosion
aluminium foil
copper foil
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201611191166.1A
Other languages
Chinese (zh)
Inventor
周润杰
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
CHANGSHU GAOJIA ENERGY TECHNOLOGY Co Ltd
Original Assignee
CHANGSHU GAOJIA ENERGY TECHNOLOGY Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by CHANGSHU GAOJIA ENERGY TECHNOLOGY Co Ltd filed Critical CHANGSHU GAOJIA ENERGY TECHNOLOGY Co Ltd
Priority to CN201611191166.1A priority Critical patent/CN106784419A/en
Publication of CN106784419A publication Critical patent/CN106784419A/en
Pending legal-status Critical Current

Abstract

The invention discloses a kind of corrosion-resistant electrokinetic cell aluminum hull and preparation method thereof, the aluminum hull includes:Aluminum hull body, the aluminum hull body includes that ecto-entad is combined aluminum base plate, aluminium foil and Copper Foil successively;It is combined by the way of cold rolling forging is closed between the aluminium foil and aluminum base plate, is combined by the way of the Rolling compund that explodes between the Copper Foil and the aluminium foil.The preparation method includes:(1)Prepare aluminum base plate;(2)Prepare aluminium foil and Copper Foil composite plate;(3)Prepare aluminum hull sheet material;(4)Drawing and forming.A kind of preparation method of corrosion-resistant electrokinetic cell aluminum hull of the present invention, it passes through rolling mill practice Rolling compund aluminium foil and Copper Foil inside aluminum is basic twice, effectively prevent contact of the lithium battery with aluminium casing, so as to suppress or delay the corrosion reaction in housing, improve the corrosion resistance of aluminum hull, Corrosion Protection to improving aluminum hull has great importance, and practicality is stronger, wide market.

Description

A kind of corrosion-resistant dynamic lithium battery aluminum hull and preparation method thereof
Technical field
The present invention relates to housing of power cell field, more particularly to a kind of corrosion-resistant electrokinetic cell aluminum hull and its preparation side Method.
Background technology
The features such as lithium ion battery has light weight, high specific energy, long-life and uses safe, becomes the power of a new generation Battery, and used in electric vehicle and energy storage field more and more.
Aluminum hull has the advantages that lightweight, good toughness, easy to process, gravimetric specific energy are high, current application than wide, Especially in the automobile power cell field that capacity is higher.But some aluminum hulls are during long-term storage or use, it may occur that rotten Erosion, causes aluminum hull leakage, not only pollutes environment, and cause very big potential safety hazard.The reason for aluminum hull corrodes mainly has contact Internal corrosion caused by the external corrosion of corrosive substance and internal generation side reaction.Wherein, internal corrosion is due to Li insertions The corrosion that loose aluminium lithium alloy produces chemical reaction to cause is formed in aluminum hull.
The content of the invention
The present invention solves the technical problem of a kind of corrosion-resistant electrokinetic cell aluminum hull of offer and preparation method thereof.
In order to solve the above technical problems, one aspect of the present invention is:A kind of corrosion-resistant electrokinetic cell is provided Aluminum hull, including:Aluminum hull body, the aluminum hull body includes that ecto-entad is combined aluminum base plate, aluminium foil and Copper Foil successively;The aluminium It is combined by the way of cold rolling forging is closed between paper tinsel and aluminum base plate, using blast Rolling compund between the Copper Foil and the aluminium foil Mode be combined.
In a preferred embodiment of the present invention, the gross thickness of the aluminium foil and Copper Foil accounts for the 1/ of the aluminum base plate thickness 7~1/10.
In a preferred embodiment of the present invention, the ratio between thickness of the aluminium foil and Copper Foil is 1:2~3.
In order to solve the above technical problems, another technical solution used in the present invention is:A kind of corrosion-resistant battery aluminium is provided The preparation method of shell, comprises the following steps:
(1)Prepare aluminum base plate:The soft state aluminium sheet for using thickness thicker is substrate;
(2)Prepare aluminium foil and Copper Foil composite plate:The aluminium foil and Copper Foil are first produced into rolling embryo, Ran Houzai through explosion composite method It is rolled into composite plate;
(3)Prepare aluminum hull sheet material:By step(2)The aluminium foil one side of the composite plate of middle preparation is attached to step(1)The aluminium of middle preparation On substrate processed, using it is cold rolling it is compound by the way of continuous rolling compound;
(4)Drawing and forming:By step(3)The composite plate of middle preparation is prepared into the aluminum hull through cold drawn stretching process.
The beneficial effects of the invention are as follows:A kind of preparation method of corrosion-resistant electrokinetic cell aluminum hull of the present invention, it passes through twice Rolling mill practice effectively prevents contact of the lithium battery with aluminium casing in the basic internal Rolling compund aluminium foil of aluminum and Copper Foil, so that Suppress or delay the corrosion reaction in housing, improve the corrosion resistance of aluminum hull, the Corrosion Protection to improving aluminum hull has weight The meaning wanted, practicality is stronger, wide market.
Brief description of the drawings
Fig. 1 is a kind of structural representation of corrosion-resistant electrokinetic cell aluminum hull housing of the present invention;
The mark of each part is as follows in accompanying drawing:1. aluminum hull housing, 11. aluminum base plates, 12. aluminium foils, 13. Copper Foils.
Specific embodiment
Presently preferred embodiments of the present invention is described in detail below in conjunction with the accompanying drawings, so that advantages and features of the invention energy It is easier to be readily appreciated by one skilled in the art, apparent is clearly defined so as to be made to protection scope of the present invention.
Fig. 1 is referred to, the embodiment of the present invention includes:
Embodiment 1
A kind of corrosion-resistant electrokinetic cell aluminum hull, including:Aluminum hull body 1, the aluminum hull body includes ecto-entad clad aluminum successively Substrate processed 11, aluminium foil 12 and Copper Foil 13;Wherein, the gross thickness of the aluminium foil 12 and Copper Foil 3 accounts for the thickness of the aluminum base plate 11 1/15~1/20;The ratio between thickness of the aluminium foil 12 and Copper Foil 13 is 1:2~3.
It is combined by the way of cold rolling forging is closed between above-mentioned aluminium foil 12 and aluminum base plate 11, is adopted between Copper Foil 13 and aluminium foil 12 It is combined with the mode of blast Rolling compund.
The preparation method of above-mentioned corrosion-resistant battery aluminum shell, comprises the following steps that:
(1)Prepare aluminum base plate:The soft state aluminium sheet for using thickness thicker is substrate;
(2)Prepare aluminium foil and Copper Foil composite plate:The aluminium foil and Copper Foil are first produced into rolling embryo, Ran Houzai through explosion composite method It is rolled into composite plate;
(3)Prepare aluminum hull sheet material:By step(2)The aluminium foil one side of the composite plate of middle preparation is attached to step(1)The aluminium of middle preparation On substrate processed, using it is cold rolling it is compound by the way of continuous rolling compound;
(4)Drawing and forming:By step(3)The composite plate of middle preparation is prepared into the aluminum hull through cold drawn stretching process.
For example,
1st, it is 2mm to use thickness first, and width is 45mm, and the trade mark is that 3003 soft state aluminium sheet is base material;
2nd, it is 45mm to use width, and thickness is the aluminium foil of 0.3mm, and it is 45mm to use width, and thickness is the Copper Foil of 0.8mm, is passed through Explosion composite method produces rolling embryo, then rolled blank is rolled into composite plate;
3rd, the aluminium foil side of the composite plate after the rolling and aluminum base plate are combined, corrosion resistant is combined into by being stacked continuous rolling Erosion plate;
4th, corrosion-resistant plate is drawn into by housing of the aluminum base plate in outside by drawing process.
Above-mentioned housing can be prevented effectively from Li and generate aluminium with reactive aluminum because of one layer of inertia copper foil layer of inner wall surface thereof Rolling compund Lithium alloy, so as to improve the corrosion resistance of housing.
Embodiments of the invention are the foregoing is only, the scope of the claims of the invention is not thereby limited, it is every to utilize this hair Equivalent structure or equivalent flow conversion that bright specification and accompanying drawing content are made, or directly or indirectly it is used in other related skills Art field, is included within the scope of the present invention.

Claims (4)

1. a kind of corrosion-resistant electrokinetic cell aluminum hull, including:Aluminum hull body, it is characterised in that the aluminum hull body is included by extroversion Aluminum base plate, aluminium foil and Copper Foil are inside combined successively;It is combined by the way of cold rolling forging is closed between the aluminium foil and aluminum base plate, institute State and be combined by the way of the Rolling compund that explodes between Copper Foil and the aluminium foil.
2. corrosion-resistant electrokinetic cell aluminum hull according to claim 1, it is characterised in that the gross thickness of the aluminium foil and Copper Foil Account for the 1/15~1/20 of the aluminum base plate thickness.
3. corrosion-resistant electrokinetic cell aluminum hull according to claim 1, it is characterised in that the thickness of the aluminium foil and Copper Foil it Than being 1:2~3.
4. the preparation method of a kind of corrosion-resistant battery aluminum shell as described in any one of claims 1 to 3, it is characterised in that including Following steps:
(1)Prepare aluminum base plate:The soft state aluminium sheet for using thickness thicker is substrate;
(2)Prepare aluminium foil and Copper Foil composite plate:The aluminium foil and Copper Foil are first produced into rolling embryo, Ran Houzai through explosion composite method It is rolled into composite plate;
(3)Prepare aluminum hull sheet material:By step(2)The aluminium foil one side of the composite plate of middle preparation is attached to step(1)The aluminium of middle preparation On substrate processed, using it is cold rolling it is compound by the way of continuous rolling compound;
(4)Drawing and forming:By step(3)The composite plate of middle preparation is prepared into the aluminum hull through cold drawn stretching process.
CN201611191166.1A 2016-12-21 2016-12-21 A kind of corrosion-resistant dynamic lithium battery aluminum hull and preparation method thereof Pending CN106784419A (en)