CN106589698A - Nanometer calcium carbonate addition reinforced modified special PVC tube used for coal mine wells, and making method thereof - Google Patents

Nanometer calcium carbonate addition reinforced modified special PVC tube used for coal mine wells, and making method thereof Download PDF

Info

Publication number
CN106589698A
CN106589698A CN201611165898.3A CN201611165898A CN106589698A CN 106589698 A CN106589698 A CN 106589698A CN 201611165898 A CN201611165898 A CN 201611165898A CN 106589698 A CN106589698 A CN 106589698A
Authority
CN
China
Prior art keywords
calcium carbonate
parts
coal mine
nano
nanometer calcium
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201611165898.3A
Other languages
Chinese (zh)
Inventor
吴跃强
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
ANHUI HUAYU PIPELINE MANUFACTURING Co Ltd
Original Assignee
ANHUI HUAYU PIPELINE MANUFACTURING Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by ANHUI HUAYU PIPELINE MANUFACTURING Co Ltd filed Critical ANHUI HUAYU PIPELINE MANUFACTURING Co Ltd
Priority to CN201611165898.3A priority Critical patent/CN106589698A/en
Publication of CN106589698A publication Critical patent/CN106589698A/en
Pending legal-status Critical Current

Abstract

The invention discloses a nanometer calcium carbonate reinforced modified special PVC tube used for coal mine wells. The PVC tube is made from, by weight, 100 parts of PVC resin, 14.7-15.7 parts of glass fibers, 3.2-3.6 parts of nanometer calcium carbonate, 1.1-1.4 parts of zinc stearate, 6-8 parts of carbon fibers, 17-21 parts of zeolite powder, 3.8-4.3 parts of samarium oxide, 2.3-2.6 parts of asphalt, 5.3-5.7 parts of methyltriethoxysilane, 1.4-1.7 parts of ethoxyquinoline, 0.9-1.3 parts of tall oil acid and a proper amount of water. Nanometer calcium carbonate is coupled with the methyltriethoxysilane, the surface of the glass fibers is coated with the methyltriethoxysilane coupled nanometer calcium carbonate used as a reinforcement material, the zeolite powder is modified with the samarium oxide and the asphalt to form a modification filler, and other effective assistants are added, so the produced PVC tube used in coal mine well environment has the advantages of good corrosion and wear resistance, high tensile strength and good antibacterial property.

Description

A kind of addition nano-calcium carbonate strengthens the coal mine special PVC pipe and its making being modified Method
Technical field
The present invention relates to PVC and preparation method thereof technical field, more particularly to a kind of addition nano-calcium carbonate enhancing Modified coal mine special PVC pipe and preparation method thereof.
Background technology
Polyvinyl chloride(PVC)Resin be thermoplastic resin most widely used in our daily lifes, that consumption is maximum it One, it has lightweight, good insulating, difficult to burn, strong mechanical performance, cheap, abundant raw material source, manufacturing process maturation etc. Feature, thus be used widely in the fields such as coal mine pipes for mining material.However, its rushing of also having that some are difficult to overcome Hit poor performance, the shortcomings of heat endurance is not good enough, in order to overcome many scholars of the disadvantages described above of polyvinyl chloride in PVC toughening modifying sides Face has carried out substantial amounts of research, and current glass fibre has been progressed in the visual field of PVC study on the modification persons, such as document《Glass The preparation of fiber/polyvinyl chloride composite materials and performance study》Glass fibre/PVC is prepared for using injection molding method(Polychlorostyrene second Alkene)Composite.Result of study shows:When shaping penetrate pressure for 130MPa, pressurize be 100MPa, back pressure be 0.5MPa, shaping temperature It is 100 DEG C and w to spend for 420 DEG C, mold temperature(Glass fibre)=15%(For composite quality)When, composite Combination property it is relatively best, its tensile strength(77.4MPa)And shear strength(57.4MPa)Relative maximum, and product table The smooth color in face is normal, and the pure PVC of bending strength ratio improves 68.4%.
It is well known that colliery is a special operating environment, dark, moist, narrow space has falling rocks sometimes, this Being accomplished by PVC will not only have enough impact strengths, also there is the property such as antistatic, fire-retardant, wear-resisting, antibacterial, anti-corrosive properties Energy.Yet with polyvinyl chloride high-insulation, its sheet resistance is up to 1014 Ω or so, and this insulating properties usually make polychlorostyrene second Alkene manufactured goods produce electrostatic and easily cause blast accident during production, accumulating, use, and do not carry out in document antistatic It is modified, in addition due to glass fibre and polyvinyl chloride poor compatibility, the shock resistance of obtained polyvinyl chloride composite materials in document Property, shear strength, tensile strength etc. cannot meet the technical indicator of coal mine pipes for mining requirement, and wear-resisting, antibacterial, anti-corrosive properties compared with Difference, disadvantages described above limits popularization and application of the polyvinyl chloride in underground coal mine.To improve disadvantages described above, need to existing production work Skill and formula rate are improved, and have the advantages that tensile strength is high, antistatic, wear-resisting, Antimicrobial preservative is ageing-resistant to prepare The mining effective modified polyvinyl chloride of underground coal mine.
The content of the invention
The object of the invention is exactly to make up the defect of prior art, there is provided a kind of addition nano-calcium carbonate strengthens modified Coal mine special PVC pipe and preparation method thereof.
The present invention is achieved by the following technical solutions:
A kind of addition nano-calcium carbonate strengthens modified coal mine special PVC pipe, is prepared by the raw materials in:PVC trees Fat 100, glass fibre 14.7-15.7, nano-calcium carbonate 3.2-3.6, zinc stearate 1.1-1.4, carbon fiber 6-8, zeolite powder 17- 21st, samarium oxide 3.8-4.3, pitch 2.3-2.6, MTES 5.3-5.7, ethoxyquinoline 1.4-1.7, tall oil Sour 0.9-1.3, appropriate amount of water.
The preparation method that a kind of described addition nano-calcium carbonate strengthens modified coal mine special PVC pipe, including it is following Step:
(1)Nano-calcium carbonate, MTES are scattered in suitable quantity of water and form dispersion liquid, added glass fiber impregnated 10-12 hours, through baking the glass fibre for obtaining nano-calcium carbonate coating after taking-up;
(2)Zeolite powder, samarium oxide are mixed in 840-930 DEG C of roasting 1-2 hour, cooling adds pitch, zinc stearate, tall oil Acid is put into ball milling 2-3 hours in ball mill, dries to obtain modified zeolite powder;
(3)Polyvinyl chloride resin is put in drying box and processes 6-8 hours in 110-115 DEG C, sealing preserve is standby;
(4)By step(3)In material input double screw extruder, step is added(1)、(2)Material and other residual components meltings It is blended and granulates and to obtain stuff and other stuff;
(5)Finally by step(4)Stuff and other stuff is put into injection mo(u)lding in plastic injection molding machine, discharging.
It is an advantage of the invention that:Nano-calcium carbonate Jing MTESs are coupled and are coated on glass fibre by the present invention Surface is added in raw material as reinforcing material, on the one hand improves compatibility of the glass fibre in PVC matrix, the opposing party Face, when during external impacts, the impulsive force that PVC matrix is subject to is transferred to be undertaken on glass fibre and by it, causes glass Glass fibrous fracture absorbs substantial amounts of energy from PVC matrix, so as to reach the purpose of toughness reinforcing;Simultaneously the present invention is also by zeolite powder Oxidized samarium, asphalt modification process are added in raw material as modified filler, improve the toughness and wearability of product, then compatibility Add other pvc pipes obtained in effective auxiliary agent in the well environment of colliery, it is excellent with anticorrosion antiwear, tensile strength height and antibacterial etc. Point.
Specific embodiment
A kind of addition nano-calcium carbonate strengthens modified coal mine special PVC pipe, is prepared by the raw materials in: Polyvinyl chloride resin 100, glass fibre 14.7, nano-calcium carbonate 3.2, zinc stearate 1.1, carbon fiber 6, zeolite powder 17, samarium oxide 3.8, Pitch 2.3, MTES 5.3, ethoxyquinoline 1.4, tall oil acid 0.9, appropriate amount of water.
The preparation method that a kind of described addition nano-calcium carbonate strengthens modified coal mine special PVC pipe, including it is following Step:
(1)Nano-calcium carbonate, MTES are scattered in suitable quantity of water and form dispersion liquid, added glass fiber impregnated 10-12 hours, through baking the glass fibre for obtaining nano-calcium carbonate coating after taking-up;
(2)Zeolite powder, samarium oxide are mixed in 840-930 DEG C of roasting 1-2 hour, cooling adds pitch, zinc stearate, tall oil Acid is put into ball milling 2-3 hours in ball mill, dries to obtain modified zeolite powder;
(3)Polyvinyl chloride resin is put in drying box and processes 6-8 hours in 110-115 DEG C, sealing preserve is standby;
(4)By step(3)In material input double screw extruder, step is added(1)、(2)Material and other residual components meltings It is blended and granulates and to obtain stuff and other stuff;
(5)Finally by step(4)Stuff and other stuff is put into injection mo(u)lding in plastic injection molding machine, discharging.
Using the surface of coal mine special PVC pipe obtained in the present invention is smooth and color normal, combination property is relatively best, Its tensile strength is 79.6 MPa;Shear strength is 59.6 MPa;The pure pvc pipe of bending strength ratio improves 69.9%.

Claims (2)

1. a kind of addition nano-calcium carbonate strengthens modified coal mine special PVC pipe, it is characterised in that by the original of following weight portion Material is made:Polyvinyl chloride resin 100, glass fibre 14.7-15.7, nano-calcium carbonate 3.2-3.6, zinc stearate 1.1-1.4, carbon fiber 6-8, zeolite powder 17-21, samarium oxide 3.8-4.3, pitch 2.3-2.6, MTES 5.3-5.7, ethoxyquinoline 1.4-1.7, tall oil acid 0.9-1.3, appropriate amount of water.
2. a kind of addition nano-calcium carbonate according to claim 1 strengthens the making side of modified coal mine special PVC pipe Method, it is characterised in that comprise the following steps:
(1)Nano-calcium carbonate, MTES are scattered in suitable quantity of water and form dispersion liquid, added glass fiber impregnated 10-12 hours, through baking the glass fibre for obtaining nano-calcium carbonate coating after taking-up;
(2)Zeolite powder, samarium oxide are mixed in 840-930 DEG C of roasting 1-2 hour, cooling adds pitch, zinc stearate, tall oil Acid is put into ball milling 2-3 hours in ball mill, dries to obtain modified zeolite powder;
(3)Polyvinyl chloride resin is put in drying box and processes 6-8 hours in 110-115 DEG C, sealing preserve is standby;
(4)By step(3)In material input double screw extruder, step is added(1)、(2)Material and other residual components meltings It is blended and granulates and to obtain stuff and other stuff;
(5)Finally by step(4)Stuff and other stuff is put into injection mo(u)lding in plastic injection molding machine, discharging.
CN201611165898.3A 2016-12-16 2016-12-16 Nanometer calcium carbonate addition reinforced modified special PVC tube used for coal mine wells, and making method thereof Pending CN106589698A (en)