CN106584293A - Camera glass panel polishing brush and polishing method thereof - Google Patents

Camera glass panel polishing brush and polishing method thereof Download PDF

Info

Publication number
CN106584293A
CN106584293A CN201610883013.7A CN201610883013A CN106584293A CN 106584293 A CN106584293 A CN 106584293A CN 201610883013 A CN201610883013 A CN 201610883013A CN 106584293 A CN106584293 A CN 106584293A
Authority
CN
China
Prior art keywords
cashmere
collodion silk
polishing
face glass
photographic head
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201610883013.7A
Other languages
Chinese (zh)
Other versions
CN106584293B (en
Inventor
韩伟
谢智敏
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Bourne High Tech (huizhou) Co Ltd
Original Assignee
Bourne High Tech (huizhou) Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Bourne High Tech (huizhou) Co Ltd filed Critical Bourne High Tech (huizhou) Co Ltd
Priority to CN201610883013.7A priority Critical patent/CN106584293B/en
Publication of CN106584293A publication Critical patent/CN106584293A/en
Application granted granted Critical
Publication of CN106584293B publication Critical patent/CN106584293B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention relates to the technical field of camera glass panel polishing, in particular to a camera glass panel polishing brush and a polishing method thereof. The polishing brush comprises bristles and a disc-shaped abrasive disk used for fixing the bristles. The bristles comprise cashmere and collodion silk which are each averagely divided into four areas arranged on the abrasive disk at intervals. The cashmere is 3-10 mm shorter than the collodion silk. The diameter of the cashmere is 5-10 times that of the collodion silk. The purpose of the invention is to provide the camera glass panel polishing brush and the polishing method thereof. With the adoption of the technical scheme, the excellence rate of camera glass panels can be increased, the defective products of camera glass panels are reduced, and machining cost is reduced.

Description

A kind of photographic head face glass polishing hairbrush and its finishing method
Technical field
The present invention relates to photographic head face glass polishing technology field, more particularly to a kind of photographic head face glass polishing hair Brush and its finishing method.
Background technology
The photographic effect of photographic head depends not only on camera internal reference number, additionally depends on the face glass at photographic head position Optical flat effect.If the face glass polishing at photographic head position has out-of-flatness, face glass optical flat effect is poor, and photographic effect can be deposited In rainbow phenomena.
The polishing hairbrush that prior art is adopted adopts the cashmere brush of a diameter of 3.0mm made by cashmere, and pure cashmere brush can be right Glass surface plate face type effect causes to be damaged, and is only 30%-40% using the face glass yield of the hairbrush polishing.
The content of the invention
The goal of the invention of the present invention is to provide a kind of photographic head face glass polishing hairbrush and its finishing method, using this The technical scheme that invention is provided can improve photographic head face glass acceptance rate, reduce face glass defective products, reduce being processed into This.
In order to solve above-mentioned technical problem, one aspect of the present invention provides a kind of photographic head face glass and polishes hairbrush, including Bristle and the discoid mill for fixing the bristle;The bristle includes cashmere and collodion silk;The cashmere and collodion silk are put down It is divided into four regions to be disposed on the mill;The length of the cashmere 3~10mm shorter than the length of the collodion silk;Institute State a diameter of described collodion silk of cashmere 5~10 times of diameter.
Preferably, the length of the cashmere is 30mm;The length of the collodion silk is 35mm.
Preferably, a diameter of 1.5mm of the cashmere;A diameter of 0.3mm of the collodion silk.
Preferably, the cashmere and the area ratio of collodion silk are 3:2.
Preferably, the collodion silk is Pilus Sus domestica.
Preferably, the liquid outlet of sprinkling polishing fluid is provided with four regions that the cashmere and collodion silk are divided into.
Another aspect of the present invention also provides a kind of photographic head face glass finishing method, and the method adopts above-mentioned photographic head glass Glass panel polishes hairbrush, comprises the following steps:
1), photographic head face glass is fixed on polishing clamp;
2), polishing clamp is placed on polishing machine base;
3) buffing machine, mill sprinkling polishing fluid, are opened, and is pressed on polishing clamp, make end and the collodion silk of cashmere End is parallel, and contacts with photographic head face glass;
4), mill rotational time is 30min, and rotating speed is 35 turns/min;
5), stop buffing machine, complete polishing process.
Therefore, using the technical scheme of the embodiment of the present invention, have the advantages that:The hairbrush that the present invention is adopted is adopted The structure mixed with cashmere and collodion silk, the cashmere that diameter is big and length is short is used to be polished face glass, and diameter is little and long The long collodion silk of degree is used to repair the face glass after polishing, and cashmere and collodion silk replace contact and grind with face glass respectively Mill, repeats polishing and repair action so that face glass completes polishing process, and the hairbrush provided using the present invention improves glass The optical flat effect of panel, yield can reach 99%, substantially increase the optical flat processing yield of face glass, considerably reduces and adds Work cost.
Description of the drawings
In order to be illustrated more clearly that the embodiment of the present invention or technical scheme of the prior art, below will be to present invention enforcement Example or the accompanying drawing to be used needed for description of the prior art are briefly described.It should be evident that drawings in the following description are only Only it is a part of embodiment of the present invention, for those of ordinary skill in the art, in the premise for not paying creative work Under, can be with according to these other accompanying drawings of accompanying drawings acquisition.
Fig. 1 is that the embodiment of the present invention polishes hair brush structure schematic diagram;
Fig. 2 is embodiment of the present invention finishing method FB(flow block).
Specific embodiment
Describe the polishing hairbrush of the face glass of embodiment of the present invention in detail below with reference to the accompanying drawings.Additionally, in accompanying drawing Explanation in, to essentially identical configuration or parts mark identical label, it is appropriate sometimes omit that a part repeats say Bright and part known in those skilled in the art or structure.Although in addition, retouching to the present invention with reference to specific embodiment State, it will be appreciated that, the description is not intended as limiting the invention to described embodiment.Conversely, the description is intended to cover Cover replacement, improvement and the equivalent that may include in the spirit and scope of the present invention being defined by the appended claims.This Field it is to be understood by the skilled artisans that realize that the present invention is not required for all these part, and can be without departing from this Any change is made to the type and arrangement of these parts under bright spirit and scope.
As shown in figure 1, the invention discloses a kind of photographic head face glass polishing hairbrush, including bristle and for fixing State the discoid mill 10 of bristle.Bristle includes cashmere 21 and collodion silk 22, and the cashmere 21 and collodion silk 22 are divided into four Region is disposed on the mill 10.Length 3~the 10mm shorter than the length of the collodion silk 22 of wherein described cashmere 21, institute State a diameter of described collodion silk 22 of cashmere 21 5~10 times of diameter.Four be divided in the cashmere 21 and collodion silk 22 The liquid outlet 23 of sprinkling polishing fluid is provided with region.
With reference to above-mentioned polishing hairbrush, as shown in Fig. 2 the present invention also provides a kind of photographic head face glass finishing method, bag Include following steps:
1), photographic head face glass is fixed on polishing clamp, and is placed on polishing machine base;
2) buffing machine, mill sprinkling polishing fluid, are opened, and is pressed on polishing clamp;Because collodion silk length is more than cashmere Length so that mill is depressed into the dynamics hinge structure of face glass and substantially increases, after pushing, for repair glue The end bending of silk, the end of collodion silk is parallel with the end of cashmere, and contacts with photographic head face glass;
3), mill rotational time is 30min, and rotating speed is 35 turns/min;Mill rotational time extends relative to prior art 20%, rotating cycle reaches 1000 turns, and mill rotation is turned around, and face glass completes four polishings and repair action, rotation 1000 turns then complete 4000 polishings and repair action, coordinate with said brush, improve face glass acceptance rate;
4), stop buffing machine, complete polishing process;
5) face glass after polishing, is removed, outward appearance and optical flat detection is carried out.
In steps of 5
Outward appearance detection refers to that the outer surface of range estimation face glass, with the presence or absence of scratch or crackle, if any being then defective products, is needed Again polishing or calcellation is processed.
Optical flat refers to the right cylindrical with two (or one) optical measurement planes or rectangular gauge, refers specifically to glass Glass surface roughness value and flatness.The all minimum glass planar of surface roughness value and flatness error, can produce Interference fringe, optical flat detection is the detection method that glass planar degree error is measured using optical interference phenomenon, is also called flat Brilliant interferometric method.When optical flat is detected, optical flat is placed on measured surface, and the wedge angle of a very little is formed with measured surface, with list Color light source can produce interference fringe when irradiating.The position of interference fringe is relevant with the angle of incidence of light.As incident ray perpendicular to Gap very little between measured surface, and optical flat and measured surface, the then light for being reflected by optical flat measuring surface P reflects with measured surface Light interfere in measuring surface P and bright or dark interference fringe occur.If under white light, there is Color Interfering Fringes By Use. As interference fringe is straight, it is parallel to each other, and is evenly distributed, then it represents that the flatness of measured surface is fine;As interference fringe bends, Then represent that flatness is bad.Its error amount is f=(v/ ω) × (λ/2), and λ is optical wavelength, and the mean wavelength of white light is 0.58 μ M, ν are interference fringe amount of bow, and ω is interorder distance.The flatness error of optical measurement plane is:1 class precision for 0.03~ 0.05 micron;2 class precisions for 0.1 micron.Present invention polishing hairbrush is used for the polishing of the face glass of photographic head, in step Optical flat accuracy of detection in rapid 5 is 2 class precisions.
Three kinds mixed with cashmere with reference to collodion silk, cashmere and collodion silk polish hairbrush and are polished processing, using throwing Light method is the finishing method of above-mentioned photographic head face glass;Inspection is sampled simultaneously, and the unit product of sampling inspection is throwing The face glass that light is machined, sample size is 100, and quantity of sampling quantity is 50, and the quality testing of unit product is outward appearance detection With optical flat detection, wherein optical flat detection method is above-mentioned optical flat interferometric method:
Embodiment 1
Experiment hairbrush be collodion silk hairbrush, a diameter of 0.3mm of collodion silk, length is 35mm, and mill pushes pressure in finishing method Power is 280kg, and rotating speed is 30rpm, and rotational time is 35min, and outward appearance yield and optical flat detection yield experimental data are as follows:
Experiment sequence number Quantity of sampling quantity The qualified quantity of outward appearance Outward appearance yield The qualified quantity of optical flat Optical flat yield
1 50 1 2% 0 0%
2 50 0 0% 0 0%
3 50 1 2% 1 2%
Embodiment 2
Experiment hairbrush be cashmere hairbrush, a diameter of 3mm of cashmere, length is 30mm, the down force pressure of mill in finishing method For 280kg, rotating speed is 30rpm, and rotational time is 35min, and outward appearance yield and optical flat detection yield experimental data are as follows:
Experiment sequence number Quantity of sampling quantity The qualified quantity of outward appearance Outward appearance yield The qualified quantity of optical flat Optical flat yield
1 50 34 68% 16 32%
2 50 32 64% 18 36%
3 50 33 66% 17 34%
Embodiment 3
Experiment hairbrush is cashmere and collodion silk mixing hairbrush, a diameter of 3mm of cashmere, and length is 30mm, and collodion silk is a diameter of 0.3mm, length is 35mm, and the down force pressure of mill is 280kg in finishing method, and rotating speed is 30rpm, and rotational time is 35min, Outward appearance yield and optical flat detection yield experimental data are as follows:
Experiment sequence number Quantity of sampling quantity The qualified quantity of outward appearance Outward appearance yield The qualified quantity of optical flat Optical flat yield
1 50 42 84% 35 70%
2 50 44 88% 34 68%
3 50 43 86% 36 72%
Embodiment 4
Experiment hairbrush is cashmere and collodion silk mixing hairbrush, a diameter of 1.5mm of cashmere, and length is 30mm, and collodion silk is a diameter of 0.3mm, length is 30mm, and the down force pressure of mill is 280kg in finishing method, and rotating speed is 30rpm, and rotational time is 35min, Outward appearance yield and optical flat detection yield experimental data are as follows:
Experiment sequence number Quantity of sampling quantity The qualified quantity of outward appearance Outward appearance yield The qualified quantity of optical flat Optical flat yield
1 50 45 90% 37 74%
2 50 46 92% 39 78%
3 50 43 86% 36 72%
Embodiment 5
Experiment hairbrush is cashmere and collodion silk mixing hairbrush, a diameter of 1.5mm of cashmere, and length is 30mm, and collodion silk is a diameter of 0.3mm, length is 35mm, and the down force pressure of mill is 280kg in finishing method, and rotating speed is 30rpm, and rotational time is 35min, Outward appearance yield and optical flat detection yield experimental data are as follows:
Experiment sequence number Quantity of sampling quantity The qualified quantity of outward appearance Outward appearance yield The qualified quantity of optical flat Optical flat yield
1 50 46 92% 50 100%
2 50 45 90% 49 98%
3 50 47 94% 50 100%
Knowable to above-mentioned experimental data, in embodiment 1 and embodiment 2 mono-material hair commonly used in the prior art is used Brush.Wherein the outward appearance yield of collodion silk hairbrush and optical flat yield close 0%, it is impossible to complete the polishing to face glass;Cashmere hair The outward appearance yield and optical flat yield of brush is printed with lifting relative to collodion silk, but optical flat yield is only 35% or so, still can be produced More defective products.The outward appearance yield and optical flat yield of the hairbrush of above two mono-material is unable to reach process requirements, only makees For matched group.
Embodiment 3-5 uses cashmere and collodion silk mixing hairbrush, and outward appearance yield and optical flat yield are equal relative to matched group Have and significantly lifted.The hairbrush mixed using cashmere and collodion silk, the cashmere that diameter is big and length is short is used to enter face glass Row polishing, diameter is little and collodion silk of length length is used to repair the face glass after polishing, cashmere and collodion silk respectively with glass The alternately contact grinding of glass panel, repeats polishing and repair action so that face glass completes polishing process.Wherein in embodiment 5 Outward appearance yield reaches more than 90%, and optical flat yield close 100% mixes hairbrush as preferred, and the length of cashmere is 30mm, directly Footpath is 1.5mm;The length of collodion silk is 35mm, a diameter of 0.3mm.
In addition when cashmere is 1 with the area ratio of collodion silk:When 1, face glass acceptance rate reaches 85%~90%;Work as cashmere It is 3 with the area ratio of collodion silk:When 2, face glass acceptance rate mixes hairbrush, cashmere and collodion silk up to 99% as preferred Area ratio be 3:2.
By above-described embodiment, during the hairbrush being combined into using above-mentioned cashmere and collodion silk, through experiment employing is drawn The cashmere of above-mentioned preferred length, diameter and ratio and the hairbrush of collodion silk combination improve the outward appearance and optical flat effect of face glass Really, the acceptance rate of face glass is greatly improved.
Embodiments described above, does not constitute the restriction to the technical scheme protection domain.It is any in above-mentioned enforcement Modification, equivalent and improvement made within the spirit and principle of mode etc., should be included in the protection model of the technical scheme Within enclosing.

Claims (7)

1. a kind of photographic head face glass polishes hairbrush, it is characterised in that:
Discoid mill including bristle and for fixing the bristle;
The bristle includes cashmere and collodion silk;
The cashmere and collodion silk are divided into four regions and are disposed on the mill;
The length of the cashmere 3~10mm shorter than the length of the collodion silk;
5~10 times of the diameter of a diameter of described collodion silk of the cashmere.
2. a kind of photographic head face glass according to claim 1 polishes hairbrush, it is characterised in that:
The length of the cashmere is 30mm;
The length of the collodion silk is 35mm.
3. a kind of photographic head face glass according to claim 2 polishes hairbrush, it is characterised in that:
A diameter of 1.5mm of the cashmere;
A diameter of 0.3mm of the collodion silk.
4. a kind of photographic head face glass according to claim 1 polishes hairbrush, it is characterised in that:
The cashmere is 3 with the area ratio of collodion silk:2.
5. a kind of photographic head face glass according to claim 1 polishes hairbrush, it is characterised in that:
The collodion silk is Pilus Sus domestica.
6. a kind of photographic head face glass according to claim 1 polishes hairbrush, it is characterised in that:
The liquid outlet of sprinkling polishing fluid is provided with four regions that the cashmere and collodion silk are divided into.
7. the finishing method of hairbrush is polished using the photographic head face glass described in any one of claim 1-6, it is characterised in that Comprise the following steps:
1), photographic head face glass is fixed on polishing clamp;
2), polishing clamp is placed on polishing machine base;
3) buffing machine, mill sprinkling polishing fluid, are opened, and is pressed on polishing clamp, make the end of cashmere and the end of collodion silk It is parallel, and contact with photographic head face glass;
4), mill rotational time is 30min, and rotating speed is 35 turns/min;
5), stop buffing machine, complete polishing process.
CN201610883013.7A 2016-10-08 2016-10-08 A kind of camera glass panel polishing hairbrush and its polishing method Active CN106584293B (en)