CN106497218A - A kind of manufacture method of Environmental-protection water-based ink - Google Patents

A kind of manufacture method of Environmental-protection water-based ink Download PDF

Info

Publication number
CN106497218A
CN106497218A CN201510594609.0A CN201510594609A CN106497218A CN 106497218 A CN106497218 A CN 106497218A CN 201510594609 A CN201510594609 A CN 201510594609A CN 106497218 A CN106497218 A CN 106497218A
Authority
CN
China
Prior art keywords
water
color
agent
environmental
resin
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201510594609.0A
Other languages
Chinese (zh)
Inventor
周军辉
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Tysan Packaging Co Ltd
Original Assignee
Tysan Packaging Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Tysan Packaging Co Ltd filed Critical Tysan Packaging Co Ltd
Priority to CN201510594609.0A priority Critical patent/CN106497218A/en
Publication of CN106497218A publication Critical patent/CN106497218A/en
Pending legal-status Critical Current

Abstract

The present invention provides a kind of manufacture method of Environmental-protection water-based ink, and Environmental-protection water-based ink component includes:Quick-drying color resin 20 one 30%, into touching wear-resisting waterproof resin 15-20%, emulsifying resins 10-15%, mill base 25-30%, water 8-15%, auxiliary agent 2-5%;Mixed, and stirred, placement 2-3 minutes are formed paste mixture;The viscosity of test paste mixture;Examination color is carried out according to color sample, examination color is carried out on corrugated paper by color development wheel;Obtain final product water color ink.Good effect:Water color ink is nontoxic, do not contain organic solvent so that the noxious substance of leaflet such as packing box remained on surface greatly reduces, while add defoamer or foam inhibitor in the water color ink, to solve water color ink foaming phenomena;Add the rate of drying that dry agent can adjust water color ink, while printer rotation speed requirements, improve production efficiency is reached anti-wear agent is added.

Description

A kind of manufacture method of Environmental-protection water-based ink
Technical field
A kind of the invention belongs to technical field of ink, more particularly to manufacture method of Environmental-protection water-based ink.
Background technology
Water color ink is by the uniform slurry like material of the material compositions such as link stuff, pigment, auxiliary agent.Link stuff provides ink Necessary transfer performance, pigment give ink with color.The link stuff of water color ink is broadly divided into two types:Water is dilute Release type and water-dispersion type, the resinous type that the former can use has many kinds, such as malein acid ester resin, lac, Maleic acid resin Modified Shell-lac for Cuprous Surface Anticorrosion, urethane, water soluble acrylic resin and water-compatible amino resin etc..The company of water-dispersion type Ramming material is polymerized gained by the monomer of emulsifying in water, and it is two-phase system, wherein oil phase with graininess in water phase Dispersion, though can not be dissolved in water, can be diluted with water, so it is also assumed that being oil-in-water emulsion type.
Pigment imparts ink colors feature, meets requirement of the printing to color, general organic pigment and inorganic face Material can be used in water color ink.As the resin of water color ink is mostly alkali-soluble, so when selecting pigment, must make Pigment with energy alkali resistance.But, in ink, the distribution density of pigment is much greater compared with solvent type ink, and the table of water Face tension force and polarity are all big with solvent difference so that pigment dispersion is more difficult, directly influence ink stability, Viscosity and pH value, the viscosity of ink and pH value need precise control, and when pH value is higher than 9.5, alkalescence is too strong, The viscosity of ink can reduce, and rate of drying is slack-off, water resistance is deteriorated;When pH value is less than 8, alkalescence is again too weak, The viscosity of ink is raised, and rate of drying is accelerated, and can cause the defects such as dirty version, scumming, foaming.Select in printing process When using pigment, should select that the gorgeous bright, viscosity of color and luster in pigment is low, stable system senior pigment to be making water color ink.
Traditional water color ink makes, and is not added with auxiliary agent or adds that auxiliary agent is not comprehensive, affect resin and water affinity and Mill base and the affinity of resin, so as to the stability of water color ink is also poor, and meanwhile also more complicated in processing technology, Added value is low.
Content of the invention
Present invention aim at for the defect of prior art, there is provided for the deficiencies in the prior art, the invention provides A kind of manufacture method of Environmental-protection water-based ink, its objective is the component and step by Environmental-protection water-based ink, realizes resin With the affinity of the affinity and mill base of water and resin, so as to improve the stability of water color ink.
The present invention is achieved by the following technical solutions, have developed a kind of manufacture method of Environmental-protection water-based ink, and which is special Levy and be, comprise the following steps:
(1) Environmental-protection water-based ink component includes:Quick-drying color resin 20-30%, into touching wear-resisting waterproof resin 15- 20%, emulsifying resins 10-15%, mill base 25-30%, water 8-15%, auxiliary agent 2-5%;
(2) by quick-drying color resin, mixed into touching wear-resisting waterproof resin, emulsifying resins, mill base and water, And stir, placement 2-3 minutes form paste mixture;
(3) auxiliary agent will be added in the paste mixture described in step 2 again, is stirred after adding auxiliary agent;
(4) viscosity of paste mixture is tested;
(5) examination color is carried out according to color sample, examination color is carried out on corrugated paper by color development wheel;
(6) water color ink is obtained final product, and sealing is simultaneously labelled.
Auxiliary agent in the step 1 is defoamer, anti-wear agent, quick dry agent, levelling agent, and wherein defoamer is 0.5- 0.8%th, anti-wear agent be 0.1-0.4%, quick dry agent be 0.2-1%, levelling agent be 1.1-2.0%.
Quick-drying color resin in the step 2, mixed into touching wear-resisting waterproof resin, emulsifying resins, mill base and water Stirring is closed, the speed of stirring is 500-700 rev/min, and mixing time is 2-3 minutes;Add in the step 3 The speed stirred after auxiliary agent is 600-700 rev/min, and mixing time is 3-5 minutes.
Water in the step 1 is pure water.
The good effect of invention is:Water color ink of the invention uses water as dissolving carrier, aqueouss oil compared with prior art Ink have significant Environmental Safety feature, nontoxic, do not fire not quick-fried, during for printing hardly in air dissipate Volatile organic gas (VOC) are sent out, while water color ink does not contain organic solvent so that leaflet such as packing box remained on surface Noxious substance greatly reduce, such as require in sanitary conditions such as cigarette, wine, food, beverage, medicine, toys for children tight Packing box in the Packaging Printing Product of lattice more embodies good healthy and safe property.
Add water and excessively all can with printing technology personnel when stirring in the manufacture method step 2 of Environmental-protection water-based ink and step 3 There is air bubble problem, the phenomenons such as leaflet shows money or valuables one carries unintentionally, inking amount is few occur when bubble is larger, has a strong impact on printing quality, At this moment add defoamer or foam inhibitor in water color ink, be used in mixed way for two kinds using one kind sometimes according to bubble situation sometimes, To solve water color ink foaming phenomena.
Water color ink is too fast due to the different or machine rotational speed from resin producer in use, is likely to result in water Property ink setting speed slower, adding quick dry agent can adjust the rate of drying of water color ink, while reaching anti-wear agent is added Arrive printer rotation speed requirements, improve production efficiency.
Specific embodiment
Embodiment 1
First prepare Environmental-protection water-based ink component, quick-drying color resin 20%, into touching wear-resisting waterproof resin 20%, emulsifying tree Fat 15%, mill base 27%, water 15%;By quick-drying color resin, into touching wear-resisting waterproof resin, emulsifying resins, mill base Mixed with water, and stirred, the speed of stirring is 500 revs/min, and mixing time is 3 minutes, Place and form within 2 minutes paste mixture, then defoamer will be added in described paste mixture again for 0.8%, anti-wear agent It is that 0.9%, levelling agent is 1.1% for 0.2%, quick dry agent, stirs after adding auxiliary agent, the speed of stirring is 600 Rev/min, mixing time is 5 minutes, and the viscosity for testing paste mixture by flow cup is entered according to color sample Row examination color, carries out examination color on corrugated paper by color development wheel, obtains final product the stability of water color ink more than 80%, during printing Layer of ink wearability is more than 85%.
Make large red water color ink
Quick-drying color resin 20%, into touching wear-resisting waterproof resin 20%, emulsifying resins 15%, large red mill base 21.7%, Crocus mill base 5%, blue mill base 0.3%, water 15%;By quick-drying color resin, into touching wear-resisting waterproof resin, breast Change resin, mill base and water to be mixed, and stir, the speed of stirring is 500 revs/min, during stirring Between for 3 minutes, place 2 minutes and form paste mixture, then by defoamer is added in described paste mixture be again 0.8%th, anti-wear agent be 0.2%, quick dry agent be 0.9%, levelling agent be 1.1%, add auxiliary agent after stir, stir The speed that mixes is 600 revs/min, and mixing time is 5 minutes, the viscosity for testing paste mixture by flow cup, Color according to large red carries out examination color, carries out trying color into large red by color development wheel, obtain final product large red on corrugated paper Water color ink.
Embodiment 2
First prepare Environmental-protection water-based ink component, quick-drying color resin 25%, into touching wear-resisting waterproof resin 15%, emulsifying tree Fat 13%, mill base 30%, water 13%;By quick-drying color resin, into touching wear-resisting waterproof resin, emulsifying resins, mill base Mixed with water, and stirred, the speed of stirring is 600 revs/min, and mixing time is 2 minutes, Place and form within 3 minutes paste mixture, then defoamer will be added in described paste mixture again for 0.6%, anti-wear agent It is that 1.0%, levelling agent is 2.0% for 0.4%, quick dry agent, stirs after adding auxiliary agent, the speed of stirring is 650 Rev/min, mixing time is 3 minutes, and the viscosity for testing paste mixture by flow cup is entered according to color sample Row examination color, carries out examination color on corrugated paper by color development wheel, obtains final product the stability of water color ink more than 85%, during printing Layer of ink wearability is more than 88%.
Make bottle green water color ink
Quick-drying color resin 25%, into touching wear-resisting waterproof resin 15%, emulsifying resins 13%, blue mill base 15%, Green mill base 10%, middle yellow mill base 5%, water 13%;By quick-drying color resin, into touching wear-resisting waterproof resin, breast Change resin, mill base and water to be mixed, and stir, the speed of stirring is 600 revs/min, during stirring Between for 2 minutes, place 3 minutes and form paste mixture, then by defoamer is added in described paste mixture be again 0.6%th, anti-wear agent be 0.4%, quick dry agent be 1.0%, levelling agent be 2.0%, add auxiliary agent after stir, stir The speed that mixes is 650 revs/min, and mixing time is 3 minutes, the viscosity for testing paste mixture by flow cup, Examination color is carried out according to bottle-green color, color is tried on corrugated paper into bottle green by color development wheel, bottle green aqueouss are obtained final product Ink.
Embodiment 3
First prepare Environmental-protection water-based ink component, quick-drying color resin 30%, into touching wear-resisting waterproof resin 18%, emulsifying tree Fat 10%, mill base 25%, water 14%;By quick-drying color resin, into touching wear-resisting waterproof resin, emulsifying resins, mill base Mixed with water, and stirred, the speed of stirring is 700 revs/min, and mixing time is 3 minutes, Place and form within 3 minutes paste mixture, then defoamer will be added in described paste mixture again for 0.5%, anti-wear agent It is that 0.5%, levelling agent is 1.9% for 0.1%, quick dry agent, stirs after adding auxiliary agent, the speed of stirring is 700 Rev/min, mixing time is 4 minutes, and the viscosity for testing paste mixture by flow cup is entered according to color sample Row examination color, carries out examination color on corrugated paper by color development wheel, obtains final product the stability of water color ink more than 90%, during printing Layer of ink wearability is more than 90%.
Make sky blue water color ink
Quick-drying color resin 30%, into touching wear-resisting waterproof resin 18%, emulsifying resins 10%, sky blue mill base 9%, White colorant 15%, middle yellow mill base 1%, water 14%;By quick-drying color resin, into touching wear-resisting waterproof resin, breast Change resin, mill base and water to be mixed, and stir, the speed of stirring is 700 revs/min, during stirring Between for 3 minutes, place 3 minutes and form paste mixture, then by defoamer is added in described paste mixture be again 0.5%th, anti-wear agent be 0.1%, quick dry agent be 0.5%, levelling agent be 1.9%, add auxiliary agent after stir, stir The speed that mixes is 700 revs/min, and mixing time is 4 minutes, the viscosity for testing paste mixture by flow cup, Examination color is carried out according to sapphire color, color is tried on corrugated paper into sky blue by color development wheel, sky blue aqueouss are obtained final product Ink.
In actual applications, those skilled in the art completely can in technical scheme, reasonable selection its His parameter, but identical with the technical scheme substance protected by the present invention, still fall within protection scope of the present invention.

Claims (4)

1. a kind of manufacture method of Environmental-protection water-based ink, it is characterised in that comprise the following steps:
(1) Environmental-protection water-based ink component includes:Quick-drying color resin 20-30%, into touching wear-resisting waterproof resin 15-20%, emulsifying resins 10-15%, mill base 25-30%, water 8-15%, auxiliary agent 2-5%;
(2) by quick-drying color resin, mixed into touching wear-resisting waterproof resin, emulsifying resins, mill base and water Stirring, and stir, placement 2-3 minutes form paste mixture;
(3) auxiliary agent will be added again in the paste mixture described in step (2), is stirred after adding auxiliary agent;
(4) viscosity of paste mixture is tested;
(5) examination color is carried out according to color sample, examination color is carried out on corrugated paper by color development wheel;
(6) water color ink is obtained final product, and sealing is simultaneously labelled.
2. the manufacture method of a kind of Environmental-protection water-based ink according to claim 1, it is characterised in that:Institute It is defoamer, anti-wear agent, quick dry agent, levelling agent to state the auxiliary agent in step (1), and wherein defoamer is 0.5 - 0.8%, anti-wear agent be 0.1-0.4%, quick dry agent be 0.2-1%, levelling agent be 1.1-2.0%.
3. the manufacture method of a kind of Environmental-protection water-based ink according to claim 1, it is characterised in that:Institute State the quick-drying color resin in step (2), carry out into touching wear-resisting waterproof resin, emulsifying resins, mill base and water Mix, the speed of stirring is 500-700 rev/min, and mixing time is 2-3 minutes;The step (3) speed stirred after adding auxiliary agent in is 600-700 rev/min, and mixing time is 3-5 minutes.
4. the manufacture method of a kind of Environmental-protection water-based ink according to claim 1, it is characterised in that:Institute It is pure water to state the water in step (1).
CN201510594609.0A 2015-09-08 2015-09-08 A kind of manufacture method of Environmental-protection water-based ink Pending CN106497218A (en)