CN106381674A - Desizing processing method for super-fine denier nylon fabric - Google Patents
Desizing processing method for super-fine denier nylon fabric Download PDFInfo
- Publication number
- CN106381674A CN106381674A CN201610785164.9A CN201610785164A CN106381674A CN 106381674 A CN106381674 A CN 106381674A CN 201610785164 A CN201610785164 A CN 201610785164A CN 106381674 A CN106381674 A CN 106381674A
- Authority
- CN
- China
- Prior art keywords
- weight portion
- weight
- parts
- desizing
- fabric
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses a desizing processing method for a super-fine denier nylon fabric, wherein the method comprises the following steps: 1) successively adding 1 to 2 parts by weight of sucrose fatty acid ester, 1.2 parts by weight of methyl cellulose, 1.5 parts by weight of iso-fatty alcohol polyoxyethylene ether, 0.8 part by weight of potassium tetraborate and 21 parts by weight of amylase into 65 parts by weight of deionized water, and stirring evenly; 2) then successively adding 1.2 parts by weight of a binuclear manganese complex, 0.9 part by weight of zinc chloride, 1.3 parts by weight of stearic acid polyoxyethylene ester, and 0.4 part by weight of alkyl dimethyl aryl ammonium chloride, and continuing to stir to fully and evenly mix, to prepare a desizing liquid; and 3) carrying out padding treatment of the fabric in the desizing slurry, taking out the fabric, washing with water, and air-drying. The desizing processing method for the super-fine denier nylon fabric has high desizing rate; the fabric after desizing treatment has relatively high capillary effect and mechanical properties.
Description
Technical field
The present invention relates to the desizing processing method of superfine denier nylon.
Background technology
The warp thread of the fabrics such as cotton, viscose glue and synthetic fibers, mostly first passes through sizing before weaving.Slurry is in dyeing and finishing process
The middle wettability that can affect fabric, and hinder chemicals to fiber contacts, therefore fabric dye previous as all carry out at desizing
Reason.
Content of the invention
It is an object of the invention to provide a kind of desizing processing method of superfine denier nylon, its desizing rate height, desizing
Fabric after process has higher capillary effect and mechanical property, is conducive to the carrying out of follow-up dyeing and printing process it is ensured that follow-up print and dye
Quality;And the effective removal because of slurry, improves the feel of fabric.
For achieving the above object, the technical scheme is that the desizing process side designing a kind of superfine denier nylon
Method, comprises the steps:
1) by 1~2 parts by weight of sucrose fatty acid ester, 1.2 weight portion methylcellulose, 1.5 weight portion isomery poly alkyl alcohols
Oxygen vinyl Ether, 0.8 weight portion dipotassium tetraborate, 21 weight starch enzymes put in 65 parts by weight of deionized water successively, stir;
2) 1.2 weight portion double-core manganese complexes, 0.9 weight portion zinc chloride, 1.3 weight portion stearic acid polyoxies are put into again successively
Vinyl acetate, 0.4 weight portion alkyl dimethyl aryl ammonium chloride, continue stirring, uniform to being sufficiently mixed, prepared desizing liquid;
3) fabric is padded process in desizing liquid, wash after taking-up and dry.
Preferably, the desizing processing method of superfine denier nylon, comprises the steps:
1) by 1 parts by weight of sucrose fatty acid ester, 1.2 weight portion methylcellulose, 1.5 weight portion isomery fatty alcohol polyoxy second
Alkene ether, 0.8 weight portion dipotassium tetraborate, 21 weight starch enzymes put in 65 parts by weight of deionized water successively, stir;
2) 1.2 weight portion double-core manganese complexes, 0.9 weight portion zinc chloride, 1.3 weight portion stearic acid polyoxies are put into again successively
Vinyl acetate, 0.4 weight portion alkyl dimethyl aryl ammonium chloride, continue stirring, uniform to being sufficiently mixed, prepared desizing liquid;
3) fabric is padded process in desizing liquid, wash after taking-up and dry.
Preferably, the desizing processing method of superfine denier nylon, comprises the steps:
1) by 2 parts by weight of sucrose fatty acid esters, 1.2 weight portion methylcellulose, 1.5 weight portion isomery fatty alcohol polyoxy second
Alkene ether, 0.8 weight portion dipotassium tetraborate, 21 weight starch enzymes put in 65 parts by weight of deionized water successively, stir;
2) 1.2 weight portion double-core manganese complexes, 0.9 weight portion zinc chloride, 1.3 weight portion stearic acid polyoxies are put into again successively
Vinyl acetate, 0.4 weight portion alkyl dimethyl aryl ammonium chloride, continue stirring, uniform to being sufficiently mixed, prepared desizing liquid;
3) fabric is padded process in desizing liquid, wash after taking-up and dry.
Preferably, the desizing processing method of superfine denier nylon, comprises the steps:
1) by 1.2 parts by weight of sucrose fatty acid esters, 1.2 weight portion methylcellulose, 1.5 weight portion isomery fatty alcohol polyoxies
Vinyl Ether, 0.8 weight portion dipotassium tetraborate, 21 weight starch enzymes put in 65 parts by weight of deionized water successively, stir;
2) 1.2 weight portion double-core manganese complexes, 0.9 weight portion zinc chloride, 1.3 weight portion stearic acid polyoxies are put into again successively
Vinyl acetate, 0.4 weight portion alkyl dimethyl aryl ammonium chloride, continue stirring, uniform to being sufficiently mixed, prepared desizing liquid;
3) fabric is padded process in desizing liquid, wash after taking-up and dry.
Advantages of the present invention and having the beneficial effects that:There is provided a kind of desizing processing method of superfine denier nylon, it moves back
Slurry rate is high, and the fabric after desizing is processed has higher capillary effect and mechanical property, be conducive to the carrying out of follow-up dyeing and printing process it is ensured that
Follow-up printing quality;And the effective removal because of slurry, improves the feel of fabric.
The performance of " desizing liquid " and purposes are determined by its component and proportioning, and the different component meeting in " desizing liquid "
Influence each other, component and its proportioning can determine the final performance of " desizing liquid ", such as fruit component and its proportioning be not mutually coordinated, single
The beneficial effect that component is brought, even can be eliminated by other components abatement, when serious, different component is mutually conflicted, and rises
Less than whole synthesis effect, produce negative interaction and substandard products.The present invention passes through a large amount of creative works, repeatedly verifies, obtains " desizing
The optimal component of liquid " and proportioning so that multiple component combine, mutually coordinated and produce positive comprehensive effect.
Specific embodiment
With reference to embodiment, the specific embodiment of the present invention is further described.Following examples are only used for more
Plus clearly demonstrate technical scheme, and can not be limited the scope of the invention with this.
The technical scheme that the present invention is embodied as is:
Embodiment 1
The desizing processing method of superfine denier nylon, comprises the steps:
1) by 1~2 parts by weight of sucrose fatty acid ester, 1.2 weight portion methylcellulose, 1.5 weight portion isomery poly alkyl alcohols
Oxygen vinyl Ether, 0.8 weight portion dipotassium tetraborate, 21 weight starch enzymes put in 65 parts by weight of deionized water successively, stir;
2) 1.2 weight portion double-core manganese complexes, 0.9 weight portion zinc chloride, 1.3 weight portion stearic acid polyoxies are put into again successively
Vinyl acetate, 0.4 weight portion alkyl dimethyl aryl ammonium chloride, continue stirring, uniform to being sufficiently mixed, prepared desizing liquid;
3) fabric is padded process in desizing liquid, wash after taking-up and dry.
Embodiment 2
The desizing processing method of superfine denier nylon, comprises the steps:
1) by 1 parts by weight of sucrose fatty acid ester, 1.2 weight portion methylcellulose, 1.5 weight portion isomery fatty alcohol polyoxy second
Alkene ether, 0.8 weight portion dipotassium tetraborate, 21 weight starch enzymes put in 65 parts by weight of deionized water successively, stir;
2) 1.2 weight portion double-core manganese complexes, 0.9 weight portion zinc chloride, 1.3 weight portion stearic acid polyoxies are put into again successively
Vinyl acetate, 0.4 weight portion alkyl dimethyl aryl ammonium chloride, continue stirring, uniform to being sufficiently mixed, prepared desizing liquid;
3) fabric is padded process in desizing liquid, wash after taking-up and dry.
Embodiment 3
The desizing processing method of superfine denier nylon, comprises the steps:
1) by 2 parts by weight of sucrose fatty acid esters, 1.2 weight portion methylcellulose, 1.5 weight portion isomery fatty alcohol polyoxy second
Alkene ether, 0.8 weight portion dipotassium tetraborate, 21 weight starch enzymes put in 65 parts by weight of deionized water successively, stir;
2) 1.2 weight portion double-core manganese complexes, 0.9 weight portion zinc chloride, 1.3 weight portion stearic acid polyoxies are put into again successively
Vinyl acetate, 0.4 weight portion alkyl dimethyl aryl ammonium chloride, continue stirring, uniform to being sufficiently mixed, prepared desizing liquid;
3) fabric is padded process in desizing liquid, wash after taking-up and dry.
Embodiment 4
The desizing processing method of superfine denier nylon, comprises the steps:
1) by 1.2 parts by weight of sucrose fatty acid esters, 1.2 weight portion methylcellulose, 1.5 weight portion isomery fatty alcohol polyoxies
Vinyl Ether, 0.8 weight portion dipotassium tetraborate, 21 weight starch enzymes put in 65 parts by weight of deionized water successively, stir;
2) 1.2 weight portion double-core manganese complexes, 0.9 weight portion zinc chloride, 1.3 weight portion stearic acid polyoxies are put into again successively
Vinyl acetate, 0.4 weight portion alkyl dimethyl aryl ammonium chloride, continue stirring, uniform to being sufficiently mixed, prepared desizing liquid;
3) fabric is padded process in desizing liquid, wash after taking-up and dry.
The desizing rate of the various embodiments described above is high, and the fabric after desizing is processed has higher capillary effect and mechanical property, favorably
In follow-up dyeing and printing process carrying out it is ensured that follow-up printing quality;And the effective removal because of slurry, improves the handss of fabric
Sense.
The above is only the preferred embodiment of the present invention it is noted that ordinary skill people for the art
For member, on the premise of without departing from the technology of the present invention principle, some improvements and modifications can also be made, these improvements and modifications
Also should be regarded as protection scope of the present invention.
Claims (4)
1. the desizing processing method of superfine denier nylon is it is characterised in that comprise the steps:
1) by 1~2 parts by weight of sucrose fatty acid ester, 1.2 weight portion methylcellulose, 1.5 weight portion isomery fatty alcohol polyoxy second
Alkene ether, 0.8 weight portion dipotassium tetraborate, 21 weight starch enzymes put in 65 parts by weight of deionized water successively, stir;
2) 1.2 weight portion double-core manganese complexes, 0.9 weight portion zinc chloride, 1.3 weight portion stearic acid polyoxyethylenes are put into again successively
Ester, 0.4 weight portion alkyl dimethyl aryl ammonium chloride, continue stirring, uniform to being sufficiently mixed, prepared desizing liquid;
3) fabric is padded process in desizing liquid, wash after taking-up and dry.
2. the desizing processing method of superfine denier nylon according to claim 1 is it is characterised in that include following walking
Suddenly:
1) by 1 parts by weight of sucrose fatty acid ester, 1.2 weight portion methylcellulose, 1.5 weight portion isomery aliphatic alcohol polyethenoxies
Ether, 0.8 weight portion dipotassium tetraborate, 21 weight starch enzymes put in 65 parts by weight of deionized water successively, stir;
2) 1.2 weight portion double-core manganese complexes, 0.9 weight portion zinc chloride, 1.3 weight portion stearic acid polyoxyethylenes are put into again successively
Ester, 0.4 weight portion alkyl dimethyl aryl ammonium chloride, continue stirring, uniform to being sufficiently mixed, prepared desizing liquid;
3) fabric is padded process in desizing liquid, wash after taking-up and dry.
3. the desizing processing method of superfine denier nylon according to claim 1 is it is characterised in that include following walking
Suddenly:
1) by 2 parts by weight of sucrose fatty acid esters, 1.2 weight portion methylcellulose, 1.5 weight portion isomery aliphatic alcohol polyethenoxies
Ether, 0.8 weight portion dipotassium tetraborate, 21 weight starch enzymes put in 65 parts by weight of deionized water successively, stir;
2) 1.2 weight portion double-core manganese complexes, 0.9 weight portion zinc chloride, 1.3 weight portion stearic acid polyoxyethylenes are put into again successively
Ester, 0.4 weight portion alkyl dimethyl aryl ammonium chloride, continue stirring, uniform to being sufficiently mixed, prepared desizing liquid;
3) fabric is padded process in desizing liquid, wash after taking-up and dry.
4. the desizing processing method of superfine denier nylon according to claim 1 is it is characterised in that include following walking
Suddenly:
1) by 1.2 parts by weight of sucrose fatty acid esters, 1.2 weight portion methylcellulose, 1.5 weight portion isomery aliphatic alcohol polyethenoxies
Ether, 0.8 weight portion dipotassium tetraborate, 21 weight starch enzymes put in 65 parts by weight of deionized water successively, stir;
2) 1.2 weight portion double-core manganese complexes, 0.9 weight portion zinc chloride, 1.3 weight portion stearic acid polyoxyethylenes are put into again successively
Ester, 0.4 weight portion alkyl dimethyl aryl ammonium chloride, continue stirring, uniform to being sufficiently mixed, prepared desizing liquid;
3) fabric is padded process in desizing liquid, wash after taking-up and dry.