CN106269277A - A kind of efficiently except the rock phosphate in powder collecting agent in reverse floatation of calcite - Google Patents

A kind of efficiently except the rock phosphate in powder collecting agent in reverse floatation of calcite Download PDF

Info

Publication number
CN106269277A
CN106269277A CN201610642129.1A CN201610642129A CN106269277A CN 106269277 A CN106269277 A CN 106269277A CN 201610642129 A CN201610642129 A CN 201610642129A CN 106269277 A CN106269277 A CN 106269277A
Authority
CN
China
Prior art keywords
calcite
collecting agent
rock phosphate
powder collecting
reverse floatation
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201610642129.1A
Other languages
Chinese (zh)
Inventor
王仁宗
熊良峰
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Hubei Forbon Technology Co Ltd
Original Assignee
Hubei Forbon Technology Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Hubei Forbon Technology Co Ltd filed Critical Hubei Forbon Technology Co Ltd
Priority to CN201610642129.1A priority Critical patent/CN106269277A/en
Publication of CN106269277A publication Critical patent/CN106269277A/en
Pending legal-status Critical Current

Abstract

The present invention relates to a kind of efficiently except the rock phosphate in powder collecting agent in reverse floatation of calcite, by mass percentage, by 80~90% modified fat acid and 10~20% complexed surfactant compounding form;Wherein modified fat acid is formed by 50% turkey red oil and 50% trihydroxy ethylamine oleate soap are compounding, and complexed surfactant is compounded formed by 20% sulfonated oil, 30% fatty alcohol-polyoxyethylene ether AEO 3,20% Palmic acid formicester sodium sulfonate, 30% alhpa olefin sodium sulfonate.The present invention is applicable to phosphorite and removes the reverse floatation process of calcite, has selectivity excellent, the feature that the concentrate response rate is high.

Description

A kind of efficiently except the rock phosphate in powder collecting agent in reverse floatation of calcite
Technical field
The present invention relates to a kind of rock phosphate in powder collecting agent in reverse floatation, especially relate to efficiently remove calcite from rock phosphate in powder Collecting agent.Belong to surfactant field.
Background technology
Phosphorus ore is important strategic resource, is mainly used in and prepares phosphate and phosphate fertilizer.The production of phosphate and phosphate fertilizer is right The requirement of rock phosphate in powder raw material is P2O5Content is more than 30%, and content of MgO is below 2%.In nature, it is possible to reach so to refer to Target rock phosphate in powder is limited, and most mid low grade phosphate rock stone needs to carry out ore dressing, to reaching the requirement of high-quality rock phosphate in powder.Foam floats Choosing is a kind of ore dressing mode that current sulphur dioxide of phosphor chemical industry should be with the most use, the most general except the technique of dolomite with reverse flotation the most again Time.This technique is only applicable to the phosphorite that dolomite content is higher.Nature exists dolomite content is relatively low, calcite content Higher Sedimentary phosphate rock.For such Ore, maximally effective ore dressing mode is to remove calcite by reverse flotation, makes final P in concentrate2O5Content is promoted to more than 30%.Except the collecting agent of calcite plays conclusive effect in this floatation process.Cause This, developing a kind of has certain using value except the rock phosphate in powder collecting agent in reverse floatation of calcite.
Summary of the invention
It is an object of the invention to provide a kind of efficiently except the rock phosphate in powder collecting agent in reverse floatation of calcite, dolomite is contained Measure relatively low and that calcite content is higher phosphorite, by reverse floatation process, the collecting agent of the application present invention, remove calcite, Can be by the P in concentrate2O5Content is promoted to more than 30%, has fine selectivity, the feature that the concentrate response rate is high.
The technical scheme is that
1, a kind of efficiently except the rock phosphate in powder collecting agent in reverse floatation of calcite, by mass percentage, by 80~90% change Property fatty acid and 10~the complexed surfactant of 20%, by the way of compounding, obtains final products.
2, the acid of the modified fat in above-mentioned 1 by 50% turkey red oil and 50% trihydroxy ethylamine oleate soap compounding and Become.
3, the complexed surfactant in above-mentioned 1 by 20% sulfonated oil, the fatty alcohol-polyoxyethylene ether AEO 3 of 30%, The Palmic acid formicester sodium sulfonate of 20% and 30% alpha-olefin sodium sulfonate compound and form.
4, the alpha-olefin sodium sulfonate in above-mentioned 3, carbon number distribution is C14 or C16.
The present invention is applicable to phosphorite and removes the reverse floatation process of calcite, has selectivity excellent, the high spy of the concentrate response rate Point.
Detailed description of the invention
Embodiment 1 takes 80g turkey red oil, 80g trihydroxy ethylamine oleate soap, 8g sulfonated oil, 12g aliphatic alcohol polyethenoxy Ether AEO 3,8g Palmic acid formicester sodium sulfonate, 12g 30%C14 alpha-olefin sodium sulfonate add in 500ml flask, stir 15min, Make material in flask be sufficiently mixed uniformly, obtain rock phosphate in powder reverse flotation except calcite collecting agent.
Utilize the rock phosphate in powder reverse flotation that the present embodiment 1 prepares except calcite collecting agent is to P2O5Content is 21.90%, and MgO contains Amount is 0.51%, CaO content be 51.80% phosphorite add 1.0kg by raw ore per ton and carry out reverse flotation except calcite, obtain P2O5Content is 30.48%, and content of MgO is 0.41%, and CaO content is the concentrate of 51.15%, the response rate 91.32%.
Embodiment 2 takes 85g turkey red oil, 85g trihydroxy ethylamine oleate soap, 6g sulfonated oil, 9g fatty alcohol-polyoxyethylene ether AEO 3,6g Palmic acid formicester sodium sulfonate, 9g 30%C16 alpha-olefin sodium sulfonate add in 500ml flask, stir 15min, make burning Vial material is sufficiently mixed uniformly, obtains rock phosphate in powder reverse flotation except calcite collecting agent.
Utilize the rock phosphate in powder reverse flotation that the present embodiment 2 prepares except calcite collecting agent is to P2O5Content is 21.90%, and MgO contains Amount is 0.51%, CaO content be 51.80% phosphorite raw ore per ton add 1.0kg and carry out reverse flotation except calcite, obtain P2O5Content is 31.48%, and content of MgO is 0.31%, and CaO content is the concentrate of 51.46%, the response rate 92.32%.
Embodiment 3 takes 90g turkey red oil, 90g trihydroxy ethylamine oleate soap, 4g sulfonated oil, 6g fatty alcohol-polyoxyethylene ether AEO 3,4g Palmic acid formicester sodium sulfonate, 6g 30%C16 alpha-olefin sodium sulfonate add in 500ml flask, stir 15min, make burning Vial material is sufficiently mixed uniformly, obtains rock phosphate in powder reverse flotation except calcite collecting agent.
Utilize the rock phosphate in powder reverse flotation that the present embodiment 3 prepares except calcite collecting agent is to P2O5Content is 21.90%, and MgO contains Amount is 0.51%, CaO content be 51.80% phosphorite add 1.0kg by raw ore per ton and carry out reverse flotation except calcite, obtain P2O5Content is 31.25%, and content of MgO is 0.38%, and CaO content is the concentrate of 51.18%, the response rate 91.87%.

Claims (4)

1. one kind efficiently except the rock phosphate in powder collecting agent in reverse floatation of calcite, it is characterised in that by mass percentage, by 80~ 90% modified fat acid and 10~20% complexed surfactant compounding form.
The most according to claim 1 a kind of efficiently except the rock phosphate in powder collecting agent in reverse floatation of calcite, it is characterised in that by matter Amount percentages, described modified fat acid is formed by 50% turkey red oil and 50% trihydroxy ethylamine oleate soap are compounding.
The most according to claim 1 a kind of efficiently except the rock phosphate in powder collecting agent in reverse floatation of calcite, it is characterised in that by matter Amount percentages, described complexed surfactant is by 20% sulfonated oil, 30% fatty alcohol-polyoxyethylene ether AEO 3,20% palm fibre Palmitic acid acid formicester sodium sulfonate, 30% alhpa olefin sodium sulfonate are compounding to be formed.
The most according to claim 3 a kind of efficiently except the rock phosphate in powder collecting agent in reverse floatation of calcite, it is characterised in that 30% Alhpa olefin sodium sulfonate, carbon number distribution is C14 or C16.
CN201610642129.1A 2016-08-08 2016-08-08 A kind of efficiently except the rock phosphate in powder collecting agent in reverse floatation of calcite Pending CN106269277A (en)