CN106242489B - The preparation method of Environment-friendlymagnesium magnesium oxide decorative panel - Google Patents

The preparation method of Environment-friendlymagnesium magnesium oxide decorative panel Download PDF

Info

Publication number
CN106242489B
CN106242489B CN201610613126.5A CN201610613126A CN106242489B CN 106242489 B CN106242489 B CN 106242489B CN 201610613126 A CN201610613126 A CN 201610613126A CN 106242489 B CN106242489 B CN 106242489B
Authority
CN
China
Prior art keywords
base material
parts
magnesia
sanding
magnesium oxide
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201610613126.5A
Other languages
Chinese (zh)
Other versions
CN106242489A (en
Inventor
方德
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Dongguan huafuli decoration building materials Co., Ltd
Original Assignee
Dongguan Top Industrial Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Dongguan Top Industrial Co Ltd filed Critical Dongguan Top Industrial Co Ltd
Priority to CN201610613126.5A priority Critical patent/CN106242489B/en
Publication of CN106242489A publication Critical patent/CN106242489A/en
Application granted granted Critical
Publication of CN106242489B publication Critical patent/CN106242489B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses the preparation methods of Environment-friendlymagnesium magnesium oxide decorative panel.This method comprises the following steps:Magnesia base material is provided, the magnesia base material, which is placed in sander, carries out sanding, removes the miscellaneous dirt of magnesia substrate surface;Two surfaces of magnesia base material are respectively coated for cohesive resin;By the magnesia base material of coated with resins quickly through baking oven;Last layer melamine paper is covered in the first face of magnesia base material, the second face is covered with a layer equilibration paper, forms intermediate product;Multiple intermediate product are stacked, suppress 2min 30min naturally;The intermediate product are placed in hot press, the pressure and temperature of hot press is adjusted, suppress 0.5h 5h, form semi-finished product;The redundance at the semi-finished product edge is cut off, and removes the burr on surface, obtains the Environment-friendlymagnesium magnesium oxide decorative panel.The method of the invention is simple for process, and the magnesia decorative board structure of production is stablized, and using not removing and tilting for a long time, decoration performance is good.

Description

The preparation method of Environment-friendlymagnesium magnesium oxide decorative panel
Technical field
The present invention relates to decorative panel technical fields, and in particular to a kind of preparation method of Environment-friendlymagnesium magnesium oxide decorative panel.
Background technology
Environment friendly decoration board includes partition material, ceiling material, furniture material, pavement etc., due to the environmental protection of its material, Low cost, appearance are varied, are liked by people as ornament materials.Magnesium oxide plate is a kind of novel multi-functional builds Material, because of its not only lightweight and flexibility and cycling processability with wooden class organic plates, but also the fire line with inorganic plate and resistance to It is aqueous, it is applied in wall, furred ceiling, floor liner plate and other finishings for having fire protection requirement position.
The main component of current magnesium oxide plate be fiberglass gridding cloth (main source of the dynamics of plate), magnesia, Magnesium chloride, perlite, fiberfill fibers and property-modifying additive so that substrate material good weatherability.But it as the decorative panel of exterior wall, Ask its appearance that can reach user's requirement, it is necessary to be covered with decorative layer on the surface of base material.But in the case where exposing to the weather, surface Decorative layer exist easily tilt, stripping the defects of, cause its decorative appearance performance to substantially reduce.
Invention content
Based on this, the present invention provides a kind of preparation method of Environment-friendlymagnesium magnesium oxide decorative panel, simple for process, the oxidation of production Magnesium decorative board stable structure, using not removing and tilting for a long time, decoration performance is good.
In order to achieve the object of the present invention, the present invention uses following technical scheme:
A kind of preparation method of Environment-friendlymagnesium magnesium oxide decorative panel comprising following steps:
Magnesia base material is provided, the magnesia base material, which is placed in sander, carries out sanding, then removes the magnesia The miscellaneous dirt of substrate surface;
Two surfaces of magnesia base material are respectively coated for cohesive resin, the coated weight of the resin is 100g/m2- 120g/m2
By the magnesia base material of coated with resins quickly through the baking oven of 100 DEG C -110 DEG C of temperature in 80s-110s, to oxygen The resin changed on magnesium substrates is toasted;
Last layer melamine paper is covered in the first face of magnesia base material, it is flat to cover last layer in the second face of magnesia base material Weigh paper, forms intermediate product;
Multiple above-mentioned intermediate product are stacked, suppress 2min-30min naturally;
The intermediate product are placed in hot press, the pressure for adjusting hot press is 1.0kg/cm2-1.5kg/cm2, temperature is 190 DEG C -200 DEG C, 0.5h-5h is suppressed under these conditions, forms semi-finished product;
The redundance at the semi-finished product edge is cut off, and removes the burr on surface, obtains the Environment-friendlymagnesium magnesium oxide decoration Plate.
In wherein some embodiments, the magnesia base material sanding is first to use the sand paper of 80 mesh to carry out sanding, then adopt Sanding is carried out with the sand paper of 120 mesh, the sand paper of 180 mesh is finally used to carry out sanding.
In wherein some embodiments, the magnesia base material includes the component of following parts by weight:100 parts of magnesia, nothing 25-50 parts of aqueous magnesium chloride, 10-15 parts of sawdust, 10-15 parts of flyash, 3-10 parts of zeolite, 7-15 parts of calcium oxide, calcium stearate 0.5-1 parts, 30-50 parts of Adlerika, 3-10 parts of foaming agent, 2-8 parts of fire retardant, 5-15 parts of foaming control agent.
In wherein some embodiments, the magnesia base material includes the component of following parts by weight:100 parts of magnesia, nothing 40 parts of aqueous magnesium chloride, 12 parts of sawdust, 12 parts of flyash, 8 parts of zeolite, 10 parts of calcium oxide, 0.8 part of calcium stearate, Adlerika 40 parts, 7 parts of foaming agent, 5 parts of fire retardant, 10 parts of foaming control agent.
In wherein some embodiments, the preparation method of the magnesia base material is:
Magnesia, anhydrous magnesium chloride, calcium oxide, Adlerika, foaming agent and foaming control agent are mixed, It is placed in closed container and is stirred, gas is filled in whipping process, bubble is formed in the slurry of stirring;
Sawdust, flyash, zeolite, calcium stearate, fire retardant are added in above-mentioned closed container, are heated to 50 DEG C -60 DEG C, And be stirred, obtain raw material slurry;
Above-mentioned raw materials are starched and are added in the mold of press, heating mould is cold when keeping temperature 5h-7h to 100 DEG C -120 DEG C But it takes out afterwards, obtains semi-finished product;
The semi-finished product are stacked, place -5 days 3 days naturally at room temperature to get the magnesia base material.
The present invention also adopts the following technical scheme that:
A kind of preparation method of Environment-friendlymagnesium magnesium oxide decorative panel comprising following steps:
The process units of Environment-friendlymagnesium magnesium oxide decorative panel is provided, including:Conveying mechanism, the conveying mechanism include conveying frame And the feeder motor of the transfer member and the driving transfer member operation in the conveying frame;Mechanism of sanding machine, The mechanism of sanding machine includes sanding rack, the cabinet in the sanding rack, the sanding component being installed in the cabinet And the pumping dirt component being connected to the interior of equipment cabinet;The conveying mechanism part wears the cabinet;The sanding component Several rotating rollers including sanding motor, by the sanding motor-driven rotation and the sand paper that is set around in the rotating roller, There is gap between the rotating roller and the transfer member of the conveying mechanism;The pumping dirt component includes being located at the cabinet top The pumping dirt wind turbine in portion and several sweep-up pipes being connected to the pumping dirt wind turbine;Rubber-coated mechanism, the rubber-coated mechanism include gluing Rack, upper roller and bottom roller in the gluing rack have gap between the upper roller and bottom roller;It is described Gap between conveying mechanism and the upper roller and bottom roller is connected;Toast mechanism, the baking mechanism include toast rack, Baking conveyer belt and baking oven in the baking rack, the baking conveyer belt wear the baking oven;Windrow mechanism;Heat Press mechanism, the hot pressing mechanism include several pressing plates, temperature control unit and Pressure Control Unit, the adjacent pressing plate it Between have gap;
Magnesia base material is provided, the magnesia base material is placed on conveying mechanism, sander is delivered to by conveying mechanism Cabinet in, sanding component in cabinet carries out sanding to magnesia base material, then takes out the operation of dirt component, is stayed in after removing sanding The miscellaneous dirt of the magnesia substrate surface;
Magnesia base material after sanding is delivered between the upper roller of rubber-coated mechanism and bottom roller by conveying mechanism, upper roller Two surfaces of magnesia base material are coated in the resin on bottom roller, the coated weight of resin is 100g/m2-120g/m2
Magnesia base material after gluing is delivered in the baking rack of baking mechanism by conveying mechanism, toasts belt-driven Magnesia base material, quickly through the baking oven of 100 DEG C -110 DEG C of temperature, carries out the resin on magnesia base material in 80s-110s Toast drying;
Last layer melamine paper is covered in the first face of magnesia base material, the second face is covered with a layer equilibration paper, is formed intermediate Product;
Above-mentioned intermediate product are delivered to windrow mechanism by conveying mechanism so that multiple intermediate product are stacked, natural Suppress 2min-30min;
Between the intermediate product are delivered to the two panels pressing plate of hot pressing mechanism by conveying mechanism, the pressure of hot pressing mechanism is adjusted For 1.0kg/cm2-1.5kg/cm2, temperature is 190 DEG C -200 DEG C, suppresses 0.5h-5h under these conditions, forms semi-finished product;
The redundance at the semi-finished product edge is cut off, and removes the burr on surface, obtains the Environment-friendlymagnesium magnesium oxide decoration Plate.
In wherein some embodiments, the rotating roller includes the first rotating roller, the second rotating roller and third rotating roller, 80 the first sand paper of purpose of winding in first rotating roller, 120 the second sand paper of purpose of winding in second rotating roller, described The third sand paper of 180 mesh of winding in three rotating rollers.
In wherein some embodiments, the windrow mechanism includes liftable folding frame, is set to the folding frame On windrow board, the delivery roller that is installed on the windrow board, the windrow board is connected with the conveying mechanism;Institute It includes the folding leg and hydraulic cylinder for being separately connected the board both sides to state folding frame, the folding leg include first leg with Second supporting leg, the first leg are pivotally connected with the second supporting leg, and the first leg of two folding legs is connected by a connecting rod, The fixing end of the hydraulic cylinder is fixedly connected with the connecting rod, and the movable end of the hydraulic cylinder is connect with second supporting leg, When the hydraulic cylinder action, the folding leg can be driven to fold or open, folding leg board decline when folding is described Folding leg board rising when opening.
In wherein some embodiments, the windrow mechanism includes rickstand, the portal frame that is located at the rickstand And suction component, the rickstand are equipped with material wheel;The portal frame include set on the rickstand both sides column and The spreader of the column is connected, the spreader is equipped with sliding rail;The suction component include connecting rod and be located at the connection The windrow sucker of boom end, the windrow sucker are equipped with several windrow suction nozzles, and the connecting rod is connect with a sliding part, described Sliding part is slidably connected with the sliding rail.
In wherein some embodiments, the windrow mechanism includes liftable transport platform, bearing frame and several cylinders, The transport platform is equipped with several delivery wheels;The bearing frame is set to the top of the transport platform, and the bearing frame includes successively First side, second side, third side and the four side of connection, the second side, four side respectively with it is described First side, the flexible connection of third side, the cylinder connect with the second side, four side, for driving described the Dual side-edge, four side are moved towards the direction close to or away from the first side, third side;The second of the bearing frame Be respectively equipped with several conveying rollers on the inside of side and four side, the second side and the conveying roller at four side it Between have gap.
The preparation method of Environment-friendlymagnesium magnesium oxide decorative panel of the present invention, processing step is easy, is all made of conventional method, Low to technology requirement, manufacturing cost is low;In process of production by resin rapid draing, cover melamine paper and balance paper, heap Folded nature compacting and hot pressing so that resin can be firmly combined together with outer layer decorative layer, and the decoration of preparation is hardened Structure is stablized, and using long-time and is not easily stripped and tilts after exposing to the weather, and ensures that its performance is stablized.
In some other embodiment, the component rational proportion of magnesia base material, between interact, the base material of production is not It is only fire-retardant, fire protecting performance is good, and hardness is high, heat-proof quality is good;It is discharged without pernicious gas in manufacturing process, good environmental protection.
Description of the drawings
Fig. 1 is the overall structure signal of the process units of the Environment-friendlymagnesium magnesium oxide decorative panel described in a preferred embodiment of the present invention Figure;
Fig. 2 is the mechanism of sanding machine structural schematic diagram of the process units of the Environment-friendlymagnesium magnesium oxide decorative panel described in Fig. 1;
Fig. 3 is the windrow mechanism side structure schematic diagram of the process units of the Environment-friendlymagnesium magnesium oxide decorative panel described in Fig. 1;
Fig. 4 is the structural schematic diagram at another visual angle of the windrow mechanism described in Fig. 3;
Fig. 5 is that the windrow mechanism of the process units of the Environment-friendlymagnesium magnesium oxide decorative panel described in another preferred embodiment of the present invention bows View;
Fig. 6 is the overall structure diagram of windrow mechanism described in Fig. 5;
Fig. 7 is the positive structure schematic of the windrow mechanism of the process units of the Environment-friendlymagnesium magnesium oxide decorative panel described in Fig. 1;
Fig. 8 is the cladding plate mechanism side structure schematic diagram of the process units of the Environment-friendlymagnesium magnesium oxide decorative panel described in Fig. 1;
Fig. 9 is the cladding plate bench structure signal of the cladding plate mechanism of the process units of the Environment-friendlymagnesium magnesium oxide decorative panel described in Fig. 1 Figure;
Figure 10 is the cladding plate board side structure schematic diagram of cladding plate mechanism described in Fig. 9;
Figure 11 is the turning part structural schematic diagram of cladding plate mechanism described in Fig. 9;
Figure 12 is the vertical view of the turning part of cladding plate mechanism described in Figure 11.
Specific implementation mode
It to facilitate the understanding of the present invention, below will be to invention is more fully described.The present invention can be with many not With form realize, however it is not limited to embodiment described herein.Make to this on the contrary, purpose of providing these embodiments is The understanding of the disclosure of invention is more thorough and comprehensive.
Unless otherwise defined, all of technologies and scientific terms used here by the article and belong to the technical field of the present invention The normally understood meaning of technical staff is identical.Used term is intended merely to description tool in the description of the invention herein The purpose of the embodiment of body, it is not intended that in the limitation present invention.
The preparation method of Environment-friendlymagnesium magnesium oxide decorative panel of the present invention comprising following steps:
Magnesia base material is provided, the magnesia base material, which is placed in sander, carries out sanding, then removes the magnesia The miscellaneous dirt of substrate surface;
Two surfaces of magnesia base material are respectively coated for cohesive resin, the coated weight of the resin is 100g/m2- 120g/m2
By the magnesia base material of coated with resins quickly through the baking oven of 100 DEG C -110 DEG C of temperature in 80s-110s, to oxygen The resin changed on magnesium substrates is toasted;
Last layer melamine paper is covered in the first face of magnesia base material, the second face is covered with a layer equilibration paper, is formed intermediate Product;
Multiple above-mentioned intermediate product are stacked, suppress 2min-30min naturally;
The intermediate product are placed in hot press, the pressure for adjusting hot press is 1.0kg/cm2-1.5kg/cm2, temperature is 190 DEG C -200 DEG C, 0.5h-5h is suppressed under these conditions, forms semi-finished product;
The redundance at the semi-finished product edge is cut off, and removes the burr on surface, obtains the Environment-friendlymagnesium magnesium oxide decoration Plate.
Wherein, the magnesia base material sanding be first use 80 mesh sand paper carry out sanding, then using 120 mesh sand paper into Row sanding finally uses the sand paper of 180 mesh to carry out sanding.
Wherein, the magnesia base material includes the component of following parts by weight:100 parts of magnesia, anhydrous magnesium chloride 25-50 Part, 10-15 parts of sawdust, 10-15 parts of flyash, 3-10 parts of zeolite, 7-15 parts of calcium oxide, 0.5-1 parts of calcium stearate, magnesium sulfate are molten 30-50 parts of liquid, 3-10 parts of foaming agent, 2-8 parts of fire retardant, 5-15 parts of foaming control agent.
Wherein, the magnesia base material includes the component of following parts by weight:100 parts of magnesia, 40 parts of anhydrous magnesium chloride, wood Bits 12 parts, 12 parts of flyash, 8 parts of zeolite, 10 parts of calcium oxide, 0.8 part of calcium stearate, 40 parts of Adlerika, 7 parts of foaming agent, 5 parts of fire retardant, 10 parts of foaming control agent.
Wherein, the preparation method of the magnesia base material is:Magnesia, anhydrous magnesium chloride, calcium oxide, magnesium sulfate is molten Liquid, foaming agent and foaming control agent mix, and are placed in closed container and are stirred, and gas is filled in whipping process Body forms bubble in the slurry of stirring;Above-mentioned closed container is added in sawdust, flyash, zeolite, calcium stearate, fire retardant It is interior, 50 DEG C -60 DEG C are heated to, and be stirred, obtain raw material slurry;Above-mentioned raw materials are starched and are added in the mold of press, heated mould Tool is to 100 DEG C -120 DEG C, when keeping temperature 5h-7h, is taken out after cooling, obtains semi-finished product;The semi-finished product are stacked, - 5 days 3 days are placed naturally at room temperature to get the magnesia base material.
Following technical solution also can be used:The preparation method of Environment-friendlymagnesium magnesium oxide decorative panel comprising following steps:
The process units of Environment-friendlymagnesium magnesium oxide decorative panel is provided, including:Conveying mechanism, the conveying mechanism include conveying frame And the feeder motor of the transfer member and the driving transfer member operation in the conveying frame;Mechanism of sanding machine, The mechanism of sanding machine includes sanding rack, the cabinet in the sanding rack, the sanding component being installed in the cabinet And the pumping dirt component being connected to the interior of equipment cabinet by the top of the cabinet;The conveying mechanism part wears described Cabinet;The sanding component include sanding motor, by the sanding motor-driven rotation several rotating rollers and be set around institute The sand paper in rotating roller is stated, is had for by between plank between the rotating roller and the transfer member of the conveying mechanism Gap;The dirt component of taking out includes several dust suctions for being located at the pumping dirt wind turbine of the enclosure top and being connected to the pumping dirt wind turbine Pipe;Rubber-coated mechanism, the rubber-coated mechanism include gluing rack, upper roller and bottom roller in the gluing rack, institute Stating between upper roller and bottom roller has for the gap by plank;The conveying mechanism and the upper roller and bottom roller it Between gap linking;Mechanism is toasted, the baking mechanism includes toasting rack, the baking conveyer belt in the baking rack And baking oven, the baking conveyer belt wear the baking oven;Windrow mechanism;Hot pressing mechanism, if the hot pressing mechanism includes dry-pressing Plate, temperature control unit and Pressure Control Unit have for the gap by plank between the adjacent pressing plate;
Magnesia base material is provided, the magnesia base material is placed on conveying mechanism, sander is delivered to by conveying mechanism Cabinet in, sanding component in cabinet carries out sanding to magnesia base material, then takes out the operation of dirt component, is stayed in after removing sanding The miscellaneous dirt of the magnesia substrate surface;
Magnesia base material after sanding is delivered between the upper roller of rubber-coated mechanism and bottom roller by conveying mechanism, upper roller Two surfaces of magnesia base material are coated in the resin on bottom roller, the coated weight of resin is 100g/m2-120g/m2
Magnesia base material after gluing is delivered in the baking rack of baking mechanism by conveying mechanism, toasts belt-driven Magnesia base material, quickly through the baking oven of 100 DEG C -110 DEG C of temperature, carries out the resin on magnesia base material in 80s-110s Toast drying;
Last layer melamine paper is covered in the first face of magnesia base material, the second face is covered with a layer equilibration paper, is formed intermediate Product;
Above-mentioned intermediate product are delivered to windrow mechanism by conveying mechanism so that multiple intermediate product are stacked, natural Suppress 2min-30min;
Between the intermediate product are delivered to the two panels pressing plate of hot pressing mechanism by conveying mechanism, the pressure of hot pressing mechanism is adjusted For 1.0kg/cm2-1.5kg/cm2, temperature is 190 DEG C -200 DEG C, suppresses 0.5h-5h under these conditions, forms semi-finished product;
The redundance at the semi-finished product edge is cut off, and removes the burr on surface, obtains the Environment-friendlymagnesium magnesium oxide decoration Plate.
Wherein, the rotating roller includes the first rotating roller, the second rotating roller and third rotating roller, first rotating roller 80 the first sand paper of purpose of upper winding, 120 the second sand paper of purpose of winding in second rotating roller, winding in the third rotating roller The third sand paper of 180 mesh.
Wherein, the windrow mechanism includes liftable folding frame, the windrow board on the folding frame, peace Loaded on the delivery roller on the windrow board, the windrow board is connected with the conveying mechanism;The folding frame includes It is separately connected the folding leg and hydraulic cylinder of the board both sides, the folding leg includes first leg and the second supporting leg, described First leg is pivotally connected with the second supporting leg, and the first leg of two folding legs is connected by a connecting rod, the hydraulic cylinder Fixing end is fixedly connected with the connecting rod, and the movable end of the hydraulic cylinder is connect with second supporting leg, and the hydraulic cylinder is dynamic When making, the folding leg can be driven to fold or open, folding leg board decline when folding, when the folding leg is opened The board rises.
Wherein, the windrow mechanism include rickstand, the portal frame that is located at the rickstand and suction component, institute It states rickstand and is equipped with material wheel;The portal frame includes the cross of the column and the connection column set on the rickstand both sides Column, the spreader are equipped with sliding rail;The suction component include connecting rod and positioned at it is described connection boom end windrow sucker, The windrow sucker is equipped with several windrow suction nozzles, and the connecting rod is connect with a sliding part, the sliding part and the sliding rail It is slidably connected.
Wherein, the windrow mechanism includes liftable transport platform, bearing frame and several cylinders, is set in the transport platform There are several delivery wheels;The bearing frame be set to the transport platform top, the bearing frame include sequentially connected first side, Second side, third side and four side, the second side, four side respectively with the first side, third side Side is flexibly connected, and the cylinder is connect with the second side, four side, for driving the second side, four side It is moved towards the direction close to or away from the first side, third side;The second side of the bearing frame and four side Inside be respectively equipped with several conveying rollers, there is gap between the conveying roller at the second side and four side.
Please refer to Fig. 1 to Figure 12, the process units of above-mentioned Environment-friendlymagnesium magnesium oxide decorative panel comprising conveying mechanism 10, sand Ray machine structure 20, rubber-coated mechanism 30, baking mechanism 40, windrow mechanism 50 and hot pressing mechanism 60;Conveying mechanism 10 is used for delivery board Material, mechanism of sanding machine 20 are used to carry out sanding to plank and remove the remaining miscellaneous dirt of sanding rear surface;Rubber-coated mechanism 30 will be for that will set Fat is coated in the surface of magnesia base material;Baking mechanism 40 is for resin to be dried;Windrow mechanism 50 will be for after handling Magnesia base material stacked, processed with carrying out next cloth process;Hot pressing mechanism 60 is for pressing the plank after overlapping System, to form the decorative panel of complete structure.
Conveying mechanism 10 includes conveying frame 12 and the transfer member 13 in conveying frame 12 and driving transmission The feeder motor (not shown) that component 13 is run, conveying mechanism 10 is through in whole equipment, the plate after being processed to each process Material is conveyed.In the present embodiment, transfer member 13 is conveyer belt or transfer roller.
Referring once again to Fig. 1 and Fig. 2, mechanism of sanding machine 20 include sanding rack 21, the cabinet 22 in sanding rack 21, The sanding component 23 and the pumping dirt component 24 by being connected to inside the top of cabinet 22 and cabinet 22 being installed in cabinet 22, it is defeated It send 10 part of mechanism to wear cabinet 22, the magnesia base material of sanding will be needed to be sent into 22 inside of cabinet and carry out sanding.Sanding Component 23 includes sanding motor 231, several rotating rollers rotated by the driving of sanding motor 231 and the sand being set around in rotating roller Have between the transfer member 13 of paper, rotating roller and conveying mechanism 10 for the gap by plank, the driving of sanding motor 231 turns Dynamic roller rotation, sand paper are rotated with rotating roller, to carry out sanding to the magnesia base material of rotating roller bottom.In the present embodiment In, rotating roller includes the first rotating roller 25, the second rotating roller 26 and third rotating roller 27,80 mesh of winding in the first rotating roller 25 The first sand paper 251,120 the second sand paper of purpose 261 of winding in the second rotating roller 26,180 purpose of winding in third rotating roller 27 Third sand paper 271.To successively carry out magnesia base material three times by slightly to thin sanding operation.It includes being located to take out dirt component 24 The pumping dirt wind turbine 241 at 22 top of cabinet and several sweep-up pipes 242 being connected to pumping dirt wind turbine 241.In the present embodiment, in machine The top of cabinet 22 is equipped with perforation, and sweep-up pipe 242 is pierced by cabinet 22 by the perforation.After taking out dirt component 24 and taking out dirt, shakeout can be removed Light step remains in the miscellaneous dirt of magnesia substrate surface so that subsequent processing process is more convenient.
Fig. 1 is please referred to, rubber-coated mechanism 30 includes gluing rack 31, the upper roller 32 in gluing rack 31 and lower rolling Wheel 33 has between upper roller 32 and bottom roller 33 for the gap by plank;Conveying mechanism 10 and upper roller 32 and lower rolling Gap linking between wheel 33 so that the magnesia base material for needing gluing can be delivered on rubber-coated mechanism 30 by conveying mechanism 10, The resin coated will be needed to be poured on upper roller 32 and bottom roller 33, you can resin is coated on magnesia base material.
Please refer to Fig. 1, baking mechanism 40 include baking rack 41, the baking conveyer belt 42 in baking rack 41 and Baking oven 43, baking conveyer belt 42 are arranged along the length direction of baking rack 41 and are moved along baking rack 41, toast conveyer belt 42 wear baking oven 43, and magnesia base material is driven across baking oven 43 by baking conveyer belt 42, and baking drying is carried out by baking oven 43.
Fig. 8 to Figure 12 is please referred to, in the present embodiment, cladding plate machine is additionally provided between baking mechanism 40 and windrow mechanism 50 Structure 70, for melamine paper and balance paper to be overlying on magnesia base material automatically.Cladding plate mechanism 70 includes cladding plate board 71, position 72 liters of the sliding rail 73 and driving cladding plate sucker that cladding plate sucker 72 and cladding plate sucker 72 above cladding plate board 71 are slidably connected The driving part 74 of drop, cladding plate sucker 72 are equipped with several cladding plate suction nozzles 75, need the base material for covering acrylic board by conveying mechanism 10 are delivered on cladding plate board 71, and cladding plate sucker 72 acts, and draw acrylic board, cladding plate board is moved to then along sliding rail 73 Then 71 top drops to base material by the driving of driving part 74 again, acrylic board is overlying in the one side of base material, then will The base material is overturn, and after overturning, cladding plate sucker 72 continues to act, then acrylic board is overlying on the another side of base material.Overturning Method can be manual overturning, can also be the setting turning part 76 on cladding plate board 71.
In the present embodiment, turning part 76 includes the shaft 761 for being set to cladding plate board 71, connect with shaft 761 first Clamp bar group 762, the second clamp bar group 763 and third clamp bar group 764, the 4th clamp bar group 765 and inductor 766, the first clamp bar 762 homonymies that are corresponding with third clamp bar group 764 and being located at shaft 761 of group, the second clamp bar group 763 and the 4th clamp bar group 765 Homonymy that is corresponding and being located at shaft 761.First clamp bar group 762 includes several spaced first clamp bars 7621, third Clamp bar group 764 includes several spaced third clamp bars 7641, and every one first clamp bar 7621 corresponds to a third clamp bar 7641, Angle with 15-40 degree between first clamp bar 7621 and third clamp bar 7641, in order to which substrate can be inserted in the first clamp bar Between 7621 and third clamp bar 741, the angle is 25 degree in the present embodiment;Second clamp bar group 763 is arranged including several intervals The second clamp bar 7631, the 4th clamp bar group 765 includes several spaced 4th clamp bars 7651, and every one second clamp bar 7631 Corresponding one the 4th clamp bar 7651, the angle with 15-40 degree between the second clamp bar 7631 and the 4th clamp bar 7651, in order to substrate It can be inserted between the second clamp bar 7631 and the 4th clamp bar 7651, the angle is 25 degree in the present embodiment.Cladding plate board 71 It is equipped with conveyer belt 710, when base material after being covered with acrylic board on one side, conveyer belt 710 acts, and base material is driven to enter the first clamp bar Between 721 and third clamp bar 741, the inductor 766 in rack 10 senses that base material enters the first clamp bar 7621 and third clamp bar When 7641, control shaft 761 rotates, and the first clamp bar 7621 is driven to be overturn to the second of cladding plate board 71 with third clamp bar 7641 End to corresponding position stops, and continues to carry out cladding plate to base material, subsequent processing is delivered to after the completion of cladding plate.Thus it recycles, you can real The overturning of existing substrate.In the present embodiment, cladding plate board 71 is equipped with two groups of conveyer belts 710, the shaft of panel turnover mechanism 76 761 Between two groups of conveyer belts 710.Each conveyer belt 710 is equipped at least two inductors 766.And inductor 766 is set to board The side of 71 upper conveyor belts 710, facilitates induction substrate, and does not influence the work of panel turnover mechanism 76.Close to both ends on cladding plate board 71 Position be additionally provided with the fixture 77 for clamping plank, cladding plate board 71 is equipped with the fixture hole 711 of several strips, fixture 77 The limiting cylinder moved along fixture hole 711 including the limited post 771 being limited in fixture hole 711 and driving limited post 771.When When substrate is located on cladding plate board 71, limiting cylinder action, driving limited post 771 moves in fixture hole 711, to approach base Plate, clamping substrate.Cladding plate board 71 is elongate in shape, and turning part 76 is located at the medium position of cladding plate board 71.
Fig. 3 and Fig. 4 are please referred to, windrow mechanism 50 includes liftable folding frame 51, the heap on folding frame 51 Material board 52, the delivery roller 53 being installed on windrow board 52 and inductor 54, windrow board 52 are held in the mouth with conveying mechanism 10 It connects so that the magnesia base material after sanding and dust removal process on conveying mechanism 10 can be delivered on windrow board 52. Folding frame 51 includes being separately connected the folding leg 511 and hydraulic cylinder 512 of 52 both sides of windrow board, and folding leg 511 includes the One supporting leg 513 and the second supporting leg 514, first leg 513 and the second supporting leg 514 are pivotally connected in medium position, and the of two folding legs One supporting leg 513 is connected by a connecting rod 515, and the fixing end of hydraulic cylinder 512 is fixedly connected with connecting rod 515, hydraulic cylinder 512 Movable end is connect with the second supporting leg 514, and when hydraulic cylinder 512 acts, movable end driving can drive the second supporting leg 514 so that the Two supporting legs 514 pull first leg 513, and then first leg 513 is folded up with the second supporting leg 514, when folding leg 511 folds Windrow board 52 decline, play the role of windrow, when folding leg 511 is opened windrow board 52 rising so that whole equipment after Reforwarding row.Inductor 54 is electrically connected with a controller, for incuding whether magnesia base material arrived windrow board 52, to give Controller signals bring into operation to control subsequent equipment.
Fig. 5 and Fig. 6 are please referred to, in other embodiments, windrow mechanism 50 includes liftable transport platform 55, bearing frame 56 And several cylinders 57, transport platform 55 are equipped with several delivery wheels 551, for conveying the magnesia base material after sanding.Bearing frame 56 are set to the top of transport platform 55, and bearing frame 56 includes sequentially connected first side 561, second side 562, third side 563 and four side 564, second side 562, four side 564 respectively with first side 561,563 activity of third side even It connects, you can connect with pulling and pushing, cylinder 57 is connect with second side 562, four side 564, for driving second side 562, Four side 564 is towards the direction movement close to or away from first side 561, third side 563, when second side 562, the 4th side When side 564 is directed away from the direction movement of first side 561, third side 563, transport platform 55 rises to same with bearing frame 36 Plane, then second side 562, four side 564 are defeated towards the direction movement close to first side 561, third side 563 The magnesia base material on platform 55 is sent to be moved on bearing frame 56, equipment continues to run with.The second side 562 and the 4th of bearing frame 56 The inside of side 564 is respectively equipped with several conveying rollers 565, the conveying roller 565 at second side 562 and four side 564 Between have gap, when magnesia base material is moved on bearing frame 56, by conveying roller 565 carry out support.Above-mentioned transport platform 55 Lifting universal up-down mode can be used, details are not described herein.One is additionally provided with towards bearing frame 56 in the bottom of bearing frame 56 Middle part tabletting 58, tabletting 58 connect with a wherein cylinder, in the presence of cylinder towards close to or away from bearing frame 56 The direction at middle part is moved, to clamp or unclamp the foam base plate being placed on bearing frame 56.
Fig. 1 and Fig. 7 are please referred to, in further embodiments, windrow mechanism 50 includes rickstand 501, is located at rickstand Portal frame 502 at 501 and suction component 503, rickstand 501 are equipped with material wheel 504;Portal frame 502 includes being set to windrow The column 505 of 501 both sides of frame and the spreader 506 for connecting column 505, spreader 506 are equipped with sliding rail 507;Suction component 503 wraps Connecting rod 508 and the windrow sucker 509 positioned at 508 end of connecting rod are included, windrow sucker 509 is equipped with several windrow suction nozzles 519, connecting rod 508 is connect with a sliding part 518, and sliding part 518 is slidably connected with sliding rail 507, the plank heap after the completion of rolling It folds in the plane, after the completion of the windrow time, suction component 503 can draw the plank after the completion of rolling to the table top of subsequent processing On, to carry out the processing of subsequent processing.
Fig. 1 is please referred to, hot pressing mechanism 60 includes several pressing plates 61, temperature control unit 62 and Pressure Control Unit 63, Have for the gap by plank between adjacent pressing plate 61, Pressure Control Unit 63 controls between two adjacent pressing plates 61 Pressure, thus adjust to cold pressing mechanism 60 to the pressure of plank, temperature control unit 62 to control the temperature of pressing plate 61, To adjust temperature of the cold pressing mechanism 60 to plank.Temperature control unit 62 and Pressure Control Unit 63 are electrically connected with a controller It connects, the temperature and pressure for adjusting or monitoring cold pressing mechanism 60 on the controller.
Process units using above-mentioned PVC foam fire-proof plate is come the method for producing PVC foam fire-proof plate:
Magnesia base material is provided, magnesia base material is sent into the machine of sander 20 by the transfer member 13 of conveying mechanism 10 In cabinet 22, it is located at below rotating roller, the sand paper in rotating roller carries out sanding to magnesia base material;Specifically magnesia base material first leads to The first rotating roller 25 is crossed, there are 80 the first sand paper of purpose 251 in the first rotating roller 25, first time sand first is carried out to magnesia base material Light;Magnesia base material has 120 the second sand paper of purpose 261, then use again by the second rotating roller 26 in second rotating roller 26 The sand paper of 120 mesh carries out second of sanding;Magnesia base material has in the second rotating roller 27 finally by third rotating roller 27 The third sand paper 271 of 180 mesh, third sand paper 271 carry out third time sanding to magnesia base material.After the completion of sanding, dirt wind turbine is taken out 241 open, by sanding rear rack 22 and the miscellaneous dirt of magnesia substrate surface is evacuated to sweep-up pipe 242, by 242 row of sweep-up pipe Go out, more effectively in the subsequent operation of magnesia base material.
Conveying mechanism 10 transfers out mechanism of sanding machine 20 by sanding and except the magnesia base material after dust, then is delivered to gluing Between the upper roller 32 and bottom roller 33 of mechanism 30, resin is poured on upper roller 41 and bottom roller 42, the two of magnesia base material Surface is respectively coated for cohesive resin, and the coated weight of resin is 100g/m2-120g/m2, wait for resin automatic drying 2min- 5min.It can be by being poured on the amount of the resin on upper roller 32 and bottom roller 33, to control the coated weight of above-mentioned resin.
Magnesia base material after coated with resins is delivered in the baking rack 41 of baking mechanism 40 by conveying mechanism 10, baking Baking conveyer belt 42 in rack 41 drive magnesia base material by 80s-110s quickly through 100 DEG C -110 DEG C of temperature Baking oven 43, baking oven 43 carry out baking drying to the resin on magnesia base material, in order to subsequent processing.
Last layer melamine paper is covered in the first face of the magnesia base material with resin using cladding plate mechanism 70, after overturning It is covered with a layer equilibration paper in the second face of magnesia base material, forms intermediate product.Switching process can be manual, can also be by turning part It completes.Melamine paper and balance paper can also be overlayed on magnesia base material manually.
Above-mentioned intermediate product are delivered at windrow mechanism 50 by conveying mechanism 10, and multiple intermediate product are stacked, and are pressed naturally 2min-30min processed so that melamine paper and balance paper are preliminarily bonded together with resin layer.
Between above-mentioned intermediate product are delivered to two pressing plates 61 of hot pressing mechanism 60 by conveying mechanism 10, pass through pressure control portion It is 1.0kg/cm that part 63, which adjusts pressure,2-1.5kg/cm2, it is 190 DEG C -200 DEG C to adjust temperature by temperature control unit 62, upper 0.5h-5h is suppressed under the conditions of stating, and forms semi-finished product;
The redundance at above-mentioned semi-finished product edge is cut off by equipment such as cutting machines, and removes the burr on surface, obtains institute State Environment-friendlymagnesium magnesium oxide decorative panel.
The technical solution that will be further illustrated the present invention below by embodiment.
Embodiment one
The preparation method of Environment-friendlymagnesium magnesium oxide decorative panel described in the present embodiment, includes the following steps:
The component of following parts by weight is provided:100 parts of magnesia, 40 parts of anhydrous magnesium chloride, 12 parts of sawdust, 12 parts of flyash, 8 parts of zeolite, 10 parts of calcium oxide, 0.8 part of calcium stearate, 40 parts of Adlerika, 7 parts of foaming agent, 5 parts of fire retardant, foaming are adjusted 10 parts of agent.Magnesia, anhydrous magnesium chloride, calcium oxide, Adlerika, foaming agent and foaming control agent are mixed, It is placed in closed container and is stirred, gas is filled in whipping process, bubble is formed in the slurry of stirring;By sawdust, Flyash, zeolite, calcium stearate, fire retardant are added in above-mentioned closed container, are heated to 50 DEG C -60 DEG C, and be stirred, obtain Raw material is starched;Above-mentioned raw materials are starched and are added in the mold of press, heating mould is cold when keeping temperature 5h-7h to 100 DEG C -120 DEG C But it takes out afterwards, obtains semi-finished product;The semi-finished product are stacked, place -5 days 3 days naturally at room temperature to get the oxidation Magnesium substrates.The component rational proportion of magnesia base material, between interact, the base material of production is not only fire-retardant, fire protecting performance is good, and Hardness is high, heat-proof quality is good.
Magnesia base material is sent by the transfer member 13 of conveying mechanism 10 in the cabinet 22 of sander 20, rotation is located at Below roller, the sand paper in rotating roller carries out sanding to magnesia base material;Specifically magnesia base material first passes through the first rotating roller 25, There are 80 the first sand paper of purpose 251 in first rotating roller 25, first time sanding first is carried out to magnesia base material;Magnesia base material is again By the second rotating roller 26, there are 120 the second sand paper of purpose 261 in the second rotating roller 26, then the is carried out using the sand paper of 120 mesh Secondary sanding;Magnesia base material is finally by third rotating roller 27, the third sand paper 271 with 180 mesh in the second rotating roller 27, Third sand paper 271 carries out third time sanding to magnesia base material.After the completion of sanding, takes out dirt wind turbine 241 and open, by sanding rear rack In 22 and the miscellaneous dirt of magnesia substrate surface is evacuated to sweep-up pipe 242, is discharged by sweep-up pipe 242, more effectively in magnesium oxide-based The subsequent operation of material.
Conveying mechanism 10 transfers out mechanism of sanding machine 20 by sanding and except the magnesia base material after dust, then is delivered to gluing Between the upper roller 32 and bottom roller 33 of mechanism 30, resin is poured on upper roller 41 and bottom roller 42, the two of magnesia base material Surface is respectively coated for cohesive resin, and the coated weight of resin is 100g/m2-120g/m2, wait for resin automatic drying 2min- 5min.It can be by being poured on the amount of the resin on upper roller 32 and bottom roller 33, to control the coated weight of above-mentioned resin.
Magnesia base material after coated with resins is delivered in the baking rack 41 of baking mechanism 40 by conveying mechanism 10, baking Baking conveyer belt 42 in rack 41 drive magnesia base material by 80s-110s quickly through 100 DEG C -110 DEG C of temperature Baking oven 43, baking oven 43 carry out baking drying to the resin on magnesia base material, in order to subsequent processing.
Last layer melamine paper is covered in the first face of the magnesia base material with resin using cladding plate mechanism 70, after overturning It is covered with a layer equilibration paper in the second face of magnesia base material, forms intermediate product.Switching process can be manual, can also be by turning part It completes.Melamine paper and balance paper can also be overlayed on magnesia base material manually.
Above-mentioned intermediate product are delivered at windrow mechanism 50 by conveying mechanism 10, and multiple intermediate product are stacked, and are pressed naturally 2min-30min processed so that melamine paper and balance paper are preliminarily bonded together with resin layer.
Between above-mentioned intermediate product are delivered to two pressing plates 61 of hot pressing mechanism 60 by conveying mechanism 10, pass through pressure control portion It is 1.0kg/cm that part 63, which adjusts pressure,2-1.5kg/cm2, it is 190 DEG C -200 DEG C to adjust temperature by temperature control unit 62, upper 0.5h-5h is suppressed under the conditions of stating, and forms semi-finished product;
The redundance at above-mentioned semi-finished product edge is cut off by equipment such as cutting machines, and removes the burr on surface, obtains institute State Environment-friendlymagnesium magnesium oxide decorative panel.
Embodiment two
The preparation method of Environment-friendlymagnesium magnesium oxide decorative panel described in the present embodiment, includes the following steps:
The component of following parts by weight is provided:100 parts of magnesia, 25 parts of anhydrous magnesium chloride, 10 parts of sawdust, 10 parts of flyash, 3 parts of zeolite, 7 parts of calcium oxide, 0.5 part of calcium stearate, 30 parts of Adlerika, 3 parts of foaming agent, 2 parts of fire retardant, foaming control agent 5 parts.Magnesia, anhydrous magnesium chloride, calcium oxide, Adlerika, foaming agent and foaming control agent are mixed, juxtaposition In being stirred in closed container, it is filled with gas in whipping process, bubble is formed in the slurry of stirring;By sawdust, fine coal Ash, zeolite, calcium stearate, fire retardant are added in above-mentioned closed container, are heated to 50 DEG C -60 DEG C, and be stirred, obtain raw material Slurry;Above-mentioned raw materials are starched and are added in the mold of press, heating mould is to 100 DEG C -120 DEG C, when keeping temperature 5h-7h, after cooling It takes out, obtains semi-finished product;The semi-finished product are stacked, place -5 days 3 days naturally at room temperature to get described magnesium oxide-based Material.The component rational proportion of magnesia base material, between interact, the base material of production is not only fire-retardant, fire protecting performance is good, and hardness Height, heat-proof quality are good.
Magnesia base material is sent by the transfer member 13 of conveying mechanism 10 in the cabinet 22 of sander 20, rotation is located at Below roller, the sand paper in rotating roller carries out sanding to magnesia base material;Specifically magnesia base material first passes through the first rotating roller 25, There are 80 the first sand paper of purpose 251 in first rotating roller 25, first time sanding first is carried out to magnesia base material;Magnesia base material is again By the second rotating roller 26, there are 120 the second sand paper of purpose 261 in the second rotating roller 26, then the is carried out using the sand paper of 120 mesh Secondary sanding;Magnesia base material is finally by third rotating roller 27, the third sand paper 271 with 180 mesh in the second rotating roller 27, Third sand paper 271 carries out third time sanding to magnesia base material.After the completion of sanding, takes out dirt wind turbine 241 and open, by sanding rear rack In 22 and the miscellaneous dirt of magnesia substrate surface is evacuated to sweep-up pipe 242, is discharged by sweep-up pipe 242, more effectively in magnesium oxide-based The subsequent operation of material.
Conveying mechanism 10 transfers out mechanism of sanding machine 20 by sanding and except the magnesia base material after dust, then is delivered to gluing Between the upper roller 32 and bottom roller 33 of mechanism 30, resin is poured on upper roller 41 and bottom roller 42, the two of magnesia base material Surface is respectively coated for cohesive resin, and the coated weight of resin is 100g/m2-120g/m2, wait for resin automatic drying 2min- 5min.It can be by being poured on the amount of the resin on upper roller 32 and bottom roller 33, to control the coated weight of above-mentioned resin.
Magnesia base material after coated with resins is delivered in the baking rack 41 of baking mechanism 40 by conveying mechanism 10, baking Baking conveyer belt 42 in rack 41 drive magnesia base material by 80s-110s quickly through 100 DEG C -110 DEG C of temperature Baking oven 43, baking oven 43 carry out baking drying to the resin on magnesia base material, in order to subsequent processing.
Last layer melamine paper is covered in the first face of the magnesia base material with resin using cladding plate mechanism 70, after overturning It is covered with a layer equilibration paper in the second face of magnesia base material, forms intermediate product.Switching process can be manual, can also be by turning part It completes.Melamine paper and balance paper can also be overlayed on magnesia base material manually.
Above-mentioned intermediate product are delivered at windrow mechanism 50 by conveying mechanism 10, and multiple intermediate product are stacked, and are pressed naturally 2min-30min processed so that melamine paper and balance paper are preliminarily bonded together with resin layer.
Between above-mentioned intermediate product are delivered to two pressing plates 61 of hot pressing mechanism 60 by conveying mechanism 10, pass through pressure control portion It is 1.0kg/cm that part 63, which adjusts pressure,2-1.5kg/cm2, it is 190 DEG C -200 DEG C to adjust temperature by temperature control unit 62, upper 0.5h-5h is suppressed under the conditions of stating, and forms semi-finished product;
The redundance at above-mentioned semi-finished product edge is cut off by equipment such as cutting machines, and removes the burr on surface, obtains institute State Environment-friendlymagnesium magnesium oxide decorative panel.
Embodiment three
The preparation method of Environment-friendlymagnesium magnesium oxide decorative panel described in the present embodiment, includes the following steps:
The component of following parts by weight is provided:100 parts of magnesia, 50 parts of anhydrous magnesium chloride, 15 parts of sawdust, 15 parts of flyash, 10 parts of zeolite, 15 parts of calcium oxide, 1 part of calcium stearate, 50 parts of Adlerika, 10 parts of foaming agent, 8 parts of fire retardant, foaming are adjusted 15 parts of agent.Magnesia, anhydrous magnesium chloride, calcium oxide, Adlerika, foaming agent and foaming control agent are mixed, It is placed in closed container and is stirred, gas is filled in whipping process, bubble is formed in the slurry of stirring;By sawdust, Flyash, zeolite, calcium stearate, fire retardant are added in above-mentioned closed container, are heated to 50 DEG C -60 DEG C, and be stirred, obtain Raw material is starched;Above-mentioned raw materials are starched and are added in the mold of press, heating mould is cold when keeping temperature 5h-7h to 100 DEG C -120 DEG C But it takes out afterwards, obtains semi-finished product;The semi-finished product are stacked, place -5 days 3 days naturally at room temperature to get the oxidation Magnesium substrates.The component rational proportion of magnesia base material, between interact, the base material of production is not only fire-retardant, fire protecting performance is good, and Hardness is high, heat-proof quality is good.
Magnesia base material is sent by the transfer member 13 of conveying mechanism 10 in the cabinet 22 of sander 20, rotation is located at Below roller, the sand paper in rotating roller carries out sanding to magnesia base material;Specifically magnesia base material first passes through the first rotating roller 25, There are 80 the first sand paper of purpose 251 in first rotating roller 25, first time sanding first is carried out to magnesia base material;Magnesia base material is again By the second rotating roller 26, there are 120 the second sand paper of purpose 261 in the second rotating roller 26, then the is carried out using the sand paper of 120 mesh Secondary sanding;Magnesia base material is finally by third rotating roller 27, the third sand paper 271 with 180 mesh in the second rotating roller 27, Third sand paper 271 carries out third time sanding to magnesia base material.After the completion of sanding, takes out dirt wind turbine 241 and open, by sanding rear rack In 22 and the miscellaneous dirt of magnesia substrate surface is evacuated to sweep-up pipe 242, is discharged by sweep-up pipe 242, more effectively in magnesium oxide-based The subsequent operation of material.
Conveying mechanism 10 transfers out mechanism of sanding machine 20 by sanding and except the magnesia base material after dust, then is delivered to gluing Between the upper roller 32 and bottom roller 33 of mechanism 30, resin is poured on upper roller 41 and bottom roller 42, the two of magnesia base material Surface is respectively coated for cohesive resin, and the coated weight of resin is 100g/m2-120g/m2, wait for resin automatic drying 2min- 5min.It can be by being poured on the amount of the resin on upper roller 32 and bottom roller 33, to control the coated weight of above-mentioned resin.
Magnesia base material after coated with resins is delivered in the baking rack 41 of baking mechanism 40 by conveying mechanism 10, baking Baking conveyer belt 42 in rack 41 drive magnesia base material by 80s-110s quickly through 100 DEG C -110 DEG C of temperature Baking oven 43, baking oven 43 carry out baking drying to the resin on magnesia base material, in order to subsequent processing.
Last layer melamine paper is covered in the first face of the magnesia base material with resin using cladding plate mechanism 70, after overturning It is covered with a layer equilibration paper in the second face of magnesia base material, forms intermediate product.Switching process can be manual, can also be by turning part It completes.Melamine paper and balance paper can also be overlayed on magnesia base material manually.
Above-mentioned intermediate product are delivered at windrow mechanism 50 by conveying mechanism 10, and multiple intermediate product are stacked, and are pressed naturally 2min-30min processed so that melamine paper and balance paper are preliminarily bonded together with resin layer.
Between above-mentioned intermediate product are delivered to two pressing plates 61 of hot pressing mechanism 60 by conveying mechanism 10, pass through pressure control portion It is 1.0kg/cm that part 63, which adjusts pressure,2-1.5kg/cm2, it is 190 DEG C -200 DEG C to adjust temperature by temperature control unit 62, upper 0.5h-5h is suppressed under the conditions of stating, and forms semi-finished product;
The redundance at above-mentioned semi-finished product edge is cut off by equipment such as cutting machines, and removes the burr on surface, obtains institute State Environment-friendlymagnesium magnesium oxide decorative panel.
Several embodiments of the invention above described embodiment only expresses, the description thereof is more specific and detailed, but simultaneously Cannot the limitation to the scope of the claims of the present invention therefore be interpreted as.It should be pointed out that for those of ordinary skill in the art For, without departing from the inventive concept of the premise, various modifications and improvements can be made, these belong to the guarantor of the present invention Protect range.Therefore, the protection domain of patent of the present invention should be determined by the appended claims.

Claims (9)

1. a kind of preparation method of Environment-friendlymagnesium magnesium oxide decorative panel, which is characterized in that include the following steps:
The process units of Environment-friendlymagnesium magnesium oxide decorative panel is provided, including:Conveying mechanism, the conveying mechanism include conveying frame and The feeder motor of transfer member and driving the transfer member operation in the conveying frame;Mechanism of sanding machine, it is described Mechanism of sanding machine include sanding rack, the cabinet in the sanding rack, the sanding component being installed in the cabinet and The pumping dirt component being connected to the interior of equipment cabinet;The conveying mechanism part wears the cabinet;The sanding component includes Sanding motor, several rotating rollers by the sanding motor-driven rotation and the sand paper that is set around in the rotating roller, it is described There is gap between rotating roller and the transfer member of the conveying mechanism;The dirt component of smoking includes being located at the enclosure top Several sweep-up pipes taken out dirt wind turbine and be connected to the pumping dirt wind turbine;Rubber-coated mechanism, the rubber-coated mechanism include gluing rack, Upper roller and bottom roller in the gluing rack have gap between the upper roller and bottom roller;The conveying Gap between mechanism and the upper roller and bottom roller is connected;Mechanism is toasted, the baking mechanism includes baking rack, is located at Baking conveyer belt in the baking rack and baking oven, the baking conveyer belt wear the baking oven;Windrow mechanism;Hot press Structure, the hot pressing mechanism include several pressing plates, temperature control unit and Pressure Control Unit, are had between the adjacent pressing plate There is gap;
Magnesia base material is provided, the magnesia base material is placed on conveying mechanism, the machine of sander is delivered to by conveying mechanism In cabinet, the sanding component in cabinet carries out sanding to magnesia base material, then takes out the operation of dirt component, is stayed in after removing sanding described The miscellaneous dirt of magnesia substrate surface;
Magnesia base material after sanding is delivered between the upper roller of rubber-coated mechanism and bottom roller by conveying mechanism, and upper roller is under Resin on idler wheel is coated in two surfaces of magnesia base material, and the coated weight of resin is 100g/m2-120g/m2
Magnesia base material after gluing is delivered in the baking rack of baking mechanism by conveying mechanism, baking belt-driven oxidation Magnesium substrates, quickly through the baking oven of 100 DEG C -110 DEG C of temperature, toast the resin on magnesia base material in 80s-110s It is dry;
Last layer melamine paper is covered in the first face of magnesia base material, the second face is covered with a layer equilibration paper, forms intermediate product;
Above-mentioned intermediate product are delivered to windrow mechanism by conveying mechanism so that multiple intermediate product are stacked, and suppress naturally 2min-30min;
Between the intermediate product are delivered to the two panels pressing plate of hot pressing mechanism by conveying mechanism, the pressure for adjusting hot pressing mechanism is 1.0kg/cm2-1.5kg/cm2, temperature is 190 DEG C -200 DEG C, suppresses 0.5h-5h under these conditions, forms semi-finished product;
The redundance at the semi-finished product edge is cut off, and removes the burr on surface, obtains the Environment-friendlymagnesium magnesium oxide decorative panel.
2. the preparation method of Environment-friendlymagnesium magnesium oxide decorative panel according to claim 1, which is characterized in that the magnesia base material Sanding is first to use the sand paper of 80 mesh to carry out sanding, then carry out sanding using the sand paper of 120 mesh, finally uses the sand paper of 180 mesh Carry out sanding.
3. the preparation method of Environment-friendlymagnesium magnesium oxide decorative panel according to claim 1, which is characterized in that the magnesia base material Include the component of following parts by weight:100 parts of magnesia, 25-50 parts of anhydrous magnesium chloride, 10-15 parts of sawdust, 10-15 parts of flyash, 3-10 parts of zeolite, 7-15 parts of calcium oxide, 0.5-1 parts of calcium stearate, 30-50 parts of Adlerika, 3-10 parts of foaming agent, fire retardant 2-8 parts, 5-15 parts of foaming control agent.
4. the preparation method of Environment-friendlymagnesium magnesium oxide decorative panel according to claim 3, which is characterized in that the magnesia base material Include the component of following parts by weight:100 parts of magnesia, 40 parts of anhydrous magnesium chloride, 12 parts of sawdust, 12 parts of flyash, 8 parts of zeolite, 10 parts of calcium oxide, 0.8 part of calcium stearate, 40 parts of Adlerika, 7 parts of foaming agent, 5 parts of fire retardant, 10 parts of foaming control agent.
5. the preparation method of Environment-friendlymagnesium magnesium oxide decorative panel according to claim 3 or 4, which is characterized in that the magnesia The preparation method of base material is:
Magnesia, anhydrous magnesium chloride, calcium oxide, Adlerika, foaming agent and foaming control agent are mixed, juxtaposition In being stirred in closed container, it is filled with gas in whipping process, bubble is formed in the slurry of stirring;
Sawdust, flyash, zeolite, calcium stearate, fire retardant are added in above-mentioned closed container, 50 DEG C -60 DEG C is heated to, goes forward side by side Row stirring obtains raw material slurry;
Above-mentioned raw materials are starched and are added in the mold of press, heating mould is to 100 DEG C -120 DEG C, when keeping temperature 5h-7h, after cooling It takes out, obtains semi-finished product;
The semi-finished product are stacked, place -5 days 3 days naturally at room temperature to get the magnesia base material.
6. the preparation method of Environment-friendlymagnesium magnesium oxide decorative panel according to claim 1, which is characterized in that the rotating roller includes First rotating roller, the second rotating roller and third rotating roller, 80 the first sand paper of purpose of winding in first rotating roller, described 120 the second sand paper of purpose of winding in two rotating rollers, the third sand paper of 180 mesh of winding in the third rotating roller.
7. the preparation method of Environment-friendlymagnesium magnesium oxide decorative panel according to claim 1, which is characterized in that windrow mechanism packet Include liftable folding frame, the windrow board on the folding frame, the transmission rolling being installed on the windrow board Wheel, the windrow board are connected with the conveying mechanism;The folding frame includes the folding for being separately connected the board both sides Leg and hydraulic cylinder, the folding leg include first leg and the second supporting leg, and the first leg is pivotally connected with the second supporting leg, two The first leg of the folding leg is connected by a connecting rod, and the fixing end of the hydraulic cylinder is fixedly connected with the connecting rod, The movable end of the hydraulic cylinder is connect with second supporting leg, when hydraulic cylinder action, can drive the folding leg fold or It opens, folding leg board decline when folding, folding leg board rising when opening.
8. the preparation method of Environment-friendlymagnesium magnesium oxide decorative panel according to claim 1, which is characterized in that windrow mechanism packet Rickstand, the portal frame being located at the rickstand and suction component are included, the rickstand is equipped with material wheel;Described gantry Frame includes the spreader of the column and the connection column set on the rickstand both sides, and the spreader is equipped with sliding rail;It is described Suction component includes that connecting rod and the windrow sucker positioned at the connection boom end, the windrow sucker are equipped with several windrows Suction nozzle, the connecting rod are connect with a sliding part, and the sliding part is slidably connected with the sliding rail.
9. the preparation method of Environment-friendlymagnesium magnesium oxide decorative panel according to claim 1, which is characterized in that windrow mechanism packet Liftable transport platform, bearing frame and several cylinders are included, the transport platform is equipped with several delivery wheels;The bearing frame is set to The top of the transport platform, the bearing frame include sequentially connected first side, second side, third side and the 4th side Side, the second side, four side are flexibly connected with the first side, third side respectively, the cylinder and described the Dual side-edge, four side connection, for drive the second side, four side towards close to or away from the first side, It moves in the direction of third side;Several conveying rollers are respectively equipped on the inside of the second side of the bearing frame and four side, There is gap between conveying roller at the second side and four side.
CN201610613126.5A 2016-07-28 2016-07-28 The preparation method of Environment-friendlymagnesium magnesium oxide decorative panel Active CN106242489B (en)