CN106242436A - A kind of energy-conservation dry-mixed plastering mortar and manufacture method - Google Patents
A kind of energy-conservation dry-mixed plastering mortar and manufacture method Download PDFInfo
- Publication number
- CN106242436A CN106242436A CN201610762962.XA CN201610762962A CN106242436A CN 106242436 A CN106242436 A CN 106242436A CN 201610762962 A CN201610762962 A CN 201610762962A CN 106242436 A CN106242436 A CN 106242436A
- Authority
- CN
- China
- Prior art keywords
- sand
- energy
- machine
- plastering mortar
- mixed plastering
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
A kind of energy-conservation dry-mixed plastering mortar of the present invention and manufacture method; sand difficulty is adopted in order to solve natural sand; the adverse effect of heavy damage ecological balance; in order to preferably protect environment barren rock sand to replace partial natural sands, remaining micropowder replaces admixture, is configured to a kind of energy-conservation motar; solve natural sand well and adopt sand difficulty; the adverse effect of heavy damage ecological balance, preferably protection environment barren rock sand replaces partial natural sands, and remaining micropowder replaces admixture.
Description
Technical field
The present invention relates to building material field, particularly relate to a kind of energy-conservation motar, a kind of energy-conservation
Dry-mixed plastering mortar and manufacture method.
Background technology
Dry-mixed plastering mortar with high grade cement for master bond base material, the river sand accurately sieving and drying, be equipped with high-quality
Water-keeping thickening material, through accurate measurement dispensing, uses forced double-axis blender to be mixed, and is to use high-quality polymerization
The improvement of special dry powder and mortar that thing design produces, need only be stirred can be used with machinery on request after building site adds water.Mesh
Before, in dry-mixed plastering mortar, major part uses natural river sand, natural river sand shortage of resources, adopts sand destructible ecological environment, due to
Natural river sand rise in price in recent years so that supply bottleneck.
Summary of the invention
The invention aims to solve natural sand and adopt sand difficulty, the adverse effect of heavy damage ecological balance, in order to more
Good protection environment barren rock sand replaces partial natural sands, and remaining micropowder replaces admixture, is configured to a kind of energy-conservation plastering
Mortar.
The technical scheme that the present invention takes is:
A kind of energy-conservation dry-mixed plastering mortar and manufacture method, every raw material that test uses:
1. cement (32.5 grades of PC cement),
2. admixture (the remaining micropowder of sand processed),
3. Machine-made Sand (barren rock sand),
4. natural sand (medium sand),
5. additive (densification powder),
The most every raw material is siccative.
Referring specifically to scalar is:
Project | Grade or ratio |
Dry-mixed plastering mortar strength grade | DPM5-DPM20 |
32.5 grades of PC cement | 13.0%-21.0% |
Additive (densification powder) | 0.7%-0.8% |
The remaining micropowder of sand processed | 0.8%-7.5% |
Barren rock sand (Machine-made Sand) | 20%-40% |
Natural river sand | 32.2%-60% |
First barren rock is carried out sand processed by specialty sand making machine, screen by vibrosieve, carry out classification, then sand by powder concentrator
Putting in storage respectively with powder, natural river sand is dried by dedicated drying machine, is then selected into storehouse by Vibration Screen.Product is through micro computer essence
Really metering, after mixing and stirring, by the regulation detection of JGJ/T70-2009 building mortar key property method.
Beneficial effect acquired by the present invention:
The present invention solves natural sand well and adopts sand difficulty, the adverse effect of heavy damage ecological balance, preferably protects
Retaining ring border barren rock sand replaces partial natural sands, and remaining micropowder replaces admixture.
The ultimate principle of the present invention and principal character and advantages of the present invention have more than been shown and described.The technology of the industry
Personnel, it should be appreciated that the present invention is not restricted to the described embodiments, simply illustrating this described in above-described embodiment and description
The principle of invention, without departing from the spirit and scope of the present invention, the present invention also has various changes and modifications, and these become
Change and improvement both falls within scope of the claimed invention.Claimed scope by appending claims and
Equivalent defines.
Detailed description of the invention
Below in conjunction with specific embodiment, the invention will be further described, the illustrative examples invented at this and explanation
It is used for explaining the present invention, but not as a limitation of the invention.
Every raw material that test uses:
1. cement (32.5 grades of PC cement),
2. admixture (the remaining micropowder of sand processed),
3. Machine-made Sand (barren rock sand),
4. natural sand (medium sand),
5. additive (densification powder),
The most every raw material is siccative.
Referring specifically to scalar is:
Project | Grade or ratio |
Dry-mixed plastering mortar strength grade | DPM5-DPM20 |
32.5 grades of PC cement | 13.0%-21.0% |
Additive (densification powder) | 0.7%-0.8% |
The remaining micropowder of sand processed | 0.8%-7.5% |
Barren rock sand (Machine-made Sand) | 20%-40% |
Natural river sand | 32.2%-60% |
First barren rock is carried out sand processed by specialty sand making machine, screen by vibrosieve, carry out classification, then sand by powder concentrator
Putting in storage respectively with powder, natural river sand is dried by dedicated drying machine, is then selected into storehouse by Vibration Screen.Product is through micro computer essence
Really metering, after mixing and stirring, by the regulation detection of JGJ/T70-2009 building mortar key property method.
Claims (6)
1. an energy-conservation dry-mixed plastering mortar, it is characterised in that: every raw-material proportion is 32.5 grades of PC cement 13.0%-
21.0%, admixture 0.8%-7.5%, medium sand 32.2%-60%, additive 0.7%-0.8%, Machine-made Sand 20%-40% with
Upper every raw material is siccative.
A kind of energy-conservation dry-mixed plastering mortar the most according to claim 1, it is characterised in that described Machine-made Sand is barren rock system
Sand.
A kind of energy-conservation dry-mixed plastering mortar the most according to claim 1, it is characterised in that described medium sand is natural river
Sand.
A kind of energy-conservation dry-mixed plastering mortar the most according to claim 1, it is characterised in that described additive is thickening
Powder.
A kind of energy-conservation dry-mixed plastering mortar the most according to claim 1, it is characterised in that described admixture is more than sand processed
Stay micropowder.
6. an energy-conservation dry-mixed plastering mortar manufacture method, it is characterised in that: comprise the steps:
A. processing mechanism sand: first barren rock is carried out sand processed by specialty sand making machine, with vibrosieve screening, is carried out point by powder concentrator
Level, obtains Machine-made Sand and the remaining micropowder of sand processed, and then Machine-made Sand and the remaining micropowder of sand processed are put in storage respectively;
B. medium sand is processed: medium sand is dried by dedicated drying machine, is then selected into storehouse by Vibration Screen;
C. mix and blend: by 32.5 grades of PC cement, admixture, medium sand, additive, Machine-made Sand through micro computer accurate measurement, pour into
In mixing and blending machine after mixing and stirring, making finished product, finished product presses JGJ/T70-2009 building mortar key property method rule
Regular inspection is surveyed.