CN106183517A - Promote technique and the electronic equipment of water depositing process coating surface silk-screen adhesive force - Google Patents
Promote technique and the electronic equipment of water depositing process coating surface silk-screen adhesive force Download PDFInfo
- Publication number
- CN106183517A CN106183517A CN201610592602.XA CN201610592602A CN106183517A CN 106183517 A CN106183517 A CN 106183517A CN 201610592602 A CN201610592602 A CN 201610592602A CN 106183517 A CN106183517 A CN 106183517A
- Authority
- CN
- China
- Prior art keywords
- water
- silk
- coating surface
- adhesive force
- depositing process
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The present invention discloses a kind of technique promoting water depositing process coating surface silk-screen adhesive force, relates to product surface processing technology field.The technique of this lifting water depositing process coating surface silk-screen adhesive force includes water depositing process and the silk screen printing process carrying out plastic cement material, roughening process process was carried out, to strengthen the adhesion between plastic surface and water plating coating before plastic cement material is carried out water depositing process process.Meanwhile, housing prepared by a kind of technique using this lifting water depositing process coating surface silk-screen adhesive force and the electronic equipment with this housing are also disclosed.Invention enhances the adhesion between plastic surface and water plating coating, improve water depositing process coating surface silk-screen adhesive force, solve the existing water depositing process caducous problem of coating surface silk-screen.
Description
Technical field
The present invention relates to product surface processing technology field, particularly relate to a kind of lifting water depositing process coating surface silk-screen attached
Electronic equipment prepared by the technique puted forth effort and the technique using this lifting water depositing process coating surface silk-screen adhesive force.
Background technology
Current product, for the aesthetic property designed, it would be desirable at the water plating coating surface silk formed through water depositing process
Print some patterns or word.But, existing water depositing process coating surface silk-screen poor adhesive force, the pattern of silk-screen or word are not
Can be perfectly adhered to water depositing process coating surface, it is easy to come off, the appearance power and the quality that have had a strong impact on product are wanted
Ask.
Summary of the invention
First purpose of the present invention is to propose a kind of technique promoting water depositing process coating surface silk-screen adhesive force, to solve
The certainly existing water depositing process caducous problem of coating surface silk-screen.
Second object of the present invention is that proposition is a kind of uses above-mentioned lifting water depositing process coating surface silk-screen adhesive force
Electronic equipment prepared by technique.
For reaching this purpose, the present invention by the following technical solutions:
A kind of technique promoting water depositing process coating surface silk-screen adhesive force, including the water depositing process carrying out plastic cement material
And silk screen printing process, before plastic cement material is carried out water depositing process process, carry out roughening process process, with strengthen plastic surface with
Adhesion between water plating coating.
As the preferred version of a kind of technique promoting water depositing process coating surface silk-screen adhesive force, comprise the following steps:
Material is prepared by injection molding process;
Material is carried out roughening process process;
Material is carried out water depositing process process;
Water plating coating is carried out silk screen printing process process;
Anti-oxidant treatment obtains product.
As the preferred version of a kind of technique promoting water depositing process coating surface silk-screen adhesive force, described by being molded into
Type technique prepares material particularly as follows: use ABS material by injection mold injection mo(u)lding, obtains product material.
As the preferred version of a kind of technique promoting water depositing process coating surface silk-screen adhesive force, described by injection
After moulding process prepares material, further comprising the steps of before material is carried out roughening process process: material is surpassed
Sound wave oil removal treatment.
As the preferred version of a kind of technique promoting water depositing process coating surface silk-screen adhesive force, described material is carried out
Water depositing process processes particularly as follows: use trivalent chromium water plating solution that material carries out water depositing process process, and material surface forms water plating and is coated with
Layer.
As the preferred version of a kind of technique promoting water depositing process coating surface silk-screen adhesive force, described, material is entered
After row water depositing process processes, further comprising the steps of before water plating coating is carried out silk screen printing process process: after water plating, to use
Hot water by the water plating solution of ultrasonic waves for cleaning material remained on surface.
As the preferred version of a kind of technique promoting water depositing process coating surface silk-screen adhesive force, described to water plating coating
Carry out silk screen printing process process to comprise the following steps:
Material water plating coating surface is carried out laser carving process, carves out pattern or the character area of silk-screen;
The laser carving region of material is carried out ink printing process.
As the preferred version of a kind of technique promoting water depositing process coating surface silk-screen adhesive force, the described radium to material
Carving region carries out ink printing process and comprises the following steps:
Prepare ink liquid;
The ink liquid of preparation is passed through the half tone even print laser carving region on water plating coating surface.
As the preferred version of a kind of technique promoting water depositing process coating surface silk-screen adhesive force, described anti-oxidant treatment
Obtain product particularly as follows: be baked to ink liquid to be in drying regime, to whole product surface spray coating antioxidant, finally give product
Product.
A kind of electronic equipment, described electronic equipment uses lifting water depositing process coating surface silk-screen as described above attachment
The technique of power is prepared from.
The invention have the benefit that
The present invention proposes a kind of technique promoting water depositing process coating surface silk-screen adhesive force and uses lifting water depositing process
Electronic equipment prepared by the technique of coating surface silk-screen adhesive force, the present invention is before carrying out water depositing process process to plastic cement material
Carry out roughening process process, enhance the adhesion between plastic surface and water plating coating, improve water depositing process coating surface
Silk-screen adhesive force, solves the existing water depositing process caducous problem of coating surface silk-screen.
Accompanying drawing explanation
Fig. 1 is the flow process of the technique promoting water depositing process coating surface silk-screen adhesive force that the embodiment of the present invention two provides
Figure.
Detailed description of the invention
Technical scheme and the technique effect reached for making to present invention solves the technical problem that, using are clearer, below
By combining accompanying drawing, the technical scheme of the embodiment of the present invention is described in further detail, it is clear that described embodiment is only
It is a part of embodiment of the present invention rather than whole embodiments.Based on the embodiment in the present invention, those skilled in the art exist
Do not make the every other embodiment obtained under creative work premise, broadly fall into the scope of protection of the invention.
Embodiment one
The present embodiment proposes the first technique promoting water depositing process coating surface silk-screen adhesive force, and it includes plastic cement element
Water depositing process that material is carried out and silk screen printing process, carried out roughening process process before plastic cement material is carried out water depositing process process,
To strengthen the adhesion between plastic surface and water plating coating.
Comparing with existing water depositing process coating surface silk screen printing process, the present embodiment is carrying out water plating work to plastic cement material
Skill carries out roughening process process before processing, and enhances the adhesion between plastic surface and water plating coating, improves water plating work
Skill coating surface silk-screen adhesive force, solves the existing water depositing process caducous problem of coating surface silk-screen.
Embodiment two
The present embodiment proposes the second and promotes the technique of water depositing process coating surface silk-screen adhesive force, as it is shown in figure 1, include
Following steps:
Material is prepared by injection molding process.
Concrete, use ABS material by injection mold injection mo(u)lding, obtain product material.
Material is carried out ultrasonic oil removal process, it is ensured that material cleans up.
Material is carried out roughening process process, enhances the good combination power of plastic surface and water plating coating.
Concrete, the material after oil removing is put into equipped with chromic anhydride 350-400g/L and the roughening of sulphuric acid 350-400g/L solution
In groove, it is roughened 7-15 minute under 66-70 DEG C of air stirring, and sets up trivalent chromium electrolysis unit.The optional pottery of electrolysis unit
Diaphragm electrolysis apparatus etc., this device can control trivalent chromium in the range of 0-10g/L, make roughening steady quality.Chromium mist can be set up return
Receiving apparatus, reclaims the chromium mist that roughening groove evaporates.
Roughening process processes and improves water depositing process coating surface silk-screen adhesive force, solves existing water depositing process coating table
The caducous problem of face silk-screen.
Material is carried out water depositing process process.
Concrete, use trivalent chromium water plating solution that material carries out water depositing process process, material surface forms one layer of water plating and is coated with
Layer.
After water plating, use hot water and by the water plating solution of ultrasonic waves for cleaning material remained on surface.Use ultrasonic waves for cleaning, clearly
Wash better.
Water plating coating is carried out silk screen printing process process, is greatly improved appearance power and the class sense of product.
Concrete, silk screen printing process comprises the following steps:
Material water plating coating surface is carried out laser carving process, carves out pattern or the character area of silk-screen;Radium to material
Carving region carries out ink printing process.
Printing treatment mainly comprises the steps for preparing ink liquid;The ink liquid of preparation is existed by half tone even print
The laser carving region on water plating coating surface.
Wherein, ink liquid is to use firming agent to form according to part by weight 1:10 hybrid modulation with water plating type ink.
Anti-oxidant treatment obtains product.
Concrete, it is baked to ink liquid and is in drying regime, to whole product surface spray coating antioxidant, finally give product
Product.The product of final gained has stronger corrosion resistance and ruggedness, and service life is long.
The present embodiment proposes a kind of housing, and this housing is to use the lifting water plating work as described in embodiment one or embodiment two
The technique of skill coating surface silk-screen adhesive force is prepared from.This housing be disposed with from the bottom to top material layer, roughening metal level,
Water plating coating, ink printed layer and anti oxidation layer.It is attached that the housing using above-mentioned technique to prepare improves water plating coating surface silk-screen
Put forth effort, strengthen the adhesion between material and water plating coating, it is to avoid the water plating coating surface caducous problem of silk-screen.
The present embodiment proposes a kind of electronic equipment, and this electronic equipment has housing as described above.Wherein, electronics sets
Standby can be the electric equipments such as mobile phone, computer, audio amplifier, refrigerator, air-conditioning, washing machine.
To describe the know-why of the present invention in conjunction with specific embodiments.These describe and are intended merely to explain that the present invention's is former
Reason, and limiting the scope of the invention can not be construed to by any way.Based on explanation herein, those skilled in the art
Member need not pay performing creative labour and can associate other detailed description of the invention of the present invention, and these modes fall within this
Within the protection domain of invention.
Claims (10)
1. the technique promoting water depositing process coating surface silk-screen adhesive force, including the water depositing process that plastic cement material is carried out and
Silk screen printing process, it is characterised in that carried out roughening process process before plastic cement material is carried out water depositing process process, moulds to strengthen
Adhesion between glue surface and water plating coating.
The technique of lifting water depositing process coating surface silk-screen adhesive force the most according to claim 1, it is characterised in that include
Following steps:
Material is prepared by injection molding process;
Material is carried out roughening process process;
Material is carried out water depositing process process;
Water plating coating is carried out silk screen printing process process;
Anti-oxidant treatment obtains product.
The technique of lifting water depositing process coating surface silk-screen adhesive force the most according to claim 2, it is characterised in that described
Prepare material by injection molding process particularly as follows: use ABS material by injection mold injection mo(u)lding, obtain product material.
The technique of lifting water depositing process coating surface silk-screen adhesive force the most according to claim 2, it is characterised in that in institute
State after preparing material by injection molding process, further comprising the steps of before material is carried out roughening process process: right
Material carries out ultrasonic oil removal process.
The technique of lifting water depositing process coating surface silk-screen adhesive force the most according to claim 2, it is characterised in that described
Material is carried out water depositing process process particularly as follows: use trivalent chromium water plating solution that material carries out water depositing process process, material surface
Form water plating coating.
The technique of lifting water depositing process coating surface silk-screen adhesive force the most according to claim 2, it is characterised in that in institute
State after material is carried out water depositing process process, further comprising the steps of before water plating coating is carried out silk screen printing process process:
After water plating, use hot water and by the water plating solution of ultrasonic waves for cleaning material remained on surface.
The technique of lifting water depositing process coating surface silk-screen adhesive force the most according to claim 2, it is characterised in that described
Water plating coating carries out silk screen printing process process comprise the following steps:
Material water plating coating surface is carried out laser carving process, carves out pattern or the character area of silk-screen;
The laser carving region of material is carried out ink printing process.
The technique of lifting water depositing process coating surface silk-screen adhesive force the most according to claim 7, it is characterised in that described
The laser carving region of material carries out ink printing process and comprise the following steps:
Prepare ink liquid;
The ink liquid of preparation is passed through the half tone even print laser carving region on water plating coating surface.
The technique of lifting water depositing process coating surface silk-screen adhesive force the most according to claim 2, it is characterised in that described
Anti-oxidant treatment obtains product particularly as follows: be baked to ink liquid to be in drying regime, to whole product surface spray coating antioxidant,
Finally give product.
10. an electronic equipment, it is characterised in that described electronic equipment uses the lifting as described in any one of claim 1 to 9
The technique of water depositing process coating surface silk-screen adhesive force is prepared from.