CN106078529B - A method of handling bathroom cabinet plank using bottom abrasive material - Google Patents
A method of handling bathroom cabinet plank using bottom abrasive material Download PDFInfo
- Publication number
- CN106078529B CN106078529B CN201610384250.9A CN201610384250A CN106078529B CN 106078529 B CN106078529 B CN 106078529B CN 201610384250 A CN201610384250 A CN 201610384250A CN 106078529 B CN106078529 B CN 106078529B
- Authority
- CN
- China
- Prior art keywords
- board surface
- abrasive material
- high pressure
- slurry
- parts
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Active
Abstract
The present invention provides a kind of method handling bathroom cabinet plank using bottom abrasive material, and steps are as follows:Suitable water is added into bottom abrasive material, mechanical agitation 5 minutes or more, slurry is made, then slurry is pumped into high steam spray gun, slurry lasting stirring during being pumped into, slurry is broken up by high steam in high steam spray gun and goes out with jet-impingement, and high pressure draught directly acts on board surface, including polishing stage and spraying stage in a manner of uniformly strafing.The bottom abrasive material of the application is using high steam as carrier, it is injected in board surface, burnishing action first is formed to board surface, fine and close bottom is formed in board surface again, as the process layer between batch grieshoch or paint low layer and plank, the air of board surface can be emptied, plank is avoided to degenerate, adhesion strength is strong, as transition zone, can avoid batch grieshoch or paint low layer and is detached from plank.
Description
Technical field
The present invention relates to bathroom cabinet production technology field more particularly to a kind of handling bathroom cabinet plank using bottom abrasive material
Method.
Background technology
Bathroom cabinet is placed on the cabinet used in bathroom, can be chronically in the environment of dark humidity, wooden boards make
Made of cabinet the problems such as being easy to happen mould rotten deformation.Wooden boards cooperating microorganisms in the environment of darkness moistening, lead to plate
Batch grieshoch or priming paint on material surface are easy to fall off.In process, surface adhesion has various greasy dirts, particle sundries etc. to plank,
The problems such as being mixed in and criticize between grieshoch or priming paint and plank, being easy to cause layering, gas shell.And wooden material surface does not pass through
Polishing, the poor adhesion with batch between grieshoch or priming paint, is also susceptible to phenomena such as falling off.
Invention content
The purpose of the present invention is to provide a kind of methods handling bathroom cabinet plank using bottom abrasive material, to solve above-mentioned skill
Art problem.
The technical problems to be solved by the invention are realized using following technical scheme:
A method of handling bathroom cabinet plank using bottom abrasive material, which is characterized in that steps are as follows:
It is added suitable water into bottom abrasive material, mechanical agitation 5 minutes or more is made slurry, slurry is then pumped into height
It presses in steam spraying gun, slurry is lasting during being pumped into be stirred, and slurry is broken up by high steam in high steam spray gun and with gas
Stream ejects, and high pressure draught directly acts on board surface, including polishing stage and spraying stage in a manner of uniformly strafing,
Polishing stage, high pressure draught act on board surface in a manner of jet stream, air velocity be 550m/s~560m/s,
High pressure gas temperature is 130 DEG C~145 DEG C, jet length 15mm, the angle that high pressure draught acts on board surface is 15 °~
30°;
Spraying stage, high pressure draught act on board surface in a manner of jet stream, air velocity be 500m/s~510m/s,
High pressure gas temperature is 100 DEG C~115 DEG C, jet length 35mm, the angle that high pressure draught acts on board surface is 45 °~
75 °, the fine and close bottom that thickness is 0.15mm~0.25mm is formed in board surface.
The bottom abrasive material is made of the raw material of following parts by weight:
Carry 6 parts of silver-bearing copper silica gel, 1.3 parts of glass fiber powder, 0.6 part of sodium carboxymethylcellulose, 12 parts of tung oil, 5 parts of wood wax oil,
5.5 parts of silicon dioxide powder, 0.6 part of bamboo charcoal powder, 15 parts of land plaster, 1.2 parts of gas-phase silica;
Above-mentioned each raw material mixture in proportion stirs evenly under the conditions of 85 DEG C.
The wood wax oil is to carry silver-bearing copper wood wax oil, and the preparation method for carrying silver-bearing copper wood wax oil is:
It is 9: 12 that agitation and dropping concentration, which is the molar ratio of 0.2mol/l, in the wood wax oil for 10 volumes that temperature is 48 DEG C
Copper nitrate and silver nitrate solution amount to 6 volumes, temperature be 65 DEG C under the conditions of be stirred for 1.5h, above-mentioned mixed liquor is placed in super
Be ultrasonically treated 15min under acoustic frequency 40kHz, power 50W, taking-up be cooled to room temperature to get.
It is described carry silver-bearing copper silica gel preparation method be:Agitation and dropping concentration is equal in temperature is the silica gel of 48 DEG C of 10 volumes
The copper nitrate and silver nitrate solution that molar ratio for 0.2mol/l is 9: 12 amount to 4.5 volumes, under the conditions of temperature is 65 DEG C again
1.5h to be stirred, above-mentioned mixed liquor is placed under supersonic frequency 40kHz, power 50W and is ultrasonically treated 15min, taking-up is cooled to room temperature,
To obtain the final product.
In use, suitable water is added into bottom abrasive material, slurry is made, then by slurry in mechanical agitation 5 minutes or more
It is pumped into high steam spray gun, slurry is lasting during being pumped into be stirred, and slurry is broken up in high steam spray gun by high steam
And go out with jet-impingement, high pressure draught injects directly on board surface, under the effect of high pressure draught purging, board surface adherency
Sundries be eliminated, while board surface is humidified and is sterilized by vapor, the bottom abrasive material broken up in high pressure draught, to plank
Surface is played used in polishing, and board surface wood fibre is made more to be exposed, and increases board surface adhesion strength;
After air pressure reduces, bottom abrasive material uniform adhesion is in board surface, and well into the wood fibre of board surface
In, fill wood fibre between gap, the air of board surface is discharged, with bottom abrasive material adherency it is more and more, in wood
Plate surface adheres to one layer of fine and close bottom, after bottom solidification, you can criticizes ash on its surface or does paint low layer.
The beneficial effects of the invention are as follows:
The bottom abrasive material of the application is injected in board surface, is first formed to board surface using high steam as carrier
Burnishing action, then fine and close bottom is formed in board surface, as the process layer between batch grieshoch or paint low layer and plank, can arrange
The air of empty board surface, avoids plank from degenerating, and adhesion strength is strong, as transition zone, can avoid batch grieshoch or paint low layer and plank
It is detached from.
Specific implementation mode
In order to make the technical means, the creative features, the aims and the efficiencies achieved by the present invention be easy to understand, tie below
Specific embodiment is closed, the present invention is further explained, but following embodiments are only the preferred embodiment of the present invention, and not all.
Based on the implementation example in the implementation mode, those skilled in the art's obtained other realities without making creative work
Example is applied, protection scope of the present invention is belonged to.
A method of bathroom cabinet plank being handled using bottom abrasive material, is made of the raw material of following parts by weight:
Carry 6 parts of silver-bearing copper silica gel, 1.3 parts of glass fiber powder, 0.6 part of sodium carboxymethylcellulose, 12 parts of tung oil, 5 parts of wood wax oil,
5.5 parts of silicon dioxide powder, 0.6 part of bamboo charcoal powder, 15 parts of land plaster, 1.2 parts of gas-phase silica;
Above-mentioned each raw material mixture in proportion stirs evenly under the conditions of 85 DEG C.
Wood wax oil is to carry silver-bearing copper wood wax oil, and the preparation method for carrying silver-bearing copper wood wax oil is:
It is 9: 12 that agitation and dropping concentration, which is the molar ratio of 0.2mol/l, in the wood wax oil for 10 volumes that temperature is 48 DEG C
Copper nitrate and silver nitrate solution amount to 6 volumes, temperature be 65 DEG C under the conditions of be stirred for 1.5h, above-mentioned mixed liquor is placed in super
Be ultrasonically treated 15min under acoustic frequency 40kHz, power 50W, taking-up be cooled to room temperature to get.
Carry silver-bearing copper silica gel preparation method be:Agitation and dropping concentration is in temperature is the silica gel of 48 DEG C of 10 volumes
The copper nitrate and silver nitrate solution that the molar ratio of 0.2mol/l is 9: 12 amount to 4.5 volumes, are stirred again under the conditions of temperature is 65 DEG C
1.5h is mixed, above-mentioned mixed liquor is placed under supersonic frequency 40kHz, power 50W and is ultrasonically treated 15min, taking-up is cooled to room temperature, i.e.,
.
The method for handling board surface using bottom abrasive material, step are:Suitable water is added into bottom abrasive material, machinery stirs
It mixes 5 minutes or more, slurry is made, then slurry is pumped into high steam spray gun, slurry lasting stirring, slurry during being pumped into
It is broken up by high steam in high steam spray gun and goes out with jet-impingement, high pressure draught is directly made in a manner of uniformly strafing
For board surface, including polish stage and spraying stage,
Polishing stage, high pressure draught act on board surface in a manner of jet stream, air velocity be 550m/s~560m/s,
High pressure gas temperature is 130 DEG C~145 DEG C, jet length 15mm, the angle that high pressure draught acts on board surface is 15 °~
30°;
Spraying stage, high pressure draught act on board surface in a manner of jet stream, air velocity be 500m/s~510m/s,
High pressure gas temperature is 100 DEG C~115 DEG C, jet length 35mm, the angle that high pressure draught acts on board surface is 45 °~
75 °, the fine and close bottom that thickness is 0.15mm~0.25mm is formed in board surface.
The basic principles, main features and advantages of the present invention have been shown and described above.The technology of the industry
For personnel it should be appreciated that the present invention is not limited to the above embodiments, described in the above embodiment and specification is only the present invention
Preference, be not intended to limit the present invention, without departing from the spirit and scope of the present invention, the present invention also has various
Changes and improvements, these changes and improvements all fall within the protetion scope of the claimed invention.The claimed scope of the invention is by institute
Attached claims and its equivalent thereof.
Claims (3)
1. a kind of method handling bathroom cabinet plank using bottom abrasive material, which is characterized in that steps are as follows:
It is added suitable water into bottom abrasive material, slurry is made, and slurry, which is then pumped into high pressure, steams in mechanical agitation 5 minutes or more
In vapour spray gun, slurry is lasting during being pumped into be stirred, and slurry is broken up by high steam in high steam spray gun and sprayed with air-flow
It being shot out, high pressure draught directly acts on board surface, including polishing stage and spraying stage in a manner of uniformly strafing,
Polishing stage, high pressure draught act on board surface in a manner of jet stream, and air velocity is 550m/s~560m/s, high pressure
Gas temperature is 130 DEG C~145 DEG C, jet length 15mm, and the angle that high pressure draught acts on board surface is 15 °~30 °;
Spraying stage, high pressure draught act on board surface in a manner of jet stream, and air velocity is 500m/s~510m/s, high pressure
Gas temperature is 100 DEG C~115 DEG C, jet length 35mm, and the angle that high pressure draught acts on board surface is 45 °~75 °,
The fine and close bottom that thickness is 0.15mm~0.25mm is formed in board surface;
The bottom abrasive material is made of the raw material of following parts by weight:
Carry 6 parts of silver-bearing copper silica gel, 1.3 parts of glass fiber powder, 0.6 part of sodium carboxymethylcellulose, 12 parts of tung oil, 5 parts of wood wax oil, dioxy
5.5 parts of SiClx powder, 0.6 part of bamboo charcoal powder, 15 parts of land plaster, 1.2 parts of gas-phase silica;
Above-mentioned each raw material mixture in proportion stirs evenly under the conditions of 85 DEG C.
2. the method according to claim 1 for handling bathroom cabinet plank using bottom abrasive material, it is characterised in that:The haze tallow
To carry silver-bearing copper wood wax oil, the preparation method for carrying silver-bearing copper wood wax oil is oil:
The nitre that the molar ratio that agitation and dropping concentration is 0.2mol/l in the wood wax oil for 10 volumes that temperature is 48 DEG C is 9: 12
Sour copper and silver nitrate solution amount to 6 volumes, are stirred for 1.5h under the conditions of temperature is 65 DEG C, above-mentioned mixed liquor is placed in supersonic frequency
Be ultrasonically treated 15min under rate 40kHz, power 50W, taking-up be cooled to room temperature to get.
3. the method according to claim 1 for handling bathroom cabinet plank using bottom abrasive material, it is characterised in that:The load silver
The preparation method of copper silica gel is:Agitation and dropping concentration is mole of 0.2mol/l in temperature is the silica gel of 48 DEG C of 10 volumes
Than for 9: 12 copper nitrate and silver nitrate solution amount to 4.5 volumes, temperature be 65 DEG C under the conditions of be stirred for 1.5h, will it is above-mentioned mix
Liquid is closed to be placed under supersonic frequency 40kHz, power 50W and is ultrasonically treated 15min, taking-up be cooled to room temperature to get.