CN106009830A - Computer advertising art design sample surface protection coating material - Google Patents
Computer advertising art design sample surface protection coating material Download PDFInfo
- Publication number
- CN106009830A CN106009830A CN201610523361.3A CN201610523361A CN106009830A CN 106009830 A CN106009830 A CN 106009830A CN 201610523361 A CN201610523361 A CN 201610523361A CN 106009830 A CN106009830 A CN 106009830A
- Authority
- CN
- China
- Prior art keywords
- parts
- coating material
- art design
- design sample
- protective coating
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention relates to a computer advertising art design sample surface protection coating material. The material is composed of chlorinated polyethylene, polydimethylsiloxane, heterogeneous decanol polyoxyethylene ether, isocyanate, propylparaben, ethoxyquin, montmorillonoid, vinyl acetate, toluene diisocyanate, sorbic acid, phenolic resin diisopropanolamine, quartz powder, polyvinyl butyral, acrylic acid, tricresyl phosphate, aluminum hydroxide powder, dibasic lead phthalate, polyamide-imide, potassium acetate, tea saponin, 2,2-dipyridyl, tebuconazole, difenoconazole, stearin, octamethylcyclotetrasiloxane, nitrile rubber, triphenyl phosphate, trioctyl trimellitate, zinc borate and epoxidized soybean oil. The material has excellent flame retarding, acid and base resisting, anti-mildew and anti-microbial properties, and product performance is improved.
Description
Technical field
The present invention relates to a kind of computer Advertising art design sample surfaces protective coating material, belong to computer advertising art
Design field.
Background technology
" computer advertisement project ", neither " Computer Design ", is not " advertisement project ".Computer advertisement sets
Meter refers to use Computer Multimedia Technology design advertisement, and these advertisements comprise billboard, television advertising, network
The multiple advertisement form such as advertisement, outdoor advertising.In other words, computer advertisement refers to utilize Computer Multimedia Technology
By multimedia messages such as text required in advertisement, figure, image, animation, audio frequency, videos according to certain advertisement
Strategy, advertising creative are digitized gathering, make, process, compress, are stored in the wide of the processed such as application
Accuse performance.In computer Advertising art design, it is necessary to use some design samples, these design sample matrix materials are each
Different in order to preferably use model sample to show its effect, in order to protect these design samples, it is necessary to use
Suitably coating material.
Summary of the invention
It is an object of the invention to provide a kind of computer Advertising art design sample surfaces protective coating material, in order to more preferably
Realize the defencive function of computer Advertising art design sample surfaces protective coating material.
To achieve these goals, technical scheme is as follows.
A kind of computer Advertising art design sample surfaces protective coating material, is made up of the component of following mass fraction: chlorine
Change polyethylene 14~18 parts, polydimethylsiloxane 16~20 parts, isomery ten polyoxyethylenated alcohol 12~16 parts, different
Cyanate 10~14 parts, propylparaben 16~20 parts, ethoxy quinoline 12~16 parts, montmorillonite 10~14 parts,
Vinyl acetate 16~20 parts, toluene-2,4-diisocyanate 12~16 parts, sorbic acid 10~14 parts, phenolic resin two are different
Propanolamine 16~20 parts, silica flour 12~16 parts, polyvinyl butyral resin 12~16 parts, acrylic acid 10~14 parts,
Tricresyl phosphate 16~20 parts, aluminium-hydroxide powder 12~16 parts, Dythal 10~14 parts,
Polyamidoimide 16~20 parts, potassium acetate 12~16 parts, tea saponin 10~14 parts, 2,2-bipyridyl 16~20 parts,
Tebuconazole 12~16 parts, Difenoconazole 10~14 parts, tristerin 16~20 parts, prestox ring four silica
Alkane 12~16 parts, nitrile rubber triphenyl phosphate 12~16 parts, trioctyl trimellitate (TOTM) 12~16 parts, Firebrake ZB 12~
16 parts, epoxy soybean oil 12~16 parts.
Further, above computer Advertising art design sample surfaces protective coating material, by the group of following mass fraction
It is grouped into: chlorinated polyethylene 14 parts, polydimethylsiloxane 16 parts, isomery ten polyoxyethylenated alcohol 12 parts, isocyanide
Acid esters 10 parts, propylparaben 16 parts, ethoxy quinoline 12 parts, montmorillonite 10 parts, vinyl acetate 16 parts,
Toluene-2,4-diisocyanate 12 parts, sorbic acid 10 parts, phenolic resin diisopropanolamine (DIPA) 16 parts, silica flour 12 parts, poly-second
Enol butyral 12 parts, 10 parts of acrylic acid, tricresyl phosphate 16 parts, aluminium-hydroxide powder 12 parts, dibasic are adjacent
10 parts of phthalic acid lead, polyamidoimide 16 parts, potassium acetate 12 parts, tea saponin 10 parts, 2,2-bipyridyl 16
Part, Tebuconazole 12 parts, Difenoconazole 10 parts, tristerin 16 parts, octamethylcy-clotetrasiloxane 12 parts,
Nitrile rubber triphenyl phosphate 12 parts, trioctyl trimellitate (TOTM) 12 parts, Firebrake ZB 12 parts, epoxy soybean oil 12 parts.
Further, above computer Advertising art design sample surfaces protective coating material, by the group of following mass fraction
It is grouped into: chlorinated polyethylene 16 parts, polydimethylsiloxane 18 parts, isomery ten polyoxyethylenated alcohol 14 parts, isocyanide
Acid esters 12 parts, propylparaben 18 parts, ethoxy quinoline 14 parts, montmorillonite 12 parts, vinyl acetate 18 parts,
Toluene-2,4-diisocyanate 14 parts, sorbic acid 12 parts, phenolic resin diisopropanolamine (DIPA) 18 parts, silica flour 14 parts, poly-second
Enol butyral 14 parts, 12 parts of acrylic acid, tricresyl phosphate 18 parts, aluminium-hydroxide powder 14 parts, dibasic are adjacent
12 parts of phthalic acid lead, polyamidoimide 18 parts, potassium acetate 14 parts, tea saponin 12 parts, 2,2-bipyridyl 18
Part, Tebuconazole 14 parts, Difenoconazole 12 parts, tristerin 18 parts, octamethylcy-clotetrasiloxane 14 parts,
Nitrile rubber triphenyl phosphate 14 parts, trioctyl trimellitate (TOTM) 14 parts, Firebrake ZB 14 parts, epoxy soybean oil 14 parts.
Further, above computer Advertising art design sample surfaces protective coating material, by the group of following mass fraction
It is grouped into: chlorinated polyethylene 18 parts, polydimethylsiloxane 20 parts, isomery ten polyoxyethylenated alcohol 16 parts, isocyanide
Acid esters 14 parts, propylparaben 20 parts, ethoxy quinoline 16 parts, montmorillonite 14 parts, vinyl acetate 20 parts,
Toluene-2,4-diisocyanate 16 parts, sorbic acid 14 parts, phenolic resin diisopropanolamine (DIPA) 20 parts, silica flour 16 parts, poly-second
Enol butyral 16 parts, 14 parts of acrylic acid, tricresyl phosphate 20 parts, aluminium-hydroxide powder 16 parts, dibasic are adjacent
14 parts of phthalic acid lead, polyamidoimide 20 parts, potassium acetate 16 parts, tea saponin 14 parts, 2,2-bipyridyl 20
Part, Tebuconazole 16 parts, Difenoconazole 14 parts, tristerin 20 parts, octamethylcy-clotetrasiloxane 16 parts,
Nitrile rubber triphenyl phosphate 16 parts, trioctyl trimellitate (TOTM) 16 parts, Firebrake ZB 16 parts, epoxy soybean oil 16 parts.
Further, above computer Advertising art design sample surfaces protective coating material preparation method step is as follows:
(1) by the chlorinated polyethylene of described mass fraction, polydimethylsiloxane, isomery ten polyoxyethylenated alcohol, different
Cyanate, propylparaben, ethoxy quinoline, montmorillonite, vinyl acetate, toluene-2,4-diisocyanate, sorbic acid,
Phenolic resin diisopropanolamine (DIPA), silica flour, 2,2-bipyridyl, Tebuconazole, Difenoconazole, tristerin, eight
Methyl cyclotetrasiloxane, nitrile rubber triphenyl phosphate, trioctyl trimellitate (TOTM), Firebrake ZB, epoxy soybean oil are mixed
Closing, ultrasonic high speed dispersion, ultrasonic frequency is 20~40KHz, rate of dispersion 5000~about 5400r/min, dispersion
Time is 30~60min;
(2) polyvinyl butyral resin of described mass fraction, acrylic acid, tricresyl phosphate, aluminium hydrate powder are added
End, ultrasonic high speed dispersion, ultrasonic frequency is 20~35KHz, rate of dispersion 4800~about 5200r/min, dispersion
Time is 30~50min;
(3) Dythal of described mass fraction, polyamidoimide, potassium acetate, tea saponin are added,
Ultrasonic high speed dispersion, ultrasonic frequency is 20~30KHz, rate of dispersion 4600~about 4800r/min, jitter time
It is 20~40min;This product is prepared after mix homogeneously.
This beneficial effect of the invention is: the present invention relates to a kind of computer Advertising art design sample surfaces protective coating material
Material, composed of the following components: chlorinated polyethylene, polydimethylsiloxane, isomery ten polyoxyethylenated alcohol, isocyanates,
Propylparaben, ethoxy quinoline, montmorillonite, vinyl acetate, toluene-2,4-diisocyanate, sorbic acid, phenolic resin
Diisopropanolamine (DIPA), silica flour, polyvinyl butyral resin, acrylic acid, tricresyl phosphate, aluminium-hydroxide powder, disalt
Base lead phthalate, polyamidoimide, potassium acetate, tea saponin, 2,2-bipyridyl, Tebuconazole, Difenoconazole,
Tristerin, octamethylcy-clotetrasiloxane, nitrile rubber triphenyl phosphate, trioctyl trimellitate (TOTM), Firebrake ZB,
Epoxy soybean oil.This computer Advertising art design sample surfaces protective coating material preparation process method is simple, prepared
Product there is the most superior fire-retardant, acid and alkali-resistance, anti-mildew anti-microbial property, improve properties of product.
Detailed description of the invention
Below in conjunction with embodiment, the detailed description of the invention of the present invention is described, in order to be better understood from the present invention.
Embodiment 1
Computer Advertising art design sample surfaces protective coating material in the present embodiment, by the group of following mass fraction
It is grouped into: chlorinated polyethylene 14 parts, polydimethylsiloxane 16 parts, isomery ten polyoxyethylenated alcohol 12 parts, isocyanide
Acid esters 10 parts, propylparaben 16 parts, ethoxy quinoline 12 parts, montmorillonite 10 parts, vinyl acetate 16 parts,
Toluene-2,4-diisocyanate 12 parts, sorbic acid 10 parts, phenolic resin diisopropanolamine (DIPA) 16 parts, silica flour 12 parts, poly-second
Enol butyral 12 parts, 10 parts of acrylic acid, tricresyl phosphate 16 parts, aluminium-hydroxide powder 12 parts, dibasic are adjacent
10 parts of phthalic acid lead, polyamidoimide 16 parts, potassium acetate 12 parts, tea saponin 10 parts, 2,2-bipyridyl 16
Part, Tebuconazole 12 parts, Difenoconazole 10 parts, tristerin 16 parts, octamethylcy-clotetrasiloxane 12 parts,
Nitrile rubber triphenyl phosphate 12 parts, trioctyl trimellitate (TOTM) 12 parts, Firebrake ZB 12 parts, epoxy soybean oil 12 parts.
Above computer Advertising art design sample surfaces protective coating material preparation method step is as follows:
(1) by the chlorinated polyethylene of described mass fraction, polydimethylsiloxane, isomery ten polyoxyethylenated alcohol, different
Cyanate, propylparaben, ethoxy quinoline, montmorillonite, vinyl acetate, toluene-2,4-diisocyanate, sorbic acid,
Phenolic resin diisopropanolamine (DIPA), silica flour, 2,2-bipyridyl, Tebuconazole, Difenoconazole, tristerin, eight
Methyl cyclotetrasiloxane, nitrile rubber triphenyl phosphate, trioctyl trimellitate (TOTM), Firebrake ZB, epoxy soybean oil are mixed
Closing, ultrasonic high speed dispersion, ultrasonic frequency is 20kHz, rate of dispersion about 5400r/min, and jitter time is 60min;
(2) polyvinyl butyral resin of described mass fraction, acrylic acid, tricresyl phosphate, aluminium hydrate powder are added
End, ultrasonic high speed dispersion, ultrasonic frequency is 20kHz, rate of dispersion about 5200r/min, and jitter time is 50min;
(3) Dythal of described mass fraction, polyamidoimide, potassium acetate, tea saponin are added,
Ultrasonic high speed dispersion, ultrasonic frequency is 20kHz, rate of dispersion about 4800r/min, and jitter time is 40min;
This product is prepared after mix homogeneously.
Embodiment 2
Computer Advertising art design sample surfaces protective coating material in the present embodiment, by the component of following mass fraction
Composition: chlorinated polyethylene 16 parts, polydimethylsiloxane 18 parts, isomery ten polyoxyethylenated alcohol 14 parts, Carbimide.
Ester 12 parts, propylparaben 18 parts, ethoxy quinoline 14 parts, montmorillonite 12 parts, vinyl acetate 18 parts, two
TI 14 parts, sorbic acid 12 parts, phenolic resin diisopropanolamine (DIPA) 18 parts, silica flour 14 parts, polyethylene
Butyral 14 parts, 12 parts of acrylic acid, tricresyl phosphate 18 parts, aluminium-hydroxide powder 14 parts, dibasic neighbour's benzene
Diformazan lead plumbate 12 parts, polyamidoimide 18 parts, potassium acetate 14 parts, tea saponin 12 parts, 2,2-bipyridyl 18 parts,
Tebuconazole 14 parts, Difenoconazole 12 parts, tristerin 18 parts, octamethylcy-clotetrasiloxane 14 parts, butyronitrile
Rubber triphenyl phosphate 14 parts, trioctyl trimellitate (TOTM) 14 parts, Firebrake ZB 14 parts, epoxy soybean oil 14 parts.
Above computer Advertising art design sample surfaces protective coating material preparation method step is as follows:
(1) by the chlorinated polyethylene of described mass fraction, polydimethylsiloxane, isomery ten polyoxyethylenated alcohol, different
Cyanate, propylparaben, ethoxy quinoline, montmorillonite, vinyl acetate, toluene-2,4-diisocyanate, sorbic acid,
Phenolic resin diisopropanolamine (DIPA), silica flour, 2,2-bipyridyl, Tebuconazole, Difenoconazole, tristerin, eight
Methyl cyclotetrasiloxane, nitrile rubber triphenyl phosphate, trioctyl trimellitate (TOTM), Firebrake ZB, epoxy soybean oil are mixed
Closing, ultrasonic high speed dispersion, ultrasonic frequency is 30kHz, rate of dispersion about 5200r/min, and jitter time is 45min;
(2) polyvinyl butyral resin of described mass fraction, acrylic acid, tricresyl phosphate, aluminium hydrate powder are added
End, ultrasonic high speed dispersion, ultrasonic frequency is 27kHz, rate of dispersion about 5000r/min, and jitter time is 40min;
(3) Dythal of described mass fraction, polyamidoimide, potassium acetate, tea saponin are added,
Ultrasonic high speed dispersion, ultrasonic frequency is 25kHz, rate of dispersion about 4700r/min, and jitter time is 30min;
This product is prepared after mix homogeneously.
Embodiment 3
Computer Advertising art design sample surfaces protective coating material in the present embodiment, by the group of following mass fraction
It is grouped into: chlorinated polyethylene 18 parts, polydimethylsiloxane 20 parts, isomery ten polyoxyethylenated alcohol 16 parts, isocyanide
Acid esters 14 parts, propylparaben 20 parts, ethoxy quinoline 16 parts, montmorillonite 14 parts, vinyl acetate 20 parts,
Toluene-2,4-diisocyanate 16 parts, sorbic acid 14 parts, phenolic resin diisopropanolamine (DIPA) 20 parts, silica flour 16 parts, poly-second
Enol butyral 16 parts, 14 parts of acrylic acid, tricresyl phosphate 20 parts, aluminium-hydroxide powder 16 parts, dibasic are adjacent
14 parts of phthalic acid lead, polyamidoimide 20 parts, potassium acetate 16 parts, tea saponin 14 parts, 2,2-bipyridyl 20
Part, Tebuconazole 16 parts, Difenoconazole 14 parts, tristerin 20 parts, octamethylcy-clotetrasiloxane 16 parts,
Nitrile rubber triphenyl phosphate 16 parts, trioctyl trimellitate (TOTM) 16 parts, Firebrake ZB 16 parts, epoxy soybean oil 16 parts.
Above computer Advertising art design sample surfaces protective coating material preparation method step is as follows:
(1) by the chlorinated polyethylene of described mass fraction, polydimethylsiloxane, isomery ten polyoxyethylenated alcohol, different
Cyanate, propylparaben, ethoxy quinoline, montmorillonite, vinyl acetate, toluene-2,4-diisocyanate, sorbic acid,
Phenolic resin diisopropanolamine (DIPA), silica flour, 2,2-bipyridyl, Tebuconazole, Difenoconazole, tristerin, eight
Methyl cyclotetrasiloxane, nitrile rubber triphenyl phosphate, trioctyl trimellitate (TOTM), Firebrake ZB, epoxy soybean oil are mixed
Closing, ultrasonic high speed dispersion, ultrasonic frequency is 40kHz, rate of dispersion 5000r/min, and jitter time is 30min;
(2) polyvinyl butyral resin of described mass fraction, acrylic acid, tricresyl phosphate, aluminium hydrate powder are added
End, ultrasonic high speed dispersion, ultrasonic frequency is 35kHz, rate of dispersion 4800r/min, and jitter time is 30min;
(3) Dythal of described mass fraction, polyamidoimide, potassium acetate, tea saponin are added,
Ultrasonic high speed dispersion, ultrasonic frequency is 30kHz, rate of dispersion about 4600r/min, and jitter time is 20min;
This product is prepared after mix homogeneously.
Performance measurement is carried out for the product in embodiment 1, embodiment 2 and embodiment 3 and certain commercially available prod, measured
Data as shown in table 1.Fire protection flame retarding level estimate uses UL94 standard.
Table 1 the performance test results
Visible, product of the present invention has the most corrosion-resistant, fire protection flame retarding, anti-mildew, anti-microbial property.
The above is the preferred embodiment of the present invention, it is noted that come for those skilled in the art
Saying, under the premise without departing from the principles of the invention, it is also possible to make some improvements and modifications, these improvements and modifications also regard
For protection scope of the present invention.
Claims (5)
- null1. a computer Advertising art design sample surfaces protective coating material,It is characterized in that: be made up of the component of following mass fraction: chlorinated polyethylene 14~18 parts、Polydimethylsiloxane 16~20 parts、Isomery ten polyoxyethylenated alcohol 12~16 parts、Isocyanates 10~14 parts、Propylparaben 16~20 parts、Ethoxy quinoline 12~16 parts、Montmorillonite 10~14 parts、Vinyl acetate 16~20 parts、Toluene-2,4-diisocyanate 12~16 parts、Sorbic acid 10~14 parts、Phenolic resin diisopropanolamine (DIPA) 16~20 parts、Silica flour 12~16 parts、Polyvinyl butyral resin 12~16 parts、Acrylic acid 10~14 parts、Tricresyl phosphate 16~20 parts、Aluminium-hydroxide powder 12~16 parts、Dythal 10~14 parts、Polyamidoimide 16~20 parts、Potassium acetate 12~16 parts、Tea saponin 10~14 parts、2,2-bipyridyl 16~20 parts、Tebuconazole 12~16 parts、Difenoconazole 10~14 parts、Tristerin 16~20 parts、Octamethylcy-clotetrasiloxane 12~16 parts、Nitrile rubber triphenyl phosphate 12~16 parts、Trioctyl trimellitate (TOTM) 12~16 parts、Firebrake ZB 12~16 parts、Epoxy soybean oil 12~16 parts.
- nullComputer Advertising art design sample surfaces protective coating material the most according to claim 1,It is characterized in that: described computer Advertising art design sample surfaces protective coating material is made up of the component of following mass fraction: chlorinated polyethylene 14 parts、Polydimethylsiloxane 16 parts、Isomery ten polyoxyethylenated alcohol 12 parts、Isocyanates 10 parts、Propylparaben 16 parts、Ethoxy quinoline 12 parts、Montmorillonite 10 parts、Vinyl acetate 16 parts、Toluene-2,4-diisocyanate 12 parts、Sorbic acid 10 parts、Phenolic resin diisopropanolamine (DIPA) 16 parts、Silica flour 12 parts、Polyvinyl butyral resin 12 parts、10 parts of acrylic acid、Tricresyl phosphate 16 parts、Aluminium-hydroxide powder 12 parts、Dythal 10 parts、Polyamidoimide 16 parts、Potassium acetate 12 parts、Tea saponin 10 parts、2,2-bipyridyl 16 parts、Tebuconazole 12 parts、Difenoconazole 10 parts、Tristerin 16 parts、Octamethylcy-clotetrasiloxane 12 parts、Nitrile rubber triphenyl phosphate 12 parts、Trioctyl trimellitate (TOTM) 12 parts、Firebrake ZB 12 parts、Epoxy soybean oil 12 parts.
- null3. according to the computer Advertising art design sample surfaces protective coating material described in claim 1 to 2,It is characterized in that: described computer Advertising art design sample surfaces protective coating material is made up of the component of following mass fraction: chlorinated polyethylene 16 parts、Polydimethylsiloxane 18 parts、Isomery ten polyoxyethylenated alcohol 14 parts、Isocyanates 12 parts、Propylparaben 18 parts、Ethoxy quinoline 14 parts、Montmorillonite 12 parts、Vinyl acetate 18 parts、Toluene-2,4-diisocyanate 14 parts、Sorbic acid 12 parts、Phenolic resin diisopropanolamine (DIPA) 18 parts、Silica flour 14 parts、Polyvinyl butyral resin 14 parts、12 parts of acrylic acid、Tricresyl phosphate 18 parts、Aluminium-hydroxide powder 14 parts、Dythal 12 parts、Polyamidoimide 18 parts、Potassium acetate 14 parts、Tea saponin 12 parts、2,2-bipyridyl 18 parts、Tebuconazole 14 parts、Difenoconazole 12 parts、Tristerin 18 parts、Octamethylcy-clotetrasiloxane 14 parts、Nitrile rubber triphenyl phosphate 14 parts、Trioctyl trimellitate (TOTM) 14 parts、Firebrake ZB 14 parts、Epoxy soybean oil 14 parts.
- null4. according to the computer Advertising art design sample surfaces protective coating material described in claims 1 to 3,It is characterized in that: described computer Advertising art design sample surfaces protective coating material is made up of the component of following mass fraction: chlorinated polyethylene 18 parts、Polydimethylsiloxane 20 parts、Isomery ten polyoxyethylenated alcohol 16 parts、Isocyanates 14 parts、Propylparaben 20 parts、Ethoxy quinoline 16 parts、Montmorillonite 14 parts、Vinyl acetate 20 parts、Toluene-2,4-diisocyanate 16 parts、Sorbic acid 14 parts、Phenolic resin diisopropanolamine (DIPA) 20 parts、Silica flour 16 parts、Polyvinyl butyral resin 16 parts、14 parts of acrylic acid、Tricresyl phosphate 20 parts、Aluminium-hydroxide powder 16 parts、Dythal 14 parts、Polyamidoimide 20 parts、Potassium acetate 16 parts、Tea saponin 14 parts、2,2-bipyridyl 20 parts、Tebuconazole 16 parts、Difenoconazole 14 parts、Tristerin 20 parts、Octamethylcy-clotetrasiloxane 16 parts、Nitrile rubber triphenyl phosphate 16 parts、Trioctyl trimellitate (TOTM) 16 parts、Firebrake ZB 16 parts、Epoxy soybean oil 16 parts.
- Computer Advertising art design sample surfaces protective coating material the most according to claim 1, it is characterised in that: described computer Advertising art design sample surfaces protective coating material preparation method step is as follows:(1) by the chlorinated polyethylene of described mass fraction, polydimethylsiloxane, isomery ten polyoxyethylenated alcohol, isocyanates, propylparaben, ethoxy quinoline, montmorillonite, vinyl acetate, toluene-2,4-diisocyanate, sorbic acid, phenolic resin diisopropanolamine (DIPA), silica flour, 2, 2-bipyridyl, Tebuconazole, Difenoconazole, tristerin, octamethylcy-clotetrasiloxane, nitrile rubber triphenyl phosphate, trioctyl trimellitate (TOTM), Firebrake ZB, epoxy soybean oil is mixed, ultrasonic high speed dispersion, ultrasonic frequency is 20~40KHz, rate of dispersion about 5000~5400r/min, jitter time is 30~about 60min;(2) polyvinyl butyral resin of described mass fraction, acrylic acid, tricresyl phosphate, aluminium-hydroxide powder are added, ultrasonic high speed dispersion, ultrasonic frequency is 20~35KHz, and rate of dispersion is about 4800~5200r/min, and jitter time is 30~about 50min;(3) adding the Dythal of described mass fraction, polyamidoimide, potassium acetate, tea saponin, ultrasonic high speed dispersion, ultrasonic frequency is 20~30KHz, and rate of dispersion is about 4600~4800r/min, and jitter time is 20~about 40min;This product is prepared after mix homogeneously.