CN105904563B - A kind of processing method of wild jujube wood gold thread timber - Google Patents

A kind of processing method of wild jujube wood gold thread timber Download PDF

Info

Publication number
CN105904563B
CN105904563B CN201610477945.1A CN201610477945A CN105904563B CN 105904563 B CN105904563 B CN 105904563B CN 201610477945 A CN201610477945 A CN 201610477945A CN 105904563 B CN105904563 B CN 105904563B
Authority
CN
China
Prior art keywords
wild jujube
lumber
flat
jujube wood
grain
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201610477945.1A
Other languages
Chinese (zh)
Other versions
CN105904563A (en
Inventor
黄晓东
黄俊昆
刘雁
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Hubei thousand Sichuan doors and windows Co., Ltd.
Original Assignee
Fujian Agriculture and Forestry University
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Fujian Agriculture and Forestry University filed Critical Fujian Agriculture and Forestry University
Priority to CN201610477945.1A priority Critical patent/CN105904563B/en
Publication of CN105904563A publication Critical patent/CN105904563A/en
Application granted granted Critical
Publication of CN105904563B publication Critical patent/CN105904563B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The present invention relates to a kind of processing method of wild jujube wood gold thread timber.First, by wild jujube timber, bark and debris is removed, the wild jujube wood flat-grain lumber with mountain line is made after intercept;Secondly, wild jujube flat-grain lumber is after giant rinses, soaks dimethicone, soak again through warm water, dry after immerse in fool's bronze phenolic resin mixed liquor, the process such as pressurized dipping, dry, two-sided thicknesser processing, side gluing, large format wild jujube plain-sawed lumber jigsaw is made;Finally, repaired with fool's bronze edible vegetable oil mending paste, be sent into the fixed thick sanding of sander, it is compound with Solid Door framework, after japanning solidifies, the wild jujube Solid Door with beautiful gold thread decorative effect is made.This process technology handles through special process using aboundresources, cheap wild jujube timber, produces the wild jujube Solid Door with beautiful gold thread decorative effect, this technology is capable of the scientific and technological content and added value of product of General Promotion Solid Door industry.Therefore, there is vast potential for future development.

Description

A kind of processing method of wild jujube wood gold thread timber
Technical field
The invention belongs to wood processing field, and in particular to a kind of processing method of wild jujube wood gold thread timber.
Background technology
Wild jujube timber inverted " v " decorative pattern caused by its chord plane has by growth ring, material is stable, is unlikely to deform cracking, resistance to Rotten power is strong, while is easy to scrape, smooth surface, light after scraping, can absorb paint and colouring agent well, and easily glue Close.It is high-quality fitment material for family.
The technology of the present invention is handled, in wild jujube plain-sawed lumber using aboundresources, cheap wild jujube timber through special process Fool's bronze is injected in the pore for the beautiful mountain line pattern that material surface is formed, pore shape is relied on whole wild jujube flat-grain lumber surface Into continuous strip gold thread(Whole piece conduit is cut)With point-like Venus(Conduit is laterally cut off), produce with beautiful gold thread and gold The wild jujube Solid Door of star decorative effect, meet compatriots and open the door and see golden good hope and the hope to good life, this skill Art is capable of the scientific and technological content and added value of product of General Promotion Solid Door industry.Therefore, there is vast potential for future development.
The content of the invention
It is an object of the invention to provide a kind of processing method of wild jujube wood gold thread timber, this method using aboundresources, Cheap wild jujube timber, is handled through special process, in the pore for the beautiful mountain line pattern that wild jujube flat-grain lumber surface is formed Middle injection fool's bronze, relies on pore to form continuous strip gold thread on whole wild jujube flat-grain lumber surface(Whole piece conduit is cut) With point-like Venus(Conduit is laterally cut off), the wild jujube Solid Door with beautiful gold thread and Venus decorative effect is produced, is met Compatriots, which open the door, sees golden good hope and the hope to good life, and this technology is capable of the science and technology of General Promotion Solid Door industry Content and added value of product.Therefore, there is vast potential for future development.
The invention provides a kind of processing method of wild jujube wood gold thread timber, comprise the following steps:
Step 1:Fresh wild jujube timber is felled, removes the bark of appearance and other debris, wild jujube timber is cut into 2.2 meters The juggle of length;
Step 2:Wild jujube juggle is processed into the thick bands of 15mm using equipment such as sport car band saw, joiner pony hand-saw and thicknessers The wild jujube wood flat-grain lumber of mountain line, it is standby;
Step 3:After the wild jujube flat-grain lumber with mountain line made of giant rinsing step 2, by wild jujube plain-sawed lumber Material is put into tank, and adding the dimethicone of outsourcing makes wild jujube flat-grain lumber be completely submerged in oil, after soaking 5~10 hours Take out, be placed in 60~80 DEG C of warm water and soak again 1~2 hour, take out wild jujube flat-grain lumber, it is drained and standby;
Step 4:The wild jujube flat-grain lumber that step 3 treats is put into lumber kiln and dried, drying temperature 60-75 DEG C, 48~100 hours drying times, the moisture control of wild jujube flat-grain lumber is in 8-10wt% after drying;
Step 5:Take fool's gold ore(Pyrite FeS2), 200 mesh sieve are crossed after crushing, by fool's bronze:Outsourcing phenolic aldehyde Resin adhesive=30:70(Mass ratio)Mixing, stirs, standby;
Step 6:Wild jujube flat-grain lumber made of step 4 is placed in layer frame prefabricated in metal can and fixed, Fool's bronze-phenolic resin mixed liquor made of step 5 is poured into metal can, the liquid level of glue should be higher by wild jujube flat-grain lumber Stacking top layer about 20~30cm, close the opening of metal can;
Step 7:The adjustable speed motor on metal can top is started, the rotating speed of motor is controlled at 3000~4000 revs/min; The ball valve above closed metal tank with air compressor machine connecting tube is opened simultaneously to switch, open air compressor machine power switch and start to Injecting compressed air in closed metal tank, the Stress control of the pressure gauge on air compressor machine is in 0.5~1MPa;
Step 8:After closed pressurization 30~60 minutes, air compressor machine and adjustable speed motor power supply are closed, opens closed metal tank Opening, remaining fool's bronze-phenolic resin mixed liquor in closed metal tank is drawn back into storage glue groove with vane pump, by wild jujube string Cutting plate material takes out, and is put into special drip and drips glue on the net;
Step 9:After the glue for no longer occurring dripping downwards to be placed to the wild jujube flat-grain lumber for dripping online drips, by wild jujube plain-sawed lumber Material is sent into lumber kiln dry solidification, and the temperature of dry solidification is 135~145 DEG C, 24~48 hours dry solidification time, is done The moisture control of wild jujube flat-grain lumber is in 6~8wt% after dry;
Step 10:Dried wild jujube flat-grain lumber is sent into two-sided thicknesser, determines the wild jujube string that thickness is processed into thickness 13mm Cutting plate material;
Step 11:Tai Er splicing adhesives are brushed in wild jujube flat-grain lumber side thick 13mm, being sent into plate joggling apparatus after assembly is made Large format wild jujube plain-sawed lumber jigsaw;
Step 12:By fool's bronze of step 5:Edible vegetable oil=1:1(Mass ratio)Paste is stirred into after mixing, it is uniform with grey knife Ground blade coating unintelligible place of gold thread on large format wild jujube plain-sawed lumber jigsaw, treats that the compound of fool's bronze and edible vegetable oil fully solidifies Afterwards, it is thick to 12mm to be sent into the fixed thick sanding of sander;
Step 13:There is the wild jujube plain-sawed lumber panel and solid wood door frame of gold thread decorative effect using surface made of step 12 Frame is compound, and after japanning solidifies, the wild jujube Solid Door with beautiful gold thread decorative effect is made.
The purpose for rinsing wild jujube flat-grain lumber using giant in the step 3 is that the saw of plate surface is crushed into bits Remove, prevent above-mentioned chip from blocking timber pore during impregnating by pressure, influence final wild jujube flat-grain lumber surface gold thread Form effect.
Wild jujube flat-grain lumber is put into tank in the step 3, adding the dimethicone of outsourcing makes wild jujube plain-sawed lumber Material is completely submerged in oil, and the purpose of immersion is that the resinoid blocked in wild jujube wooden pipe hole can be dissolved using dimethicone The characteristics of, the pore passage in wild jujube wood is combed, is that fool's bronze-phenolic resin mixed liquor smoothly enters inside wild jujube wooden pipe hole Lay the first stone.
To ensure dimethicone to the abundant dissolving of the resinoid blocked in wild jujube wooden pipe hole in the step 3, Added after dimethicone should being heated to 60~80 DEG C, its to the dissolubility of resinoid that is blocked in wild jujube wooden pipe hole most It is good.
The wild jujube flat-grain lumber of completion dimethyl-silicon oil processing, which must be placed in 60~80 DEG C of warm water, in the step 3 soaks Bubble 1~2 hour, remove the dimethyl-silicon oil substances of plate surface adhesion;In order to more thoroughly remove the two of plate surface adhesion Methyl-silicone oil material, 0.1~0.2% sodium hydrate particle can be added in warm water(Mass ratio).
Outsourcing synvaren is water-soluble resin in the step 5, is provided by Foochow wood-based plate company, and it solidifies Thing content 53wt%, free formaldehyde content<0.15wt%, resin pH value 9.0.
Fool's bronze-phenolic resin mixed liquor is poured into metal can in the step 6, the liquid level of glue should be higher by wild jujube Flat-grain lumber stacking top layer about 20~30cm, it is defined, is prevented because adjusting by the buncher bottom that the generation of rotation liquid level is recessed at a high speed Speed motor rotates at a high speed, and the liquid surface hollow at metal can center is less than wild jujube flat-grain lumber stacking top layer, causes wild jujube flat-grain lumber The defects of local dipping effect is bad.
The adjustable speed motor on metal can top is started in the step 7, by the control of the rotating speed of motor 3000~4000 turns/ Minute, it is therefore an objective to prevent because the rotating speed of motor is too low, fool's bronze in impregnating agent fool bronze-phenolic resin mixed liquor is because certainly Reprecipitation gets off, and influences the dipping effect of wild jujube flat-grain lumber.
, can be with vane pump by closed gold to be cost-effective after the impregnation that wild jujube flat-grain lumber is completed in the step 8 Remaining fool's bronze-phenolic resin mixed liquor draws back storage glue groove reuse in category tank, deficiency part is available newly prepare it is stupid People's bronze-phenolic resin mixed liquor supplement.
By fool's bronze in the step 12:Edible vegetable oil=1:1(Mass ratio)Paste is stirred into after mixing, with grey knife equably Blade coating unintelligible place of gold thread on large format wild jujube plain-sawed lumber jigsaw, makes the gold thread that eventually appears on wild jujube plain-sawed lumber jigsaw clear It is clear coherent, increase the aesthetic of decoration wood door.
The advantage of the invention is that:This method is using aboundresources, cheap wild jujube timber, at special process Reason, fool's bronze is injected in the pore for the beautiful mountain line pattern that wild jujube flat-grain lumber surface is formed, in whole wild jujube plain-sawed lumber Material surface relies on pore to form continuous strip gold thread(Whole piece conduit is cut)With point-like Venus(Conduit is laterally cut off), produce Wild jujube Solid Door with beautiful gold thread and Venus decorative effect, meet compatriots and open the door and see the good hope of gold and to fine life Hope living, this technology are capable of the scientific and technological content and added value of product of General Promotion Solid Door industry.Therefore, have wide Development prospect.
Embodiment
For the further open rather than limitation present invention, below in conjunction with example, the present invention is described in further detail.
A kind of specific production stage of the processing method of wild jujube wood gold thread timber is:
Step 1:Fresh wild jujube timber is felled, removes the bark of appearance and other debris, wild jujube timber is cut into 2.2 meters The juggle of length;
Step 2:Wild jujube juggle is processed into the thick bands of 15mm using equipment such as sport car band saw, joiner pony hand-saw and thicknessers The wild jujube wood flat-grain lumber of mountain line, it is standby;
Step 3:After the wild jujube flat-grain lumber with mountain line made of giant rinsing step 2, by wild jujube plain-sawed lumber Material is put into tank, and adding the dimethicone of outsourcing makes wild jujube flat-grain lumber be completely submerged in oil, after soaking 5~10 hours Take out, be placed in 60~80 DEG C of warm water and soak again 1~2 hour, take out wild jujube flat-grain lumber, it is drained and standby;
Step 4:The wild jujube flat-grain lumber that step 3 treats is put into lumber kiln and dried, drying temperature 60-75 DEG C, 48~100 hours drying times, the moisture control of wild jujube flat-grain lumber is in 8-10wt% after drying;
Step 5:Take fool's gold ore(Pyrite FeS2), 200 mesh sieve, in mass ratio fool's bronze are crossed after crushing:Outside Purchase synvaren=30:70 mixing, stir, standby;
Step 6:Wild jujube flat-grain lumber made of step 4 is placed in layer frame prefabricated in metal can and fixed, Fool's bronze-phenolic resin mixed liquor made of step 5 is poured into metal can, the liquid level of glue should be higher by wild jujube flat-grain lumber Stacking top layer about 20~30cm, close the opening of metal can;
Step 7:The adjustable speed motor on metal can top is started, the rotating speed of motor is controlled at 3000~4000 revs/min; The ball valve above closed metal tank with air compressor machine connecting tube is opened simultaneously to switch, open air compressor machine power switch and start to Injecting compressed air in closed metal tank, the Stress control of the pressure gauge on air compressor machine is in 0.5~1MPa;
Step 8:After closed pressurization 30~60 minutes, air compressor machine and adjustable speed motor power supply are closed, opens closed metal tank Opening, remaining fool's bronze-phenolic resin mixed liquor in closed metal tank is drawn back into storage glue groove with vane pump, by wild jujube string Cutting plate material takes out, and is put into special drip and drips glue on the net;
Step 9:After the glue for no longer occurring dripping downwards to be placed to the wild jujube flat-grain lumber for dripping online drips, by wild jujube plain-sawed lumber Material is sent into lumber kiln dry solidification, and the temperature of dry solidification is 135~145 DEG C, 24~48 hours dry solidification time, is done The moisture control of wild jujube flat-grain lumber is in 6~8wt% after dry;
Step 10:Dried wild jujube flat-grain lumber is sent into two-sided thicknesser, determines the wild jujube string that thickness is processed into thickness 13mm Cutting plate material;
Step 11:Tai Er splicing adhesives are brushed in wild jujube flat-grain lumber side thick 13mm, being sent into plate joggling apparatus after assembly is made Large format wild jujube plain-sawed lumber jigsaw;
Step 12:By fool's bronze:Edible vegetable oil=1:1(Mass ratio)Paste is stirred into after mixing, is equably scratched with grey knife The unintelligible place of gold thread on large format wild jujube plain-sawed lumber jigsaw, after edible vegetable oil fully solidifies, the fixed thick sanding of sander is sent into 12mm It is thick;
Step 13:Using manufactured surface there is the wild jujube plain-sawed lumber panel of gold thread decorative effect and Solid Door framework to answer Close, after japanning solidifies, the wild jujube Solid Door with beautiful gold thread decorative effect is made.
Preferably, the purpose for rinsing wild jujube flat-grain lumber using giant in the step 3 is by the saw of plate surface Crush bits to remove, prevent above-mentioned chip from blocking timber pore during impregnating by pressure, influence final wild jujube flat-grain lumber table The formation effect of face gold thread.
Preferably, wild jujube flat-grain lumber is put into tank in the step 3, adding the dimethicone of outsourcing makes wild jujube Flat-grain lumber is completely submerged in oil, and the purpose of immersion is that the natural gum blocked in wild jujube wooden pipe hole can be dissolved using dimethicone The characteristics of shape material, the pore passage in wild jujube wood is combed, smoothly enter wild jujube wooden pipe for fool's bronze-phenolic resin mixed liquor Laid the first stone inside hole.
Preferably, in the step 3 to ensure dimethicone filling to the resinoid that is blocked in wild jujube wooden pipe hole Point dissolving, is added, it is to the resinoid that is blocked in wild jujube wooden pipe hole after dimethicone should being heated to 60~80 DEG C Dissolubility is best.
Preferably, the wild jujube flat-grain lumber for dimethyl-silicon oil processing being completed in the step 3 must be placed at 60~80 DEG C Soaked 1~2 hour in warm water, remove the dimethyl-silicon oil substances of plate surface adhesion;In order to more thoroughly remove plate surface The dimethyl-silicon oil substances of adhesion, 0.1~0.2% sodium hydrate particle can be added in warm water(Mass ratio).
Preferably, outsourcing synvaren is water-soluble resin in the step 5, and by Foochow, wood-based plate company carries For, its solidfied material content 53wt%, free formaldehyde content<0.15wt%, resin pH value 9.0.
Preferably, fool's bronze-phenolic resin mixed liquor is poured into metal can in the step 6, the liquid level of glue should Wild jujube flat-grain lumber stacking top layer about 20~30cm is higher by, is defined by the buncher bottom that the generation of rotation liquid level is recessed at a high speed, Prevent that the liquid surface hollow at metal can center is less than wild jujube flat-grain lumber stacking top layer, causes wild jujube because buncher rotates at a high speed The defects of flat-grain lumber part dipping effect is bad.
Preferably, the adjustable speed motor on metal can top is started in the step 7, by the control of the rotating speed of motor 3000~ 4000 revs/min, it is therefore an objective to prevent because the rotating speed of motor is too low, the fool in impregnating agent fool bronze-phenolic resin mixed liquor Bronze influences the dipping effect of wild jujube flat-grain lumber because deadweight precipitates.
Preferably, after the impregnation that wild jujube flat-grain lumber is completed in the step 8, it is cost-effective, vane pump can be used Remaining fool's bronze-phenolic resin mixed liquor in closed metal tank is drawn back into storage glue groove to reuse, deficiency part is available new Fool's bronze of preparation-phenolic resin mixed liquor supplement.
Preferably, by fool's bronze in the step 12:Edible vegetable oil=1:1(Mass ratio)Paste is stirred into after mixing, with grey knife The unintelligible place of gold thread on large format wild jujube plain-sawed lumber jigsaw is equably scratched, makes to eventually appear on wild jujube plain-sawed lumber jigsaw Gold thread clearly links up, and increases the aesthetic of decoration wood door.
Embodiment 1
A kind of processing method of wild jujube wood gold thread timber, comprises the following steps:
Step 1:Fresh wild jujube timber is felled, removes the bark of appearance and other debris, wild jujube timber is cut into 2.2 meters The juggle of length;
Step 2:Wild jujube juggle is processed into the thick band mountains of 15mm using sport car band saw, joiner pony hand-saw and thicknesser equipment The wild jujube wood flat-grain lumber of line, it is standby;
Step 3:After the wild jujube flat-grain lumber with mountain line made of giant rinsing step 2, by wild jujube plain-sawed lumber Material is put into tank, and adding dimethicone makes wild jujube flat-grain lumber be completely submerged in silicone oil, and immersion is taken out after 5 hours, is put Put and soaked again in 60 DEG C of warm water 1 hour, take out wild jujube flat-grain lumber, it is drained and standby;
Step 4:The wild jujube flat-grain lumber that step 3 treats is put into lumber kiln and dried, 60 DEG C of drying temperature, is done The moisture control of wild jujube flat-grain lumber is in 8wt% after dry;
Step 5:Fool's gold ore is taken, 200 mesh sieve, in mass ratio fool's bronze are crossed after crushing:Synvaren= 30:70 mixing, stir, standby;
Step 6:Wild jujube flat-grain lumber made of step 4 is placed in the layer frame in metal can and fixed, will be walked Fool's bronze-phenolic resin mixed liquor is poured into metal can made of rapid 5, and the liquid level of mixed liquor is higher by wild jujube flat-grain lumber stacking Top layer 20cm, close the opening of metal can;
Step 7:The adjustable speed motor on metal can top is started, the rotating speed of motor is controlled at 3000 revs/min, beaten simultaneously Open the ball valve above closed metal tank with air compressor machine connecting tube to switch, open air compressor machine power switch and start to closed gold Belong to injecting compressed air in tank, the Stress control of the pressure gauge on air compressor machine is in 0.5MPa;
Step 8:After closed pressurization 30 minutes, air compressor machine and adjustable speed motor power supply are closed, opens opening for closed metal tank Mouthful, remaining fool's bronze-phenolic resin mixed liquor in closed metal tank is drawn back into storage glue groove with vane pump, by wild jujube plain-sawed lumber Material takes out, and is put into special drip and drips glue on the net;
Step 9:After the glue for no longer occurring dripping downwards to be placed to the wild jujube flat-grain lumber for dripping online drips, by wild jujube plain-sawed lumber Material is sent into lumber kiln dry solidification, and the temperature of dry solidification is 135 DEG C, the moisture control of wild jujube flat-grain lumber after drying In 6wt%;
Step 10:Dried wild jujube flat-grain lumber is sent into two-sided thicknesser, determines the wild jujube string that thickness is processed into thickness 13mm Cutting plate material;
Step 11:Plate joggling apparatus is sent into after the thick wild jujube flat-grain lumber side brushing splicing adhesives of 13mm, assembly to be made significantly Face wild jujube plain-sawed lumber jigsaw;
Step 12:By the fool's bronze and edible vegetable oil in mass ratio 1 of step 5:Paste is stirred into after 1 mixing, it is uniform with grey knife Ground blade coating unintelligible place of gold thread on large format wild jujube plain-sawed lumber jigsaw, treats that the compound of fool's bronze and edible vegetable oil fully solidifies Afterwards, it is thick to 12mm to be sent into the fixed thick sanding of sander;
Step 13:There is the wild jujube plain-sawed lumber panel and solid wood door frame of gold thread decorative effect using surface made of step 12 Frame is compound, and after japanning solidifies, the wild jujube Solid Door with beautiful gold thread decorative effect is made.
Dimethyl-silicon oil temperature described in step 3 is 60 DEG C.
Warm water described in step 3 is that mass ratio is sodium hydroxide:Water=0.1:100 aqueous solution.
Synvaren described in step 5 is water-soluble resin, its solidfied material content 53wt%, free formaldehyde content< 0.15wt%, resin pH value 9.0.
Fool's bronze-phenolic resin mixed liquor is poured into metal can described in step 6, the liquid level of mixed liquor is higher by wild jujube Flat-grain lumber stacking top layer 20cm, it is defined by the buncher bottom that the generation of rotation liquid level is recessed at a high speed.
Embodiment 2
A kind of processing method of wild jujube wood gold thread timber, comprises the following steps:
Step 1:Fresh wild jujube timber is felled, removes the bark of appearance and other debris, wild jujube timber is cut into 2.2 meters The juggle of length;
Step 2:Wild jujube juggle is processed into the thick band mountains of 15mm using sport car band saw, joiner pony hand-saw and thicknesser equipment The wild jujube wood flat-grain lumber of line, it is standby;
Step 3:After the wild jujube flat-grain lumber with mountain line made of giant rinsing step 2, by wild jujube plain-sawed lumber Material is put into tank, and adding dimethicone makes wild jujube flat-grain lumber be completely submerged in silicone oil, and immersion is taken out after 8 hours, is put Put and soaked again in 70 DEG C of warm water 1.5 hours, take out wild jujube flat-grain lumber, it is drained and standby;
Step 4:The wild jujube flat-grain lumber that step 3 treats is put into lumber kiln and dried, 70 DEG C of drying temperature, is done The moisture control of wild jujube flat-grain lumber is in 9wt% after dry;
Step 5:Fool's gold ore is taken, 200 mesh sieve, in mass ratio fool's bronze are crossed after crushing:Synvaren= 30:70 mixing, stir, standby;
Step 6:Wild jujube flat-grain lumber made of step 4 is placed in the layer frame in metal can and fixed, will be walked Fool's bronze-phenolic resin mixed liquor is poured into metal can made of rapid 5, and the liquid level of mixed liquor is higher by wild jujube flat-grain lumber stacking Top layer 25cm, close the opening of metal can;
Step 7:The adjustable speed motor on metal can top is started, the rotating speed of motor is controlled at 3500 revs/min, beaten simultaneously Open the ball valve above closed metal tank with air compressor machine connecting tube to switch, open air compressor machine power switch and start to closed gold Belong to injecting compressed air in tank, the Stress control of the pressure gauge on air compressor machine is in 0.8MPa;
Step 8:After closed pressurization 45 minutes, air compressor machine and adjustable speed motor power supply are closed, opens opening for closed metal tank Mouthful, remaining fool's bronze-phenolic resin mixed liquor in closed metal tank is drawn back into storage glue groove with vane pump, by wild jujube plain-sawed lumber Material takes out, and is put into special drip and drips glue on the net;
Step 9:After the glue for no longer occurring dripping downwards to be placed to the wild jujube flat-grain lumber for dripping online drips, by wild jujube plain-sawed lumber Material is sent into lumber kiln dry solidification, and the temperature of dry solidification is 140 DEG C, the moisture control of wild jujube flat-grain lumber after drying In 7wt%;
Step 10:Dried wild jujube flat-grain lumber is sent into two-sided thicknesser, determines the wild jujube string that thickness is processed into thickness 13mm Cutting plate material;
Step 11:Plate joggling apparatus is sent into after the thick wild jujube flat-grain lumber side brushing splicing adhesives of 13mm, assembly to be made significantly Face wild jujube plain-sawed lumber jigsaw;
Step 12:By the fool's bronze and edible vegetable oil in mass ratio 1 of step 5:Paste is stirred into after 1 mixing, it is uniform with grey knife Ground blade coating unintelligible place of gold thread on large format wild jujube plain-sawed lumber jigsaw, treats that the compound of fool's bronze and edible vegetable oil fully solidifies Afterwards, it is thick to 12mm to be sent into the fixed thick sanding of sander;
Step 13:There is the wild jujube plain-sawed lumber panel and solid wood door frame of gold thread decorative effect using surface made of step 12 Frame is compound, and after japanning solidifies, the wild jujube Solid Door with beautiful gold thread decorative effect is made.
Dimethyl-silicon oil temperature described in step 3 is 70 DEG C.
Warm water described in step 3 is that mass ratio is sodium hydroxide:Water=0.15:100 aqueous solution.
Synvaren described in step 5 is water-soluble resin, its solidfied material content 53wt%, free formaldehyde content< 0.15wt%, resin pH value 9.0.
Fool's bronze-phenolic resin mixed liquor is poured into metal can described in step 6, the liquid level of mixed liquor is higher by wild jujube Flat-grain lumber stacking top layer 25cm, it is defined by the buncher bottom that the generation of rotation liquid level is recessed at a high speed.
Embodiment 3
A kind of processing method of wild jujube wood gold thread timber, comprises the following steps:
Step 1:Fresh wild jujube timber is felled, removes the bark of appearance and other debris, wild jujube timber is cut into 2.2 meters The juggle of length;
Step 2:Wild jujube juggle is processed into the thick band mountains of 15mm using sport car band saw, joiner pony hand-saw and thicknesser equipment The wild jujube wood flat-grain lumber of line, it is standby;
Step 3:After the wild jujube flat-grain lumber with mountain line made of giant rinsing step 2, by wild jujube plain-sawed lumber Material is put into tank, and adding dimethicone makes wild jujube flat-grain lumber be completely submerged in silicone oil, and immersion is taken out after 10 hours, is put Put and soaked again in 80 DEG C of warm water 2 hours, take out wild jujube flat-grain lumber, it is drained and standby;
Step 4:The wild jujube flat-grain lumber that step 3 treats is put into lumber kiln and dried, 75 DEG C of drying temperature, is done The moisture control of wild jujube flat-grain lumber is in 10wt% after dry;
Step 5:Fool's gold ore is taken, 200 mesh sieve, in mass ratio fool's bronze are crossed after crushing:Synvaren= 30:70 mixing, stir, standby;
Step 6:Wild jujube flat-grain lumber made of step 4 is placed in the layer frame in metal can and fixed, will be walked Fool's bronze-phenolic resin mixed liquor is poured into metal can made of rapid 5, and the liquid level of mixed liquor is higher by wild jujube flat-grain lumber stacking Top layer 30cm, close the opening of metal can;
Step 7:The adjustable speed motor on metal can top is started, the rotating speed of motor is controlled at 4000 revs/min, beaten simultaneously Open the ball valve above closed metal tank with air compressor machine connecting tube to switch, open air compressor machine power switch and start to closed gold Belong to injecting compressed air in tank, the Stress control of the pressure gauge on air compressor machine is in 1MPa;
Step 8:After closed pressurization 60 minutes, air compressor machine and adjustable speed motor power supply are closed, opens opening for closed metal tank Mouthful, remaining fool's bronze-phenolic resin mixed liquor in closed metal tank is drawn back into storage glue groove with vane pump, by wild jujube plain-sawed lumber Material takes out, and is put into special drip and drips glue on the net;
Step 9:After the glue for no longer occurring dripping downwards to be placed to the wild jujube flat-grain lumber for dripping online drips, by wild jujube plain-sawed lumber Material is sent into lumber kiln dry solidification, and the temperature of dry solidification is 145 DEG C, the moisture control of wild jujube flat-grain lumber after drying In 8wt%;
Step 10:Dried wild jujube flat-grain lumber is sent into two-sided thicknesser, determines the wild jujube string that thickness is processed into thickness 13mm Cutting plate material;
Step 11:Plate joggling apparatus is sent into after the thick wild jujube flat-grain lumber side brushing splicing adhesives of 13mm, assembly to be made significantly Face wild jujube plain-sawed lumber jigsaw;
Step 12:By the fool's bronze and edible vegetable oil in mass ratio 1 of step 5:Paste is stirred into after 1 mixing, it is uniform with grey knife Ground blade coating unintelligible place of gold thread on large format wild jujube plain-sawed lumber jigsaw, treats that the compound of fool's bronze and edible vegetable oil fully solidifies Afterwards, it is thick to 12mm to be sent into the fixed thick sanding of sander;
Step 13:There is the wild jujube plain-sawed lumber panel and solid wood door frame of gold thread decorative effect using surface made of step 12 Frame is compound, and after japanning solidifies, the wild jujube Solid Door with beautiful gold thread decorative effect is made.
Dimethyl-silicon oil temperature described in step 3 is 80 DEG C.
Warm water described in step 3 is that mass ratio is sodium hydroxide:Water=0.2:100 aqueous solution.
Synvaren described in step 5 is water-soluble resin, its solidfied material content 53wt%, free formaldehyde content< 0.15wt%, resin pH value 9.0.
Fool's bronze-phenolic resin mixed liquor is poured into metal can described in step 6, the liquid level of mixed liquor is higher by wild jujube Flat-grain lumber stacking top layer 30cm, it is defined by the buncher bottom that the generation of rotation liquid level is recessed at a high speed.
The wild jujube wood gold thread timber prepared by the present invention, using aboundresources, cheap wild jujube timber, through special PROCESS FOR TREATMENT, fool's bronze is injected in the pore for the beautiful mountain line pattern that wild jujube flat-grain lumber surface is formed, in whole wild jujube Flat-grain lumber surface relies on pore to form continuous strip gold thread(Whole piece conduit is cut)With point-like Venus(Conduit is laterally cut off), The wild jujube Solid Door with beautiful gold thread and Venus decorative effect is produced, compatriots is met and opens the door and see the good hope and right of gold The hope of good life, this technology are capable of the scientific and technological content and added value of product of General Promotion Solid Door industry.Therefore, have Vast potential for future development.
The foregoing is only presently preferred embodiments of the present invention, all equivalent changes done according to scope of the present invention patent with Modification, it should all belong to the covering scope of the present invention.

Claims (5)

1. a kind of processing method of wild jujube wood gold thread timber, it is characterised in that comprise the following steps:
Step 1:Fresh wild jujube timber is felled, removes the bark of appearance and other debris, wild jujube timber is cut into 2.2 meters of length Juggle;
Step 2:Using sport car band saw, joiner pony hand-saw and thicknesser equipment by wild jujube juggle be processed into 15mm it is thick with mountain line Wild jujube wood flat-grain lumber, it is standby;
Step 3:After the wild jujube wood flat-grain lumber with mountain line made of giant rinsing step 2, by wild jujube wood plain-sawed lumber Material is put into tank, and adding dimethicone makes wild jujube wood flat-grain lumber be completely submerged in dimethicone, and immersion 5~10 is small When after take out, be placed in 60~80 DEG C of warm water and soak again 1~2 hour, take out wild jujube wood flat-grain lumber, it is drained and standby;
Step 4:The wild jujube wood flat-grain lumber that step 3 treats is put into lumber kiln and dried, 60-75 DEG C of drying temperature, 48~100 hours drying times, the moisture control of wild jujube wood flat-grain lumber is in 8-10wt% after drying;
Step 5:Fool's gold ore is taken, 200 mesh sieve, in mass ratio fool's bronze are crossed after crushing:Synvaren=30: 70 mixing, stir, standby;
Step 6:Wild jujube wood flat-grain lumber made of step 4 is placed in the layer frame in metal can and fixed, by step 5 Manufactured fool's bronze-phenolic resin mixed liquor is poured into metal can, and the liquid level of mixed liquor is higher by wild jujube wood flat-grain lumber stacking 20~30cm of top layer, close the opening of metal can;
Step 7:The adjustable speed motor on metal can top is started, the rotating speed of motor is controlled at 3000~4000 revs/min, simultaneously Open the ball valve above closed metal tank with air compressor machine connecting tube to switch, open air compressor machine power switch and start to closed Injecting compressed air in metal can, the Stress control of the pressure gauge on air compressor machine is in 0.5~1MPa;
Step 8:After closed pressurization 30~60 minutes, air compressor machine and adjustable speed motor power supply are closed, opens opening for closed metal tank Mouthful, remaining fool's bronze-phenolic resin mixed liquor in closed metal tank is drawn back into storage glue groove with vane pump, by wild jujube wood flat-cut Sheet material takes out, and is put into special drip and drips glue on the net;
Step 9:After the glue for no longer occurring dripping downwards to be placed to the wild jujube wood flat-grain lumber for dripping online drips, by wild jujube wood plain-sawed lumber Material is sent into lumber kiln dry solidification, and the temperature of dry solidification is 135~145 DEG C, 24~48 hours dry solidification time, is done The moisture control of wild jujube wood flat-grain lumber is in 6~8wt% after dry;
Step 10:Dried wild jujube wood flat-grain lumber is sent into two-sided thicknesser, determines the wild jujube wood string that thickness is processed into thickness 13mm Cutting plate material;
Step 11:Plate joggling apparatus is sent into after the thick wild jujube wood flat-grain lumber side brushing splicing adhesives of 13mm, assembly, and large format is made Wild jujube wood plain-sawed lumber jigsaw;
Step 12:By the fool's bronze and edible vegetable oil in mass ratio 1 of step 5:Paste is stirred into after 1 mixing, is equably scraped with grey knife The unintelligible place of gold thread on large format wild jujube wood plain-sawed lumber jigsaw is coated in, after the compound of fool's bronze and edible vegetable oil fully solidifies, It is thick to 12mm to be sent into the fixed thick sanding of sander;
Step 13:There is the wild jujube wood plain-sawed lumber panel and Solid Door framework of gold thread decorative effect using surface made of step 12 It is compound, after japanning solidifies, the wild jujube Solid Door with beautiful gold thread decorative effect is made.
A kind of 2. processing method of wild jujube wood gold thread timber according to claim 1, it is characterised in that:Described in step 3 Dimethyl-silicon oil temperature is 60~80 DEG C.
A kind of 3. processing method of wild jujube wood gold thread timber according to claim 1, it is characterised in that:Described in step 3 Warm water is that mass ratio is sodium hydroxide:Water=0.1-0.2:100 aqueous solution.
A kind of 4. processing method of wild jujube wood gold thread timber according to claim 1, it is characterised in that:Described in step 5 Synvaren is water-soluble resin, its solidfied material content 53wt%, free formaldehyde content<0.15wt%, resin pH value 9.0。
A kind of 5. processing method of wild jujube wood gold thread timber according to claim 1, it is characterised in that:Described in step 6 Fool's bronze-phenolic resin mixed liquor is poured into metal can, the liquid level of mixed liquor is higher by wild jujube wood flat-grain lumber stacking top layer 20~30cm, it is defined by the buncher bottom that the generation of rotation liquid level is recessed at a high speed.
CN201610477945.1A 2016-06-28 2016-06-28 A kind of processing method of wild jujube wood gold thread timber Active CN105904563B (en)