CN105644110B - Rapid glass method for adhering film - Google Patents

Rapid glass method for adhering film Download PDF

Info

Publication number
CN105644110B
CN105644110B CN201610012055.3A CN201610012055A CN105644110B CN 105644110 B CN105644110 B CN 105644110B CN 201610012055 A CN201610012055 A CN 201610012055A CN 105644110 B CN105644110 B CN 105644110B
Authority
CN
China
Prior art keywords
glass
film
pad pasting
layer
dry ice
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201610012055.3A
Other languages
Chinese (zh)
Other versions
CN105644110A (en
Inventor
樊晖
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
ZHENGZHOU XINCHUANG GLASS TECHNOLOGY Co.,Ltd.
Original Assignee
Dongguan Songling Glass Crack-Resist Technologies Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Dongguan Songling Glass Crack-Resist Technologies Ltd filed Critical Dongguan Songling Glass Crack-Resist Technologies Ltd
Priority to CN201610012055.3A priority Critical patent/CN105644110B/en
Publication of CN105644110A publication Critical patent/CN105644110A/en
Application granted granted Critical
Publication of CN105644110B publication Critical patent/CN105644110B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The present invention relates to a kind of rapid glass method for adhering film, it comprises the following steps:The dirt on glass that will treat pad pasting with water, which cleans, to be finished, and processing is dried in the glass for then treating pad pasting, removes the water on surface;Stand-by film is taken out, tears the protective layer of film off;On the glass for treating pad pasting, film is towards uniformly smearing one layer of volatile liquid of one layer of dry ice or spraying on the surface of glass respectively;Film is placed on glass to be pasted and gently drags adjustment position;With generating heat, smooth disk roller carries out rolling processing on pad pasting glass.Present invention dry ice or volatile liquid, film can move freely adjustment position when just starting, quickly volatilized from periphery automatically afterwards and produce the globule not between film and glass, serve the effect of natural drying and heat drying machine drying, reduce technique, reduce process time, adhering film to glass efficiency is improved while ensure that adhering film to glass quality.

Description

Rapid glass method for adhering film
Technical field
The present invention relates to glass technology field, more particularly to a kind of using liquid or the rapid glass pad pasting of solid state medium Method.
Background technology
In order to reduce the light transmittance of glass either in order to play protective glass and improve the needs of strength of glass, often Can there are manual pad pasting and mechanical pad pasting two ways in the film on surface of glass, the pad pasting mode typically used.Adhering film to glass is Typically one layer of masking liquid is sprayed on surface, be easy to film to move adjustment position on glass, improve pad pasting quality.It is well-known , the moisture that the masking liquid of present adhering film to glass use contains is higher, and either heat dryer is used using natural drying Drying moisture is carried out to it, but entirely the drying cycle is all long, influences production efficiency, and easily there is bubble, influence Pad pasting quality;The drying mode of heat dryer can have an impact to the intensity of glass, reduce the service life of glass.
The content of the invention
Based on this, it is necessary to the problem of existing for traditional rapid glass method for adhering film, there is provided one kind is efficient, will not go out Existing bubble, the rapid glass method for adhering film of high-quality.
A kind of rapid glass method for adhering film, comprises the following steps:
First step:The dirt on glass that will treat pad pasting with water, which cleans, to be finished, and the glass for then treating pad pasting enters Row drying process;
Second step:Stand-by film is taken out, tears the protective layer of the film off;
Third step:Finish on the glass for treating pad pasting in cleaning, the film towards on the surface of the glass respectively One layer of dry ice of even application;
Four steps:The film is placed on the glass for treating pad pasting and gently drags adjustment position;
5th step:With the smooth disk roller of heating rolling processing is carried out on the glass for completing pad pasting.
In one of the embodiments, the surface temperature of the smooth disk roller is 5 DEG C~80 DEG C, the rolling of the smooth disk roller Dynamic speed is 1~8 m/min;The time of the rolling processing is 1~60 second.
Above-mentioned rapid glass method for adhering film, treating that one layer of the uniform smearing of surface difference that the glass of pad pasting is in contact with film is dry One layer of volatile liquid of ice or spraying;Dry ice or volatile liquid can play the painting used in traditional glass pad pasting Liquid, the viscosity of film is reduced when dry ice starts can move adjustment position on glass, and dry ice melts evaporation at normal temperatures afterwards, extensive Multiple viscosity completes pad pasting;Volatile liquid plays a part of barrier film when starting, liquid, which quickly volatilizees, afterwards completes pad pasting.By It can quickly be volatilized from periphery automatically because of the physical characteristic of itself in dry ice and liquid and will not produce water between film and glass Pearl, the effect of natural drying and heat drying machine drying is served, reduces technique, reduces process time, improves pad pasting Efficiency.Smooth disk roller increases its temperature simultaneously to film extruding ground, accelerates dry ice and the peritropous evaporation rate of liquid, also squeezes The bubble of the inside has been extruded, has further increased pad pasting efficiency and pad pasting quality.
Glass after being handled due to rolling carries out key performance detection, further ensures the quality of adhering film to glass, improves Qualification rate.
Brief description of the drawings
Fig. 1 is the flow chart of rapid glass method for adhering film embodiment one of the present invention;
Fig. 2 is the flow chart of rapid glass method for adhering film embodiment two of the present invention.
Embodiment
For the ease of understanding the present invention, the present invention is described more fully below with reference to relevant drawings.In accompanying drawing Give presently preferred embodiments of the present invention.But the present invention can realize in many different forms, however it is not limited to this paper institutes The embodiment of description.On the contrary, the purpose for providing these embodiments is to make the understanding to the disclosure more thorough Comprehensively.
It should be noted that when element is referred to as " being fixed on " another element, it can be directly on another element Or there may also be element placed in the middle.When an element is considered as " connection " another element, it can be directly connected to To another element or it may be simultaneously present centering elements.
Unless otherwise defined, all of technologies and scientific terms used here by the article is with belonging to technical field of the invention The implication that technical staff is generally understood that is identical.Term used in the description of the invention herein is intended merely to description tool The purpose of the embodiment of body, it is not intended that in the limitation present invention.
The flow chart of rapid glass method for adhering film shown in reference picture 1, embodiments of the invention one are:
First step:The glass for treating pad pasting is transported on glass cleaning machine with glass conveyer, band is treated into pad pasting with water Glass on dirt cleaning finish, then treat patch glass processing is dried, with dry cloth or blower fan removing surface water.
Second step:Stand-by film is taken out, tears the protective layer of film off, makes the sticking face of tool of film expose.
Third step:On the glass for treating pad pasting, even application one is distinguished on the sticking surface of the tool of film towards glass Layer volatile liquid, liquid layer thickness is 2~3mm.It is volatile for alcohol or ether, during from alcohol, alcohol concentration is More than 99%, the preferably alcohol at concentrations up to more than 99.5%, this alcohol are absolute alcohol, easily from surrounding volatilize and will not Produce the globule, it is not necessary to which roasting film process is dried, and improves efficiency;When using ether, lucifuge is carried out to processing environment Processing, in order to avoid ether accelerates oxidation under light, produce dangerous.
Four steps:Film is had into sticking surface to be placed on the glass for treating pad pasting, film can gently drag adjustment position, Corner is set to align.
5th step:Rolling processing is carried out on pad pasting glass with the smooth disk roller that generates heat, the surface temperature of smooth disk roller is 5 DEG C~80 DEG C, the present embodiment is preferably 30 DEG C~50 DEG C, according to the different types of membrane change temperature pasted;The rolling of smooth disk roller Dynamic speed is 1~8 m/min, and mode is rolled toward renaturation rolling mode or one-way according to selection is actually needed;Rolling processing Time is 1~60 second, and this example is preferably 21~41 seconds.Preferably, in order to reduce smooth disk roller because of the frictional force between film, One layer of thin paper is placed between film and smooth disk roller.
6th step:Glass after handling rolling carries out key performance detection, it is desirable to which overlay film surface reaches bright, flat Sliding, non-wrinkle, bubble-free etc.;
7th step:The glass up to standard to pad pasting carries out packing processes.
Refer to rapid glass method for adhering film of the present invention, embodiment two shown in Fig. 2 is:
First step:The glass for treating pad pasting is transported on glass cleaning machine with glass conveyer, band is treated into pad pasting with water Glass on dirt cleaning finish, then treat patch glass processing is dried, with dry cloth or blower fan removing surface water.
Second step:Stand-by film is taken out, tears the protective layer of film off, makes the sticking face of tool of film expose.
Third step:On the glass for treating pad pasting, even application one is distinguished on the sticking surface of the tool of film towards glass Layer dry ice, dry ice layer thickness is 0.1~1mm.
Four steps:Film is had into sticking surface to be placed on the glass for treating pad pasting, dry ice reduces the viscosity of film during beginning, Film can gently drag adjustment position, corner is alignd, and viscosity is replied in dry ice evaporation under normal temperature afterwards.
5th step:Rolling processing is carried out on pad pasting glass with the smooth disk roller that generates heat, the surface temperature of smooth disk roller is 5 DEG C~80 DEG C, the present embodiment is preferably 30 DEG C~50 DEG C, according to the different types of membrane change temperature pasted;The rolling of smooth disk roller Dynamic speed is 1~8 m/min, and mode is rolled toward renaturation rolling mode or one-way according to selection is actually needed;Rolling processing Time is that 1~60 second the present embodiment is preferably 21~41 seconds.Preferably, in order to reduce smooth disk roller because of the friction between film Power, one layer of thin paper is placed between film and smooth disk roller
Embodiment three is:Third step in embodiment one and embodiment two is changed to smear one on the glass for treat pad pasting Layer dry ice, in one layer of alcohol of the sticking surface spraying of the tool of film towards glass or ether;Can also treat the glass of pad pasting One layer of alcohol of upper spraying or ether, has sticking one layer of dry ice of surface smear in film.This scheme can be according to treating pad pasting glass The position relationship selective binding of glass and film uses dry ice and alcohol, ether.
Foregoing invention is treated pad pasting glass cleaning and also manually can directly operate cleaning or be cleaned using ultrasonic wave, ultrasonic wave The effect of cleaning is good, and cleannes are high, and cleaning speed is fast, also should not drying process, to workpiece surface not damaged, reduce and be produced into This.By the rapid glass method for adhering film in embodiment one, two and three, relative to traditional rapid glass method for adhering film, dry ice The masking liquid used in traditional glass pad pasting can be played with volatile liquid, the viscosity that film is reduced when dry ice starts can be in glass Adjustment position is moved on glass, dry ice melts evaporation at normal temperatures afterwards, recovers viscosity and completes pad pasting;When volatile liquid starts Play a part of barrier film, liquid, which quickly volatilizees, afterwards completes pad pasting.Because dry ice and liquid can be because of the physical characteristics of itself Automatically quickly volatilized from periphery and the globule will not be produced between pad pasting and glass, served natural drying and heat dryer dries Dry effect, reduces technique, reduces process time, improves pad pasting efficiency, reduces cost input.Smooth disk roller is to film Extruding ground increases its temperature simultaneously, accelerates dry ice and the peritropous evaporation rate of liquid, has also squeezed out the bubble of the inside, Further increase pad pasting efficiency and pad pasting quality.
Each technical characteristic of embodiment described above can be combined arbitrarily, to make description succinct, not to above-mentioned reality Apply all possible combination of each technical characteristic in example to be all described, as long as however, the combination of these technical characteristics is not deposited In contradiction, the scope that this specification is recorded all is considered to be.
Embodiment described above only expresses the several embodiments of the present invention, and its description is more specific and detailed, but simultaneously Can not therefore it be construed as limiting the scope of the patent.It should be pointed out that come for one of ordinary skill in the art Say, without departing from the inventive concept of the premise, various modifications and improvements can be made, these belong to the protection of the present invention Scope.Therefore, the protection domain of patent of the present invention should be determined by the appended claims.

Claims (2)

1. a kind of rapid glass method for adhering film, it is characterised in that comprise the following steps:
First step:The dirt on glass that will treat pad pasting with water, which cleans, to be finished, and the glass for then treating pad pasting is done Dry processing;
Second step:Stand-by film is taken out, tears the protective layer of the film off;
Third step:Finish on the glass for treating pad pasting in cleaning, the film is towards uniform respectively on the surface of the glass Spray one layer of dry ice;
Four steps:The film is placed on the glass for treating pad pasting and gently drags adjustment position;
5th step:With the smooth disk roller of heating rolling processing is carried out on the glass for completing pad pasting.
2. rapid glass method for adhering film according to claim 1, it is characterised in that the surface temperature of the smooth disk roller is 5 DEG C~80 DEG C, the rolling speed of the smooth disk roller is 1~8 m/min;The time of the rolling processing is 1~60 second.
CN201610012055.3A 2016-01-07 2016-01-07 Rapid glass method for adhering film Active CN105644110B (en)