CN104278520B - Water-repellent finishing method for clothes - Google Patents

Water-repellent finishing method for clothes Download PDF

Info

Publication number
CN104278520B
CN104278520B CN201410552582.4A CN201410552582A CN104278520B CN 104278520 B CN104278520 B CN 104278520B CN 201410552582 A CN201410552582 A CN 201410552582A CN 104278520 B CN104278520 B CN 104278520B
Authority
CN
China
Prior art keywords
parts
clothes
water
hours
impregnation liquid
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201410552582.4A
Other languages
Chinese (zh)
Other versions
CN104278520A (en
Inventor
钱永忠
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
HUZHOU ZHILI CHILDREN'S CLOTHING DEVELOPMENT CO LTD
Huzhou Youchuang Technology Co Ltd
Original Assignee
SUZHOU ZONEJOY CLOTHING Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by SUZHOU ZONEJOY CLOTHING Co Ltd filed Critical SUZHOU ZONEJOY CLOTHING Co Ltd
Priority to CN201410552582.4A priority Critical patent/CN104278520B/en
Publication of CN104278520A publication Critical patent/CN104278520A/en
Application granted granted Critical
Publication of CN104278520B publication Critical patent/CN104278520B/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a kind of water-repellent finishing method for clothes, comprise the steps: 1) by 30 parts of water, 1~2 part of alkylolamides polyethylene oxide ether, 2~3 parts of acrylic resins, 3~4 parts of polyvinylpyrrolidones, 4~5 parts of isopropanolamine mixing, then 7~8 parts of PAMAs, 1~2 part of ethylene glycol monostearate, 6~7 parts of HPC-1 finishing agents, 8~9 parts of dihydroxymethyl ethylene ureas, 1~2 part of glyceryl monostearate it are slowly added, feed intake in 35 minutes complete, continue mixing 2.5 hours, prepare impregnation liquid;2) clothes padding process in impregnation liquid, pressure 2.3MPa, liquid carrying rate 71%, by clothes 143 DEG C of constant temperature 3 hours after drying。The clothes that the present invention arranges has water repellency and good endurance。

Description

Water-repellent finishing method for clothes
Technical field
The present invention relates to the water-repellent finishing method for clothes。
Background technology
Being currently used for the water-repellent finishing method of clothes, it is bad that water durability refused by the clothes of its arrangement。
Summary of the invention
It is an object of the invention to provide a kind of water-repellent finishing method for clothes, the clothes of its arrangement has water repellency and good endurance。
For achieving the above object, the technical scheme is that a kind of water-repellent finishing method for clothes of design, comprise the steps:
1) by 30 parts of water, 1~2 part of alkylolamides polyethylene oxide ether, 2~3 parts of acrylic resins, 3~4 parts of polyvinylpyrrolidones, 4~5 parts of isopropanolamine mixing, then 7~8 parts of PAMAs, 1~2 part of ethylene glycol monostearate, 6~7 parts of HPC-1 finishing agents, 8~9 parts of dihydroxymethyl ethylene ureas, 1~2 part of glyceryl monostearate it are slowly added, feed intake in 35 minutes complete, continue mixing 2.5 hours, prepare impregnation liquid;
2) clothes padding process in impregnation liquid, pressure 2.3MPa, liquid carrying rate 71%, by clothes 143 DEG C of constant temperature 3 hours after drying。
Preferably, for the water-repellent finishing method of clothes, comprise the steps:
1) by 30 parts of water, 1.2 parts of alkylolamides polyethylene oxide ethers, 2.3 parts of acrylic resins, 3.4 parts of polyvinylpyrrolidones, 4.5 parts of isopropanolamine mixing, then 7.8 parts of PAMAs, 1.2 parts of ethylene glycol monostearates, 6.7 parts of HPC-1 finishing agents, 8.9 parts of dihydroxymethyl ethylene ureas, 1.2 parts of glyceryl monostearates it are slowly added, feed intake in 35 minutes complete, continue mixing 2.5 hours, prepare impregnation liquid;
2) clothes padding process in impregnation liquid, pressure 2.3MPa, liquid carrying rate 71%, by clothes 143 DEG C of constant temperature 3 hours after drying。
Preferably, for the water-repellent finishing method of clothes, comprise the steps:
1) by 30 parts of water, 2 parts of alkylolamides polyethylene oxide ethers, 3 parts of acrylic resins, 4 parts of polyvinylpyrrolidones, 5 parts of isopropanolamine mixing, then 8 parts of PAMAs, 2 parts of ethylene glycol monostearates, 7 parts of HPC-1 finishing agents, 9 parts of dihydroxymethyl ethylene ureas, 2 parts of glyceryl monostearates it are slowly added, feed intake in 35 minutes complete, continue mixing 2.5 hours, prepare impregnation liquid;
2) clothes padding process in impregnation liquid, pressure 2.3MPa, liquid carrying rate 71%, by clothes 143 DEG C of constant temperature 3 hours after drying。
Preferably, for the water-repellent finishing method of clothes, comprise the steps:
1) by 30 parts of water, 1 part of alkylolamides polyethylene oxide ether, 2 parts of acrylic resins, 3 parts of polyvinylpyrrolidones, 4 parts of isopropanolamine mixing, then 7 parts of PAMAs, 1 part of ethylene glycol monostearate, 6 parts of HPC-1 finishing agents, 8 parts of dihydroxymethyl ethylene ureas, 1 part of glyceryl monostearate it are slowly added, feed intake in 35 minutes complete, continue mixing 2.5 hours, prepare impregnation liquid;
2) clothes padding process in impregnation liquid, pressure 2.3MPa, liquid carrying rate 71%, by clothes 143 DEG C of constant temperature 3 hours after drying。
Advantages of the present invention and having the beneficial effects that: providing a kind of water-repellent finishing method for clothes, the clothes of its arrangement has water repellency and good endurance。
Detailed description of the invention
Below in conjunction with embodiment, the specific embodiment of the present invention is further described。Following example are only for clearly illustrating technical scheme, and can not limit the scope of the invention with this。
The technical scheme that the present invention is embodied as is:
Embodiment 1
For the water-repellent finishing method of clothes, comprise the steps:
1) by 30 parts of water, 1.2 parts of alkylolamides polyethylene oxide ethers, 2.3 parts of acrylic resins, 3.4 parts of polyvinylpyrrolidones, 4.5 parts of isopropanolamine mixing, then 7.8 parts of PAMAs, 1.2 parts of ethylene glycol monostearates, 6.7 parts of HPC-1 finishing agents, 8.9 parts of dihydroxymethyl ethylene ureas, 1.2 parts of glyceryl monostearates it are slowly added, feed intake in 35 minutes complete, continue mixing 2.5 hours, prepare impregnation liquid;
2) clothes padding process in impregnation liquid, pressure 2.3MPa, liquid carrying rate 71%, by clothes 143 DEG C of constant temperature 3 hours after drying。
Embodiment 2
For the water-repellent finishing method of clothes, comprise the steps:
1) by 30 parts of water, 2 parts of alkylolamides polyethylene oxide ethers, 3 parts of acrylic resins, 4 parts of polyvinylpyrrolidones, 5 parts of isopropanolamine mixing, then 8 parts of PAMAs, 2 parts of ethylene glycol monostearates, 7 parts of HPC-1 finishing agents, 9 parts of dihydroxymethyl ethylene ureas, 2 parts of glyceryl monostearates it are slowly added, feed intake in 35 minutes complete, continue mixing 2.5 hours, prepare impregnation liquid;
2) clothes padding process in impregnation liquid, pressure 2.3MPa, liquid carrying rate 71%, by clothes 143 DEG C of constant temperature 3 hours after drying。
Embodiment 3
For the water-repellent finishing method of clothes, comprise the steps:
1) by 30 parts of water, 1 part of alkylolamides polyethylene oxide ether, 2 parts of acrylic resins, 3 parts of polyvinylpyrrolidones, 4 parts of isopropanolamine mixing, then 7 parts of PAMAs, 1 part of ethylene glycol monostearate, 6 parts of HPC-1 finishing agents, 8 parts of dihydroxymethyl ethylene ureas, 1 part of glyceryl monostearate it are slowly added, feed intake in 35 minutes complete, continue mixing 2.5 hours, prepare impregnation liquid;
2) clothes padding process in impregnation liquid, pressure 2.3MPa, liquid carrying rate 71%, by clothes 143 DEG C of constant temperature 3 hours after drying。
The above is only the preferred embodiment of the present invention; it should be pointed out that, for those skilled in the art, under the premise without departing from the technology of the present invention principle; can also making some improvements and modifications, these improvements and modifications also should be regarded as protection scope of the present invention。

Claims (4)

1. for the water-repellent finishing method of clothes, it is characterised in that comprise the steps:
1) by 30 parts of water, 1~2 part of alkylolamides polyethylene oxide ether, 2~3 parts of acrylic resins, 3~4 parts of polyvinylpyrrolidones, 4~5 parts of isopropanolamine mixing, then 7~8 parts of PAMAs, 1~2 part of ethylene glycol monostearate, 6~7 parts of HPC-1 finishing agents, 8~9 parts of dihydroxymethyl ethylene ureas, 1~2 part of glyceryl monostearate it are slowly added, feed intake in 35 minutes complete, continue mixing 2.5 hours, prepare impregnation liquid;
2) clothes padding process in impregnation liquid, pressure 2.3MPa, liquid carrying rate 71%, by clothes 143 DEG C of constant temperature 3 hours after drying。
2. the water-repellent finishing method for clothes according to claim 1, it is characterised in that comprise the steps:
1) by 30 parts of water, 1.2 parts of alkylolamides polyethylene oxide ethers, 2.3 parts of acrylic resins, 3.4 parts of polyvinylpyrrolidones, 4.5 parts of isopropanolamine mixing, then 7.8 parts of PAMAs, 1.2 parts of ethylene glycol monostearates, 6.7 parts of HPC-1 finishing agents, 8.9 parts of dihydroxymethyl ethylene ureas, 1.2 parts of glyceryl monostearates it are slowly added, feed intake in 35 minutes complete, continue mixing 2.5 hours, prepare impregnation liquid;
2) clothes padding process in impregnation liquid, pressure 2.3MPa, liquid carrying rate 71%, by clothes 143 DEG C of constant temperature 3 hours after drying。
3. the water-repellent finishing method for clothes according to claim 1, it is characterised in that comprise the steps:
1) by 30 parts of water, 2 parts of alkylolamides polyethylene oxide ethers, 3 parts of acrylic resins, 4 parts of polyvinylpyrrolidones, 5 parts of isopropanolamine mixing, then 8 parts of PAMAs, 2 parts of ethylene glycol monostearates, 7 parts of HPC-1 finishing agents, 9 parts of dihydroxymethyl ethylene ureas, 2 parts of glyceryl monostearates it are slowly added, feed intake in 35 minutes complete, continue mixing 2.5 hours, prepare impregnation liquid;
2) clothes padding process in impregnation liquid, pressure 2.3MPa, liquid carrying rate 71%, by clothes 143 DEG C of constant temperature 3 hours after drying。
4. the water-repellent finishing method for clothes according to claim 1, it is characterised in that comprise the steps:
1) by 30 parts of water, 1 part of alkylolamides polyethylene oxide ether, 2 parts of acrylic resins, 3 parts of polyvinylpyrrolidones, 4 parts of isopropanolamine mixing, then 7 parts of PAMAs, 1 part of ethylene glycol monostearate, 6 parts of HPC-1 finishing agents, 8 parts of dihydroxymethyl ethylene ureas, 1 part of glyceryl monostearate it are slowly added, feed intake in 35 minutes complete, continue mixing 2.5 hours, prepare impregnation liquid;
2) clothes padding process in impregnation liquid, pressure 2.3MPa, liquid carrying rate 71%, by clothes 143 DEG C of constant temperature 3 hours after drying。
CN201410552582.4A 2014-10-20 2014-10-20 Water-repellent finishing method for clothes Expired - Fee Related CN104278520B (en)