CN104152597A - Fur machining method - Google Patents

Fur machining method Download PDF

Info

Publication number
CN104152597A
CN104152597A CN201410419041.4A CN201410419041A CN104152597A CN 104152597 A CN104152597 A CN 104152597A CN 201410419041 A CN201410419041 A CN 201410419041A CN 104152597 A CN104152597 A CN 104152597A
Authority
CN
China
Prior art keywords
fur
skin
time
concentration
pickling
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201410419041.4A
Other languages
Chinese (zh)
Other versions
CN104152597B (en
Inventor
张江山
郑超斌
郑红超
郝安生
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Beijing Fanbo Science & Technology Co ltd
Original Assignee
Beijing Fanbo Science & Technology Co ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Beijing Fanbo Science & Technology Co ltd filed Critical Beijing Fanbo Science & Technology Co ltd
Priority to CN201410419041.4A priority Critical patent/CN104152597B/en
Publication of CN104152597A publication Critical patent/CN104152597A/en
Application granted granted Critical
Publication of CN104152597B publication Critical patent/CN104152597B/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention relates to the field of fur production machining industries, in particular to a fur machining method. According to the fur machining method, in the machining process of fur, the salt-free pickling and aldehyde-free chromium-free tanning technology is adopted. Neutral inorganic salt (sodium chloride and sodium sulfate) is not used in the processes of soaking, degreasing, softening, pickling and the like, and the machining processes are achieved by adding corresponding organic reagents (penetrating agents, degreasing agents, pickling additives and softening enzyme). Therefore, the problem that in the prior art, when fur is machined, a large amount of inorganic salt (especially neutral salt) needs to be used, and the environment is polluted is solved. In addition, in the whole fur machining process, due to the fact that the neutral salt is not used, the production cost is greatly reduced, the cost for waste water treating is reduced, the environment is protected, and the quality of the machined fur is not affected.

Description

The working method of fur
Technical field
The present invention relates to fur process for processing industry field, in particular to a kind of working method of fur.
Background technology
In the technological process of process for processing fur, in the process of especially softening in pickling and immersion, conventionally can use a large amount of neutral salt (mainly comprising sodium-chlor and sodium sulfate).Concrete, table 1 has been listed neutral salt service condition in the process of 1 ton of raw material skin of processing of correlation technique.
The conventional 1 ton of fur technology neutral salt service condition table of table 1
Operation Raw hide is anticorrosion Immersion Pickling is softening Tanning
Water consumption (L) 0 20000 20000 20000
Neutral salt operation parameter Tare weight 20% 15g/L 60g/L 50g/L
Neutral salt consumption (Kg) 200 300 1200 1000
Can find out by table 1, process 1 ton of raw material skin and need to consume 2.0-3.0 ton neutral salt, and then make neutral salt content in the sewage after fur manufacturing higher (can up to 15g/L).Contain a large amount of neutral salt sewage and be difficult to process, its long-term accumulation can make water and soil salinization gradually, biological electrolysis dysequilibrium, and final water and soil salinization, destroys ecotope.
Summary of the invention
The object of the present invention is to provide a kind of working method of fur, with the above-mentioned technical problem solving.
The working method that fur is provided in an embodiment of the present invention, comprises the following steps: 1), fur is immersed in the water that permeate agent concentration is 0.5-1.0g/L, soak for the first time, after being soaked for the first time, expect skin; 2), material skin after described immersion is for the first time immersed to permeate agent concentration is in 0.5-1.0g/L, the grease-removing agent concentration water that is 0.5-2.0g/L, soaks for the second time, after being soaked for the second time, expects skin; 3), material skin after described immersion is for the second time added to grease-removing agent concentration is in 2.0-3.0g/L, the soda ash concentration water that is 0.5-2.0g/L, carries out degreasing, obtain expecting skin after degreasing; 4), soften expecting after described degreasing that skin immerses in the water that the concentration of macerating enzyme NM is 0.5-1.0g/L, obtain softening after material skin; 5), by described softening after material skin to join auxiliary pickling agent ADC concentration be that the concentration of 4.0-4.5g/L, macerating enzyme ARS is in the concentration of 1.5-2.0g/L, the macerating enzyme BRH water that is 0.3-0.5g/L, carry out pickling, obtain expecting skin after pickling; 6), will after described pickling, expect that skin carries out, without aldehyde chrome-free tanning, obtaining processing rear fur.
The working method of this fur provided by the invention, it has adopted salt-free pickling, technique without aldehyde chrome-free tanning in the process of processing.In the processes such as immersion, degreasing, softening, pickling, all do not use neutral inorganic (sodium-chlor and sodium sulfate), but by adding corresponding organic medicament (permeate agent, grease-removing agent, auxiliary pickling agent and macerating enzyme) to realize the course of processing.Therefore overcome in prior art the problem of environmental pollution that need to use a large amount of inorganic salt (especially neutral salt) and then bring in processing fur.
In addition, in the process of the application's whole fur manufacturing, owing to not using neutral salt, therefore, reduced greatly production cost, reduced process waste water cost, protected environment, and do not affect the quality of made fur.Therefore, the working method of this fur provided by the invention is the good examples that industry energy conservation reduces discharging, promotes quality, expands export, and contributes to bring great economic benefit to enterprise.
Optionally, in step 1) in: described permeate agent is Ai Lite wetting agent HAC; Water temperature in described immersion process is for the first time that 32-35 DEG C, time are 2-4 hour.
Optionally, in step 2) in: described permeate agent is Ai Lite wetting agent HAC; Described grease-removing agent is Ai Lite grease-removing agent H; Water temperature in described immersion process is for the second time normal temperature, and the time is 10-16 hour.
Optionally, in step 2) and step 3) between also comprise: the residual meat that described in removal, after immersion for the second time, material leaves on skin.
Optionally, in step 4) in: the water temperature in described softening process is that 35 DEG C, time are 0.5-1.5 hour.
Optionally, in step 5) in specifically comprise; In water, add described softening rear material skin, add again auxiliary pickling agent ADC, make its concentration reach 4.0-4.5g/L, after 10-16 hour, add again macerating enzyme ARS and macerating enzyme BRH, and make the concentration of described macerating enzyme ARS and described macerating enzyme BRH reach respectively 1.5-2.0g/L and 0.3-0.5g/L, and soak 16-24 hour, obtain expecting skin after pickling.
Optionally, step 4) and step 5) between, also comprise: the water that is 20-30 DEG C to material skin temperature after softening cleans.
Brief description of the drawings
In order to be illustrated more clearly in the specific embodiment of the invention or technical scheme of the prior art, to the accompanying drawing of required use in embodiment or description of the Prior Art be briefly described below, apparently, accompanying drawing in the following describes is some embodiments of the present invention, for those of ordinary skill in the art, do not paying under the prerequisite of creative work, can also obtain according to these accompanying drawings other accompanying drawing.
The working method schema of the fur that Fig. 1 provides for the embodiment of the present invention one.
Embodiment
For making the object, technical solutions and advantages of the present invention clearer; to technical scheme of the present invention be carried out to clear, complete description below; based on the embodiment in the present invention; all other embodiments that those of ordinary skill in the art obtain under the prerequisite of not making creative work, all belong to the scope that the present invention protects.
Before narration specific embodiments of the invention, it is pointed out that macerating enzyme NM refers in all embodiment of the present invention: this macerating enzyme of prestige NM; Auxiliary pickling agent ADC refers to this auxiliary pickling agent of prestige ADC; Macerating enzyme ARS refers to: this macerating enzyme of prestige ARS; Macerating enzyme BRH refers to: this macerating enzyme of prestige BRH.The fur customizations chemical product of above medicament Jun Shi Fanbo Chemicals Co., Ltd..
Embodiment mono-
Please refer to Fig. 1, the working method of this fur that the embodiment of the present invention provides, comprises the following steps:
Step 101: fur is immersed in the water that permeate agent concentration is 0.5-1.0g/L, soak for the first time, expect skin after being soaked for the first time;
In step 101, after soaking for the first time, the contained great amount of soluble albumen of fur (raw material skin), floating meat and oil film can be removed, and permeate agent infiltrates after fur the loose and water-filling of its collagen fiber structure.
Step 102: it is in 0.5-1.0g/L, the grease-removing agent concentration water that is 0.5-2.0g/L that material skin after described immersion is for the first time immersed to permeate agent concentration, soaks for the second time, expects skin after being soaked for the second time;
In step 102, the material skin after immersion has for the first time been added to certain density grease-removing agent, therefore, after expecting that after soaking for the first time skin soaks for the second time, its remaining lipid is by a large amount of removals, and then preparation enters next process.
Step 103: it is in 2.0-3.0g/L, the soda ash concentration water that is 0.5-2.0g/L that material skin after described immersion is for the second time added to grease-removing agent concentration, carries out degreasing, obtains expecting skin after degreasing;
In step 103, its main purpose is for degreasing, and then has strengthened the consumption of grease-removing agent in the process of operation, and has added soda ash, and then removes as far as possible completely remaining lipid on material skin.Concrete, grease-removing agent reacts with remaining lipid generation good fortune as tensio-active agent, and after degreasing, in skin, the hair of intracellular grease and procuticle comes off, and exposes natural careful grain; In addition, degreasing target below should as far as possible realizing in the process of degreasing: strong, without rotten skin, scarce face; Fleece is clean, and subcutis is removed clean without damaged, and skin is without unctuousness, without swelling.
Step 104: soften in the water that is 0.5-1.0g/L by the concentration of expecting skin immersion macerating enzyme NM after described degreasing, obtain softening rear material skin;
In step 104, by expecting to add macerating enzyme NM in skin and then make it softening after degreasing, to meet the demand of following process.
Step 105: by described softening after material skin to join auxiliary pickling agent ADC concentration be that the concentration of 4.0-4.5g/L, macerating enzyme ARS is in the concentration of 1.5-2.0g/L, the macerating enzyme BRH water that is 0.3-0.5g/L, carry out pickling, obtain expecting skin after pickling;
After softening operation completes, by macerating enzyme BRH and macerating enzyme ARS and the operation of auxiliary pickling agent ADC realization to material skin pickling after softening of set consumption, substitute the operation of using acid and neutral salt pickling in traditional technology, in the process of pickling, by regulating pH and then changing the electric charge sex character on pelt surface, be beneficial to penetrating of tanning agent in follow-up tannery.In addition, by two kinds of macerating enzymes, it can make to expect that the collagen fiber structure of skin is further loose, is convenient to follow-up tannery.
Step 106: will expect after described pickling that skin carries out, without aldehyde chrome-free tanning, obtaining processing rear fur.
In the process of tanning, the protein of intracutaneous carries out chemistry and physical reaction.And a series of variations occur the protein that makes intracutaneous, make collagen protein generation Denaturation.Tanned leather is both soft, firm, wear-resisting again, is not easy putrid and deteriorated.
In addition, adopt in the present invention without aldehyde chrome-free tanning, this tanning operation environmental protection, cost is low.
The working method of this fur provided by the invention, has adopted salt-free pickling, technique without aldehyde chrome-free tanning.In the processes such as immersion, degreasing, softening, pickling, all do not use neutral inorganic (sodium-chlor and sodium sulfate), but by adding corresponding organic medicament (permeate agent, grease-removing agent, auxiliary pickling agent and macerating enzyme) to realize the course of processing.Therefore overcome the problem of environmental pollution that need to use a large amount of inorganic salt (especially neutral salt) and then bring in prior art in processing fur.In addition, in the process of the application's whole fur manufacturing, owing to not using neutral salt, therefore, reduced greatly production cost, reduced process waste water cost, protected environment, and do not affect the quality of made fur.Therefore, the working method of this fur provided by the invention is the good examples that industry energy conservation reduces discharging, promotes quality, expands export, and contributes to bring great economic benefit to enterprise.
For the working method of the fur that makes the above embodiment of the present invention is better applied, more effectively be applied in leather processing field, the present invention also provides embodiment bis-on the basis of above-described embodiment, embodiment bis-has provided the further refinement of working method or the increase of the fur of above-described embodiment, is now described in detail and explains:
Embodiment bis-
In the present embodiment, the preparation method of the working method of fur comprises the following steps:
S1: fur is immersed in the water that permeate agent concentration is 0.5-1.0g/L, soak for the first time, expect skin after being soaked for the first time;
In this step, wherein, described permeate agent is Ai Lite wetting agent HAC; Water temperature in described immersion process is for the first time that 32-35 DEG C, time are 2-4 hour.
S2: it is in 0.5-1.0g/L, the grease-removing agent concentration water that is 0.5-2.0g/L that material skin after described immersion is for the first time immersed to permeate agent concentration, soaks for the second time, expects skin after being soaked for the second time;
In step 202, described permeate agent is Ai Lite wetting agent HAC; Described grease-removing agent is Ai Lite grease-removing agent H; Water temperature in described immersion process is for the second time normal temperature, and the time is 10-16 hour.
S3: it is in 2.0-3.0g/L, the soda ash concentration water that is 0.5-2.0g/L that material skin after described immersion is for the second time added to grease-removing agent concentration, carries out degreasing, obtains expecting skin after degreasing;
After step S1 and S2, material may also exist in skin all to be difficult to the residual meat of removing, if these meat are not removed, is unfavorable for follow-up degreasing and the operation such as softening.Therefore,, before carrying out step S3, also comprise: remove the rear operation of expecting the residual meat leaving on skin of immersion for the second time.
S4: soften in the water that is 0.5-1.0g/L by the concentration of expecting skin immersion macerating enzyme NM after described degreasing, obtain softening rear material skin;
In this step, preferred, the water temperature in described softening process is that 35 DEG C, time are 0.5-1.5 hour.
After completing softening operation, preferred, the water that also to comprise material skin temperature after softening be 20-30 DEG C cleans, and cleans and can carry out following operation afterwards.
S5: by described softening after material skin to join auxiliary pickling agent ADC concentration be that the concentration of 4.0-4.5g/L, macerating enzyme ARS is in the concentration of 1.5-2.0g/L, the macerating enzyme BRH water that is 0.3-0.5g/L, carry out pickling, obtain expecting skin after pickling;
Concrete, above-mentioned steps is carried out according to following operation: in water, add described softening rear material skin, add again auxiliary pickling agent ADC, make its concentration reach 4.0-4.5g/L, after 10-16 hour, then add macerating enzyme ARS and macerating enzyme BRH, and make the concentration of described macerating enzyme ARS and described macerating enzyme BRH reach respectively 1.5-2.0g/L and 0.3-0.5g/L, soak 16-24 hour, obtain expecting skin after pickling.
S6: will expect after described pickling that skin carries out, without aldehyde chrome-free tanning, obtaining processing rear fur.
To sum up, the working method of this fur that the embodiment of the present invention provides, it has used salt-free pickling, technique without aldehyde chrome-free tanning.In the processes such as immersion, degreasing, softening, pickling, all do not use neutral inorganic (sodium-chlor and sodium sulfate), but by adding corresponding organic medicament (permeate agent, grease-removing agent, auxiliary pickling agent and macerating enzyme) to realize the course of processing; Therefore overcome the problem of environmental pollution that need to use a large amount of inorganic salt (especially neutral salt) and then bring in prior art in processing fur.In addition, the method has also reduced greatly production cost, has reduced the cost of processing waste water, has protected environment, and does not affect the quality of made fur.Therefore, the working method of this fur provided by the invention is the good examples that industry energy conservation reduces discharging, promotes quality, expands export, and contributes to bring great economic benefit to enterprise.
The foregoing is only the preferred embodiments of the present invention, be not limited to the present invention, for a person skilled in the art, the present invention can have various modifications and variations.Within the spirit and principles in the present invention all, any amendment of doing, be equal to replacement, improvement etc., within all should being included in protection scope of the present invention.

Claims (7)

1. a working method for fur, is characterized in that, comprises the following steps:
1), fur is immersed in the water that permeate agent concentration is 0.5-1.0g/L, soak for the first time, after being soaked for the first time, expect skin;
2), material skin after described immersion is for the first time immersed to permeate agent concentration is in 0.5-1.0g/L, the grease-removing agent concentration water that is 0.5-2.0g/L, soaks for the second time, after being soaked for the second time, expects skin;
3), material skin after described immersion is for the second time added to grease-removing agent concentration is in 2.0-3.0g/L, the soda ash concentration water that is 0.5-2.0g/L, carries out degreasing, obtain expecting skin after degreasing;
4), soften expecting after described degreasing that skin immerses in the water that the concentration of macerating enzyme NM is 0.5-1.0g/L, obtain softening after material skin;
5), by described softening after material skin to join auxiliary pickling agent ADC concentration be that the concentration of 4.0-4.5g/L, macerating enzyme ARS is in the concentration of 1.5-2.0g/L, the macerating enzyme BRH water that is 0.3-0.5g/L, carry out pickling, obtain expecting skin after pickling;
6), will after described pickling, expect that skin carries out, without aldehyde chrome-free tanning, obtaining processing rear fur.
2. the working method of fur according to claim 1, is characterized in that, in step 1) in:
Described permeate agent is Ai Lite wetting agent HAC; Water temperature in described immersion process is for the first time that 32-35 DEG C, time are 2-4 hour.
3. the working method of fur according to claim 2, is characterized in that, in step 2) in:
Described permeate agent is Ai Lite wetting agent HAC; Described grease-removing agent is Ai Lite grease-removing agent H; Water temperature in described immersion process is for the second time normal temperature, and the time is 10-16 hour.
4. the working method of fur according to claim 3, is characterized in that, in step 2) and step 3) between also comprise:
The residual meat leaving on material skin after immersion for the second time described in removal.
5. the working method of fur according to claim 4, is characterized in that, in step 4) in:
Water temperature in described softening process is that 35 DEG C, time are 0.5-1.5 hour.
6. according to the working method of the fur described in claim 1-5 any one, it is characterized in that, in step 5) in specifically comprise:
In water, add described softening rear material skin, add again auxiliary pickling agent ADC, make its concentration reach 4.0-4.5g/L, after 10-16 hour, add again macerating enzyme ARS and macerating enzyme BRH, and make the concentration of described macerating enzyme ARS and described macerating enzyme BRH reach respectively 1.5-2.0g/L and 0.3-0.5g/L, and soak 16-24 hour, obtain expecting skin after pickling.
7. the working method of fur according to claim 6, is characterized in that, in described step 4) and step 5) between, also comprise:
Material skin after softening is cleaned with the water that temperature is 20-30 DEG C.
CN201410419041.4A 2014-08-22 2014-08-22 The working method of fur Expired - Fee Related CN104152597B (en)