Summary of the invention
For problems of the prior art, the object of the present invention is to provide a kind of technical scheme of waterproof coating.
Described a kind of waterproof coating, is characterized in that being made up of the raw material of following weight part: tetrabutyl phosphorus chloride 25-40 part, acrylate acrylate copolymer emulsion 15-30 part, PVDC latex 5-10 part, lime powder 15-22 part, styroyl phenol polyoxyethylene polyoxypropylene ether 5-10 part, alkyl benzene calcium sulfonate 6-12 part, dibutyl succinic acid sodium sulfonate 2-8 part, tartrate 3-10 part, dimethylbenzene 2-8 part, two Polyglycerine 1-6 parts, tributyl phosphate 1-6 part, Methyl Benzene-o-dicarboxylate 4-8 part, MALEIC ANHYDRIDE 3-8 part, rosin 8-15 part.
Described a kind of waterproof coating, is characterized in that being made up of the raw material of following weight part: tetrabutyl phosphorus chloride 30-35 part, acrylate acrylate copolymer emulsion 20-25 part, PVDC latex 6-9 part, lime powder 17-20 part, styroyl phenol polyoxyethylene polyoxypropylene ether 6-9 part, alkyl benzene calcium sulfonate 8-10 part, dibutyl succinic acid sodium sulfonate 4-6 part, tartrate 5-8 part, dimethylbenzene 3-7 part, two Polyglycerine 2-5 parts, tributyl phosphate 2-5 part, Methyl Benzene-o-dicarboxylate 5-7 part, MALEIC ANHYDRIDE 4-7 part, rosin 10-13 part.
Described a kind of waterproof coating, is characterized in that being made up of the raw material of following weight part: tetrabutyl phosphorus chloride 31-34 part, acrylate acrylate copolymer emulsion 21-24 part, PVDC latex 6.5-8.5 part, lime powder 18-19 part, styroyl phenol polyoxyethylene polyoxypropylene ether 7-8 part, alkyl benzene calcium sulfonate 8.5-9.5 part, dibutyl succinic acid sodium sulfonate 4.5-5.5 part, tartrate 6-7 part, dimethylbenzene 4-6 part, two Polyglycerine 3-4 parts, tributyl phosphate 3-4 part, Methyl Benzene-o-dicarboxylate 5.5-6.5 part, MALEIC ANHYDRIDE 5-6 part, rosin 11-12 part.
Described a kind of waterproof coating, is characterized in that being made up of the raw material of following weight part: tetrabutyl chlorination P33 part, 23 parts of acrylate acrylate copolymer emulsions, 7 parts, PVDC latex, 18.5 parts of lime powders, 7.5 parts, styroyl phenol polyoxyethylene polyoxypropylene ether, 9 parts of alkyl benzene calcium sulfonates, 5 parts of dibutyl succinic acid sodium sulfonates, 6.5 parts, tartrate, 5 parts of dimethylbenzene, 3.5 parts of two Polyglycerine, 3.5 parts of tributyl phosphates, 6 parts of Methyl Benzene-o-dicarboxylates, 5.5 parts of MALEIC ANHYDRIDE, 11.5 parts of rosin.
The present invention, compared with existing waterproof paint, can be used for roof waterproof, be difficult for aging, dry and cracked, be out of shape, fracture, layering; Can be for indoor waterproof, for complex-shaped place, easy construction, manifests protection well to seepage, need not reprocess for a long time, has increased the work-ing life of whole building buildings.
Embodiment
Embodiment 1
A kind of waterproof coating, is made up of the raw material of following weight part: 40 parts, tetrabutyl phosphorus chloride, 15 parts of acrylate acrylate copolymer emulsions, 5 parts, PVDC latex, 15 parts of lime powders, 5 parts, styroyl phenol polyoxyethylene polyoxypropylene ether, 6 parts of alkyl benzene calcium sulfonates, 2 parts of dibutyl succinic acid sodium sulfonates, 3 parts, tartrate, 2 parts of dimethylbenzene, 1 part of two Polyglycerine, 1 part of tributyl phosphate, 4 parts of Methyl Benzene-o-dicarboxylates, 3 parts of MALEIC ANHYDRIDE, 8 parts of rosin.
Embodiment 2
A kind of waterproof coating, is made up of the raw material of following weight part: 25 parts, tetrabutyl phosphorus chloride, 30 parts of acrylate acrylate copolymer emulsions, 10 parts, PVDC latex, 22 parts of lime powders, 10 parts, styroyl phenol polyoxyethylene polyoxypropylene ether, 12 parts of alkyl benzene calcium sulfonates, 8 parts of dibutyl succinic acid sodium sulfonates, 10 parts, tartrate, 8 parts of dimethylbenzene, 6 parts of two Polyglycerine, 6 parts of tributyl phosphates, 8 parts of Methyl Benzene-o-dicarboxylates, 8 parts of MALEIC ANHYDRIDE, 15 parts of rosin.
Embodiment 3
A kind of waterproof coating, is characterized in that being made up of the raw material of following weight part: 35 parts, tetrabutyl phosphorus chloride, 20 parts of acrylate acrylate copolymer emulsions, 6 parts, PVDC latex, 17 parts of lime powders, 6 parts, styroyl phenol polyoxyethylene polyoxypropylene ether, 8 parts of alkyl benzene calcium sulfonates, 4 parts of dibutyl succinic acid sodium sulfonates, 5 parts, tartrate, 3 parts of dimethylbenzene, 2 parts of two Polyglycerine, 2 parts of tributyl phosphates, 5 parts of Methyl Benzene-o-dicarboxylates, 4 parts of MALEIC ANHYDRIDE, 10 parts of rosin.
Embodiment 4
A kind of waterproof coating, is characterized in that being made up of the raw material of following weight part: 30 parts, tetrabutyl phosphorus chloride, 25 parts of acrylate acrylate copolymer emulsions, 9 parts, PVDC latex, 20 parts of lime powders, 9 parts, styroyl phenol polyoxyethylene polyoxypropylene ether, 10 parts of alkyl benzene calcium sulfonates, 6 parts of dibutyl succinic acid sodium sulfonates, 8 parts, tartrate, 7 parts of dimethylbenzene, 5 parts of two Polyglycerine, 5 parts of tributyl phosphates, 7 parts of Methyl Benzene-o-dicarboxylates, 7 parts of MALEIC ANHYDRIDE, 13 parts of rosin.
Embodiment 5
A kind of waterproof coating, is characterized in that being made up of the raw material of following weight part: 34 parts, tetrabutyl phosphorus chloride, 21 parts of acrylate acrylate copolymer emulsions, 6.5 parts, PVDC latex, 18 parts of lime powders, 7 parts, styroyl phenol polyoxyethylene polyoxypropylene ether, 8.5 parts of alkyl benzene calcium sulfonates, 4.5 parts of dibutyl succinic acid sodium sulfonates, 6 parts, tartrate, 4 parts of dimethylbenzene, 3 parts of two Polyglycerine, 3 parts of tributyl phosphates, 5.5 parts of Methyl Benzene-o-dicarboxylates, 5 parts of MALEIC ANHYDRIDE, 11 parts of rosin.
Embodiment 6
A kind of waterproof coating, is characterized in that being made up of the raw material of following weight part: 31 parts, tetrabutyl phosphorus chloride, 24 parts of acrylate acrylate copolymer emulsions, 8.5 parts, PVDC latex, 19 parts of lime powders, 8 parts, styroyl phenol polyoxyethylene polyoxypropylene ether, 9.5 parts of alkyl benzene calcium sulfonates, 5.5 parts of dibutyl succinic acid sodium sulfonates, 7 parts, tartrate, 6 parts of dimethylbenzene, 4 parts of two Polyglycerine, 4 parts of tributyl phosphates, 6.5 parts of Methyl Benzene-o-dicarboxylates, 6 parts of MALEIC ANHYDRIDE, 12 parts of rosin.
Embodiment 7
A kind of waterproof coating, is characterized in that being made up of the raw material of following weight part: tetrabutyl chlorination P33 part, 23 parts of acrylate acrylate copolymer emulsions, 7 parts, PVDC latex, 18.5 parts of lime powders, 7.5 parts, styroyl phenol polyoxyethylene polyoxypropylene ether, 9 parts of alkyl benzene calcium sulfonates, 5 parts of dibutyl succinic acid sodium sulfonates, 6.5 parts, tartrate, 5 parts of dimethylbenzene, 3.5 parts of two Polyglycerine, 3.5 parts of tributyl phosphates, 6 parts of Methyl Benzene-o-dicarboxylates, 5.5 parts of MALEIC ANHYDRIDE, 11.5 parts of rosin.
The present invention, compared with existing waterproof paint, can be used for roof waterproof, be difficult for aging, dry and cracked, be out of shape, fracture, layering; Can be for indoor waterproof, for complex-shaped place, easy construction, manifests protection well to seepage, need not reprocess for a long time, has increased the work-ing life of whole building buildings.