CN103693852B - 密着性强的金属塘瓷釉料 - Google Patents

密着性强的金属塘瓷釉料 Download PDF

Info

Publication number
CN103693852B
CN103693852B CN201310654346.9A CN201310654346A CN103693852B CN 103693852 B CN103693852 B CN 103693852B CN 201310654346 A CN201310654346 A CN 201310654346A CN 103693852 B CN103693852 B CN 103693852B
Authority
CN
China
Prior art keywords
mass parts
enamel
oxide
coat
adherence
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201310654346.9A
Other languages
English (en)
Other versions
CN103693852A (zh
Inventor
单佳
单永其
张文斌
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Foshan China made glaze Co., Ltd.
Original Assignee
CHANGSHU YONGDA CHEMICAL EQUIPMENT FACTORY
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by CHANGSHU YONGDA CHEMICAL EQUIPMENT FACTORY filed Critical CHANGSHU YONGDA CHEMICAL EQUIPMENT FACTORY
Priority to CN201310654346.9A priority Critical patent/CN103693852B/zh
Publication of CN103693852A publication Critical patent/CN103693852A/zh
Application granted granted Critical
Publication of CN103693852B publication Critical patent/CN103693852B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种密着性强的金属塘瓷釉料,包括塘瓷底釉和塘瓷面釉;本发明密着性强的金属塘瓷釉料,其塘瓷底釉涂覆在胚体上可以使得胚体具有耐高温的特性,同时具有较好的耐腐蚀性,釉面处在高温环境中,可长时间保持耐腐蚀的特性。

Description

密着性强的金属塘瓷釉料
技术领域
本发明涉及密着性强的金属塘瓷釉料。
背景技术
目前常用的金属塘瓷釉料,其瓷底釉和塘瓷面釉的性能都不是很理想。
发明内容
本发明的目的在于提供一种密着性强的金属塘瓷釉料,其塘瓷底釉涂覆在胚体上可以使得胚体具有耐高温的特性,同时具有较好的耐腐蚀性,釉面处在高温环境中,可长时间保持耐腐蚀的特性。
为实现上述目的,本发明的技术方案是设计一种密着性强的金属塘瓷釉料,包括塘瓷底釉和塘瓷面釉;
所述塘瓷面釉由如下组分组成:
1-2质量份三聚磷酸钠,
1-2质量份五氧化二磷,
5-6质量份氧化硼,
1-2质量份氧化钴,
1-2质量份氟硅酸钠,
4-5质量份氧化锌,
25质量份碳化硅,
1质量份三氧化二铝,
1质量份氟化钙,
30质量份一价碱性氧化物;
所述塘瓷底釉由如下组分组成:
1质量份焦磷酸钠,
2质量份钼酸钡,
65质量份二氧化硅,
13质量份三氧化二铝,
1.5质量份氧化钼,
1质量份三氧化二铁,
1质量份氧化锰,
12质量份氟化钙,
1质量份氟硅酸钠,
1质量份氧化锑,
23质量份一价碱性氧化物,
2.5质量份钼酸锌,
45质量份氧化硼。
本发明的优点和有益效果在于:提供一种密着性强的金属塘瓷釉料,其塘瓷底釉涂覆在胚体上可以使得胚体具有耐高温的特性,同时具有较好的耐腐蚀性,釉面处在高温环境中,可长时间保持耐腐蚀的特性。
具体实施方式
下面结合实施例,对本发明的具体实施方式作进一步描述。以下实施例仅用于更加清楚地说明本发明的技术方案,而不能以此来限制本发明的保护范围。
本发明具体实施的技术方案是:
实施例1
一种密着性强的金属塘瓷釉料,包括塘瓷底釉和塘瓷面釉;
所述塘瓷面釉由如下组分组成:
1质量份三聚磷酸钠,
1质量份五氧化二磷,
5质量份氧化硼,
1质量份氧化钴,
1质量份氟硅酸钠,
4质量份氧化锌,
25质量份碳化硅,
1质量份三氧化二铝,
1质量份氟化钙,
30质量份一价碱性氧化物;
所述塘瓷底釉由如下组分组成:
1质量份焦磷酸钠,
2质量份钼酸钡,
65质量份二氧化硅,
13质量份三氧化二铝,
1.5质量份氧化钼,
1质量份三氧化二铁,
1质量份氧化锰,
12质量份氟化钙,
1质量份氟硅酸钠,
1质量份氧化锑,
23质量份一价碱性氧化物,
2.5质量份钼酸锌,
45质量份氧化硼。
实施例2
一种密着性强的金属塘瓷釉料,包括塘瓷底釉和塘瓷面釉;
所述塘瓷面釉由如下组分组成:
2质量份三聚磷酸钠,
2质量份五氧化二磷,
6质量份氧化硼,
2质量份氧化钴,
2质量份氟硅酸钠,
5质量份氧化锌,
25质量份碳化硅,
1质量份三氧化二铝,
1质量份氟化钙,
30质量份一价碱性氧化物;
所述塘瓷底釉由如下组分组成:
1质量份焦磷酸钠,
2质量份钼酸钡,
65质量份二氧化硅,
13质量份三氧化二铝,
1.5质量份氧化钼,
1质量份三氧化二铁,
1质量份氧化锰,
12质量份氟化钙,
1质量份氟硅酸钠,
1质量份氧化锑,
23质量份一价碱性氧化物,
2.5质量份钼酸锌,
45质量份氧化硼。
实施例3
一种密着性强的金属塘瓷釉料,包括塘瓷底釉和塘瓷面釉;
所述塘瓷面釉由如下组分组成:
1.2质量份三聚磷酸钠,
1.2质量份五氧化二磷,
5.6质量份氧化硼,
1.2质量份氧化钴,
1.2质量份氟硅酸钠,
4.5质量份氧化锌,
25质量份碳化硅,
1质量份三氧化二铝,
1质量份氟化钙,
30质量份一价碱性氧化物;
所述塘瓷底釉由如下组分组成:
1质量份焦磷酸钠,
2质量份钼酸钡,
65质量份二氧化硅,
13质量份三氧化二铝,
1.5质量份氧化钼,
1质量份三氧化二铁,
1质量份氧化锰,
12质量份氟化钙,
1质量份氟硅酸钠,
1质量份氧化锑,
23质量份一价碱性氧化物,
2.5质量份钼酸锌,
45质量份氧化硼。
以上所述仅是本发明的优选实施方式,应当指出,对于本技术领域的普通技术人员来说,在不脱离本发明技术原理的前提下,还可以做出若干改进和润饰,这些改进和润饰也应视为本发明的保护范围。

Claims (1)

1.密着性强的金属塘瓷釉料,其特征在于,包括塘瓷底釉和塘瓷面釉;
所述塘瓷面釉由如下组分组成:
1-2质量份三聚磷酸钠,
1-2质量份五氧化二磷,
5-6质量份氧化硼,
1-2质量份氧化钴,
1-2质量份氟硅酸钠,
4-5质量份氧化锌,
25质量份碳化硅,
1质量份三氧化二铝,
1质量份氟化钙,
30质量份一价碱性氧化物;
所述塘瓷底釉由如下组分组成:
1质量份焦磷酸钠,
2质量份钼酸钡,
65质量份二氧化硅,
13质量份三氧化二铝,
1.5质量份氧化钼,
1质量份三氧化二铁,
1质量份氧化锰,
12质量份氟化钙,
1质量份氟硅酸钠,
1质量份氧化锑,
23质量份一价碱性氧化物,
2.5质量份钼酸锌,
45质量份氧化硼。
CN201310654346.9A 2013-12-09 2013-12-09 密着性强的金属塘瓷釉料 Active CN103693852B (zh)