CN103663743A - Composite corrosion and scale inhibitor for circulating cooling water - Google Patents
Composite corrosion and scale inhibitor for circulating cooling water Download PDFInfo
- Publication number
- CN103663743A CN103663743A CN201310664274.6A CN201310664274A CN103663743A CN 103663743 A CN103663743 A CN 103663743A CN 201310664274 A CN201310664274 A CN 201310664274A CN 103663743 A CN103663743 A CN 103663743A
- Authority
- CN
- China
- Prior art keywords
- parts
- cooling water
- corrosion
- composite slow
- scale resistor
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention belongs to the technical field of water treatment, and particularly relates to a composite corrosion and scale inhibitor for circulating cooling water. The composite corrosion and scale inhibitor for circulating cooling water is prepared from the following components in parts by weight: zinc sulfate, sodium salicylate, sulfhydryl benzotriazole, 2-phosphonobutane-1,2,4-tricarboxylic acid and maleic acid-acrylic acid copolymer. The composite corrosion and scale inhibitor is convenient to use, and has the advantages of small toxicity, no smell and favorable dispersibility.
Description
Technical field
The invention belongs to the technical field of water treatment, be specifically related to a kind of composite slow-corrosion scale resistor for recirculated cooling water.
Background technology
Recirculated cooling water plays the important and pivotal role in cooling system, but recirculated cooling water intensity used is high, basicity is large, have serious scale feature, under the various occasions of water temperature higher than envrionment temperature, the fouling meeting of the inorganic salt such as calcium carbonate brings serious consequence.While being used for industrial cooling circulating water system using it as heat-eliminating medium, can cause water quality deterioration, the problems such as corrosion and scaling occur, cause heat exchanger and line clogging or leakage, have a strong impact on production equipment and normally move.Along with the socioeconomic progress developing rapidly with technology, water technology comes into one's own day by day, by using effectively protection against corrosion and prevent fouling of water treatment agent, thus the utilization ratio of raising equipment and water and reach the object of saving water source and the energy.At present increasingly strict to the water treatment standard of corrosion-mitigation scale-inhibition, the feature of environmental protection of additive has also been proposed to high requirement simultaneously.
Summary of the invention
The object of the invention is to for the defect of above-mentioned existence and a kind of composite slow-corrosion scale resistor for recirculated cooling water is provided, this composite slow-corrosion scale resistor is easy to use, and toxicity is little, and tasteless dispersing property is good.
Technical scheme of the present invention is: a kind of composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
4~11 parts, zinc sulfate
1.5~6 parts of sodium salicylates
6~14 parts of sulfydryl benzotriazoles
2-phosphonate group-1,1~2 part of 2,4-butane tricarboxylate
1~3.5 part of maleic acid-acrylic acid copolymer.
The described composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
5.7 parts, zinc sulfate
2.4 parts of sodium salicylates
7.3 parts of sulfydryl benzotriazoles
2-phosphonate group-1,1.2 parts of 2,4-butane tricarboxylates
1.6 parts of maleic acid-acrylic acid copolymers.
The described composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
6.4 parts, zinc sulfate
3.8 parts of sodium salicylates
8.4 parts of sulfydryl benzotriazoles
2-phosphonate group-1,1.32 parts of 2,4-butane tricarboxylates
2.26 parts of maleic acid-acrylic acid copolymers.
The described composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
8.35 parts, zinc sulfate
4.1 parts of sodium salicylates
11.5 parts of sulfydryl benzotriazoles
2-phosphonate group-1,1.18 parts of 2,4-butane tricarboxylates
1.9 parts of maleic acid-acrylic acid copolymers.
The described composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
9.62 parts, zinc sulfate
4.7 parts of sodium salicylates
12.3 parts of sulfydryl benzotriazoles
2-phosphonate group-1,1.46 parts of 2,4-butane tricarboxylates
2.78 parts of maleic acid-acrylic acid copolymers.
Beneficial effect of the present invention is: the component toxicity of the composite slow-corrosion scale resistor for recirculated cooling water of the present invention is little, little to environmental influence, there is good corrosion inhibition, prevent the corrosion of recirculated cooling water to metallic conduit, corrosion mitigating effect reaches 99.1%~99.7%, makes its corrosion rate be reduced to 0.00247~0.0031mm/a; Also there is good scale inhibition effect simultaneously.
In sum, described composite slow-corrosion scale resistor is easy to use, and toxicity is little, and tasteless dispersing property is good.
Embodiment
Below by specific embodiment, the present invention will be described in detail.
Embodiment 1
For a composite slow-corrosion scale resistor for recirculated cooling water, by the component of following weight part, formed:
4 parts, zinc sulfate
1.5 parts of sodium salicylates
6 parts of sulfydryl benzotriazoles
2-phosphonate group-1,1 part of 2,4-butane tricarboxylate
1 part of maleic acid-acrylic acid copolymer.
Described in employing embodiment 1, composite slow-corrosion scale resistor makes corrosion mitigating effect reach 99.1%, makes its corrosion rate be reduced to 0.0031mm/a.
Embodiment 2
The described composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
5.7 parts, zinc sulfate
2.4 parts of sodium salicylates
7.3 parts of sulfydryl benzotriazoles
2-phosphonate group-1,1.2 parts of 2,4-butane tricarboxylates
1.6 parts of maleic acid-acrylic acid copolymers.
Described in employing embodiment 2, composite slow-corrosion scale resistor makes corrosion mitigating effect reach 99.21%, makes its corrosion rate be reduced to 0.0026mm/a.
Embodiment 3
The described composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
6.4 parts, zinc sulfate
3.8 parts of sodium salicylates
8.4 parts of sulfydryl benzotriazoles
2-phosphonate group-1,1.32 parts of 2,4-butane tricarboxylates
2.26 parts of maleic acid-acrylic acid copolymers.
Described in employing embodiment 3, composite slow-corrosion scale resistor makes corrosion mitigating effect reach 99.3%, makes its corrosion rate be reduced to 0.00253mm/a.
Embodiment 4
The described composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
8.35 parts, zinc sulfate
4.1 parts of sodium salicylates
11.5 parts of sulfydryl benzotriazoles
2-phosphonate group-1,1.18 parts of 2,4-butane tricarboxylates
1.9 parts of maleic acid-acrylic acid copolymers.
Described in employing embodiment 4, composite slow-corrosion scale resistor makes corrosion mitigating effect reach 99.63%, makes its corrosion rate be reduced to 0.00248mm/a.
Embodiment 5
The described composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
9.62 parts, zinc sulfate
4.7 parts of sodium salicylates
12.3 parts of sulfydryl benzotriazoles
2-phosphonate group-1,1.46 parts of 2,4-butane tricarboxylates
2.78 parts of maleic acid-acrylic acid copolymers.
Described in employing embodiment 5, composite slow-corrosion scale resistor makes corrosion mitigating effect reach 99.66%, makes its corrosion rate be reduced to 0.00251mm/a.
Embodiment 6
For a composite slow-corrosion scale resistor for recirculated cooling water, by the component of following weight part, formed:
11 parts, zinc sulfate
6 parts of sodium salicylates
14 parts of sulfydryl benzotriazoles
2-phosphonate group-1,2 parts of 2,4-butane tricarboxylates
3.5 parts of maleic acid-acrylic acid copolymers.
Described in employing embodiment 6, composite slow-corrosion scale resistor makes corrosion mitigating effect reach 99.7%, makes its corrosion rate be reduced to 0.00247mm/a.
Claims (5)
1. for a composite slow-corrosion scale resistor for recirculated cooling water, it is characterized in that, by the component of following weight part, formed:
4~11 parts, zinc sulfate
1.5~6 parts of sodium salicylates
6~14 parts of sulfydryl benzotriazoles
2-phosphonate group-1,1~2 part of 2,4-butane tricarboxylate
1~3.5 part of maleic acid-acrylic acid copolymer.
2. according to claim 1 for the composite slow-corrosion scale resistor of recirculated cooling water, it is characterized in that, by the component of following weight part, formed:
5.7 parts, zinc sulfate
2.4 parts of sodium salicylates
7.3 parts of sulfydryl benzotriazoles
2-phosphonate group-1,1.2 parts of 2,4-butane tricarboxylates
1.6 parts of maleic acid-acrylic acid copolymers.
3. according to claim 1 for the composite slow-corrosion scale resistor of recirculated cooling water, it is characterized in that, by the component of following weight part, formed:
6.4 parts, zinc sulfate
3.8 parts of sodium salicylates
8.4 parts of sulfydryl benzotriazoles
2-phosphonate group-1,1.32 parts of 2,4-butane tricarboxylates
2.26 parts of maleic acid-acrylic acid copolymers.
4. according to claim 1 for the composite slow-corrosion scale resistor of recirculated cooling water, it is characterized in that, by the component of following weight part, formed:
8.35 parts, zinc sulfate
4.1 parts of sodium salicylates
11.5 parts of sulfydryl benzotriazoles
2-phosphonate group-1,1.18 parts of 2,4-butane tricarboxylates
1.9 parts of maleic acid-acrylic acid copolymers.
5. according to claim 1 for the composite slow-corrosion scale resistor of recirculated cooling water, it is characterized in that, by the component of following weight part, formed:
9.62 parts, zinc sulfate
4.7 parts of sodium salicylates
12.3 parts of sulfydryl benzotriazoles
2-phosphonate group-1,1.46 parts of 2,4-butane tricarboxylates
2.78 parts of maleic acid-acrylic acid copolymers.