CN103663739A - Composite corrosion and scale inhibitor used for circulating cooling water - Google Patents

Composite corrosion and scale inhibitor used for circulating cooling water Download PDF

Info

Publication number
CN103663739A
CN103663739A CN201310661856.9A CN201310661856A CN103663739A CN 103663739 A CN103663739 A CN 103663739A CN 201310661856 A CN201310661856 A CN 201310661856A CN 103663739 A CN103663739 A CN 103663739A
Authority
CN
China
Prior art keywords
cooling water
corrosion
scale inhibitor
composite slow
parts
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201310661856.9A
Other languages
Chinese (zh)
Inventor
牟军平
朱娜
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
SHANDONG HWAYA ENVIRONMENTAL PROTECTION TECHNOLOGY Co Ltd
Original Assignee
SHANDONG HWAYA ENVIRONMENTAL PROTECTION TECHNOLOGY Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by SHANDONG HWAYA ENVIRONMENTAL PROTECTION TECHNOLOGY Co Ltd filed Critical SHANDONG HWAYA ENVIRONMENTAL PROTECTION TECHNOLOGY Co Ltd
Priority to CN201310661856.9A priority Critical patent/CN103663739A/en
Publication of CN103663739A publication Critical patent/CN103663739A/en
Pending legal-status Critical Current

Abstract

The invention belongs to the technical field of water processing, and specially relates to a composite corrosion and scale inhibitor used for circulating cooling water. The composite corrosion and scale inhibitor used for circulating cooling water comprises following ingredients, by weight, 11 to 17 parts of sodium tetraborate, 6 to 10 parts of sodium benzoate, 5 to 9 parts of maleic anhydride-sulfonated styrene copolymer, 2.7 to 3.8 parts of methylbenzotriazole, and 3.1 to 4.5 parts of 2-hydroxyphosphonoacetic acid. The composite corrosion and scale inhibitor is convenient for using, is low in toxicity, is high in dispersity, and is smell-less.

Description

A kind of composite slow-corrosion scale resistor for recirculated cooling water
Technical field
The invention belongs to the technical field of water treatment, be specifically related to a kind of composite slow-corrosion scale resistor for recirculated cooling water.
Background technology
Recirculated cooling water plays the important and pivotal role in cooling system, but recirculated cooling water intensity used is high, basicity is large, have serious scale feature, under the various occasions of water temperature higher than envrionment temperature, the fouling meeting of the inorganic salt such as calcium carbonate brings serious consequence.While being used for industrial cooling circulating water system using it as heat-eliminating medium, can cause water quality deterioration, the problems such as corrosion and scaling occur, cause heat exchanger and line clogging or leakage, have a strong impact on production equipment and normally move.Along with the socioeconomic progress developing rapidly with technology, water technology comes into one's own day by day, by using effectively protection against corrosion and prevent fouling of water treatment agent, thus the utilization ratio of raising equipment and water and reach the object of saving water source and the energy.At present increasingly strict to the water treatment standard of corrosion-mitigation scale-inhibition, the feature of environmental protection of additive has also been proposed to high requirement simultaneously.
Summary of the invention
The object of the invention is to for the defect of above-mentioned existence and a kind of composite slow-corrosion scale resistor for recirculated cooling water is provided, this composite slow-corrosion scale resistor is easy to use, and toxicity is little, and tasteless dispersing property is good.
Technical scheme of the present invention is: a kind of composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
The described composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
Figure BDA0000433370120000012
The described composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
Figure BDA0000433370120000021
The described composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
Figure BDA0000433370120000022
The described composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
Beneficial effect of the present invention is: the component toxicity of the composite slow-corrosion scale resistor for recirculated cooling water of the present invention is little, little to environmental influence, there is good corrosion inhibition, prevent the corrosion of recirculated cooling water to metallic conduit, corrosion mitigating effect reaches 98.8%~99.6%, makes its corrosion rate be reduced to 0.0019~0.0021mm/a; Also there is good scale inhibition effect simultaneously.
In sum, described composite slow-corrosion scale resistor is easy to use, and toxicity is little, and tasteless dispersing property is good.
Embodiment
Below by specific embodiment, the present invention will be described in detail.
Embodiment 1
For a composite slow-corrosion scale resistor for recirculated cooling water, by the component of following weight part, formed:
Figure BDA0000433370120000031
Described in employing embodiment 1, composite slow-corrosion scale resistor makes corrosion mitigating effect reach 98.8%, makes its corrosion rate be reduced to 0.0021mm/a.
Embodiment 2
The described composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
Figure BDA0000433370120000032
Described in employing embodiment 2, composite slow-corrosion scale resistor makes corrosion mitigating effect reach 98.92%, makes its corrosion rate be reduced to 0.00203mm/a.
Embodiment 3
The described composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
Figure BDA0000433370120000033
Described in employing embodiment 3, composite slow-corrosion scale resistor makes corrosion mitigating effect reach 99.15%, makes its corrosion rate be reduced to 0.00209mm/a.
Embodiment 4
The described composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
Figure BDA0000433370120000034
Described in employing embodiment 4, composite slow-corrosion scale resistor makes corrosion mitigating effect reach 99.38%, makes its corrosion rate be reduced to 0.00193mm/a.
Embodiment 5
The described composite slow-corrosion scale resistor for recirculated cooling water, is comprised of the component of following weight part:
Figure BDA0000433370120000041
Described in employing embodiment 5, composite slow-corrosion scale resistor makes corrosion mitigating effect reach 99.47%, makes its corrosion rate be reduced to 0.00198mm/a.
Embodiment 6
For a composite slow-corrosion scale resistor for recirculated cooling water, by the component of following weight part, formed:
Described in employing embodiment 6, composite slow-corrosion scale resistor makes corrosion mitigating effect reach 99.6%, makes its corrosion rate be reduced to 0.0019mm/a.

Claims (5)

1. for a composite slow-corrosion scale resistor for recirculated cooling water, it is characterized in that, by the component of following weight part, formed:
Figure FDA0000433370110000011
2. according to claim 1 for the composite slow-corrosion scale resistor of recirculated cooling water, it is characterized in that, by the component of following weight part, formed:
Figure FDA0000433370110000012
3. according to claim 1 for the composite slow-corrosion scale resistor of recirculated cooling water, it is characterized in that, by the component of following weight part, formed:
Figure FDA0000433370110000013
4. according to claim 1 for the composite slow-corrosion scale resistor of recirculated cooling water, it is characterized in that, by the component of following weight part, formed:
5. according to claim 1 for the composite slow-corrosion scale resistor of recirculated cooling water, it is characterized in that, by the component of following weight part, formed:
Figure FDA0000433370110000015
CN201310661856.9A 2013-12-09 2013-12-09 Composite corrosion and scale inhibitor used for circulating cooling water Pending CN103663739A (en)