Summary of the invention
The technical problem to be solved in the present invention provides and a kind ofly prepares the igelite tackiness agent with waste polystyrene foam and waste polyvinyl chloride, this preparation method substitutes the part polyvinyl chloride with the waste polystyrene foam, through reasonable proportioning, make the igelite tackiness agent by certain technological process.
The technical problem to be solved in the present invention is solved by following scheme: waste polystyrene foam and waste polyvinyl chloride prepare the igelite tackiness agent, it is characterized in that: pimelinketone and tetrahydrofuran (THF) are mixed with mixed solvent, add waste polyvinyl chloride, placement is spent the night, under stirring it is fully dissolved, add dibutyl phthalate, stir, make polyvinyl chloride solution; In toluene, add the waste polystyrene foam, stir and made its dissolving in 1 hour, make polystyrene solution; Polyvinyl chloride solution and polystyrene solution are mixed, stirred 0.5 hour, discharging, packing namely gets product, and wherein the mass ratio of pimelinketone, tetrahydrofuran (THF), waste polyvinyl chloride, dibutyl phthalate, toluene and waste polystyrene is 1:1:0.4: 0.04:2:0.4-2.0.
The waste polyvinyl chloride that above-mentioned waste polystyrene foam and waste polyvinyl chloride prepare in the igelite tackiness agent refers to waste polyvinyl chloride tubing, sheet material and film etc., and the waste polystyrene foam refers to: the waste polystyrene foam that wrapping waste polystyrene foam and disposable lunch-box are used etc.
Advantage of the present invention is: 1, because with waste polystyrene foam instead of part polyvinyl chloride, particularly the dissolved polystyrene foam can use cheap toluene, therefore can reduce the usage quantity of pimelinketone and tetrahydrofuran (THF), it is very low to prepare the cost of polyvinyl chloride adhesive with present method.2, a large amount of waste polystyrene foams that can effectively utilize the city to produce are made rational use of resources and are alleviated the pollution that waste causes.
Embodiment
In the mixed solvent that embodiment 1:25g pimelinketone and 25g tetrahydrofuran (THF) form, add the 10g polyvinyl chloride, placement is spent the night, and under stirring it is fully dissolved, and adds the 1g dibutyl phthalate, stirs, and makes polyvinyl chloride solution; In 50g toluene, add 50 g waste polystyrene foams, stir and made its dissolving in 1 hour, make polystyrene solution; Above-mentioned polyvinyl chloride solution and polystyrene solution are mixed, stirred 0.5 hour, discharging, packing namely gets product.
In the mixed solvent that embodiment 2:25g pimelinketone and 25g tetrahydrofuran (THF) form, add the 10g polyvinyl chloride, placement is spent the night, and under stirring it is fully dissolved, and adds the 1g dibutyl phthalate, stirs, and makes polyvinyl chloride solution; In 50g toluene, add 45 g waste polystyrene foams, stir and made its dissolving in 1 hour, make polystyrene solution; Above-mentioned polyvinyl chloride solution and polystyrene solution are mixed, stirred 0.5 hour, discharging, packing namely gets product.
In the mixed solvent that embodiment 3:25g pimelinketone and 25g tetrahydrofuran (THF) form, add the 10g polyvinyl chloride, placement is spent the night, and under stirring it is fully dissolved, and adds the 1g dibutyl phthalate, stirs, and makes polyvinyl chloride solution; In 50g toluene, add 40 g waste polystyrene foams, stir and made its dissolving in 1 hour, make polystyrene solution; Above-mentioned polyvinyl chloride solution and polystyrene solution are mixed, stirred 0.5 hour, discharging, packing namely gets product.
In the mixed solvent that embodiment 4:25g pimelinketone and 25g tetrahydrofuran (THF) form, add the 10g polyvinyl chloride, placement is spent the night, and under stirring it is fully dissolved, and adds the 1g dibutyl phthalate, stirs, and makes polyvinyl chloride solution; In 50g toluene, add 35 g waste polystyrene foams, stir and made its dissolving in 1 hour, make polystyrene solution; Above-mentioned polyvinyl chloride solution and polystyrene solution are mixed, stirred 0.5 hour, discharging, packing namely gets product.
In the mixed solvent that embodiment 5:25g pimelinketone and 25g tetrahydrofuran (THF) form, add the 10g polyvinyl chloride, placement is spent the night, and under stirring it is fully dissolved, and adds the 1g dibutyl phthalate, stirs, and makes polyvinyl chloride solution; In 50g toluene, add 30 g waste polystyrene foams, stir and made its dissolving in 1 hour, make polystyrene solution; Above-mentioned polyvinyl chloride solution and polystyrene solution are mixed, stirred 0.5 hour, discharging, packing namely gets product.
In the mixed solvent that embodiment 6:25g pimelinketone and 25g tetrahydrofuran (THF) form, add the 10g polyvinyl chloride, placement is spent the night, and under stirring it is fully dissolved, and adds the 1g dibutyl phthalate, stirs, and makes polyvinyl chloride solution; In 50g toluene, add 25 g waste polystyrene foams, stir and made its dissolving in 1 hour, make polystyrene solution; Above-mentioned polyvinyl chloride solution and polystyrene solution are mixed, stirred 0.5 hour, discharging, packing namely gets product.
In the mixed solvent that embodiment 7:25g pimelinketone and 25g tetrahydrofuran (THF) form, add the 10g polyvinyl chloride, placement is spent the night, and under stirring it is fully dissolved, and adds the 1g dibutyl phthalate, stirs, and makes polyvinyl chloride solution; In 50g toluene, add 20 g waste polystyrene foams, stir and made its dissolving in 1 hour, make polystyrene solution; Above-mentioned polyvinyl chloride solution and polystyrene solution are mixed, stirred 0.5 hour, discharging, packing namely gets product.
In the mixed solvent that embodiment 8:25g pimelinketone and 25g tetrahydrofuran (THF) form, add the 10g polyvinyl chloride, placement is spent the night, and under stirring it is fully dissolved, and adds the 1g dibutyl phthalate, stirs, and makes polyvinyl chloride solution; In 50g toluene, add 15 g waste polystyrene foams, stir and made its dissolving in 1 hour, make polystyrene solution; Above-mentioned polyvinyl chloride solution and polystyrene solution are mixed, stirred 0.5 hour, discharging, packing namely gets product.
In the mixed solvent that embodiment 9:25g pimelinketone and 25g tetrahydrofuran (THF) form, add the 10g polyvinyl chloride, placement is spent the night, and under stirring it is fully dissolved, and adds the 1g dibutyl phthalate, stirs, and makes polyvinyl chloride solution; In 50g toluene, add 10 g waste polystyrene foams, stir and made its dissolving in 1 hour, make polystyrene solution; Above-mentioned polyvinyl chloride solution and polystyrene solution are mixed, stirred 0.5 hour, discharging, packing namely gets product.