CN103132483A - 一种能净化水质的轻质砖及其制备方法 - Google Patents

一种能净化水质的轻质砖及其制备方法 Download PDF

Info

Publication number
CN103132483A
CN103132483A CN2013100382317A CN201310038231A CN103132483A CN 103132483 A CN103132483 A CN 103132483A CN 2013100382317 A CN2013100382317 A CN 2013100382317A CN 201310038231 A CN201310038231 A CN 201310038231A CN 103132483 A CN103132483 A CN 103132483A
Authority
CN
China
Prior art keywords
brick
light
weight
purify water
mixed material
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN2013100382317A
Other languages
English (en)
Other versions
CN103132483B (zh
Inventor
林小明
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Guangdong spring ecological science and Technology Group Co., Ltd.
Original Assignee
Dongguan Yueyuan Packaging Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Dongguan Yueyuan Packaging Co Ltd filed Critical Dongguan Yueyuan Packaging Co Ltd
Priority to CN201310038231.7A priority Critical patent/CN103132483B/zh
Publication of CN103132483A publication Critical patent/CN103132483A/zh
Application granted granted Critical
Publication of CN103132483B publication Critical patent/CN103132483B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明属于轻质砖技术领域,尤其涉及一种能净化水质的轻质砖,该种能净化水质的轻质砖,所述轻质砖包括砖壳和设置于砖壳内的砖芯,所述砖芯为活性碳,所述砖壳的原料采用污泥、建筑垃圾、钾长石粉、粉煤灰和水泥制成。本发明制得的轻质砖不仅质轻,而且具有很好的净化水质的功能,应用于筑河拦坝可以维持持久的生态平衡,常年水质清澈碧绿。

Description

一种能净化水质的轻质砖及其制备方法
技术领域
 本发明属于轻质砖技术领域,尤其涉及一种能净化水质的轻质砖。
背景技术
现有的砖块大都是以粘土和其它辅助材料搅拌均匀后通过压块机成型,然后烧制而成的,现有的砖块比较重,搬运费力。
后来随着技术的发展,出现了一些轻质砖,如中国发明专利申请200910027910.8公开了一种轻质节能保温砖,由下列重量份原料:低热量粗渣20-40份,粉煤灰20-30份,脱硫石膏5-20份,保温陶粒10-30份,木质纤维素1-5份,水泥10-20份,石英砂5-15份,水适量,经搅拌混合、挤压成型、养护后制得;中国发明专利申请200910117099.2公开了一种抗震轻型墙体砖的制造方法,是将页岩(粘土)、陶粒、煤矿石、锯末粉按一定比例(陶粒占60%-70%,页岩占15%-20%,煤矿石占7.5%-10%,锯末粉占7.5%-10%)加水搅拌均匀后进行挤型压制成长方体砖块,将长方体砖块在900℃-1300℃的温度下进行烧结出窑。
但是以上这些砖都没有净化功能,特别是当这些砖用于筑河拦坝时,由于水无法流动,时间长了容易造成水质变差,严重影响了正常的生态平衡。
发明内容
本发明的目的在于针对现有技术的不足而提供一种能净化水质的轻质砖。
为了实现上述目的,本发明采用如下技术方案。
 一种能净化水质的轻质砖,所述轻质砖包括砖壳和设置于砖壳内的砖芯, 
所述砖芯为活性碳,所述砖壳的原料采用污泥、建筑垃圾、钾长石粉、粉煤灰和水泥制成。
所述污泥为池塘污泥、印染污泥或糖厂污泥,这些污泥含有大量的有机成分,在焙烧颗粒中产生不连通的空隙,不仅降低轻质砖的容重,也有利于水分的透过。
所述活性碳为颗粒型活性碳。
所述建筑垃圾为砖、瓦、石块、土和混凝土块中的一种或两种以上按任意比例混合。
所述砖壳的原料具体包括以下重量份的原料:
污泥         50-60份
建筑垃圾      40-50份     
钾长石粉      40-60份
粉煤灰        20-30份   
水泥          40-50份。
所述砖壳中加入生物质焦和硅藻土,生物质焦和硅藻土内部含有大量的孔道,不仅使制得的轻质砖质轻,更有利于水分的透过。
优选的,所述砖壳的原料具体包括以下重量份的原料:
污泥         40-50份
建筑垃圾      50-60份     
钾长石粉      40-60份
生物质焦      10-20份
硅藻土        10-20份
粉煤灰        20-30份   
水泥          40-50份。
所述能净化水质的轻质砖的制备方法,它包括以下制备步骤:
a、将配方量的建筑垃圾粉碎至200目以下,与配方量的污泥、钾长石粉混合均匀后造粒,在1200-1400℃焙烧20-40分钟,冷却后得到焙烧颗粒;
b、将步骤a得到的焙烧颗粒与配方量的水泥和粉煤灰在搅拌机中搅拌均匀,得到混合物料;
c、加入占步骤b混合物料10%-30%重量百分比的水继续搅拌至均匀,得到待用混合物料;
d、将步骤c得到的待用混合物料和活性碳加入模型中成型、脱模和养护,得到所述的能净化水质的轻质砖。
优选的,所述能净化水质的轻质砖的制备方法,它包括以下制备步骤:
a、将配方量的建筑垃圾粉碎至200目以下,与配方量的污泥、钾长石粉混合均匀后造粒,在1200-1400℃焙烧20-40分钟,冷却后得到焙烧颗粒;
b、将步骤a得到的焙烧颗粒与配方量的水泥、粉煤灰、硅藻土和生物质焦在搅拌机中搅拌均匀,得到混合物料;
c、加入占步骤b混合物料10%-30%重量百分比的水继续搅拌至均匀,得到待用混合物料;
d、将步骤c得到的待用混合物料和活性碳加入模型中成型、脱模和养护,得到所述的能净化水质的轻质砖。 
与现有技术相比,本发明具有如下有益效果:
(1)本发明的轻质砖包括砖壳和设置于砖壳内的砖芯,砖壳使用的污泥含有大量的有机成分,在焙烧颗粒中产生不连通的空隙,不仅使制得的轻质砖质轻,更有利于水分透过砖壳,经过砖芯的活性碳,达到有效净化水质的目的。  
(2)本发明使用大量建筑垃圾、污泥和粉煤灰,制得的产品成本低,经济效益高,不仅可以变废为宝,而且有利于改善环境污染,符合我国固体废物处理的无害化、减量化和资源化原则,具有显著的经济效益和社会效益。
(3)本发明制备工艺通过几个步骤分别对污泥、硅藻土和生物质焦、活性碳进行处理,使制得的轻质砖净化水质的效果最佳。总之,本发明制得的轻质砖不仅质轻,而且具有很好的净化水质的功能,应用于筑河拦坝可以维持长久的生态平衡,常年水质清澈碧绿。
具体实施方式
为了便于本领域技术人员的理解,下面结合实施例对本发明作进一步的说明,实施例提及的内容并非对本发明的限定。
实施例1。
一种能净化水质的轻质砖,所述轻质砖包括砖壳和设置于砖壳内的砖芯, 
所述砖芯为颗粒型活性碳,所述砖壳的原料具体包括以下重量份的原料:印染污泥50㎏、建筑垃圾40㎏、钾长石粉40㎏、粉煤灰20㎏、水泥40㎏。
所述建筑垃圾为砖、石块、土和混凝土块中的混合物。
所述能净化水质的轻质砖的制备方法,它包括以下制备步骤:
a、将配方量的建筑垃圾粉碎至200目以下,与配方量的印染污泥、钾长石粉混合均匀后造粒,在1200℃焙烧40分钟,冷却后得到焙烧颗粒;
b、将步骤a得到的焙烧颗粒与配方量的水泥和粉煤灰在搅拌机中搅拌均匀,得到混合物料;
c、加入占步骤b混合物料10%重量百分比的水继续搅拌至均匀,得到待用混合物料;
d、根据轻质砖的大小,取步骤c得到的待用混合物料和活性碳加入模型中,活性碳的用量占整个砖壳体积的三分之一,最后经成型、脱模和养护,得到所述的能净化水质的轻质砖。
应用本实施例的技术方案所制得的轻质砖,容重为280kg/m3,应用于筑河拦坝可以维持长久的生态平衡,常年水质清澈碧绿。
实施例2。
一种能净化水质的轻质砖,所述轻质砖包括砖壳和设置于砖壳内的砖芯, 
所述砖芯为颗粒型活性碳,所述砖壳的原料具体包括以下重量份的原料:池塘污泥55㎏、建筑垃圾45㎏、钾长石粉50㎏、粉煤灰25㎏、水泥45㎏。
所述建筑垃圾为瓦、土和混凝土块中的混合物。
所述能净化水质的轻质砖的制备方法,它包括以下制备步骤:
a、将配方量的建筑垃圾粉碎至200目以下,与配方量的池塘污泥、钾长石粉混合均匀后造粒,在1300℃焙烧30分钟,冷却后得到焙烧颗粒;
b、将步骤a得到的焙烧颗粒与配方量的水泥和粉煤灰在搅拌机中搅拌均匀,得到混合物料;
c、加入占步骤b混合物料20%重量百分比的水继续搅拌至均匀,得到待用混合物料;
d、根据轻质砖的大小,取步骤c得到的待用混合物料和活性碳加入模型中,活性碳的用量占整个砖壳体积的四分之一,最后经成型、脱模和养护,得到所述的能净化水质的轻质砖。
应用本实施例的技术方案所制得的轻质砖,容重为290kg/m3,应用于筑河拦坝可以维持长久的生态平衡,常年水质清澈碧绿。
实施例3。
一种能净化水质的轻质砖,所述轻质砖包括砖壳和设置于砖壳内的砖芯, 
所述砖芯为颗粒型活性碳,所述砖壳的原料具体包括以下重量份的原料:糖厂污泥50㎏、建筑垃圾60㎏、钾长石粉60㎏、生物质焦20㎏、硅藻土20㎏、粉煤灰30㎏、水泥50㎏。
所述能净化水质的轻质砖的制备方法,它包括以下制备步骤:
a、将配方量的建筑垃圾粉碎至200目以下,所述建筑垃圾为砖、土和混凝土块中的混合物,与配方量的污泥、钾长石粉混合均匀后造粒,在1400℃焙烧40分钟,冷却后得到焙烧颗粒;
b、将步骤a得到的焙烧颗粒与配方量的糖厂水泥、粉煤灰、硅藻土和生物质焦在搅拌机中搅拌均匀,得到混合物料;
c、加入占步骤b混合物料10%重量百分比的水继续搅拌至均匀,得到待用混合物料;
d、根据轻质砖的大小,取步骤c得到的待用混合物料和活性碳加入模型中,活性碳的用量占整个砖壳体积的三分之一,最后经成型、脱模和养护,得到所述的能净化水质的轻质砖。 
应用本实施例的技术方案所制得的轻质砖,容重为270kg/m3,应用于筑河拦坝可以维持长久的生态平衡,常年水质清澈碧绿。
实施例4。
一种能净化水质的轻质砖,所述轻质砖包括砖壳和设置于砖壳内的砖芯, 
所述砖芯为颗粒型活性碳,所述砖壳的原料具体包括以下重量份的原料:糖厂污泥40㎏、建筑垃圾50㎏、钾长石粉40㎏、生物质焦10㎏、硅藻土10㎏、粉煤灰20㎏、水泥40㎏。所述建筑垃圾为砖、石块、土和混凝土块中的混合物。
所述能净化水质的轻质砖的制备方法,它包括以下制备步骤:
a、将配方量的建筑垃圾粉碎至200目以下,与配方量的污泥、钾长石粉混合均匀后造粒,在1200℃焙烧40分钟,冷却后得到焙烧颗粒;
b、将步骤a得到的焙烧颗粒与配方量的池塘水泥、粉煤灰、硅藻土和生物质焦在搅拌机中搅拌均匀,得到混合物料;
c、加入占步骤b混合物料30%重量百分比的水继续搅拌至均匀,得到待用混合物料;
d、根据轻质砖的大小,取步骤c得到的待用混合物料和活性碳加入模型中,活性碳的用量占整个砖壳体积的四分之一,最后经成型、脱模和养护,得到所述的能净化水质的轻质砖。
应用本实施例的技术方案所制得的轻质砖,容重为275kg/m3,应用于筑河拦坝可以维持长久的生态平衡,常年水质清澈碧绿。
最后应当说明的是,以上实施例仅用于说明本发明的技术方案而非对本发明保护范围的限制,尽管参照较佳实施例对本发明作了详细说明,本领域的普通技术人员应当理解,可以对本发明的技术方案进行修改或者等同替换,而不脱离本发明技术方实质和范围。

Claims (9)

1.一种能净化水质的轻质砖,其特征在于:所述轻质砖包括砖壳和设置于砖壳内的砖芯, 
所述砖芯为活性碳,所述砖壳的原料采用污泥、建筑垃圾、钾长石粉、粉煤灰和水泥制成。
2.根据权利要求1所述的能净化水质的轻质砖,其特征在于:所述污泥为池塘污泥、印染污泥或糖厂污泥。
3.根据权利要求1所述的能净化水质的轻质砖,其特征在于:所述活性碳为颗粒型活性碳。
4.根据权利要求1所述的能净化水质的轻质砖,其特征在于:所述建筑垃圾为砖、瓦、石块、土和混凝土块中的一种或两种以上按任意比例混合。
5.根据权利要求1所述的能净化水质的轻质砖,其特征在于:所述砖壳的原料具体包括以下重量份的物质:
污泥         50-60份
建筑垃圾      40-50份     
钾长石粉      40-60份
粉煤灰        20-30份   
水泥          40-50份。
6.根据权利要求1所述的能净化水质的轻质砖,其特征在于:所述砖壳的原料中还包括生物质焦和硅藻土。
7.根据权利要求6所述的能净化水质的轻质砖,其特征在于:所述砖壳的原料具体包括以下重量份的物质:
污泥         40-50份
建筑垃圾      50-60份     
钾长石粉      40-60份
生物质焦      10-20份
硅藻土        10-20份
粉煤灰        20-30份   
水泥          40-50份。
8.如权利要求5所述的能净化水质的轻质砖的制备方法,其特征在于:它包括以下制备步骤:
a、将配方量的建筑垃圾粉碎至200目以下,与配方量的污泥、钾长石粉混合均匀后造粒,在1200-1400℃焙烧20-40分钟,冷却后得到焙烧颗粒;
b、将步骤a得到的焙烧颗粒与配方量的水泥和粉煤灰在搅拌机中搅拌均匀,得到混合物料;
c、加入占步骤b混合物料10%-30%重量百分比的水继续搅拌至均匀,得到待用混合物料;
d、将步骤c得到的待用混合物料和活性碳加入模型中成型、脱模和养护,得到所述的能净化水质的轻质砖。
9.如权利要求7所述的能净化水质的轻质砖的制备方法,其特征在于:它包括以下制备步骤:
a、将配方量的建筑垃圾粉碎至200目以下,与配方量的污泥、钾长石粉混合均匀后造粒,在1200-1400℃焙烧20-40分钟,冷却后得到焙烧颗粒;
b、将步骤a得到的焙烧颗粒与配方量的水泥、粉煤灰、硅藻土和生物质焦在搅拌机中搅拌均匀,得到混合物料;
c、加入占步骤b混合物料10%-30%重量百分比的水继续搅拌至均匀,得到待用混合物料;
d、将步骤c得到的待用混合物料和活性碳加入模型中成型、脱模和养护,得到所述的能净化水质的轻质砖。
CN201310038231.7A 2013-01-31 2013-01-31 一种能净化水质的轻质砖 Active CN103132483B (zh)