CN103103766A - Real silk anti-yellowing finishing agent and preparation method thereof - Google Patents

Real silk anti-yellowing finishing agent and preparation method thereof Download PDF

Info

Publication number
CN103103766A
CN103103766A CN 201210443937 CN201210443937A CN103103766A CN 103103766 A CN103103766 A CN 103103766A CN 201210443937 CN201210443937 CN 201210443937 CN 201210443937 A CN201210443937 A CN 201210443937A CN 103103766 A CN103103766 A CN 103103766A
Authority
CN
China
Prior art keywords
parts
finishing agent
yellowing
real silk
silk
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Withdrawn
Application number
CN 201210443937
Other languages
Chinese (zh)
Inventor
钱树良
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
WUJIANG QIAN'S TEXTILE CO Ltd
Original Assignee
WUJIANG QIAN'S TEXTILE CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by WUJIANG QIAN'S TEXTILE CO Ltd filed Critical WUJIANG QIAN'S TEXTILE CO Ltd
Priority to CN 201210443937 priority Critical patent/CN103103766A/en
Publication of CN103103766A publication Critical patent/CN103103766A/en
Withdrawn legal-status Critical Current

Abstract

The invention discloses a real silk anti-yellowing finishing agent and a preparation method thereof. The real silk anti-yellowing finishing agent comprises the following components in parts by weight: 20-30 parts of dimethylaminoethyl methacrylate, 10-20 parts of polyacrylamide, 1-3 parts of potassium hydroxide, 1-3 parts of sodium polyphosphate, 10-20 parts of diethylene glycol, 3-5 parts of fatty alcohol-polyoxyethylene ether, 10-20 parts of dicyandiamide, 3-8 parts of polyethylene glycol, 10-20 parts of 1, 3-butanediol, and 100-180 parts of water. In comparison with the prior art, the real silk anti-yellowing finishing agent disclosed by the invention has the advantages of (1) good anti-yellowing effect, and incapability of affecting the style and the hand feeling of the real silk, and (2) good light fastness and incapability of yellowing and discoloring for a long-term preservation.

Description

Anti-yellowing finishing agent of a kind of real silk silk and preparation method thereof
Technical field
The invention belongs to the textile auxiliary technical field, more specifically relate to anti-yellowing finishing agent of a kind of real silk silk and preparation method thereof.
Background technology
Usually through real silk and silk broadcloth meeting yellowing variable color in storage process of refining bleaching, be mainly because the amino acid residue of the tryptophan in silk protein and TYR etc. is oxidized and painted in air.Favour impels this phenomenon to occur under the irradiation of light.Although the silk broadcloth of variable color can be bleached with sodium hydrosulfite, its character can occur deteriorated.
Summary of the invention
The object of the invention is to overcome the deficiency that prior art exists, provide a kind of real silk silk to prevent the yellowing finishing agent.
Another object of the present invention is to provide the preparation method of the anti-yellowing finishing agent of this real silk silk.
For achieving the above object, the present invention has taked following technical scheme:
A kind of real silk silk is prevented the yellowing finishing agent, and is in weight portion, composed of the following components:
Dimethylaminoethyl Methacrylate: 20~30, polyacrylamide: 10~20,
Potassium hydroxide: 1~3, sodium polyphosphate: 1~3, diethylene glycol (DEG): 10~20,
Fatty alcohol-polyoxyethylene ether: 3~5, dicyandiamide: 10~20, polyethylene glycol: 3~8,
1,3-BDO: 10~20, water: 100~180.
In technique scheme, the preparation technology of the anti-yellowing finishing agent of described real silk silk is as follows:
(1) by proportioning, Dimethylaminoethyl Methacrylate, fatty alcohol-polyoxyethylene ether, diethylene glycol (DEG), dicyandiamide and polyethylene glycol are mixed, stirred 1~3 hour;
(2) polyacrylamide and sodium polyphosphate are added to the water, mix;
(3) product with step (1) mixes with the product of step (2), is warming up to 40~60 ℃, reacts 2~3 hours;
(4) be cooled to room temperature, add all the other components, get final product to get product after mixing.
Compared with prior art, the present invention has following beneficial effect:
(1) have the good yellowing effect that prevents, and harmless its style and feel;
(2) light resistance is good, and long preservation also can the yellowing variable color.
The specific embodiment
The invention will be further described below in conjunction with specific embodiment, but the present invention's scope required for protection is not limited to the scope that embodiment describes.
Embodiment 1
A kind of real silk silk is prevented the yellowing finishing agent, and is in weight portion, composed of the following components:
Dimethylaminoethyl Methacrylate: 20, polyacrylamide: 10,
Potassium hydroxide: 1, sodium polyphosphate: 1, diethylene glycol (DEG): 10,
Fatty alcohol-polyoxyethylene ether: 3, dicyandiamide: 10, polyethylene glycol: 3,
1,3-BDO: 10, water: 100.
Embodiment 2
A kind of real silk silk is prevented the yellowing finishing agent, and is in weight portion, composed of the following components:
Dimethylaminoethyl Methacrylate: 30, polyacrylamide: 20,
Potassium hydroxide: 3, sodium polyphosphate: 3, diethylene glycol (DEG): 20,
Fatty alcohol-polyoxyethylene ether: 5, dicyandiamide: 20, polyethylene glycol: 8,
1,3-BDO: 20, water: 180.
Embodiment 3
A kind of real silk silk is prevented the yellowing finishing agent, and is in weight portion, composed of the following components:
Dimethylaminoethyl Methacrylate: 25, polyacrylamide: 16,
Potassium hydroxide: 2, sodium polyphosphate: 2, diethylene glycol (DEG): 16,
Fatty alcohol-polyoxyethylene ether: 4, dicyandiamide: 15, polyethylene glycol: 6,
1,3-BDO: 16, water: 160.
In above-described embodiment, the preparation method of the anti-yellowing finishing agent of described a kind of real silk silk comprises the steps:
(1) by proportioning, Dimethylaminoethyl Methacrylate, fatty alcohol-polyoxyethylene ether, diethylene glycol (DEG), dicyandiamide and polyethylene glycol are mixed, stirred 1~3 hour;
(2) polyacrylamide and sodium polyphosphate are added to the water, mix;
(3) product with step (1) mixes with the product of step (2), is warming up to 40~60 ℃, reacts 2~3 hours;
(4) be cooled to room temperature, add all the other components, get final product to get product after mixing.

Claims (5)

1. the anti-yellowing finishing agent of real silk silk, is characterized in that, and is in weight portion, composed of the following components:
Dimethylaminoethyl Methacrylate: 20~30, polyacrylamide: 10~20,
Potassium hydroxide: 1~3, sodium polyphosphate: 1~3, diethylene glycol (DEG): 10~20,
Fatty alcohol-polyoxyethylene ether: 3~5, dicyandiamide: 10~20, polyethylene glycol: 3~8,
1,3-BDO: 10~20, water: 100~180.
2. the anti-yellowing finishing agent of a kind of real silk silk according to claim 1, is characterized in that, and is in weight portion, composed of the following components:
Dimethylaminoethyl Methacrylate: 20, polyacrylamide: 10,
Potassium hydroxide: 1, sodium polyphosphate: 1, diethylene glycol (DEG): 10,
Fatty alcohol-polyoxyethylene ether: 3, dicyandiamide: 10, polyethylene glycol: 3,
1,3-BDO: 10, water: 100.
3. the anti-yellowing finishing agent of a kind of real silk silk according to claim 1, is characterized in that, and is in weight portion, composed of the following components:
Dimethylaminoethyl Methacrylate: 30, polyacrylamide: 20,
Potassium hydroxide: 3, sodium polyphosphate: 3, diethylene glycol (DEG): 20,
Fatty alcohol-polyoxyethylene ether: 5, dicyandiamide: 20, polyethylene glycol: 8,
1,3-BDO: 20, water: 180.
4. the anti-yellowing finishing agent of a kind of real silk silk according to claim 1, is characterized in that, and is in weight portion, composed of the following components:
Dimethylaminoethyl Methacrylate: 25, polyacrylamide: 16,
Potassium hydroxide: 2, sodium polyphosphate: 2, diethylene glycol (DEG): 16,
Fatty alcohol-polyoxyethylene ether: 4, dicyandiamide: 15, polyethylene glycol: 6,
1,3-BDO: 16, water: 160.
5. the preparation method of the anti-yellowing finishing agent of a kind of real silk silk claimed in claim 1, is characterized in that, comprises the steps:
(1) by proportioning, Dimethylaminoethyl Methacrylate, fatty alcohol-polyoxyethylene ether, diethylene glycol (DEG), dicyandiamide and polyethylene glycol are mixed, stirred 1~3 hour;
(2) polyacrylamide and sodium polyphosphate are added to the water, mix;
(3) product with step (1) mixes with the product of step (2), is warming up to 40~60 ℃, reacts 2~3 hours;
(4) be cooled to room temperature, add all the other components, get final product to get product after mixing.
CN 201210443937 2012-11-08 2012-11-08 Real silk anti-yellowing finishing agent and preparation method thereof Withdrawn CN103103766A (en)