CN102733267A CN2012102464923A CN201210246492A CN102733267A CN 102733267 A CN102733267 A CN 102733267A CN 2012102464923 A CN2012102464923 A CN 2012102464923A CN 201210246492 A CN201210246492 A CN 201210246492A CN 102733267 A CN102733267 A CN 102733267A
Authority
CN
China
Prior art keywords
leaf
paper page
water paper
layer
playing card
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN2012102464923A
Other languages
Chinese (zh)
Inventor
吴立群
周原
杨娇
刘攀
杨玉洁
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
China Haisum Engineering Co Ltd
Original Assignee
China Haisum Engineering Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by China Haisum Engineering Co Ltd filed Critical China Haisum Engineering Co Ltd
Priority to CN2012102464923A priority Critical patent/CN102733267A/en
Publication of CN102733267A publication Critical patent/CN102733267A/en
Pending legal-status Critical Current

Links

Abstract

The invention discloses a playing card paperboard, orderly comprising a surface layer wet paper page, a core layer wet paper page and a bottom layer wet paper page which are combined. The playing card paperboard is characterized in that foam glue is coated before combining the surface layer wet paper page, the core layer wet paper page and the bottom layer wet paper page; the processing method comprises the following steps: preparing each slurry into wet paper pages; preparing the foam glue by a bonding agent, dye and water and coating the foam glue on one face of the surface layer wet paper page, two faces of the core layer wet paper page, one or more faces of one face of the bottom layer wet paper page; combining each layer of wet paper pages; squeezing and dewatering each layer so as to prepare a paperboard, and drying the paperboard; coating corresponding coating material on the surface of the paperboard; and processing after-treatment so as to manufacture the playing card paperboard. According to the invention, the bonding agent used for bonding each layer of paper web and dye capable of improving opaqueness of playing card papers are coated on each layer of the wet paper page in a foam glue method; technology of adding the dye into core slurry is substituted; and dyeing pollution caused by papermaking whitewater is avoided.

Description

A kind of playing card board and processing method thereof
Technical field
The present invention relates to a kind of playing card board and processing method thereof, belong to pulp technology for making paper.
Background technology
Snipsnapsnorum is a kind of layer of all ages, the recreation that confined condition is few.Along with the enriching constantly and increase of entertainment life, the demand to playing card on the market increases very fast.According to statistics, by 2010, China became maximum in the world playing card producing country and country of consumption.At present; High-grade playing card Zhu on the market Yao Shi ?the core playing card; Its advantage is light tight; Be not easy cheating, and the body paper of present this playing card is bonded with carbon black glue mixing water by two one-side coated papers mainly, its processing technology is complicated, loss is big, cost is high, output is little and mainly rely on import.
China utility model patent ZL200720108545.X discloses a kind of playing card paper; Comprise the surface layer and the bottom that are coated with face coating layer and primary coat layer of cloth respectively; Characteristics are to be provided with blue core fibre light shield layer between surface layer and the bottom, and are compound through the binding agent press dewatering respectively between blue core fibre light shield layer and the bottom.Chinese patent CN101851876A has proposed a kind of processing method that in the core slurry, has added the block-core playing card paper of black dyes and trivalent aluminium salt simultaneously.More than two patents in the core slurry, added blueness and black dyes respectively, in order to improving the opacity of playing card paper, pollute but this kind method is prone to produce the dyestuff color and luster of mthod of white water from paper making, increase the environmental protection treatment cost; Though the latter adds trivalent aluminium salt the pollution of mthod of white water from paper making and web part of paper machine is alleviated to some extent, adding chemicals has increased production cost again; In addition; When the many net formings of paper machine are copied paper,, adopt the interlayer spraying binder to increase the bonding force of each interlayer in order to reduce the blowing phenomenon; But spray lower with the starch adesive gum concentration; Increased the dehydrating amount of wet end, and polluted felt and net easily, its lower concentration is prone to cause glue migration amount in paper excessive simultaneously.
Summary of the invention
The purpose of this invention is to provide and a kind of mthod of white water from paper making is not caused dye discoloration, lower, the high-quality playing card board of production cost and processing method thereof.
In order to achieve the above object; The invention provides a kind of playing card board; Comprise compound successively surface layer l Water Paper page or leaf, sandwich layer l Water Paper page or leaf and bottom l Water Paper page or leaf, it is characterized in that, before described surface layer l Water Paper page or leaf, sandwich layer l Water Paper page or leaf and bottom l Water Paper page or leaf are compound, all be coated with foamed glue.
Preferably, be provided with face lining l Water Paper page or leaf between described surface layer l Water Paper page or leaf and the sandwich layer l Water Paper page or leaf, be provided with end liner layer l Water Paper page or leaf between sandwich layer l Water Paper page or leaf and the bottom l Water Paper page or leaf, face lining l Water Paper page or leaf and end liner layer l Water Paper page or leaf were coated with adhesive or foamed glue before compound.
Preferably, the preparation method of said foamed glue is: the water of inciting somebody to action by percentage to the quality 1~10% adhesive, 0~2% dyestuff and surplus carries out mechanical foaming under 50-70 ℃, blowing ratio is 1: 3~1: 5.
The present invention also provides the processing method of above-mentioned playing card board, and its step is following:
The first step: preparation and preliminary treatment surface layer slurry, center stock and base pastes;
Second step: surface layer slurry, center stock and base pastes that the first step obtains are manufactured paper with pulp into surface layer l Water Paper page or leaf, sandwich layer l Water Paper page or leaf and bottom l Water Paper page or leaf;
The 6th step: at the facing surface coated face coating of the 5th cardboard that obtain of step, at bottom surface barrier coating coating;
The 7th step: the cardboard that the 6th step was obtained carries out surface waterproofing processing, surface treatment, cut paper successively, processes playing card board, it is characterized in that, and is further comprising the steps of:
The 3rd step: the water of inciting somebody to action by percentage to the quality 1~10% adhesive, 0~2% dyestuff and surplus carries out mechanical foaming, and blowing ratio is 1: 3~1: 5, processes foamed glue;
The 4th step: the 3rd foamed glue that obtain of step is coated on any one side or several times in the one side of two sides and bottom l Water Paper page or leaf of one side, sandwich layer l Water Paper page or leaf of the surface layer l Water Paper page or leaf that second step obtained;
The 5th step: surface layer l Water Paper page or leaf, sandwich layer l Water Paper page or leaf, bottom l Water Paper page or leaf that the 4th step obtained is compound successively; Surface layer l Water Paper page or leaf and bottom l Water Paper page or leaf are coated with the one side of foamed glue towards a compound side; Between each layer, carry out press dewatering then, process cardboard, drying.
Preferably, also prepare and preliminary treatment face lining slurry and end liner layer slurry in the described first step; The face lining slurry and the end liner layer slurry that also the first step are obtained in described second step are manufactured paper with pulp into face lining l Water Paper page or leaf and end liner layer l Water Paper page or leaf; Also adhesive or the 3rd foamed glue that obtain of step are coated on any one side or several times in the two sides of two sides and end liner layer l Water Paper page or leaf of the face lining l Water Paper page or leaf that second step obtained in described the 4th step; The face lining l Water Paper page or leaf that also the 4th step was obtained in described the 5th step is located between surface layer l Water Paper page or leaf and the sandwich layer l Water Paper page or leaf, and end liner layer l Water Paper page or leaf is located between sandwich layer l Water Paper page or leaf and the bottom l Water Paper page or leaf.
Preferably, it is characterized in that the binding agent in described the 3rd step is any one or a few the mixture in starch, casein, soya casein, animal glue, styrene-butadiene latex, carboxylic styrene butadiene latex, polyvinyl alcohol and the polyacrylate.
Preferably, the binding agent in described the 4th step is any one or a few the mixture in starch, casein, soya casein, animal glue, styrene-butadiene latex, carboxylic styrene butadiene latex, polyvinyl alcohol and the polyacrylate.
Preferably, the dyestuff in described the 3rd step is at least a in ACID DYES, basic-dyeable fibre and the direct dyes.
Further, the dyestuff in described the 3rd step is an ACID DYES.
Preferably, in said the 3rd step the method for mechanical foaming be wherein a kind of during static type foams with dynamic type.
Preferably, the coating process in said the 4th step is at least a in scraper type, pulley type, rubber blanket vacuum pumping-type, net belt type, cylinder and the slit.
The present invention adopts the mode of foamed glue to coat each layer l Water Paper page or leaf with the dyestuff that increases the playing card paper opacity in the bonding used adhesive of each layer paper web; Substituted the technology of in the core slurry, adding dyestuff; Avoided the dyeing of mthod of white water from paper making to pollute; Binder concn is higher in the foamed glue simultaneously, moisture is low; Can make glue-line be retained in the l Water Paper page frame table; Reduced the migration of adhesive to inside; Increased the interlayer adhesion and the elasticity of playing card board, reduced pollution paper grade (stock) wet end and felt; Also can under the situation that does not hinder its characteristic, in foamed glue, add filler, to reduce cost effectively.
The specific embodiment
For making the present invention more obviously understandable,, elaborate as follows now with preferred embodiment.
Embodiment 1
The first step: go out surface layer slurry, center stock and base pastes through size degradation, screening, purification, flotation, hot dispersion, bleaching and defibrination Processing of Preparation;
Second step: surface layer slurry, center stock and base pastes that the first step is obtained utilize folder net, cylinder, fourdrinier wire combined type former to dewater respectively on the net, process surface layer l Water Paper page or leaf, sandwich layer l Water Paper page or leaf and bottom l Water Paper page or leaf;
The 3rd step: (good biological starch Science and Technology Ltd. is believed in Hebei to 5.0% amylan that will be by percentage to the quality; LSE-3), 0.2% dyestuff (the happy chemical industry of Hangzhou card Co., Ltd; Acid black 1 94) and 94.8% water in the time of 50 ℃, mix, carry out mechanical foaming, blowing ratio is 1: 3; Process foamed glue, coat second through the mode of blade coating and go on foot on the one side of the sandwich layer l Water Paper page or leaf that obtains;
The 4th step: (good biological starch Science and Technology Ltd. is believed in Hebei to 5.0% amylan that will be by percentage to the quality; LSE-3) and 95% water in the time of 50 ℃, mix; Carry out mechanical foaming; Blowing ratio is 1: 3, processes foamed glue, coats second through the mode of blade coating and goes on foot on the bottom l Water Paper page or leaf one side that obtains;
The 5th step: the surface layer l Water Paper page or leaf that second step was obtained, sandwich layer l Water Paper page or leaf, the 4th bottom l Water Paper page or leaf that obtain of step that the 3rd step obtained are compound; It is relative with the one side of surface layer l Water Paper page or leaf that sandwich layer l Water Paper page or leaf is coated with the one side of foamed glue; Its another side is relative with the one side that bottom l Water Paper page or leaf is coated with foamed glue; Between each layer, carry out press dewatering; Make cardboard, drying;
The 6th step: at the facing surface coated face coating of the 5th cardboard that obtain of step, at bottom surface barrier coating coating;
The 7th step: the cardboard that the 6th step was obtained carries out surface waterproofing processing, surface treatment, cut paper successively, processes playing card board.
Process the quantitative 250g/m of being of the playing card board that obtains through said method 2, thickness is 261 μ m, and deflection (laterally) is 3.3mN/m, and deflection (vertically) is 6.4mN/m, and folding strength (vertically) is 92 times.The interlayer adhesion is 225J/m 2, elasticity is that 1.0mm/ opens.
Embodiment 2
The first step: go out surface layer slurry, center stock and base pastes through size degradation, screening, purification, flotation, hot dispersion, bleaching and defibrination Processing of Preparation;
Second step: surface layer slurry, center stock and base pastes that the first step is obtained utilize folder net, cylinder, fourdrinier wire combined type former to dewater respectively on the net, process surface layer l Water Paper page or leaf, sandwich layer l Water Paper page or leaf and bottom l Water Paper page or leaf;
The 3rd step: (good biological starch Science and Technology Ltd. is believed in Hebei to 10.0% amylan that will be by percentage to the quality; LSE-3), 2.0% dyestuff (the happy chemical industry of Hangzhou card Co., Ltd; Acid black 1 94) and 88% water in the time of 70 ℃, mix, carry out mechanical foaming, blowing ratio is 1: 5; Process foamed glue, coat second through the mode of blade coating and go on foot on the two sides of the sandwich layer l Water Paper page or leaf that obtains;
The 4th step: the sandwich layer l Water Paper page or leaf that surface layer l Water Paper page or leaf, bottom l Water Paper page or leaf, the 3rd step that second step was obtained obtains is compound; The one side of sandwich layer l Water Paper page or leaf is relative with the one side of surface layer l Water Paper page or leaf; Its another side is relative with the one side of bottom l Water Paper page or leaf; Between each layer, carry out press dewatering; Make cardboard, drying;
The 5th step: at the facing surface coated face coating of the 4th cardboard that obtain of step, at bottom surface barrier coating coating;
The 6th step: the cardboard that the 6th step was obtained carries out surface waterproofing processing, surface treatment, cut paper successively, processes playing card board.
Process the quantitative 260g/m of being of the playing card board that obtains through said method 2, thickness is 270 μ m, and deflection (laterally) is 3.7mN/m, and deflection (vertically) is 6.8mN/m, and folding strength (vertically) is 95 times.The interlayer adhesion is 232J/m 2, elasticity is that 0.9mm/ opens.
Embodiment 3
The first step: go out surface layer slurry, face lining slurry, center stock, end liner layer slurry and base pastes through size degradation, screening, purification, flotation, hot dispersion, bleaching and defibrination Processing of Preparation;
Second step: surface layer slurry, face lining slurry, center stock, end liner layer slurry and base pastes that the first step is obtained utilize folder net, cylinder, fourdrinier wire combined type former to dewater respectively on the net, process surface layer l Water Paper page or leaf, face lining l Water Paper page or leaf, sandwich layer l Water Paper page or leaf, end liner layer l Water Paper page or leaf and bottom l Water Paper page or leaf;
The 3rd step: (good biological starch Science and Technology Ltd. is believed in Hebei to 1.0% amylan that will be by percentage to the quality; LSE-3), 1.0% dyestuff (the happy chemical industry of Hangzhou card Co., Ltd; Acid black 1 94) and 98% water in the time of 60 ℃, mix, carry out mechanical foaming, blowing ratio is 1: 4; Process foamed glue, coat second through the mode of blade coating and go on foot on the two sides of the sandwich layer l Water Paper page or leaf that obtains;
The 4th step: (good biological starch Science and Technology Ltd. is believed in Hebei to 1.0% amylan that will be by percentage to the quality; LSE-3) and 99% water in the time of 60 ℃, mix; Carry out mechanical foaming; Blowing ratio is 1: 4, processes foamed glue, through the mode of blade coating coat second the step obtain on the one side of surface layer l Water Paper page or leaf and bottom l Water Paper page or leaf;
The 5th step: go on foot the surface layer l Water Paper page or leaf that obtains with the 4th; The face lining l Water Paper page or leaf that second step obtained; End liner layer l Water Paper page or leaf; The sandwich layer l Water Paper page or leaf that the 3rd step obtained; The bottom l Water Paper page or leaf that the 4th step obtained is compound; It is relative with the one side of face lining l Water Paper page or leaf that surface layer l Water Paper page or leaf is coated with the one side of foamed glue; The another side of face lining l Water Paper page or leaf is relative with the one side of sandwich layer l Water Paper page or leaf; The another side of sandwich layer l Water Paper page or leaf is relative with the one side of end liner layer l Water Paper page or leaf; The another side of end liner layer l Water Paper page or leaf is relative with the one side that bottom l Water Paper page or leaf is coated with foamed glue; Between each layer, carry out press dewatering; Make cardboard, drying;
The 6th step: at the facing surface coated face coating of the 5th cardboard that obtain of step, at bottom surface barrier coating coating;
The 7th step: the cardboard that the 6th step was obtained carries out surface waterproofing processing, surface treatment, cut paper successively, processes playing card board.
Process the quantitative 280g/m of being of the playing card board that obtains through said method 2, thickness is 290 μ m, and deflection (laterally) is 4.0mN/m, and deflection (vertically) is 7.6mN/m, and folding strength (vertically) is 84 times.The interlayer adhesion is 210J/m 2, elasticity is that 1.2mm/ opens.
Embodiment 4
The first step: go out surface layer slurry, face lining slurry, center stock, end liner layer slurry and base pastes through size degradation, screening, purification, flotation, hot dispersion, bleaching and defibrination Processing of Preparation;
Second step: surface layer slurry, face lining slurry, center stock, end liner layer slurry and base pastes that the first step is obtained utilize many forming device for cylinder machine to dewater respectively on the net, process surface layer l Water Paper page or leaf, face lining l Water Paper page or leaf, sandwich layer l Water Paper page or leaf, end liner layer l Water Paper page or leaf and bottom l Water Paper page or leaf;
The 3rd step: (good biological starch Science and Technology Ltd. is believed in Hebei to 8.0% amylan that will be by percentage to the quality; LSE-3), 1.5% dyestuff (the happy chemical industry of Hangzhou card Co., Ltd; Acid black 1 94) and 90.5% water in the time of 60 ℃, mix, carry out mechanical foaming, blowing ratio is 1: 4; Process foamed glue, coat through the mode of blade coating on the one side of one side and sandwich layer l Water Paper page or leaf of the second face lining l Water Paper page or leaf that obtain of step;
The 4th step: (good biological starch Science and Technology Ltd. is believed in Hebei to 6.0% amylan that will be by percentage to the quality; LSE-3) and 94% water in the time of 60 ℃, mix; Carry out mechanical foaming; Blowing ratio is 1: 4, processes foamed glue, coats through the mode of blade coating on the one side of one side and end liner layer l Water Paper page or leaf of the second surface layer l Water Paper page or leaf that obtain of step;
The 5th step: go on foot the surface layer l Water Paper page or leaf that obtains with the 4th; End liner layer l Water Paper page or leaf; The face lining l Water Paper page or leaf that the 3rd step obtained; Sandwich layer l Water Paper page or leaf; The bottom l Water Paper page or leaf that second step obtained is compound; It is relative with the one side of the uncoated foamed glue of face lining l Water Paper page or leaf that surface layer l Water Paper page or leaf is coated with the one side of foamed glue; The another side that face lining l Water Paper page or leaf is coated with foamed glue is relative with the one side of the uncoated foamed glue of sandwich layer l Water Paper page or leaf; The another side that sandwich layer l Water Paper page or leaf is coated with foamed glue is relative with the one side of the uncoated foamed glue of end liner layer l Water Paper page or leaf; The another side that end liner layer l Water Paper page or leaf is coated with foamed glue is relative with the one side of bottom l Water Paper page or leaf; Between each layer, carry out press dewatering; Make cardboard, drying;
The 6th step: at the facing surface coated face coating of the 5th cardboard that obtain of step, at bottom surface barrier coating coating;
The 7th step: the cardboard that the 6th step was obtained carries out surface waterproofing processing, surface treatment, cut paper successively, processes playing card board.
Process the quantitative 270g/m of being of the playing card board that obtains through said method 2, thickness is 280 μ m, and deflection (laterally) is 4.0mN/m, and deflection (vertically) is 7.6mN/m, and folding strength (vertically) is 93 times.The interlayer adhesion is 227J/m 2, elasticity is that 1.1mm/ opens.
Embodiment 5
The first step: go out surface layer slurry, face lining slurry, center stock, end liner layer slurry and base pastes through size degradation, screening, purification, flotation, hot dispersion, bleaching and defibrination Processing of Preparation;
Second step: surface layer slurry, face lining slurry, center stock, end liner layer slurry and base pastes that the first step is obtained utilize many forming device for cylinder machine to dewater respectively on the net, process surface layer l Water Paper page or leaf, face lining l Water Paper page or leaf, sandwich layer l Water Paper page or leaf, end liner layer l Water Paper page or leaf and bottom l Water Paper page or leaf;
The 3rd step: (good biological starch Science and Technology Ltd. is believed in Hebei to 3.0% amylan that will be by percentage to the quality; LSE-3), 1.5% dyestuff (the happy chemical industry of Hangzhou card Co., Ltd; Acid black 1 94) and 90.5% water in the time of 60 ℃, mix, carry out mechanical foaming, blowing ratio is 1: 4; Process foamed glue, coat through the mode of blade coating on the one side of one side and sandwich layer l Water Paper page or leaf of the second face lining l Water Paper page or leaf that obtain of step;
The 4th step: (good biological starch Science and Technology Ltd. is believed in Hebei, LSE-3) coats on the one side of one side and end liner layer l Water Paper page or leaf of the surface layer l Water Paper page or leaf that second step obtained through the mode of spraying with amylan;
The 5th step: go on foot the surface layer l Water Paper page or leaf that obtains with the 4th; End liner layer l Water Paper page or leaf; The face lining l Water Paper page or leaf that the 3rd step obtained; Sandwich layer l Water Paper page or leaf; The bottom l Water Paper page or leaf that second step obtained is compound; It is relative with the one side of the uncoated foamed glue of face lining l Water Paper page or leaf that surface layer l Water Paper page or leaf is coated with the one side of foamed glue; The another side that face lining l Water Paper page or leaf is coated with foamed glue is relative with the one side of the uncoated foamed glue of sandwich layer l Water Paper page or leaf; The another side that sandwich layer l Water Paper page or leaf is coated with foamed glue is relative with the one side of the uncoated foamed glue of end liner layer l Water Paper page or leaf; The another side that end liner layer l Water Paper page or leaf is coated with foamed glue is relative with the one side of bottom l Water Paper page or leaf; Between each layer, carry out press dewatering; Make cardboard, drying;
The 6th step: at the facing surface coated face coating of the 5th cardboard that obtain of step, at bottom surface barrier coating coating;
The 7th step: the cardboard that the 6th step was obtained carries out surface waterproofing processing, surface treatment, cut paper successively, processes playing card board.
Process the quantitative 270g/m of being of the playing card board that obtains through said method 2, thickness is 280 μ m, and deflection (laterally) is 3.6mN/m, and deflection (vertically) is 7.0mN/m, and folding strength (vertically) is 86 times.The interlayer adhesion is 219J/m 2, elasticity is that 1.3mm/ opens.

Claims (11)

1. a playing card board comprises compound successively surface layer l Water Paper page or leaf, sandwich layer l Water Paper page or leaf and bottom l Water Paper page or leaf, it is characterized in that, before described surface layer l Water Paper page or leaf, sandwich layer l Water Paper page or leaf and bottom l Water Paper page or leaf are compound, all is coated with foamed glue.
2. a kind of playing card board according to claim 1; It is characterized in that; Be provided with face lining l Water Paper page or leaf between described surface layer l Water Paper page or leaf and the sandwich layer l Water Paper page or leaf; Be provided with end liner layer l Water Paper page or leaf between sandwich layer l Water Paper page or leaf and the bottom l Water Paper page or leaf, face lining l Water Paper page or leaf and end liner layer l Water Paper page or leaf were coated with adhesive or foamed glue before compound.
3. according to claim 1,2 described a kind of playing card boards; It is characterized in that; The preparation method of said foamed glue is: the water of inciting somebody to action by percentage to the quality 1~10% adhesive, 0~2% dyestuff and surplus carries out mechanical foaming under 50-70 ℃, blowing ratio is 1: 3~1: 5.
4. the processing method of the described a kind of playing card board of claim 1, its step is following:
The first step: preparation and preliminary treatment surface layer slurry, center stock and base pastes;
Second step: surface layer slurry, center stock and base pastes that the first step obtains are manufactured paper with pulp into surface layer l Water Paper page or leaf, sandwich layer l Water Paper page or leaf and bottom l Water Paper page or leaf;
The 6th step: at the facing surface coated face coating of the 5th cardboard that obtain of step, at bottom surface barrier coating coating;
The 7th step: the cardboard that the 6th step was obtained carries out surface waterproofing processing, surface treatment, cut paper successively, processes playing card board, it is characterized in that, and is further comprising the steps of:
The 3rd step: the water of inciting somebody to action by percentage to the quality 1~10% adhesive, 0~2% dyestuff and surplus carries out mechanical foaming, and blowing ratio is 1: 3~1: 5, processes foamed glue;
The 4th step: the 3rd foamed glue that obtain of step is coated on any one side or several times in the one side of two sides and bottom l Water Paper page or leaf of one side, sandwich layer l Water Paper page or leaf of the surface layer l Water Paper page or leaf that second step obtained;
The 5th step: surface layer l Water Paper page or leaf, sandwich layer l Water Paper page or leaf, bottom l Water Paper page or leaf that the 4th step obtained is compound successively; Surface layer l Water Paper page or leaf and bottom l Water Paper page or leaf are coated with the one side of foamed glue towards a compound side; Between each layer, carry out press dewatering then, process cardboard, drying.
5. the processing method of a kind of playing card board according to claim 4 is characterized in that, also prepares and preliminary treatment face lining slurry and end liner layer slurry in the described first step; The face lining slurry and the end liner layer slurry that also the first step are obtained in described second step are manufactured paper with pulp into face lining l Water Paper page or leaf and end liner layer l Water Paper page or leaf; Also adhesive or the 3rd foamed glue that obtain of step are coated on any one side or several times in the two sides of two sides and end liner layer l Water Paper page or leaf of the face lining l Water Paper page or leaf that second step obtained in described the 4th step; The face lining l Water Paper page or leaf that also the 4th step was obtained in described the 5th step is located between surface layer l Water Paper page or leaf and the sandwich layer l Water Paper page or leaf, and end liner layer l Water Paper page or leaf is located between sandwich layer l Water Paper page or leaf and the bottom l Water Paper page or leaf.
6. according to the processing method of claim 4 or 5 described a kind of playing card boards; It is characterized in that the binding agent in described the 3rd step is any one or a few the mixture in starch, casein, soya casein, animal glue, styrene-butadiene latex, carboxylic styrene butadiene latex, polyvinyl alcohol and the polyacrylate.
7. the processing method of a kind of playing card board according to claim 5; It is characterized in that the binding agent in described the 4th step is any one or a few the mixture in starch, casein, soya casein, animal glue, styrene-butadiene latex, carboxylic styrene butadiene latex, polyvinyl alcohol and the polyacrylate.
8. the processing method of a kind of playing card board according to claim 4 is characterized in that, the dyestuff in described the 3rd step is at least a in ACID DYES, basic-dyeable fibre and the direct dyes.
9. the processing method of a kind of playing card board according to claim 4 is characterized in that, the dyestuff in described the 3rd step is an ACID DYES.
10. according to the processing method of claim 4 or 5 described a kind of playing card boards, it is characterized in that, in said the 3rd step the method for mechanical foaming be wherein a kind of during static type foams with dynamic type.
11. the processing method according to claim 4 or 5 described a kind of playing card boards is characterized in that, the coating process in said the 4th step is at least a in scraper type, pulley type, rubber blanket vacuum pumping-type, net belt type, cylinder and the slit.
CN2012102464923A 2012-07-16 2012-07-16 Playing card paperboard and processing method thereof Pending CN102733267A (en)

Priority Applications (1)

Application Number Priority Date Filing Date Title
CN2012102464923A CN102733267A (en) 2012-07-16 2012-07-16 Playing card paperboard and processing method thereof

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
CN2012102464923A CN102733267A (en) 2012-07-16 2012-07-16 Playing card paperboard and processing method thereof

Publications (1)

Publication Number Publication Date
CN102733267A true CN102733267A (en) 2012-10-17

Family

ID=46989526

Family Applications (1)

Application Number Title Priority Date Filing Date
CN2012102464923A Pending CN102733267A (en) 2012-07-16 2012-07-16 Playing card paperboard and processing method thereof

Country Status (1)

Country Link
CN (1) CN102733267A (en)

Cited By (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN102926286A (en) * 2012-11-20 2013-02-13 中国海诚工程科技股份有限公司 Playing card paperboard and production method thereof
CN104594108A (en) * 2014-12-17 2015-05-06 金东纸业(江苏)股份有限公司 Preparation method of playing card paper, matrix paper and playing card paper
CN112609488A (en) * 2020-12-25 2021-04-06 镇江大东纸业有限公司 Method for producing multilayer paper with high interlayer bonding strength
CN113939626A (en) * 2019-05-14 2022-01-14 斯道拉恩索公司 Method for applying starch to paper or paperboard web
CN113939626B (en) * 2019-05-14 2024-04-26 斯道拉恩索公司 Method for applying starch to paper or paperboard web

Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN1173893A (en) * 1995-02-14 1998-02-18 泡沫技术联合公司 Stable and water-resistance aqueous foam composition
JP2000141576A (en) * 1998-11-10 2000-05-23 Tokushu Paper Mfg Co Ltd Perfectly opaque paper
CN201082942Y (en) * 2007-04-25 2008-07-09 宁波亚洲浆纸业有限公司 Playing card paper
CN101356316A (en) * 2006-01-05 2009-01-28 西巴控股有限公司 Reactive dye grafted binders
CN201512724U (en) * 2009-05-08 2010-06-23 东莞玖龙纸业有限公司 Coated white paperboard with laminated structure

Patent Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN1173893A (en) * 1995-02-14 1998-02-18 泡沫技术联合公司 Stable and water-resistance aqueous foam composition
JP2000141576A (en) * 1998-11-10 2000-05-23 Tokushu Paper Mfg Co Ltd Perfectly opaque paper
CN101356316A (en) * 2006-01-05 2009-01-28 西巴控股有限公司 Reactive dye grafted binders
CN201082942Y (en) * 2007-04-25 2008-07-09 宁波亚洲浆纸业有限公司 Playing card paper
CN201512724U (en) * 2009-05-08 2010-06-23 东莞玖龙纸业有限公司 Coated white paperboard with laminated structure

Cited By (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN102926286A (en) * 2012-11-20 2013-02-13 中国海诚工程科技股份有限公司 Playing card paperboard and production method thereof
CN102926286B (en) * 2012-11-20 2015-04-29 中国海诚工程科技股份有限公司 Playing card paperboard and production method thereof
CN104594108A (en) * 2014-12-17 2015-05-06 金东纸业(江苏)股份有限公司 Preparation method of playing card paper, matrix paper and playing card paper
CN113939626A (en) * 2019-05-14 2022-01-14 斯道拉恩索公司 Method for applying starch to paper or paperboard web
CN113939626B (en) * 2019-05-14 2024-04-26 斯道拉恩索公司 Method for applying starch to paper or paperboard web
CN112609488A (en) * 2020-12-25 2021-04-06 镇江大东纸业有限公司 Method for producing multilayer paper with high interlayer bonding strength

Similar Documents

Publication Publication Date Title
CN102212983B (en) High-intensity environment-friendly craft paper and manufacturing method thereof
CN103321096B (en) A kind of coated white cardboard and production technology thereof
CN102277776B (en) Method for making slightly-coated elegant pure paper
WO2015007098A1 (en) Waterproof recycled paper and production method thereof
CN111005262B (en) All-cotton transfer printing base paper and production method thereof
CN104846684B (en) Environment-friendly plastics-absorption double-surface coated white board paper and preparation technology thereof
CN109706778B (en) Production process of engineering copying base paper
CN106087523B (en) A kind of papermaking process of on-line coater water-transfer printing paper base stock body paper
CN103614949A (en) High-permeability super black decorated base paper and preparation method thereof
CN101768896B (en) Preparation method of Stefan parchment paper
CN106948208A (en) A kind of environmentally friendly light basis weight coated duplex board with grey back and preparation method thereof
CN103103860B (en) Imitated rice paper production method
CN104894912A (en) Papermaking process
CN102733267A (en) Playing card paperboard and processing method thereof
CN105484106B (en) A kind of high-strength water-resistance environmental protection craft paper and preparation method
CN104499355A (en) Textured base paper dipping production technology
CN104532680B (en) High-grade environment-friendly super-sense paper and preparation process thereof
CN111005258B (en) Light coated craft paper and production method thereof
CN103790069A (en) Paperboard for anti-counterfeit cigarette
CN103103871A (en) Preparation method for producing decorative pearly-luster body paper in in-pulp dying mode
CN102433801A (en) Production method of color imitation parchment paper
CN108411704A (en) A kind of high interfacial bonding strength dumb light U.S. line paper and preparation method thereof
CN105155327A (en) Production method for hydrophilic transfer printing body paper
CN109653023A (en) It is a kind of for manufacturing the translucent suction pipe paper and preparation method of translucent suction pipe
CN114541170A (en) Coating composition for papermaking, gravure light coated paper and manufacturing method thereof

Legal Events

Date Code Title Description
C06 Publication
PB01 Publication
C10 Entry into substantive examination
SE01 Entry into force of request for substantive examination
C12 Rejection of a patent application after its publication
RJ01 Rejection of invention patent application after publication