CN102701839A - 改善径流水质的屋顶绿化用基质及制备方法 - Google Patents

改善径流水质的屋顶绿化用基质及制备方法 Download PDF

Info

Publication number
CN102701839A
CN102701839A CN2012101575416A CN201210157541A CN102701839A CN 102701839 A CN102701839 A CN 102701839A CN 2012101575416 A CN2012101575416 A CN 2012101575416A CN 201210157541 A CN201210157541 A CN 201210157541A CN 102701839 A CN102701839 A CN 102701839A
Authority
CN
China
Prior art keywords
roof greening
water quality
medium
runoff water
matrix
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN2012101575416A
Other languages
English (en)
Inventor
李贺
刘守城
何兆芳
张烨
倪淑梅
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
China MCC17 Group Co Ltd
Original Assignee
China MCC17 Group Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by China MCC17 Group Co Ltd filed Critical China MCC17 Group Co Ltd
Priority to CN2012101575416A priority Critical patent/CN102701839A/zh
Publication of CN102701839A publication Critical patent/CN102701839A/zh
Pending legal-status Critical Current

Abstract

本发明公开了一种改善径流水质的屋顶绿化用基质及制备方法,各组分的重量分数为:泥炭土20-30,珍珠岩10-15,粗纤维腐殖质30-40,陶粒15-20,凹凸棒土5-10。还可包含杀虫剂、杀菌剂和肥力缓释剂。将泥炭土、珍珠岩、粗纤维腐殖质、陶粒和凹凸棒土按比例混合并搅拌均匀,然后将杀虫剂、杀菌剂和肥力缓释剂按用量与基质混合均匀,将基质均匀铺撒在屋顶绿化种植区内,种植屋顶绿化植物。使用本发明基质,可有效改善径流水质,有机污染物去除率在15-35%,营养物质的去除率在10-15%。同时基质较轻,不超过780kg/m3,饱水状态下的重量不超过1300kg/m3,可满足简单屋顶绿化建筑屋顶通常荷载较低的条件。可广泛的应用于各种类型的屋顶绿化。

Description

改善径流水质的屋顶绿化用基质及制备方法
技术领域
本发明涉及一种绿化用基质,具体地说,涉及一种环保型屋顶绿化植物栽培基质及制备方法,用于改善屋顶径流水质,避免污染环境。可在屋顶绿化中广泛应用。
 
背景技术
随着人们物质生活水平的日益提高,人们对居住区、办公区、休闲区绿化、美化的要求及欣赏水平也越来越高,屋顶绿化日益受到不同国家、不同地区人们的青睐和重视。
屋顶绿化是一种在建筑屋面上种植花草、灌木甚至小型乔木使屋面具有像花园一般的园林景观的屋面。可分为简单式绿化和花园式绿化。简单式绿化是指栽种低矮灌木或草坪、地被植物,不设置园林小品等,一般不允许非管理维修人员活动的简单绿化。花园式绿化与简单式绿化的区别在于栽培小型乔木等以形成植物群落复层结构,设置园路、座椅和园林小品,提供游人游览及休憩空间。屋顶绿化能较好地减轻排水压力,减少环境污染。由于植被增加了对雨水的截留作用和栽培基质对雨水的吸收作用,可大幅削减屋面径流峰值,推迟暴雨径流峰值出现时间,减轻对环境的污染。
不污染环境是进行屋顶绿化的基本要求。屋顶绿化基质要求要选择清洁材料和无害化工艺,要做到基质不会对环境造成污染。过去的人工栽培基质原料,常常对环境造成污染。
目前,屋顶绿化基质常常被赋予单一的植物栽培功能,很少被用于改善径流水质的作用,因此,开发屋顶绿化改善径流水质的基质成为了亟需破解的问题。
发明内容
本发明的目的就是为了解决现有技术存在的上述问题,而提供一种轻质、高效保水、清洁环保、能够改善径流水质的屋顶绿化用基质。
本发明的另一目的是提供上述屋顶绿化用基质的制备方法。
为了实现本发明目的,本发明改善径流水质的屋顶绿化用基质采用以下技术方案。
本发明改善径流水质的屋顶绿化用基质包括以下组分,各组分的重量分数为:
泥炭土        20-30
珍珠岩        10-15
粗纤维腐殖质  30-40
陶粒          15-20
凹凸棒土      5-10。
其中,所述原料均为市售商品。
本发明改善径流水质的屋顶绿化用基质的优化配方中,各组分的重量分数为:
泥炭土        20
珍珠岩        15
粗纤维腐殖质  45
陶粒          15
凹凸棒土       5。
为了防止病虫害的发生,保证基质中肥力的缓慢释放,保持肥力长久,在上述基质组分中还含有杀虫剂、杀菌剂和肥力缓释剂。其中,所述杀虫剂为高效、无公害的广谱土壤专用杀虫剂,每立方用量2-4克;杀菌剂为无公害、无残留、低毒性的农药,每立方用量0.6-1.2克;肥力缓释剂为长效缓释复合肥料,每立方用量30-50克。
本发明的制备方法为,将泥炭土、珍珠岩、粗纤维腐殖质、陶粒和凹凸棒土按比例混合并搅拌均匀,然后将杀虫剂、杀菌剂和肥力缓释剂按用量与基质混合均匀。
本发明基质在屋顶绿化中的应用:将基质均匀铺撒在屋顶绿化种植区内,根据所种植的植物不同,选取铺设厚度,将基质耙平并压实后,种植屋顶绿化植物。
本发明提供的改善径流水质的屋顶绿化用基质的优点在于:
(1)基质中的凹凸棒土,可有效改善径流水质,有机污染物去除率在15-35%,营养物质的去除率在10-15%。
(2)基质中的陶粒,5天内保持基质的含水率在45%以上,在简单式屋顶绿化基质层较薄的情况下,能满足绿化植物的正常生长的水分需求。
(3)基质重量较轻,不超过780kg/m3,饱水状态下的重量不超过1300kg/m3,可以满足简单屋顶绿化建筑屋顶通常荷载较低的条件。
(4)本发明改善径流水质的屋顶绿化用基质还能够有效防止病虫害的发生,保持肥力,无异味。
具体实施方式
为进一步描述本发明,下面结合实施例对本发明改善径流水质的屋顶绿化用基质作进一步详细说明。
以下实例用于说明本发明,但不用来限制本发明的范围。
实施例1
在一个屋顶绿化工程中,按比例称取下述重量份的原料:泥炭土20、珍珠岩15、粗纤维腐殖质40、陶粒15和凹凸棒土5,其中所述原料均为市售商品。将上述原料搅拌均匀,之后加入杀虫剂闻到死,用量2g/m3;杀菌剂恶霉灵,用量0.6g/m3,清除土壤中可能存在的虫体、虫卵以及有害菌;以及,施可丰长效缓释复合肥料(肥力缓释剂),用量40g/m3,混合均匀。然后装袋运输至工程现场,将基质均匀铺撒与屋顶绿化种植区域内,根据所种植的植物,选取铺设厚度,将基质耙平并压实后,种植绿化植物。
实施例2
在一个屋顶绿化工程中,按比例称取下述重量份的原料:泥炭土30、珍珠岩10、粗纤维腐殖质30、陶粒15和凹凸棒土10,其中所述原料均为市售商品。将上述原料搅拌均匀,之后加入杀虫剂闻到死,用量3g/m3;杀菌剂恶霉灵,用量1.2g/m3,清除土壤中可能存在的虫体、虫卵以及有害菌;以及,施可丰长效缓释复合肥料(肥力缓释剂),用量50g/m3,混合均匀。其余同实施例1。
实施例3
在一个屋顶绿化工程中,按比例称取下述重量份的原料:泥炭土30、珍珠岩10、粗纤维腐殖质40、陶粒5和凹凸棒土10,其中所述原料均为市售商品。将上述原料搅拌均匀,之后加入杀虫剂闻到死,用量4g/m3;杀菌剂恶霉灵,用量1.0g/m3,清除土壤中可能存在的虫体、虫卵以及有害菌;以及,施可丰长效缓释复合肥料(肥力缓释剂),用量30g/m3,混合均匀。其余同实施例1。
虽然,上文中已经用一般性说明及具体实施方案对本发明作了详尽的描述,但在本发明基础上,可以对之作一些修改或改进,这对本领域技术人员而言是显而易见的。因此,在不偏离本发明主旨的基础上所做的这些修改或改进,均属于本发明要求保护的范畴。

Claims (5)

1.一种改善径流水质的屋顶绿化用基质,其特征在于包括以下组分,各组分的重量分数为:
泥炭土        20-30
珍珠岩        10-15
粗纤维腐殖质  30-40
陶粒          15-20
凹凸棒土      5-10。
2.如权利要求1所述的改善径流水质的屋顶绿化用基质,其特征在于各组分的重量分数为:
泥炭土        20
珍珠岩        15
粗纤维腐殖质  45
陶粒          15
凹凸棒土       5。
3.如权利要求1或2所述的改善径流水质的屋顶绿化用基质,其特征在于:还含有杀虫剂、杀菌剂和肥力缓释剂。
4.如权利要求3所述的改善径流水质的屋顶绿化用基质,其特征在于:所述杀虫剂为高效、无公害的广谱土壤专用杀虫剂,每立方用量2-4克;杀菌剂为无公害、无残留、低毒性的农药,每立方用量0.6-1.2克;肥力缓释剂为长效缓释复合肥料,每立方用量30-50克。
5.如权利要求4所述的改善径流水质的屋顶绿化用基质的制备方法,其特征在于:将泥炭土、珍珠岩、粗纤维腐殖质、陶粒和凹凸棒土按比例混合并搅拌均匀,然后将杀虫剂、杀菌剂和肥力缓释剂按用量与基质混合均匀。
CN2012101575416A 2012-05-21 2012-05-21 改善径流水质的屋顶绿化用基质及制备方法 Pending CN102701839A (zh)