CN102698948B - Three-stage spraying method of bamboo craft - Google Patents

Three-stage spraying method of bamboo craft Download PDF

Info

Publication number
CN102698948B
CN102698948B CN 201210205368 CN201210205368A CN102698948B CN 102698948 B CN102698948 B CN 102698948B CN 201210205368 CN201210205368 CN 201210205368 CN 201210205368 A CN201210205368 A CN 201210205368A CN 102698948 B CN102698948 B CN 102698948B
Authority
CN
China
Prior art keywords
coating
spraying
spray
wood product
artistic bamboo
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN 201210205368
Other languages
Chinese (zh)
Other versions
CN102698948A (en
Inventor
罗潺潺
陈桂福
罗粤涛
陈桂道
罗成坤
罗晓玲
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
TAICANG DELAN TREE PIECE PAINTING EQUIPMENT TECHNOLOGY CO LTD
Original Assignee
TAICANG DELAN TREE PIECE PAINTING EQUIPMENT TECHNOLOGY CO LTD
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by TAICANG DELAN TREE PIECE PAINTING EQUIPMENT TECHNOLOGY CO LTD filed Critical TAICANG DELAN TREE PIECE PAINTING EQUIPMENT TECHNOLOGY CO LTD
Priority to CN 201210205368 priority Critical patent/CN102698948B/en
Publication of CN102698948A publication Critical patent/CN102698948A/en
Application granted granted Critical
Publication of CN102698948B publication Critical patent/CN102698948B/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention provides a spraying method, in particular a method for carrying out three-stage spraying on the surfaces of bamboo and wood materials and articles. Problems that a mixed coating containing no fine particles has been not added to a bamboo craft coating and a series of factors unfavorable for spraying, such as poor surface flatness, weak smoothness, small plumpness, low adhesion forceand large discharge capacity, exist in a multi-layer classified spraying process in the prior art are solved; a set of brand new three-stage spraying method of a bamboo craft is designed; and therefore, the flatness, smoothness, plumpness and adhesion force of the coating are obviously improved, so that powerful support is provided for the high-grade bamboo craft. As the three-stage spraying method is adopted, atomizing loss of the coating is greatly reduced, the coating is saved and the discharge capacity is reduced.

Description

A kind of three grades of spraying methods of artistic bamboo-wood product
Technical field
The present invention relates to a kind of spraying method, especially carry out the method for three grades of sprayings at bamboo matter, wood materials and article surface.
Background technology
The spraying of known artistic bamboo-wood product, be that spray gun by nitrocellulose primer, varnish and air press is directly to the spraying of artistic bamboo-wood product surface, but it is rare in coating, adding the coating and the multi-level classification spraying coating process that contain the thin not mixing of particle, the present invention is directed to existing spraying method and innovate recreation, invent a kind of three grades of spraying methods of artistic bamboo-wood product, filled up the industry blank.
Summary of the invention
At prior art still unresolvedly add in artistic bamboo-wood product coating that the surface smoothness that exists in the mixed coating contain thin not particle and the multi-level classification spraying coating process is poor, a little less than the fineness, a series of factors of spraying of being unfavorable for such as plumpness is little, adhesive force is low, blowdown flow rate is big, and design three grades of brand-new spraying methods of a cover.
The technical scheme that the present invention addresses the above problem is to select back cover layer coating, intermediate layer coating and the finishing coat coating that is exclusively used in the artistic bamboo-wood product for use, and what it adopted is three grades of spraying methods:
One, one-level back cover layer coating spraying
(1), select air compressor: power is more than 5, the tolerance abundance, pressure 4-7Kg/ square centimeter, be with three tracheaes, can satisfy the above needs that back cover layer coating, intermediate layer coating and finishing coat coating are constructed synchronously of three people, three tracheaes are numbered: back cover layer coating tracheae is that q1, intermediate layer coating tracheae are that q2, finishing coat coating tracheae are q3.
(2), debugging coating spray gun: capacity required 500ml, capacity can not be too big, otherwise too heavy, operation inconvenience, the little then speed of application of bore is slow, may delay the duration, unsuitable large-area construction.
(3), adorn coating fully: the back cover layer coating that is made into will be loaded in the hydraulic tank standby.
(4), by dress coating spray gun: in order to adapt to different construction, spray more preferably effect.By dress q2 6mm bore nozzle, because selecting different nozzles, the more little then spraying effect of bore is more smooth evenly at spray gun, and greatly then the flower point is more big for bore, and the convex-concave sense is more strong.
(5), polishing: artistic bamboo-wood product top layer is polished with 1000 order carpenter sand paper.
Temperature when (6), constructing: temperature can not be lower than-10 ℃.
(7), begin to spray the back cover layer: will spray back cover layer twice, midfeather is no more than 1 hour, and thickness is no more than 120 microns, spraying height 2-3mm.
(8), in dry: sprayed the artistic bamboo-wood product of back cover layer coating, and be seated in when indoor, temperature can not be lower than-10 ℃, and air drying is 8 hours.
Two, secondary intermediate layer coating spraying
(1), selects the coating spray gun for use: press dress q2 8mm bore nozzle, pressure 4-7 kilogram/square centimeter at spray gun.
(2), adorn the intermediate layer coating fully: the intermediate layer coating that is made into will be loaded in the hydraulic tank fully.
(3), begin to spray the intermediate layer coating: spray intermediate layer coating twice, midfeather 2 hours sprays height 5-10mm, and thickness is no more than 150 microns.
(4), polishing: can polish after dry 8 hours, adopt 400--600 order sand paper, the sand grains of floating intermediate layer coating surface projection gets final product gently.Noting firmly can not be too violent, otherwise can destroy coating, causes that the bottom is loosening, can cause adhesive force bad when serious, coating shedding.
(5), drying: the polished artistic bamboo-wood product of intermediate layer coating of spraying, be seated in when indoor, temperature can not be lower than in-8 ℃, be 26 hours drying time.
Three, three grades of finishing coat coating sprayings
(1), finishing coat coating spraying construction ground and requirement: be applicable to the artistic bamboo-wood product, the surface should be smooth, clean, and have intensity preferably, can construct behind the impurity such as elder generation's removal dust grease.
(2), adorn the finishing coat coating fully: the finishing coat coating that is made into is loaded in the hydraulic tank fully.
Temperature when (3), constructing: temperature can not be lower than-8 ℃
(4), begin to spray the finishing coat coating: spray finishing coat coating twice, midfeather 1 hour sprays height 4-6mm, and thickness is no more than 110 microns.
(5), drying: sprayed the artistic bamboo-wood product of finishing coat coating, and be seated in when indoor, temperature can not be lower than-10 ℃, and the air drying time is 26 hours.
Three grades of spraying methods of a kind of artistic bamboo-wood product of the present invention also are for different artistic bamboo-wood shape of products, and the method for best spray-on coating is arranged.
(1), rectangle artistic bamboo-wood product spraying: design earlier artistic bamboo-wood shape of product size on request, carry out the rectangle model with wooden frame then, to be sleeved in the rectangle model at rectangle artistic bamboo-wood product, successively rectangle artistic bamboo-wood product are sprayed back cover layer coating, intermediate layer coating and finishing coat coating by three grades of spraying method processes again, before the finishing coat coating does not also have surface drying, take off wooden frame at last and get final product.
(2), rhombus artistic bamboo-wood product spraying: with spray gun to draw a circle method, apart from rhombus artistic bamboo-wood product 30cm-40cm, laterally draw the circle spraying with the about 15cm of radius, and shake spray gun frequently up and down, the speed of spraying like this is fast and even, and it is easy to control, if adopt the overlapping spraying of main formula by rows, speed is slow, and the difficult control in junction evenly up and down, to influence outward appearance, cause holiday.
(3), cylindrical artistic bamboo-wood product sprayings: because it is cylindrical, thus with spray gun with " M " linear spraying, apart from 40cm, spray gun is wanted vertical cylinder spraying, from top to bottom, the good one side of spray turns to another side again, steering angle 60 degree.
(4), square artistic bamboo-wood product spraying: because the square column corner angle are clearly demarcated, be easy to blur because spraying the irregular square artistic bamboo-wood product corner angle that make, convenient for making spraying, with the distance spraying square artistic bamboo-wood product corner angle of 50cm, because of remote spraying, mist is spent diffusing as to open, and area is big and even, if distance is too near, do not note to spray thick slightly, spray inhomogeneously, square artistic bamboo-wood product arris fillet can not manifested, lost original square artistic bamboo-wood product overall appearance aesthetic feeling.
(5), the spraying of artistic bamboo-wood product circles beads bangle: modern artistic bamboo-wood product beads bangle decoration, all to spray coating, because it is small and exquisite, have ornamental, also more careful to their spraying coating process.Do artistic bamboo-wood product beads bangle, distance is too near, and the bottom can't positive spray at all, so can't reach ideal effect by general conventional spray method.Small nozzle is selected in spraying for use; apart from 40cm; sprayed coating fast looses; the one side one side is sprayed from top to bottom; can not positive spray; with the method for shake spray gun, make it spray coating on every side as far as possible, flat coating is brushed with hairbrush in the bottom; the place that is not sprayed onto also can be with the light one deck of spreading of hairbrush; loose with spray gun again and spray one time, can not be too thin, can not be too thick; covering brush mark gets final product; thin can not play good protection effect, thick then cover in original lines aesthetic feeling, undesirable appearance phenomenons such as crack also may occur.
The invention has the beneficial effects as follows: a kind of spraying method, the method for especially carrying out three grades of sprayings at bamboo matter, wood materials and article surface.Solved that prior art adds as yet that the surface smoothness that exists in the mixed coating that contains thin not particle and the multi-level classification spraying coating process is poor in the artistic bamboo-wood product coating, a little less than the fineness, a series of factors of spraying of being unfavorable for such as plumpness is little, adhesive force is low, blowdown flow rate is big, overlap brand-new three grades of spraying methods of artistic bamboo-wood product and design one, improved planarization, fineness, plumpness and the adhesive force of coating significantly, superior with strong support to the artistic bamboo-wood product.Because three grades of spraying methods that adopt, the atomizing of coating run off and subtract greatly, save coating, have reduced blowdown flow rate.
The specific embodiment
The present invention is described in further detail below in conjunction with embodiment:
Embodiment one
The present invention selects back cover layer coating, intermediate layer coating and the finishing coat coating that is exclusively used in the artistic bamboo-wood product for use, and what it adopted is three grades of spraying methods:
One, one-level back cover layer coating spraying
(1), select air compressor: power is more than 5, the tolerance abundance, pressure 4-7Kg/ square centimeter, be with three tracheaes, can satisfy the above needs that back cover layer coating, intermediate layer coating and finishing coat coating are constructed synchronously of three people, three tracheaes are numbered: back cover layer coating tracheae is that q1, intermediate layer coating tracheae are that q2, finishing coat coating tracheae are q3.
(2), debugging coating spray gun: capacity required 500ml, capacity can not be too big, otherwise too heavy, operation inconvenience, the little then speed of application of bore is slow, may delay the duration, unsuitable large-area construction.
(3), adorn coating fully: the back cover layer coating that is made into will be loaded in the hydraulic tank standby.
(4), by dress coating spray gun: in order to adapt to different construction, spray more preferably effect.By dress q2 6mm bore nozzle, because selecting different nozzles, the more little then spraying effect of bore is more smooth evenly at spray gun, and greatly then the flower point is more big for bore, and the convex-concave sense is more strong.
(5), polishing: artistic bamboo-wood product top layer is polished with 1000 order carpenter sand paper.
Temperature when (6), constructing: temperature can not be lower than-10 ℃.
(7), begin to spray the back cover layer: will spray back cover layer twice, midfeather is no more than 1 hour, and thickness is no more than 120 microns, spraying height 2-3mm.
(8), drying: sprayed the artistic bamboo-wood product of back cover layer coating, and be seated in when indoor, temperature can not be lower than-10 ℃, and air drying is 8 hours.
Two, secondary intermediate layer coating spraying
(1), selects the coating spray gun for use: press dress q2 8mm bore nozzle, pressure 4-7 kilogram/square centimeter at spray gun.
(2), adorn the intermediate layer coating fully: the intermediate layer coating that is made into will be loaded in the hydraulic tank fully.
(3), begin to spray the intermediate layer coating: spray intermediate layer coating twice, midfeather 2 hours sprays height 5-10mm, and thickness is no more than 150 microns.
(4), polishing: can polish after dry 8 hours, adopt 400--600 order sand paper, the sand grains of floating intermediate layer coating surface projection gets final product gently.Noting firmly can not be too violent, otherwise can destroy coating, causes that the bottom is loosening, can cause adhesive force bad when serious, coating shedding.
(5), drying: the polished artistic bamboo-wood product of intermediate layer coating of spraying, be seated in when indoor, temperature can not be lower than in-8 ℃, be 26 hours drying time.
Three, three grades of finishing coat coating sprayings
(1), finishing coat coating spraying construction ground and requirement: be applicable to the artistic bamboo-wood product, the surface should be smooth, clean, and have intensity preferably, can construct behind the impurity such as elder generation's removal dust grease.
(2), adorn the finishing coat coating fully: the finishing coat coating that is made into is loaded in the hydraulic tank fully.
Temperature when (3), constructing: temperature can not be lower than-8 ℃
(4), begin to spray the finishing coat coating: spray finishing coat coating twice, midfeather 1 hour sprays height 4-6mm, and thickness is no more than 110 microns.
(5), drying: sprayed the artistic bamboo-wood product of finishing coat coating, and be seated in when indoor, temperature can not be lower than-10 ℃, and the air drying time is 26 hours.
Embodiment two
Three grades of spraying methods of a kind of artistic bamboo-wood product of the present invention also are for different artistic bamboo-wood shape of products, and the method for best spray-on coating is arranged.
(1), rectangle artistic bamboo-wood product spraying: design earlier artistic bamboo-wood shape of product size on request, carry out the rectangle model with wooden frame then, to be sleeved in the rectangle model at rectangle artistic bamboo-wood product, successively rectangle artistic bamboo-wood product are sprayed back cover layer coating, intermediate layer coating and finishing coat coating by three grades of spraying method processes again, before the finishing coat coating does not also have surface drying, take off wooden frame at last and get final product.
(2), rhombus artistic bamboo-wood product spraying: with spray gun to draw a circle method, apart from rhombus artistic bamboo-wood product 30cm-40cm, laterally draw the circle spraying with the about 15cm of radius, and shake spray gun frequently up and down, the speed of spraying like this is fast and even, and it is easy to control, if adopt the overlapping spraying of main formula by rows, speed is slow, and the difficult control in junction evenly up and down, to influence outward appearance, cause holiday.
(3), cylindrical artistic bamboo-wood product sprayings: because it is cylindrical, thus with spray gun with " M " linear spraying, apart from 40cm, spray gun is wanted vertical cylinder spraying, from top to bottom, the good one side of spray turns to another side again, steering angle 60 degree.
(4), square artistic bamboo-wood product spraying: because the square column corner angle are clearly demarcated, be easy to blur because spraying the irregular square artistic bamboo-wood product corner angle that make, convenient for making spraying, with the distance spraying square artistic bamboo-wood product corner angle of 50cm, because of remote spraying, mist is spent diffusing as to open, and area is big and even, if distance is too near, do not note to spray thick slightly, spray inhomogeneously, square artistic bamboo-wood product arris fillet can not manifested, lost original square artistic bamboo-wood product overall appearance aesthetic feeling.
(5), the spraying of artistic bamboo-wood product circles beads bangle: modern artistic bamboo-wood product beads bangle decoration, all to spray coating, because it is small and exquisite, have ornamental, also more careful to their spraying coating process.Do artistic bamboo-wood product beads bangle, distance is too near, and the bottom can't positive spray at all, so can't reach ideal effect by general conventional spray method.Small nozzle is selected in spraying for use; apart from 40cm; sprayed coating fast looses; the one side one side is sprayed from top to bottom; can not positive spray; with the method for shake spray gun, make it spray coating on every side as far as possible, flat coating is brushed with hairbrush in the bottom; the place that is not sprayed onto also can be with the light one deck of spreading of hairbrush; loose with spray gun again and spray one time, can not be too thin, can not be too thick; covering brush mark gets final product; thin can not play good protection effect, thick then cover in original lines aesthetic feeling, undesirable appearance phenomenons such as crack also may occur.
In sum; three grades of spraying methods of a kind of artistic bamboo-wood product of the present invention; though explain with reference to embodiment; but; technical staff of the same trade is to be understood that; the invention is not restricted to illustrated each flow process details and method, can make and change and change and do not depart from protection scope of the present invention.

Claims (2)

1. three of artistic bamboo-wood product grades of spraying methods is characterized in that the present invention selects back cover layer coating, intermediate layer coating and the finishing coat coating that is exclusively used in the artistic bamboo-wood product for use, and what it adopted is three grades of spraying methods:
One, one-level back cover layer coating spraying
(1), select air compressor: power is more than 5, the tolerance abundance, pressure 4-7Kg/ square centimeter, be with three tracheaes, can satisfy the above needs that back cover layer coating, intermediate layer coating and finishing coat coating are constructed synchronously of three people, three tracheaes are numbered: back cover layer coating tracheae is that q1, intermediate layer coating tracheae are that q2, finishing coat coating tracheae are q3;
(2), debugging coating spray gun: capacity required 500ml;
(3), adorn coating fully: the back cover layer coating that is made into will be loaded in the hydraulic tank standby;
(4), by dress coating spray gun: in order to adapt to different construction, spray more preferably effect, press dress q2 6mm bore nozzle at spray gun;
(5), polishing: artistic bamboo-wood product top layer is polished with 1000 order carpenter sand paper;
Temperature when (6), constructing: temperature can not be lower than-10c;
(7), begin to spray the back cover layer: will spray back cover layer twice, midfeather is no more than 1 hour, and thickness is no more than 120 microns, spraying height 2-3mm;
(8), drying: sprayed the artistic bamboo-wood product of back cover layer coating, and be seated in when indoor, temperature can not be lower than-10 ℃, and air drying is 8 hours;
Two, secondary intermediate layer coating spraying
(1), selects the coating spray gun for use: press dress q2 8mm bore nozzle, pressure 4-7Kg/ square centimeter at spray gun;
(2), adorn the intermediate layer coating fully: the intermediate layer coating that is made into will be loaded in the hydraulic tank fully;
(3), begin to spray the intermediate layer coating: spray intermediate layer coating twice, midfeather 2 hours sprays height 5-10mm, and thickness is no more than 150 microns;
(4), polishing: can polish after dry 8 hours, adopt 400--600 order sand paper, the sand grains of floating intermediate layer coating surface projection gets final product gently;
(5), drying: the polished artistic bamboo-wood product of intermediate layer coating of spraying, be seated in when indoor, temperature can not be lower than in-8 ℃, be 26 hours drying time;
Three, three grades of finishing coat coating sprayings
(1), finishing coat coating spraying construction ground and requirement: be applicable to the artistic bamboo-wood product, the surface should be smooth, clean, and have intensity preferably, can construct behind the impurity such as elder generation's removal dust grease;
(2), adorn the finishing coat coating fully: the finishing coat coating that is made into is loaded in the hydraulic tank fully;
Temperature when (3), constructing: temperature can not be lower than-8c;
(4), begin to spray the finishing coat coating: spray finishing coat coating twice, midfeather 1 hour sprays height 4-6mm, and thickness is no more than 110 microns;
(5), drying: sprayed the artistic bamboo-wood product of finishing coat coating, and be seated in when indoor, temperature can not be lower than-10c, and the air drying time is 26 hours.
2. three of a kind of artistic bamboo-wood product according to claim 1 grades of spraying methods are further characterized in that for different artistic bamboo-wood shape of products, and the method for best spray-on coating is arranged,
(1), rectangle artistic bamboo-wood product spraying: design earlier artistic bamboo-wood shape of product size on request, carry out the rectangle model with wooden frame then, to be sleeved in the rectangle model at rectangle artistic bamboo-wood product, successively rectangle artistic bamboo-wood product are sprayed back cover layer coating, intermediate layer coating and finishing coat coating by three grades of spraying method processes again, before the finishing coat coating does not also have surface drying, take off wooden frame at last and get final product;
(2), rhombus artistic bamboo-wood product spray: spray gun to draw a circle method, apart from rhombus artistic bamboo-wood product 30cm-40cm, is laterally drawn the circle spraying with the about 15cm of radius, and shaken spray gun frequently up and down, and the speed of spraying like this is fast and even, and easy to control;
(3), cylindrical artistic bamboo-wood product sprayings: because it is cylindrical, thus with spray gun with " M " linear spraying, apart from 40cm, spray gun is wanted vertical cylinder spraying, from top to bottom, the good one side of spray turns to another side again, steering angle 60 degree;
(4), square artistic bamboo-wood product spraying: because the square column corner angle are clearly demarcated, be easy to blur because spraying the irregular square artistic bamboo-wood product corner angle that make, for making spraying conveniently, with the distance spraying square artistic bamboo-wood product corner angle of 50cm;
(5), artistic bamboo-wood product circle beads bangle spraying: small nozzle is selected in spraying for use, apart from 40cm, fast diffusing sprayed coating, the one side one side is sprayed from top to bottom, can not positive spray, method with the shake spray gun, make and spray coating around it as far as possible, flat coating is brushed with hairbrush in the bottom, and the place that is not sprayed onto also can be with the light one deck of spreading of hairbrush, loose with spray gun again and spray one time, cover brush mark and get final product.
CN 201210205368 2012-06-21 2012-06-21 Three-stage spraying method of bamboo craft Expired - Fee Related CN102698948B (en)