CN102041325A - Wax emulsion as leather finishing addictive and preparation method thereof - Google Patents

Wax emulsion as leather finishing addictive and preparation method thereof Download PDF

Info

Publication number
CN102041325A
CN102041325A CN2009100360580A CN200910036058A CN102041325A CN 102041325 A CN102041325 A CN 102041325A CN 2009100360580 A CN2009100360580 A CN 2009100360580A CN 200910036058 A CN200910036058 A CN 200910036058A CN 102041325 A CN102041325 A CN 102041325A
Authority
CN
China
Prior art keywords
leather
wax emulsion
wax
water
distilled water
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN2009100360580A
Other languages
Chinese (zh)
Inventor
蒋马小
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN2009100360580A priority Critical patent/CN102041325A/en
Publication of CN102041325A publication Critical patent/CN102041325A/en
Pending legal-status Critical Current

Abstract

The invention discloses a wax emulsion as a leather finishing addictive, in particular the constituents of the wax emulsion as the leather finishing addictive and a preparation method. The wax emulsion comprises the following raw materials in percentage by weight: 21.00-49.00 bee wax, 9.00-21.00 cera flava, 0.88-2.04 perogol O-20, 0.32-0.76 span-800 and 28.8-67.20 distilled water. The wax emulsion can be prepared by the following steps of: adding the span-80 and the perogol O-20 in a container, heating, melting, uniformly stirring and adding in an emulsor; adding the bee wax and the cera flava in the emulsor, heating, melting and uniformly stirring; dropping distilled water by stirring; stopping stirring after finishing adding water; and filtering the obtained materials to obtain a finished product. The wax emulsion as the leather finishing addictive can be applied to slurry for decorating the bottom layer, the intermediate layer and the top layer of leather, can greatly improve the hand feeling of the leather, has various functions of preventing sticking, smoothening, resisting water, softening, filling, glazing and the like and can also improve the dry and wet wiping resistance of the leather. The wax emulsion is a high-grade leather finishing addictive for producing pig, cow and sheet light-color leather or white leather.

Description

A kind of EFFECTS OF LEATHER FINISHING auxiliary agent wax emulsion and preparation method
Technical field
The present invention relates to a kind of EFFECTS OF LEATHER FINISHING auxiliary agent wax emulsion, comprise the composition and the preparation method of this EFFECTS OF LEATHER FINISHING auxiliary agent wax emulsion.
Background technology
The leather wax emulsion is a kind of important promoter material of process hides ornamenting operation.Domestic many tanneries still adopt natural montanin wax and soap flakes to prepare at present.Because look black, the system instability can not adapt to the requirement that high-grade leather is produced.Commercial goods wax mainly contains paraffin, ceresine, insect wax, beeswax, palm wax, montanin wax etc. at present.From chemical structure analysis, these waxes approximately are divided into three kinds, and a kind of is compound based on the fatty acids ester structure, and a kind of is the pure carbon hydrogen compound, another is the alkanes that had both contained hydrocarbon polymer, contains the mixture of fatty acid or lipid acid and aliphatic alcohols again.Above-mentioned three kinds of wax performances are single, all can not satisfy the ornamenting requirement of high-grade leather (especially light color and white leather).
Summary of the invention
For solving problem, the present invention proposes a kind of EFFECTS OF LEATHER FINISHING auxiliary agent wax emulsion and preparation method thereof.
1, the present invention is an EFFECTS OF LEATHER FINISHING auxiliary agent wax emulsion, and it is to be prepared from by following raw materials according (W%):
Beeswax 21.00-49.00 river wax 9.00-21.00 paregal O-20 0.88-2.04
Benzene-80 0.32-0.76 of department distilled water 28.8-67.20.
2, preferable proportioning raw materials (W%) is in said ratio:
Beeswax 28.00-42.00 river wax 12.00-18.00 paregal O-20 1.16-1.75
Benzene-80 0.43-0.64 of department distilled water 38.40-57.60.
3, better proportioning raw materials (W%) is in said ratio:
Beeswax 35.00 river wax 15.00 paregal Os-20 1.46
Department's benzene-80 0.54 distilled water 48.00.
4, for guaranteeing to reach the designed effect of the present invention, conveniently use, EFFECTS OF LEATHER FINISHING auxiliary agent wax emulsion of the present invention and preparation method thereof should be by following processing method preparation.
(1) takes by weighing following raw materials according (W%);
Beeswax 21.00-49.00 river wax 9.00-21.00 paregal O-20 0.88-2.04
Benzene-80 0.32-0.76 of department distilled water 28.8-67.20.
(2) will take charge of that benzene-80 and peregal O-20 put into vessel in heating fusing and the postcooling that stirs is standby;
(3) (2) gained mixture, beeswax, river wax are put into emulsor, after the heat fused, stir;
(4) under agitation in (3) gained mixture, drip distilled water;
(5) treat to stop after water adds to stir;
(6) (5) gained material filtering is got finished product.
5, method according to claim 4, in its step (3), the heating medium temperature is 120-150 ℃, churning time is no less than 5 minutes;
6, method according to claim 4, in its step (4), it is 0.5Kg/min that the initial stage adds water speed, stirring velocity is 300rpm;
7, method according to claim 4 in its step (4), when adding water to the material retrogradation, adds water speed and transfers to 0.8Kg/min, and stirring velocity is 500rpm;
8, method according to claim 4 in its step (4), when continuing to add water to material when thinning, adds water speed and transfers to 6Kg/min, and stirring velocity is 800rpm, all adds until water.
EFFECTS OF LEATHER FINISHING auxiliary agent wax emulsion of the present invention system adopts two kinds of natural waxs, in addition suitable emulsifying agent, a kind of EFFECTS OF LEATHER FINISHING auxiliary agent that is prepared from through special emulsifying process.At the bottom of adding leather, in, use in the slurry of top finishing, can improve the feel of finished leather widely, have multiple functions such as antiseized, smooth, waterproof, softness, filling, glazing, can also improve finished leather anti-ly do, the wet rubbing ability.This wax emulsion is main raw material with the natural wax, selects different wax proportionings, can make rigid wax emulsion and soft wax emulsion; Select suitable two kinds of nonionic emulsifier and property-modifying additive for use, the wax emulsion that forms through particular emulsifier and emulsifying process emulsification is to manufacture the high-grade EFFECTS OF LEATHER FINISHING auxiliary agent of pig, ox, sheep light color leather or white leather.
Specific implementation method
(1) take by weighing following raw materials according (W%) by processing compound:
Beeswax 35.00 river wax 15.00 paregal Os-20 1.46
Department's benzene-80 0.54 distilled water 48.00.
(2) will take charge of that benzene-80 and peregal O-20 put into vessel in heating fusing and the postcooling that stirs is standby;
(3) (2) gained mixture, beeswax, river wax are put into emulsor, after the heat fused, stir; The heating medium temperature is 120-150 ℃, and churning time is no less than 5 minutes;
(4) under agitation in (3) gained mixture, drip distilled water; It is 0.5Kg/min that initial stage adds water speed, and stirring velocity is 300rpm; When adding water to the material retrogradation, add water speed and transfer to 0.8Kg/min, stirring velocity is 500rpm; When continuing to add water to material when thinning, add water speed and transfer to 6Kg/min, stirring velocity is 800rpm, all adds until water.
(5) treat to stop after water adds to stir;
(6) (5) gained material filtering is got finished product.

Claims (8)

1. EFFECTS OF LEATHER FINISHING auxiliary agent wax emulsion is characterized in that it is to be prepared from by following raw materials according (W%):
Beeswax 21.00-49.00 river wax 9.00-21.00 paregal O-20 0.88-2.04
Benzene-80 0.32-0.76 of department distilled water 28.8-67.20.
2. EFFECTS OF LEATHER FINISHING auxiliary agent wax emulsion according to claim 1 is characterized in that (W%):
Beeswax 28.00-42.00 river wax 12.00-18.00 paregal O-20 1.16-1.75
Benzene-80 0.43-0.64 of department distilled water 38.40-57.60.
3. EFFECTS OF LEATHER FINISHING auxiliary agent wax emulsion according to claim 1 and 2 is characterized in that (W%);
Beeswax 35.00 river wax 15.00 paregal Os-20 1.46
Department's benzene-80 0.54 distilled water 48.00.
4. EFFECTS OF LEATHER FINISHING auxiliary agent wax emulsion and preparation method thereof:
(1) take by weighing following raw materials according (W%).
Beeswax 21.00-49.00 river wax 9.00-21.00 paregal O-20 0.88-2.04
Benzene-80 0.32-0.76 of department distilled water 28.8-67.20.
(2) will take charge of that benzene-80 and peregal O-20 put into vessel in heating fusing and the postcooling that stirs is standby;
(3) (2) gained mixture, beeswax, river wax are put into emulsor, after the heat fused, stir;
(4) under agitation in (3) gained mixture, drip distilled water;
(5) treat to stop after water adds to stir;
(6) (5) gained material filtering is got finished product.
5. method according to claim 4, in its step (3), the heating medium temperature is 120-150 ℃, churning time is no less than 5 minutes.
6. method according to claim 4, in its step (4), it is 0.5Kg/min that the initial stage adds water speed, stirring velocity is 300rpm.
7. method according to claim 4 in its step (4), when adding water to the material retrogradation, adds water speed and transfers to 0.8Kg/min, and stirring velocity is 500rpm.
8. method according to claim 4 in its step (4), when continuing to add water to material when thinning, adds water speed and transfers to 6Kg/min, and stirring velocity is 800rpm, all adds until water.
CN2009100360580A 2009-10-16 2009-10-16 Wax emulsion as leather finishing addictive and preparation method thereof Pending CN102041325A (en)