CN101736608B - Pigment printing thickener and method for preparing same - Google Patents

Pigment printing thickener and method for preparing same Download PDF

Info

Publication number
CN101736608B
CN101736608B CN200910273337A CN200910273337A CN101736608B CN 101736608 B CN101736608 B CN 101736608B CN 200910273337 A CN200910273337 A CN 200910273337A CN 200910273337 A CN200910273337 A CN 200910273337A CN 101736608 B CN101736608 B CN 101736608B
Authority
CN
China
Prior art keywords
parts
component
printing
minutes
kilograms
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN200910273337A
Other languages
Chinese (zh)
Other versions
CN101736608A (en
Inventor
徐春翼
万安
刘礼华
郭秋萍
郑晓宇
黄先宁
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
JINZHOU TIANYI FINE CHEMISTRY INDUSTRY DEVELOPMENT Co Ltd
Original Assignee
JINZHOU TIANYI FINE CHEMISTRY INDUSTRY DEVELOPMENT Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by JINZHOU TIANYI FINE CHEMISTRY INDUSTRY DEVELOPMENT Co Ltd filed Critical JINZHOU TIANYI FINE CHEMISTRY INDUSTRY DEVELOPMENT Co Ltd
Priority to CN200910273337A priority Critical patent/CN101736608B/en
Publication of CN101736608A publication Critical patent/CN101736608A/en
Application granted granted Critical
Publication of CN101736608B publication Critical patent/CN101736608B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention provides a pigment printing thickener and a method for preparing the same. The method comprises the following steps of: preparing a water phase containing monomers, a crosslinking agent and an initiator and an oil phase containing solvent oil and an activator; shearing-emulsifying the water phase and the oil phase at a high speed in an atmosphere of argon gas; initializing the solution by sulfur dioxide, heating the solution to the temperature of between 50 and 60 DEG C, keeping the solution warm, adding an emulsifier, stirring the mixed solution for 10 to 30 minutes, adding the mixed solution to the solvent oil containing sodium polyacrylate and the activator, and evenly stirring the mixed solution to obtain the finished product of the pigment printing thickener. The pigment printing thickener has the advantages of small dosage, strong thickening effect and good thixotropic property, has a simple preparation process and is suitable for mass industrialized production.

Description

Paint thickener for printing and preparation method thereof
Technical field
The present invention relates to the auxiliary chemicals field, specially refer to paint thickener for printing and preparation method thereof.
Background technology
COAT PRINTING is meant that using binder forms resin film on fabric, mechanically be fixed on the printing method on the fabric with pigment.COAT PRINTING, no matter adopt the sort of stamp mode, its print paste is formed by pigment, adhesive, thickener and other additives.Can increase its viscosity through in print paste, adding thickener, reduce its flowability, make it have pseudoplastic behavior, this performance makes adhesive self-crosslinking or external crosslinking combine closely each other by coating particles, improves rub resistance and fastness to washing.Paint thickener for printing is the important component in the print paste, directly affects the quality and the cost of COAT PRINTING.Thickener mainly comprises natural thickener, emulsifing thickener, synthetic thickening agent three major types at present, and wherein the natural thickener use cost is high, and depth of color, vividness, fastness to washing and fabric feeling are all unsatisfactory, eliminates gradually at present.
Summary of the invention
The object of the present invention is to provide a kind of mill base modulation convenience that has, stability is good, and the surface is skinning not, does not fill in paint thickener for printing of net and preparation method thereof during stamp.
For realizing above-mentioned purpose, technical scheme of the present invention is:
Water in the paint thickener for printing (component 1) by following material by weight component constitute:
25~40 parts in acrylic acid
5~20 parts of acrylamides
3~8 parts of methacrylic acids
1~3 part of crosslinking agent
2~4 parts of sodium acetates
0.5~2.5 part of initator
10~20 parts in NaOH
40~65 parts of deionized waters
Wherein: crosslinking agent is N, and N '-methylene acrylamide, initator are ammonium persulfate.
Oil phase in the paint thickener for printing (component 2) by following material by weight component constitute:
2~5 parts of ethyl acrylates
15~25 parts of sorbester p17s
10~30 parts of polysorbate60s
200 #35~75 parts of solvent naphthas
2~5 parts of laurate APEOs.
Component 4 in the paint thickener for printing by following material by weight component constitute:
10~16 parts in acid polyethylene sodium (dry powder)
200 #8~15 parts of solvent naphthas
5~10 parts of sorbester p18s.
The preparation method of paint thickener for printing follows these steps to carry out (following each material is parts by weight of component):
1, formulation components 1:
With 25~40 parts acrylic acid, 5~20 parts acrylamide, 3~8 parts of methacrylic acids; 1~3 part of N, N '-methylene acrylamide crosslinking agent, 2~4 parts of sodium acetates; 0.5~2.5 parts ammonium persulfate initiator, and 10~20 parts of NaOH and 40~60 parts of aqueous solution that deionized water constitutes are put in the preparatory emulsification still; The pH value to 8 of regulation system, high speed shear emulsification 10~30 minutes;
2, formulation components 2:
With 2~5 parts of ethyl acrylates, 15~25 parts sorbester p17,10~30 parts of polysorbate60s, 35~75 parts 200 #The laurate APEO of solvent naphtha and 2~5 parts dropped into preparatory emulsification still high speed emulsification pretreatment 10~30 minutes together;
3, under argon shield, component 1 and component 2 are joined in the agitated reactor simultaneously, stirred 10~30 minutes, feed sulfur dioxide and cause; Be warmed up to 50~60 ℃, and under this temperature, be incubated 3~4 hours, then add 12~30 parts NPE NP-10; Stirred 10~30 minutes, it is subsequent use to process component 3, and wherein the amount of NPE NP-10 is to confirm as follows; For example: component 1 is 100 parts, and component 2 is 100 parts, and it is 50 parts that component 3 is added up with component 4; Total umber is 250 parts, and then NPE NP-10 accounts for wherein 12~30 parts;
4, the acid polyethylene sodium (dry powder) that in another agitator, adds 10~16 parts, 8~15 parts 200 #The sorbester p18 of solvent naphtha and 5~10 parts stirred 10~30 minutes, component 3 was added again, and mixed and was the paint thickener for printing finished product.
Good effect of the present invention is:
1, paint thickener for printing can with various binder compatibilities, the printing paste of preparation is applicable to roller printing and garden, PLATE SCREAM PRINTING, and the PRINTED FABRIC pattern contour is clear, lines are meticulous, bright in colour, tinctorial yield is high, and fastness is excellent;
2, to have a residual monomer few for paint thickener for printing, has from thickening property, can directly be used for characteristics such as printing paste modulation;
3, the modulation of paint thickener for printing mill base is convenient, good stability, and the surface is skinning not, does not fill in net during stamp, and is good with stamp binder, coating and printing assistant compatibility, possesses good stable property.
The specific embodiment
Further specify the specific embodiment of the present invention below in conjunction with given embodiment.
Embodiment one
1, the preparation of component 1: with 250 kilograms acrylic acid, 200 kilograms acrylamide, 30 kilograms methacrylic acid; 10 kilograms N; N '-methylene acrylamide, 20 kilograms sodium acetate, the aqueous solution of the NaOH of 5 kilograms ammonium persulfate and 475 kilograms is put in the preparatory emulsification still; The pH value of regulation system is 8, high speed shear emulsification 10~30 minutes;
2, the preparation of component 2: with 20 kilograms ethyl acrylate, 150 kilograms sorbester p17,200 kilograms polysorbate60,600 kilograms 200 #The preparatory emulsification still of the laurate APEO input high speed emulsification pretreatment of solvent naphtha and 30 kilograms 10~30 minutes;
3, under argon shield, component 1 and component 2 are joined in the agitated reactor simultaneously; Stirred 10-30 minute, and fed sulfur dioxide and cause, be warmed up to 50~60 ℃; And under this temperature, be incubated 3~4 hours; The NPE NP-10 that then adds 150 kilograms stirred 10~30 minutes, and it is subsequent use to process component 3;
4, the Sodium Polyacrylate (dry powder) that in another agitator, adds 120 kg, 150 kilograms 200 #The sorbester p18 of solvent naphtha and 80 kilograms stirred after 10~30 minutes, component 3 was added again, and mixed and was the thickener finished product.
Embodiment two
1, the preparation of component 1: with 300 kilograms acrylic acid, 150 kilograms acrylamide, 30 kilograms methacrylic acid; 10 kilograms N; N '-methylene acrylamide, 20 kilograms sodium acetate, the aqueous solution of the NaOH of 5 kilograms ammonium persulfate and 475 kilograms is put in the preparatory emulsification still; The pH value of regulation system is 8, high speed shear emulsification 10~30 minutes;
2, the preparation of component 2: with 20 kilograms ethyl acrylate, 150 kilograms sorbester p17,200 kilograms polysorbate60,600 kilograms 200 #The preparatory emulsification still of the laurate APEO input high speed emulsification pretreatment of solvent naphtha and 30 kilograms 10~30 minutes;
3, under argon shield, component 1 and component 2 are joined in the agitated reactor simultaneously; Stirred 10-30 minute, and fed sulfur dioxide and cause, be warmed up to 50~60 ℃; And under this temperature, be incubated 3~4 hours; The NPE NP-10 that then adds 160 kilograms stirred 10~30 minutes, and it is subsequent use to process component 3;
4, the Sodium Polyacrylate (dry powder) that in another agitator, adds 100 kilograms, 150 kilograms 200 #The sorbester p18 of solvent naphtha and 80 kilograms stirred after 10~30 minutes, component 3 was added again, and mixed and was the thickener finished product.
Embodiment three
1, the preparation of component 1: with 350 kilograms acrylic acid, 100 kilograms acrylamide, 30 kilograms methacrylic acid; 10 kilograms N; N '-methylene acrylamide, 20 kilograms sodium acetate, the aqueous solution of the NaOH of 5 kilograms ammonium persulfate and 475 kilograms is put in the preparatory emulsification still; The pH value of regulation system is 8, high speed shear emulsification 10~30 minutes;
2, the preparation of component 2: with 30 kilograms ethyl acrylate, 150 kilograms sorbester p17,200 kilograms polysorbate60,600 kilograms 200 #The preparatory emulsification still of the laurate APEO input high speed emulsification pretreatment of solvent naphtha and 30 kilograms 10~30 minutes;
3, under argon shield, component 1 and component 2 are joined in the agitated reactor simultaneously; Stirred 10-30 minute, and fed sulfur dioxide and cause, be warmed up to 50~60 ℃; And under this temperature, be incubated 3~4 hours; The NPE NP-10 that then adds 160 kilograms stirred 10~30 minutes, and it is subsequent use to process component 3;
4, the Sodium Polyacrylate (dry powder) that in another agitator, adds 120 kg, 150 kilograms 200 #The sorbester p18 of solvent naphtha and 80 kilograms stirred after 10~30 minutes, component 3 was added again, and mixed and was the thickener finished product.
Example detection result:
Paint thickener for printing through the check, wherein: outward appearance be the milky white to light yellow viscous liquid, solids content is 60-70%, 1% pH value of water solution is 6-7, stability is more than 6 months.

Claims (2)

1. paint thickener for printing is characterized in that: the water in the paint thickener for printing be component 1 by following material by weight component constitute:
Figure FSB00000786696700011
Wherein: crosslinking agent is N, and N '-methylene acrylamide, initator are ammonium persulfate;
Oil phase in the paint thickener for printing is a component 2, by following material by weight component constitute:
Figure FSB00000786696700012
Component 4 in the paint thickener for printing by following material by weight component constitute:
10~16 parts in acid polyethylene sodium dry powder
200 #8~15 parts of solvent naphthas
5~10 parts of sorbester p18s.
2. paint thickener for printing according to claim 1 is characterized in that: the preparation method of paint thickener for printing follows these steps to carry out, below each material be parts by weight of component:
(1), formulation components 1:
With 25~40 parts acrylic acid, 5~20 parts acrylamide, 3~8 parts of methacrylic acids; 1~3 part of N, N '-methylene acrylamide crosslinking agent, 2~4 parts of sodium acetates; 0.5~2.5 parts ammonium persulfate initiator, and 10~20 parts of NaOH and 40~60 parts of aqueous solution that deionized water constitutes are put in the preparatory emulsification still; The pH value to 8 of regulation system, high speed shear emulsification 10~30 minutes;
(2), formulation components 2:
With 2~5 parts of ethyl acrylates, 15~25 parts sorbester p17,10~30 parts of polysorbate60s, 35~75 parts 200# solvent naphtha and 2~5 parts laurate APEO dropped into preparatory emulsification still high speed emulsification pretreatment 10~30 minutes together;
(3), under argon shield, component 1 and component 2 are joined in the agitated reactor simultaneously; Stirred 10~30 minutes, and fed sulfur dioxide and cause, be warmed up to 50~60 ℃; And under this temperature, be incubated 3~4 hours; The NPE NP-10 that then adds 12~30 parts stirred 10~30 minutes, and it is subsequent use to process component 3;
(4), in another agitator, add 10~16 parts acid polyethylene sodium (dry powder), 8~15 parts 200 #The sorbester p18 of solvent naphtha and 5~10 parts stirred 10~30 minutes, component 3 was added again, and mixed and was the paint thickener for printing finished product.
CN200910273337A 2009-12-15 2009-12-15 Pigment printing thickener and method for preparing same Active CN101736608B (en)