CN101149538A - Spacer particle dispersion liquid - Google Patents

Spacer particle dispersion liquid Download PDF

Info

Publication number
CN101149538A
CN101149538A CNA200710166707XA CN200710166707A CN101149538A CN 101149538 A CN101149538 A CN 101149538A CN A200710166707X A CNA200710166707X A CN A200710166707XA CN 200710166707 A CN200710166707 A CN 200710166707A CN 101149538 A CN101149538 A CN 101149538A
Authority
CN
China
Prior art keywords
spacer particle
dispersio
particle
liquid crystal
substrate
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CNA200710166707XA
Other languages
Chinese (zh)
Inventor
大口善之
上田伦久
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sekisui Chemical Co Ltd
Original Assignee
Sekisui Chemical Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sekisui Chemical Co Ltd filed Critical Sekisui Chemical Co Ltd
Publication of CN101149538A publication Critical patent/CN101149538A/en
Pending legal-status Critical Current

Abstract

The invention relates to an isolated particle dispersion liquid, which includes at least isolated particle and medium. The medium contains 10-80 percent weight liquid whose boiling point is above 150 centigrade thermometer under the 1 atmospheric pressure. The isolated particle dispersion liquid is used in the manufacturing method, wherein, the isolated particle dispersion liquid is ejected by the way of ink jet to configure the isolated particle on the random position of the substrate of the liquid crystal display equipment.

Description

Spacer particle dispersio
The application's application number that to be the applicant propose on March 26th, 2003 dividing an application that be 03807198.3 (PCT/JP03/03699), denomination of invention for the international application of " manufacture method of the manufacture method of liquid crystal indicator, base plate for liquid crystal display device, base plate for liquid crystal display device and, spacer particle dispersio ".
Technical field
The present invention relates to a kind ofly can spacer particle correctly be disposed at manufacture method, the base plate for liquid crystal display device of the liquid crystal indicator on the optional position of substrate, the manufacture method and the spacer particle dispersio of base plate for liquid crystal display device by ink-jetting style.
Background technology
At present, liquid crystal indicator is widely used in personal computer, the portable electronic instrument etc.
Fig. 1 is the sectional view of an example of expression liquid crystal indicator.As shown in Figure 1, generally speaking, liquid crystal indicator has following structure, promptly, the inboard disposes transparency electrode 3, alignment films 8, color filter 4, black matrix 5 etc. and the outside disposes 2 transparency carrier 1 clampings of polaroid 2 and and be equipped on the encapsulant 9 around it and disposed relatively, and enclosing in formed space thus has liquid crystal 6.In addition, transparency carrier 1 also is divided into the lightproof area that disposes pixel region pixel electrode, that become the display part and do not dispose pixel electrode.In this liquid crystal indicator, with the interval that limits 2 transparency carriers 1 and to keep liquid crystal layer suitable thickness (cell gap) be that purpose is used, be exactly spacer particle 7.
The method of configuration isolation particle 7 was in the past, had been formed with random and spreading spacer particle 7 equably on the substrate of pixel electrode.But in the method, spacer particle 7 also can be configured on the pixel electrode, that is, and and the display part of liquid crystal indicator.Because spacer particle 7 is made of synthetic resin or glass etc. usually, if therefore spacer particle is configured on the pixel electrode, then can produce following problem, promptly, polarized light can take place lose the so-called depolarization phenomenon of polarizability, so isolation part branch causes the leakage of light that perhaps the orientation of the lip-deep liquid crystal of spacer particle gets muddled and causes passing through of light because of scattering, thereby reduce contrast and tone, finally can make the display quality variation.Especially in the TFT liquid crystal indicator, when substrate bears pressure, can produce the ruined serious problem of TFT element.
At therewith, people have only carried out as the part beyond the pixel region of transparency carrier display part, promptly only at lightproof area configuration isolation particle, thereby overcome the trial of these problems.For example, the spy opens in the flat 4-198919 communique and discloses, and will have after the peristome and the lightproof area aligned in position on the substrate of mask of peristome, only in the method for mask open portion configuration isolation particle; In addition, the spy opens in the flat 6-258647 communique and discloses, on photoreceptor with the method that is transferred to transparency carrier after the electrostatic means absorption spacer particle again.But, all there is following problem in these methods, that is,, therefore can cause the alignment films on the substrate impaired owing to must on substrate, directly contact mask or photoreceptor, cause display quality to descend.
In addition, the spy opens in the flat 10-339878 communique and discloses, after impressed voltage on the pixel electrode on substrate, and the spacer particle of spreading band homopolarity electricity, thus utilize electrostatic repulsion forces, spacer particle is disposed at the method for lightproof area.But this method has following problem, that is, owing to must therefore spacer particle can not be disposed at position fully arbitrarily, thereby the kind of the liquid crystal indicator that can be suitable for be restricted along the patterned arrangement electrode of configuration.
On the other hand, the spy opens in the clear 57-58124 communique and discloses, and uses the ink jet print printing machine, and spacer particle dispersio is disposed at method on the substrate.In this method, owing to can directly not be contacted with substrate, and can therefore once be considered to very effective method with the configuration isolation particle on position arbitrarily of pattern arbitrarily.Yet, being accompanied by precise treatment, miniaturization, the variation of electronic device in recent years, liquid crystal indicator also more and more is required to become small-sized and have the contour performance of high-contrast.Thus, need the width of the lightproof area of configuration isolation particle to become about 10~30 μ m, and for configuration isolation particle optionally on such narrow region, not only the ejection precision to ink discharge device has proposed very high requirement, has also caused some problems simultaneously.
First problem is the drop size by the ink-jet method ejection can't to be controlled at below the size in the zone of preparing the configuration isolation particle.Impact diameter when generally, playing on substrate by the drop of ink-jet method ejection is about 40~200 μ m.If be contracted to this below value, then must dwindle the bore of nozzle, yet because the nozzle diameter minimum of present ink discharge device also is about 20 μ m, and the particle diameter of spacer particle is about 2~10 μ m, therefore, if nozzle diameter is contracted to below the described size, then can cause the obstruction or the phenomenon such as ejection instability etc. of nozzle.
As will correctly collecting one of the method in regulation district (position) by the drop of ink discharge device ejection, people have inquired into and have worked out control and have been ejected the method for the regulation district of face with respect to the wetting state of drop.For example, ejection liquid as ink discharge device often uses aqueous solution, and such aqueous solution has following characteristic, promptly, for the face that is ejected of the contour polarity in metal surface is can be wetting and sprawl, then nonwetting and sprawl for the face that is ejected of low polarity such as resin surface.
As the example that utilizes this characteristic, for example, the spy opens flat 6-347637 communique and discloses following printing process, promptly, in the color filter of making liquid crystal indicator,, use the printing ink of corresponding color only for the specific pixel region on the substrate that is formed with pixel region and lightproof area.In the method, form the hydrophobicity district according to the lightproof area of photoresist method on substrate, and when using ink discharge device configuration isolation particle, can similarly be suitable for this method.On the substrate of liquid crystal indicator, be formed with for example polyimide resin film that is called as alignment films of the state of orientation that is used to limit liquid crystal usually, and on this alignment films the configuration isolation particle.If will open disclosed method configuration isolation particle on substrate in the flat 6-347637 communique according to the spy, then for example can on alignment films, form filming of photonasty alkali soluble resins such as acrylic copolymer, and the enforcement photolithographic processes, only the alignment layer surface of preparing the configuration isolation particle position is carried out high polar.But in fact, in order to limit the liquid crystal aligning direction at alignment layer surface, for example, implement to utilize the friction processing of nylon or regenerated fiber etc., be very difficult and implement photoetching treatment on the alignment layer surface that has passed through such retrofit.In addition, because filming to protrude, high polarity is present on the alignment films, therefore if implement friction treatment after filming partly forming high polarity, then the high polarity of the alignment layer surface of cementability difference is filmed and can be peeled off in essence, thereby spacer particle optionally can't be disposed in the zone of regulation.Hence one can see that, in reality, must form the zone that forms opposed polarity on the filming of this special surface state of so-called alignment films, and is difficulty very technically.
Second problem is, relevant for the dispersion problem of the spacer particle in the spacer particle dispersio.Known, in the piezoelectric ink jet device of the ejection that is suitable for spacer particle dispersio in ink discharge device, the surface tension of the liquid of ejection is 25~55mN/m preferably.Yet,, therefore be difficult to be dispersed in and be suitable for surface tension that ink-jet uses than in the higher medium because in the past spacer particle is general all to be dispersed in by being prerequisite in the media of surface tension below 30mN/m such as lower alcohol or halogenated hydrocarbon, water.The spy opens and discloses in the 2000-347191 communique in the surface adsorption hydrophobic compound of spacer particle and the method that covers, and particle is also very difficult to be distributed in the high capillary medium with the single-particle state fully but these cover.And also because to be hydrophobic particle poor for the compatibility of alignment films on the substrate on the surface, therefore, it is not enough that its cohesive can become, and the spacer particle that is disposed can move after liquid crystal cells inside is hit etc., thereby can damage alignment films.In addition, also has following problem, promptly, in the covering method based on suction-operated, the surface that is difficult in spacer particle is completely fixed hydrophobic compound, for example, the part of hydrophobic compound meeting elution is to printing ink in the preservation process, and when being ejected to substrate, cover alignment films, perhaps in liquid crystal cells elution to nematic liquid crystal medium etc., thereby display quality not good that causes liquid crystal indicator.In addition, must prevent to produce the scarce luminous point that anomalous orientation caused by the liquid crystal around the spacer particle that is expressed on the pixel, and import the hydrophobic functional groups of the known function with the anomalous orientation that can effectively control liquid crystal and disperse the processing of spacer particle with the single-particle state at jetted ink in medium is opposite operation mutually.Hence one can see that, very complicated for the desired character of spacer particle at present, is extremely difficult and satisfy all requirements under the condition of the good dispersiveness of maintenance.
Summary of the invention
The object of the present invention is to provide manufacture method, the base plate for liquid crystal display device of the liquid crystal indicator on a kind of optional position that spacer particle correctly can be disposed at substrate by ink-jetting style, the manufacture method and the spacer particle dispersio of base plate for liquid crystal display device.
The present invention's 1 is, a kind of manufacture method of liquid crystal indicator, be by ink-jetting style ejection spacer particle dispersio and this spacer particle be disposed at the manufacture method of the liquid crystal indicator on the optional position on the substrate, it is characterized in that, play the impact diameter D of the described spacer particle dispersio on described substrate 1With, residual spacer particle adheres to diameter D after the described spacer particle dispersio drying 2, satisfy the relation of following formula (1).
D 2<(D 1×0.5) (1)
In the manufacture method of the present invention's 1 liquid crystal indicator, the substrate surface temperature when spacer particle dispersio is played on substrate is preferably lower more than 20 ℃ than the boiling point of the liquid of minimum boiling point contained in the described spacer particle dispersio; Substrate surface temperature when more preferably spacer particle dispersio is played on substrate, boiling point than the liquid of minimum boiling point contained in the described spacer particle dispersio is low more than 20 ℃, and the substrate surface temperature before the spacer particle dispersio bone dry is below 90 ℃.In addition, preferred described spacer particle dispersio is formed by containing medium and the spacer particle that 10~80 weight % boiling points are lower than 100 ℃ liquid, and the content of described spacer particle is 0.05~5 weight %; More preferably described spacer particle dispersio is formed at the medium and the spacer particle of the liquid more than 150 ℃ by containing liquid and 80~10 weight % boiling points that 10~80 weight % boiling points are lower than 100 ℃, and the content of described spacer particle is 0.05~5 weight %.More preferably described spacer particle dispersio is 25~70 ° with respect to the contact angle of alignment films on the substrate.
The present invention's 2 is, a kind of base plate for liquid crystal display device, it is to be formed with by according to the pixel region of certain arranged in patterns with divide the base plate for liquid crystal display device of the color filter that the lightproof area of described pixel region constitutes, wherein, be equivalent on the zone of described pixel region, existence is the alignment films of θ b with respect to the contact angle of spacer particle dispersio, and be equivalent at least a portion zone of described lightproof area, existence is the part of θ a with respect to the contact angle of spacer particle dispersio, and described θ b and θ a satisfy the relation of following formula (2) expression.
θa<θb (2)
The following method of manufacture method that belongs to the present invention's 2 base plate for liquid crystal display device also is one of the present invention, promptly, in the method, after the whole surface of substrate is formed uniformly contact angle with respect to spacer particle dispersio and is the alignment films of θ b, to needs configuration isolation particle position irradiation noncontact energy, removing alignment films or it is carried out modification, is θ a thereby make the contact angle with respect to spacer particle dispersio.The following method of manufacture method that belongs to the present invention's 2 base plate for liquid crystal display device also is one of the present invention, promptly, have on the substrate on surface that contact angle with respect to spacer particle dispersio is θ a, evenly the coating photosensitive polyimide is that resin precursor or photosensitive polyimide are resin, and expose and develop by mask, thereby needing on the configuration isolation particle position substrate surface in addition, forming by polyimide with pattern-like is the alignment films that resin constitutes, simultaneously, make described alignment layer surface reach θ b with respect to the contact angle of spacer particle dispersio.
Below, also be one of the present invention.Promptly, a kind of manufacture method of liquid crystal indicator, be to use the present invention's 2 base plate for liquid crystal display device to make the method for liquid crystal indicator, wherein, the contact angle with respect to spacer particle dispersio at described base plate for liquid crystal display device is the part of θ a, the ejection spacer particle dispersio is with the configuration isolation particle.
The present invention's 3 is, a kind of spacer particle dispersio, by inorganic be that spacer particle and the medium that combines vinyl based thermoplastic resin by graft polymerization on the surface of particulate and/or organic system particulate formed, and described spacer particle is scattered in the described medium with single-grain-shaped, wherein, the ethene base system monomer of the alkyl that this vinyl based thermoplastic resin is possess hydrophilic property functional group and/or carbon number 3~22 forms through free radical polymerization, and this medium is made up of water and/or hydrophilic organic solvent and 20 ℃ under surface tension be 25~50mN/m.Preferably contain in the described ethene base system monomer possess hydrophilic property functional group ethene base system monomer 30~80 weight % and, have ethene base system monomer 20~60 weight % of carbon number 3~22 alkyl.In addition, described hydrophilic functional group is preferably and is selected from least a in hydroxyl, carboxyl, sulfonyl, phosphono, amino, amide group, ether, mercapto and the thioether group.
Description of drawings
Fig. 1 is the sectional view of an example of expression liquid crystal indicator.
Fig. 2 is the mode chart of configuration isolation particle position on the substrate that uses among the expression embodiment 7,8.
Among the figure: 1-transparency carrier, 2-polaroid, 3-transparency electrode, 4-color filter, 5-black matrix, 6-liquid crystal, 7-spacer particle, 8-alignment films, 9-encapsulant.
Embodiment
Below, the present invention is described in detail in detail.
The present invention's 1 is, a kind of manufacture method of liquid crystal indicator, be by ink-jetting style ejection spacer particle dispersio and this spacer particle be disposed at the manufacture method of the liquid crystal indicator on the optional position on the substrate, wherein, play the impact diameter D of the spacer particle dispersio on described substrate 1With, residual spacer particle adheres to diameter D after the spacer particle dispersio drying 2Satisfy the relation of following formula (1).
D 2<(D 1×0.5) (1)
This means that after spacer particle dispersio was played on substrate, in its dry run, the spacer particle in the spacer particle dispersio accumulated near the central authorities of impact drop.Thus, have the spacer particle dispersio of the liquid-drop diameter that can utilize ink-jet method ejection, configuration isolation particle in the zone littler by ejection than liquid-drop diameter.
The inventor etc. are through with great concentration discussion and research, found to have the spacer particle dispersio of certain character by use, and the drying process after playing under certain condition on substrate, can make the impact diameter D of the spacer particle dispersio of playing on substrate 1With, residual spacer particle adheres to diameter D after the spacer particle dispersio drying 2Satisfy the relation of above-mentioned formula (1), and then finished the present invention's 1.
In addition, in this instructions, the impact diameter of so-called spacer particle dispersio is meant, plays the external diameter of the spacer particle dispersio drop on substrate, be meant and so-called spacer particle adheres to diameter, residue in the adhering range external diameter of the spacer particle on the substrate behind the dry spacer particle dispersio.
Described spacer particle dispersio is made of spacer particle and medium.There is no particular limitation to described spacer particle, for example, can enumerate the material that is made of inorganic based materials such as silicon dioxide, perhaps, and the material that constitutes by organic system materials such as resins.Wherein, the preferred spacer particle that constitutes by resin, its reason is: it has can not damage hardness alignment films, suitable that is formed on the liquid crystal display base board; Adapt to easily the variation in thickness that thermal expansion or thermal shrinkage by alignment films cause; And mobile fewer in inside, unit.
Constitute the resin of described spacer particle, can obtain by monofunctional polymerizable monomer and/or polyfunctional monomer.Wherein, consider aspects such as intensity, the multipolymer of preferred monofunctional monomer and polyfunctional monomer.At this moment, the ratio of described polyfunctional monomer is preferably below 50 weight %.More preferably below 30 weight %.
There is no particular limitation to described monofunctional monomer, for example, can enumerate following material: styrene derivatives such as styrene, α-Jia Jibenyixi, p-methyl styrene, p-chlorostyrene, 1-chloro-4-methyl-benzene; Vinyl chloride; Vinyl esters such as vinyl acetate, propionate; Unsaturated nitriles such as vinyl cyanide; (methyl) acrylate derivatives such as (methyl) methyl acrylate, (methyl) ethyl acrylate, (methyl) butyl acrylate, (methyl) 2-EHA, (methyl) octadecyl acrylate, (methyl) acrylic acid second diester, (methyl) acrylic acid trifluoro ethyl ester, (methyl) acrylic acid five fluorine propyl ester, (methyl) cyclohexyl acrylate etc.Can use these monofunctional monomers separately, also can two or more and usefulness.
Also there is no particular limitation to described polyfunctional monomer, can enumerate, for example, divinylbenzene, 1,6-hexanediol two (methyl) acrylate, trimethylolpropane tris (methyl) acrylate, tetramethylol methane three (methyl) acrylate, tetra methylol propane four (methyl) acrylate, diallyl phthalate and isomeride thereof, cyamelide triallyl and derivant thereof, trimethylolpropane tris (methyl) acrylate and derivant thereof, pentaerythrite three (methyl) acrylate, pentaerythrite four (methyl) acrylate, dipentaerythritol six (methyl) acrylate, polyglycol two (methyl) acrylate of ethylene glycol bisthioglycolate (methyl) acrylate etc., polypropylene glycol two (methyl) acrylate of propylene glycol two (methyl) acrylate etc., poly-tetramethylene glycol two (methyl) acrylate, neopentyl glycol two (methyl) acrylate, 1,3-butylene glycol two (methyl) acrylate, 2,2 of two [4-(metacryloxy ethoxy) phenyl] propane two (methyl) acrylate of 2-etc., two [4-(metacryloxy polyethoxy) phenyl] propane two (methyl) acrylate of 2-, 2, two [4-(propenyloxy group polyethoxy) phenyl] propane two (methyl) acrylate of 2-hydrogenation, 2, two [4-(propenyloxy group gathers propoxyl group) phenyl] propane two (methyl) acrylate of 2-etc.Can use these polyfunctional monomers separately, also can two or more and usefulness.
When carrying out described polymerization, can use polymerization initiator.There is no particular limitation for described initiating agent, for example can enumerate, benzoyl peroxide, dilauroyl peroxide, adjacent chlorobenzoyl peroxide, O-methoxy benzoyl peroxide, 3,5, organic peroxides such as 5-trimethyl peroxidating hexanoyl, t-butyl peroxyization-2 ethyl hexanoic acid ester, two-t-butylperoxide; Azoisobutyronitrile, azo two cyclohexanenitriles, azo two azo based compounds such as (2, the 4-methyl pentane nitrile) etc.The use amount of described polymerization initiator, with respect to polymerizable monomer 100 weight portions, preferred usually 0.1~10 weight portion that uses.
As the described monomer of polymerization and make the method for spacer particle, there is no particular limitation, can enumerate for example suspension polymerization, seed (seed) polymerization, dispersin polymerization etc.
Described suspension polymerization is meant, will be dispersed to the particle diameter that reaches required by the monomer composition that polymerizable monomer and polymerization initiator constitute and carry out polymerization in Weak solvent.According to described suspension polymerization, can obtain the wider polydisperse particle of size distribution, therefore, can produce the spacer particle of various particle diameters by the gradation operation.
As the spreading agent that uses in the described suspension polymerization, normally used is to add dispersion stabilizer in the water material.As described dispersion stabilizer, can enumerate the macromolecule that dissolves in the medium, for example polyvinyl alcohol (PVA), polyvinylpyrrolidone, methylcellulose, ethyl cellulose, polyacrylic acid, polyacrylamide, polyethylene oxide etc.In addition, also be fit to use nonionic or ionic surfactant.The polymerizing condition of described suspension polymerization, the difference with the kind of polymerization initiator or polymerizable monomer, but normally suitable condition is: polymerization temperature is that 50~80 ℃, polymerization time are 3~24 hours.
Described seeding polymerization is meant, makes by emulsifier-free polymerization or the synthetic further absorbing polymer monomer of monodispersed kind of particle of emulsion polymerization and carries out polymerization, thereby be expanded to the polymerization of the particle diameter of regulation.According to seeding polymerization, can not obtain monodisperse particle by the gradation operation yet, therefore, can make spacer particle in a large number with specified particle diameter.As the organic monomer that is used for described kind of particle, there is no particular limitation, but being separated in the time of to suppress seeding polymerization owing to the composition of planting particle, therefore, the approaching material of monomer component when preferably using with seeding polymerization, for example, for aromatic diethylene base monomer, optimization styrene system, and for propylene was multi-vinyl monomer, preferred propylene was.Owing to plant the size distribution after the size distribution of particle also can be reflected into seeding polymerization, therefore be preferably single dispersion, and the CV value be preferably below 5%.
In addition, when carrying out seeding polymerization, can use dispersion stabilizer as required.As described dispersion stabilizer, preferably dissolve in the macromolecule in the medium, can enumerate, for example, polyvinyl alcohol (PVA), polyvinylpyrrolidone, methylcellulose, ethyl cellulose, polyacrylic acid, polyacrylamide, polyethylene oxide etc.In addition, be fit to use nonionic or ionic surfactant.
In seeding polymerization,, preferably add the polymerizable monomer of 20~100 weight portions for kind of particle 1 weight portion.If below 20 weight portions, then the intensity of the spacer particle of Huo Deing will be not enough; And if more than 100 weight portions, when then carrying out seeding polymerization, because the aggegation of particle etc., it is wide that size distribution will become.
Described dispersin polymerization is meant, can the solvent polymerization monomer but can not dissolve in the Weak solvent system of resin of generation and carry out polyreaction, and by add the macromolecular dispersion stabilizer in this system, separates out the method for the polymkeric substance of generation with shape of particle.According to dispersin polymerization, can not obtain monodisperse particle by the gradation operation yet, therefore, can make spacer particle in a large number with specified particle diameter.
In dispersin polymerization, generally under the situation of using polyfunctional monomer, be easy to generate the cohesion of gained particle, and be difficult to stably obtain monodisperse cross-linked particle, but by selected appropriate condition, polymerizable contains the monomer of crosslinked composition.But, cohesion when considering polymerization and intensity etc., polyfunctional monomer is shared ratio in whole monomers, is preferably in more than the 50 weight %.If less than 50 weight %, then because the microparticle surfaces that forms during polymerization is soft in solvent, therefore, might by particulate each other conflict and lump together, mean particle dia is distributed becomes wide, perhaps even become condensed matter.In addition, even for example keep monodispersity,, then may be difficult to obtain sufficient breakdown strength as spacer particle if cross-linking density is little.
In dispersin polymerization, the medium that uses during as polymerization, can carry out suitable selection according to the polymerizable monomer that uses, but in general the organic solvent of Shi Heing is, for example, alcohols, cellosolve class, ketone or hydro carbons, and can use these individually, perhaps use the mixed solvent that mixes with other organic solvents compatible, water etc. with these.As the organic solvent that is applicable to mixed solvent, can enumerate, for example, acetonitrile, N, alcohols such as dinethylformamide, dimethyl sulfoxide (DMSO), ethyl acetate, methyl alcohol, ethanol, propyl alcohol; Cellosolve classes such as methyl cellosolve class, ethyl cellosolve; Ketones such as acetone, MEK, methyl butyl ketone, 2-butanone.
The elasticity of compression rate (10%K value) of described spacer particle when displacement 10% is preferably 2000~15000MPa.If less than 2000MPa, the pressure during then owing to the combination display element, spacer particle can deform, and can't keep suitable spacing; And if surpass 15000Mpa, then when the combination display element, the alignment films on might wounded substrate, thereby cause display abnormality.In addition, described 10%K value can be obtained by the following method, for example, show flat 6-503180 communique according to the spy, use slight compression exerciser (society of Shimadzu Seisakusho Ltd. system, PCT-200), on the level and smooth section of the cylinder of adamantine diameter 50 μ m, apply and make particulate produce the load of 10% distortion, and try to achieve thus.
For improving the contrast of display element, can carry out painted to described spacer particle.As to described spacer particle method of colouring, can enumerate, for example, make it to contain the method for carbon black, disperse dyes, acid dyes, basic-dyeable fibre, metal oxide etc.; Form the organism film on spacer particle surface, and at high temperature make it to decompose or the method for carbonization etc.In addition, under having the situation of color, can directly use the material itself that forms spacer particle and need not be painted.
Described spacer particle can be provided with adhesive linkage on its surface, also can carry out finishing for the orientation disorder that prevents peripheral liquid crystal.Implement the method for described finishing, can enumerate, for example, it is disclosed that the spy opens flat 1-247154 communique, separates out resin on the spacer particle surface and the method for modifying; Te Kaiping 9-113915 communique is disclosed, enables compound and its generation effect of reacting with the functional group on spacer particle surface, the method for modifying thus; The record of Te Kaiping 11-223821 communique, carry out the method for graft polymerization etc. on the spacer particle surface.Wherein, when forming the superficial layer with the chemical mode combination on spacer particle surface, occur in the unit of liquid crystal indicator seldom that superficial layer peels off or to the problems such as stripping of liquid crystal, therefore preferred, for example, utilize reductibility base by making the spacer particle surface and oxygenant to react and produce free radical, carry out the method for graft polymerization on the surface, it is high and have the superficial layer of enough thickness to form density, therefore preferred.
In addition, also can be formed on the surface coating that vinyl based thermoplastic resin is fixed and forms by graft polymerization formation chemical bond on the spacer particle surface.This vinyl based thermoplastic resin is that polymerising ethylene base system monomer forms.This surface coating is in the liquid of jetted ink or in the liquid crystal display unit cell, is not easy to produce peeling off or problem such as stripping of surface coating, and is therefore preferred.
As the ethene base system monomer that constitutes described vinyl based thermoplastic resin, there is no particular limitation, can enumerate, for example, 2-hydroxyethyl (methyl) acrylate, 1,4-hydroxyl butyl (methyl) acrylate, (gathering) caprolactone modification hydroxyethyl (methyl) acrylate, allyl alcohol, glycerine one allyl ether etc. have the ethene base system monomer of hydroxyl; Acrylic acid and their alpha-alkyl derivant or β-alkyl derivatives such as (methyl) acrylic acid, α-Yi Jibingxisuan, butenoic acid; Unsaturated dicarboxylic classes such as fumaric acid, maleic acid, citraconic acid, itaconic acid; Single 2-(methyl) acrylyl oxy-ethyl ester derivant of described unsaturated dicarboxylic class etc. has the ethene base system monomer of carboxyl; T-butyl acrylamide sulfonic acid, styrene sulfonic acid, 2-acrylamide-2-methyl propane sulfonic acid etc. have the ethene base system monomer of sulfonyl; The ethene base system monomer with phosphoryl of vinyl phosphate, 2-(methyl) acrylyl oxy-ethyl phosphate etc.; Dimethyl aminoethyl methacrylate, diethylamino ethyl methacrylate etc. have the ethene base system monomers such as amine of acryloyl group; The end alkyl ether of the end alkyl ether of (gathering) ethylene glycol (methyl) acrylate, (gathering) propylene glycol (methyl) acrylate, tetrahydrofurfuryl (methyl) acrylate etc. have the ethene base system monomer of ether; (methyl) acrylamide, methylol (methyl) acrylamide, vinyl pyrrolidone etc. have the ethene base system monomer of amide group; (methyl) methyl acrylate, (methyl) acrylic acid ethyl ester, (methyl) acrylic acid n-propyl diester, (methyl) acrylic acid i-propyl diester, (methyl) acrylic acid n-butyl ester, (methyl) acrylic acid i-butyl ester, (methyl) acrylic acid t-butyl ester, (methyl) acrylic acid cyclohexyl ester, (methyl) 2-ethylhexyl acrylate, (methyl) dodecylacrylate, (methyl) acrylic acid stearyl, (methyl) acrylic acid isooctadecane base ester, (methyl) acrylic acid isodecyl ester, (methyl) acrylic acid 13 decyl ester, (methyl) isobornyl acrylate, (methyl) phenyl acrylate, (methyl) acrylic acid benzyl ester, (methyl) acrylic acid methyl-α-chlorine ester, (methyl) esters of acrylic acids such as (methyl) glycidyl acrylate; Unsaturated nitrile such as vinyl cyanide, methacrylonitrile; Maleimides such as phenyl maleimide, cyclohexyl maleimide; Vinyl esters such as vinyl acetate, propionate; Vinyl ethers such as ethyl vinyl ether, butyl vinyl ether; Haloizations such as vinyl chloride, vinylidene chloride, bromine ethene are vinyl-based; Olefines such as ethene, propylene, 1-butylene, 2-butylene, butadiene; At least the ethene base system monomer that has a polymerism unsaturated double-bond in 1 molecules such as styrene such as styrene, α-Jia Jibenyixi and derivant thereof.Can use these ethene base system monomers separately, also can two or more and usefulness.
Described spacer particle content in the described spacer particle dispersio is preferably 0.05~5 weight %.If less than 0.05 weight %, the probability that does not then comprise spacer particle in Pen Chu the drop can improve; And if greater than 5 weight %, then the nozzle of ink discharge device stops up easily, perhaps the spacer particle number that comprises in Dan Zhe the dispersant liquid drop can become and too much spacer particle be moved.More preferably 0.1~2 weight %.
Described spacer particle preferably is scattered in the spacer particle dispersio with the single-particle state.If there is condensation product in the spacer particle dispersio, then not only spraying precision can descend, even serious the time, can cause the obstruction of ink discharge device nozzle.
As the medium of described spacer particle dispersio, as long as be in a liquid state under the room temperature, just there is no particular limitation, wherein, and preferred water dissolubility or hydrophilic liquid.Generally, the shower nozzle of ink discharge device has the tendency that can stablize the ejection hydrophilic liquid.When using the strong solvent of hydrophobicity, the parts that constitute shower nozzle can take place easily to corrode, situation such as perhaps the part of the bonding agent of adhering part is dissolved.In addition, described medium must not have and is penetrated in the alignment films that is formed at substrate surface or with the so-called alignment films contaminative of its dissolving.Described alignment films is made of polyamide usually, and friction treatment was carried out, the may command liquid crystal aligning in its surface.
As described water-soluble or hydrophilic liquid, except water, for example can enumerate unary alcohols such as ethanol, n-propyl alcohol, 2-propyl alcohol, 1-butanols, 2-butanols, 1-methoxyl-2-propyl alcohol, furfuryl alcohol, tetrahydrofurfuryl alcohol; The polymer of ethylene glycol such as ethylene glycol, diglycol, triethylene glycol, tetraethylene glycol; Rudimentary monoalkyl ethers such as the monomethyl ether of the polymer of ethylene glycol and ethylene glycol, single ether, single isopropyl ether, single propyl ether, monobutyl ether, lower dialkyl ethers such as dimethyl ether, diethyl ether, diisopropyl ether, dipropyl ether, alkyl esters such as monoacetate, diacetate esters; The polymer of propylene glycol such as propylene glycol, dipropylene glycol, tripropylene glycol, four propylene glycol; Rudimentary monoalkyl ethers such as the monomethyl ether of the polymer of propylene glycol and propylene glycol, single ether, single isopropyl ether, single propyl ether, monobutyl ether, lower dialkyl ethers such as dimethyl ether, diethyl ether, diisopropyl ether, dipropyl ether, alkyl esters such as monoacetate, diacetate esters; 1, ammediol, 1,2-butylene glycol, 1,3 butylene glycol, 1,4-butylene glycol, 3-methyl isophthalic acid, 5-pentanediol, 3-hexene-2,5-glycol, 1,5-pentanediol, 2,4-pentanediol, 2-methyl-2,4-pentanediol, 2,5-hexanediol, 1, glycolss such as 6-hexanediol, neopentyl glycol; The ether derivant of glycols; The acetic ester derivative of glycols; Glycerine, 1,2,4-butantriol, 1,2,6-hexanetriol, 1,2, polyalcohols such as 5-penta triol, trimethylolpropane, trimethylolethane, pentaerythrite or and ether derivant; Acetic ester derivative etc.; Dimethyl sulfoxide (DMSO), sulfo-diglycol, N-N-methyl-2-2-pyrrolidone N-, N-vinyl-2-Pyrrolidone, r-butyrolactone, 1,3-dimethyl-2-imidazolidine, sulfolane, formamide, N, N-diethylformamide, N, dinethylformamide, N-NMF, acetamide, N-methylacetamide, α-terpilenol, carbon ester vinyl acetate, carbon ester propylene ester, bis-beta-hydroxyethyl sulfone, bis-beta-hydroxyethyl urea, N, N-diethyl ethanolamine, abienol, diacetone alcohol, urea etc.
The boiling point that the medium of described spacer particle dispersio preferably contains under 1 atmospheric pressure is lower than 100 ℃ liquid.This liquid in the drying, can volatilize under lower temperature after spacer particle dispersio is ejected to substrate, therefore, can be provided with baking temperature lowlyer.By setting baking temperature lower, can prevent that medium from polluting alignment films when drying and the situation that influences the demonstration image quality of liquid crystal indicator takes place.More preferably contain boiling point more than 70 ℃, be lower than 100 ℃ organic solvent.Can enumerate as this organic solvent, for example low-grade monobasic alcohol class such as ethanol, n-propyl alcohol, 2-propyl alcohol or ketone etc.
Described boiling point is lower than 100 ℃ liquid, is preferably in below the 25mN/m 20 ℃ surface tension.Generally, when the surface tension of liquid of ejection was 25~50mN/m, ink discharge device can show good ejection precision.On the other hand, be ejected to the surface tension of the dispersant liquid drop on the substrate if bigger, then easier to be mobile at the dry run spacer particle.If boiling point is lower than 100 ℃ the surface tension of liquid below 25mN/m, then can be when ejection the surface tension of spacer particle dispersio be reduced to smaller value, thereby obtains good ejection precision; And on the other hand, quilt can earlier evaporate than other compositions in the spacer particle dispersio after being played on the substrate, and therefore, the surface tension of dispersion liquid can uprise, and moving of spacer particle also can become easy.
In the described spacer particle dispersio, described boiling point is lower than the content of 100 ℃ liquid, preferred 10~80 weight % scopes.If less than 10 weight %, then under the lower baking temperature of 1 the LCD device preparation method that is applicable to the present invention, the rate of drying of dispersion liquid will be slack-off, and production efficiency also can descend; And if greater than 80 weight %, then near the spacer particle dispersio the ink discharge device nozzle is dry easily, thus the ejection of infringement ink-jet, and perhaps dry easily when making spacer particle dispersio or in fluid box, the generation probability of agglutination particle also can improve.
The medium of described spacer particle dispersio preferably contains boiling point under 1 atmospheric pressure at the liquid more than 150 ℃.This liquid can prevent near spacer particle dispersio overdrying and cause the spraying precise decreasing ink discharge device nozzle, and is dry and produce aggregated particle in the time of can also suppressing to make spacer particle dispersio or in fluid box.More preferably contain boiling point at the liquid more than 150 ℃, below 200 ℃.Can enumerate as this liquid, for example, the lower alcohol ethers of ethylene glycol, glycol monomethyl ether, glycol dimethyl ether etc.
Described boiling point is preferably in more than the 30mN/m 20 ℃ surface tension at the liquid more than 150 ℃.If this value is more than 30mN/m, after then the drop of spacer particle dispersio is played on substrate, boiling point is lower evaporate after, can keep the high surface tension of spacer particle dispersio, thereby make the mobile of spacer particle become easy.
In the described spacer particle dispersio, described boiling point is preferably 10~80 weight % scopes at the content of the liquid more than 150 ℃.If less than 10 weight %, then be easy to cause spraying the problem of precise decreasing because of the drying of spacer particle dispersio, perhaps can produce aggregated particle etc.; And if greater than 80 weight %, then not only drying time significant prolongation and lowering efficiency, and, also easily because the pollution of alignment films causes the decline of the demonstration image quality of liquid crystal indicator.
In addition, can also contain in the medium of described spacer particle dispersio to give the bonding composition that cementability is a purpose; Also can improve the ejection precision or improve the movability of spacer particle, contain various surfactants or viscous regulator for physical characteristics such as dispersiveness, control surface tension force and the viscosity of improving spacer particle.In addition, in not hindering the scope of finishing problem of the present invention, as required, for example can contain in the medium of described spacer particle dispersio, in the various adjuvants such as viscous regulator, pH regulator agent, defoamer, antioxidant, thermal stabilizer, light stabilizer, ultraviolet light absorber, colorant more than a kind or 2 kinds.
Described spacer particle dispersio is preferably 25~70 ° with respect to the contact angle of alignment films on the substrate.If less than 25 °, after then the drop of spacer particle dispersio is played on the substrate, be difficult to make spacer particle to be moved; And if, then be difficult to good precision ejection spacer particle dispersio greater than 70 °.
Then, describe for operation in the present invention's 1 the LCD device preparation method, that described spacer particle dispersio is ejected on the substrate.
The ink discharge device that uses in 1 the LCD device preparation method as the present invention, can use, for example, utilize the vibrations ejections liquid of piezoelectric element the piezoelectricity mode, utilize the expansion of liquids that heating rapidly produces and spray the known in the past devices such as type of heating of liquid.The nozzle diameter of described ink discharge device, preferred 20~100 μ m.If, then following problem may occur less than 20 μ m, that is, at the particle diameter of ejection spacer particle when being the spacer particle dispersio of 2~10 μ m, because too small, thereby can cause the decline of ejection precision, and problem is when serious with the difference of particle diameter, also may plug nozzle; And if above 100 μ m, then because the change of the drop of ejection greatly, is played diameter and also can be become greatly, the precision of configuration isolation ion also can descend.
Liquid-drop diameter from the spacer particle dispersio of the nozzle of described ink discharge device ejection is preferably 10~80 μ m.The method of control liquid-drop diameter has, and for example, optimizes the method for nozzle diameter, perhaps the methods such as electric signal of optimal control ink discharge device.The latter is particularly important when using the ink discharge device of piezoelectricity mode.In addition, play the liquid-drop diameter on substrate, preferred 30~150 μ m.If less than 30 μ m, then nozzle diameter also must be very little, thereby the spray nozzle clogging that causes by spacer particle can occur, perhaps can have problems aspect the machining precision of nozzle.If surpass 150 μ m, then the precision of configuration isolation particle can descend.
Substrate as 1 the LCD device preparation method that is used for the present invention has no particular limits, and for example can use the material that glass plate or resin plate etc. use as the board-like substrate of liquid crystal indicator usually.
In the present invention's 1 LCD device preparation method, be preferably on the substrate surface in two substrates that constitute liquid crystal indicator the configuration isolation particle.In addition, the spacer particle on the substrate can randomly dispose, and also can carry out the patterning configuration by certain location.Result from the decline of demonstration image quality of spacer particle in order to suppress to lack luminous point etc., described spacer particle preferably is configured in the non-displaypart of substrate.As described non-displaypart, can consider to be formed at light shield layer that is called as black matrix around the pixel and the residing part of TFT element in the TFT liquid crystal indicator, still,, preferably be disposed at the black matrix part in order not destroy the TFT element.In addition, the configuration number of spacer particle, preferably every usually 1mm2 zone has 50~300.As long as satisfy the scope of this particle density, just can be configured with any pattern in any part of black matrix.
Then, illustrate in the present invention's 1 LCD device preparation method, play on substrate from described spacer particle dispersio after, the operation of the medium in the dry spacer particle dispersio.In the present invention's 1 the LCD device preparation method,, make from the spacer particle dispersio of the nozzle ejection of ink discharge device and just played impact diameter D behind substrate by drying 1, and the spacer particle dispersio drying after residual spacer particle adhere to diameter D 2Satisfy following formula (1) relation,
D 2<(D 1×0.5) (1)
If will in dry run, make near the central authorities of this spacer particle near the impact drop, importantly: as mentioned above with boiling point, the surface tension of spacer particle dispersio medium, be set at suitable condition with respect to the contact angle of alignment films and the concentration of the spacer particle in the spacer particle dispersio, simultaneously, with baking temperature be set at suitable condition drying time.Had better not select to make the sharply condition of drying of medium, in order to avoid medium just disappears in during spacer particle moves in the dry run on substrate.On the contrary, if drying time is long, the production efficiency of liquid crystal indicator is reduced.In addition, if medium at high temperature Long contact time in alignment films, thereby then may pollute the demonstration image quality that alignment films influences liquid crystal indicator.If medium is volatilization at room temperature easily, then near the spacer particle dispersio the ink discharge device nozzle can be easy to drying, thereby infringement ink-jet ejection property perhaps when making spacer particle dispersio or the drying in the fluid box, produces aggregated particle probably.
Consider these restriction conditions,, for example can enumerate that compare with the boiling point of the liquid of the contained minimum boiling point of described spacer particle dispersio, the substrate surface temperature when spacer particle dispersio is played on substrate is low more than 20 ℃ as desirable drying condition.If substrate surface temperature exceeds the temperature than low 20 ℃ of the boiling point of minimum boiling point liquid, then will sharply volatilize owing to minimum boiling point liquid, not only spacer particle can't move, in the time of serious, even because rapid boiling, can connect drop one and coexist and move on the substrate, thereby can significantly reduce the configuration precision of spacer particle.
In addition, before the spacer particle dispersio bone dry during in, substrate surface temperature is preferably in below 90 ℃.If surpass 90 ℃, thereby then can pollute the demonstration image quality that alignment films influences liquid crystal indicator.More preferably below 70 ℃.In addition, in this instructions, so-called bone dry is meant, the moment that the drop on the substrate disappears.
Use perimeter seal, will by the substrate of described method configuration isolation particle with relative with this substrate to substrate add thermo-compressed, and, can make liquid crystal indicator by to formed substrate gap filling liquid crystal.
1 LCD device preparation method according to the present invention, in the process of dry spacer particle dispersio, spacer particle can be assembled in the narrower scope of liquid-drop diameter when being disposed at than impact, therefore, at the extremely narrow non-displaypart of width also configuration isolation particle optionally.Therefore, in the liquid crystal indicator that 1 LCD device preparation method according to the present invention is made, the decline of the demonstration image quality that causes because of the scarce luminous point around the spacer particle can not appear.
The present invention's 2 is a kind of base plate for liquid crystal display device, be to be formed with by by the pixel region of certain arranged in patterns with divide the base plate for liquid crystal display device of the color filter that the lightproof area of described pixel region constitutes, wherein, be equivalent in the zone of described pixel region, existence is the alignment films of θ b with respect to the contact angle of spacer particle dispersio, and being equivalent to have at least in the zone of described lightproof area a part to have the contact angle with respect to spacer particle dispersio is the part of θ a, and described θ b and θ a satisfy the relation of following formula (2) expression.
θa<θb (2)
In addition, in this instructions, the zone that what is called is equivalent to pixel region is meant: be assembled under the state of liquid crystal indicator, make the real estate that is formed with color filter be positioned at above and under the situation of horizontal positioned display frame, be positioned at the zone under the pixel region of color filter.The zone that is equivalent to lightproof area is meant: be positioned at the zone under the lightproof area of color filter.In addition, the so-called contact angle in this instructions is meant: leave standstill under the situation of droplet of the liquid (spacer particle dispersio) as object the static contact angle in the moment that the expansion of drop is static in the plane.
Use the present invention's 2 base plate for liquid crystal display device, can make the spacer particle dispersio of ejection optionally wetting and sprawl on lightproof area, its result can optionally be disposed at lightproof area with spacer particle.If θ b and θ a do not satisfy the relation of described formula (2), then spacer particle optionally can't be disposed at lightproof area.
Described contact angle is the part of θ a, can be formed on continuously in the zone that is equivalent to lightproof area with wire, also can be with the discontinuous island that forms of arbitrary shape.In addition, described contact angle is the part of θ a, is preferably in than in the narrower scope in the zone that is equivalent to lightproof area, forms with the regional spaced around certain distance that is equivalent to lightproof area.Form and touch around the zone that is equivalent to lightproof area if contact angle is the part of θ a, then not carrying out the part of liquid crystal aligning control can extrude from the zone that is equivalent to lightproof area, thereby in being equivalent to the zone of pixel region, can generate the part that liquid crystal is not oriented control, finally cause badization of the display quality of liquid crystal indicator.
As the present invention's 2 base plate for liquid crystal display device, there is no particular limitation, for example can use the material that glass plate or resin plate etc. use as the display panel substrate of liquid crystal indicator usually.In addition, on the surface of the present invention's 2 base plate for liquid crystal display device, be formed with the resin film that is called as alignment films that is used for the regulation liquid crystal aligning usually.Described alignment films is that resin forms by polyimide usually, and by friction treatment being implemented on its surface, the orientation of control liquid crystal.
Manufacture method to the present invention's 2 base plate for liquid crystal display device, there is no particular limitation, for example can enumerate, and forms earlier after the alignment films, only, carry out the back method for processing by removal, modification, covering etc. for the alignment films that needs on the configuration isolation particle position; Only in the method that does not need to form on the configuration isolation particle position alignment films.These methods can be distinguished use separately, also can both and usefulness.
As forming alignment films earlier afterwards only for needing the alignment films on the configuration isolation particle position to carry out the back method for processing by removal, modification, covering etc., for example can enumerate on the whole surface of substrate and be formed uniformly after contact angle with respect to spacer particle dispersio is the alignment films of θ b, shine contactless energy to needs configuration isolation particle position, remove alignment films or alignment films is carried out modification, thereby make the method that changes θ a with respect to the contact angle of spacer particle dispersio into.The manufacture method of above-mentioned the present invention's 2 base plate for liquid crystal display device also is one of the present invention.
In the manufacture method of this base plate for liquid crystal display device of the present invention, preferably, at first form alignment films, and in the surface of this alignment films enforcement friction treatment, thereby carry out liquid crystal aligning control, afterwards, to the contactless energy of needs configuration isolation particle position local irradiation.
The method of the contactless energy of described irradiation, there is no particular limitation, if the focus of irradiation energy can be accumulated in below 20 microns and can be that aligning film material such as resin is implemented to decompose, evapotranspired to polyimide, burning, oxidation etc., any method can adopt, and can enumerate laser radiation, excimer laser radiation, Corona discharge Treatment, low-temperature plasma processing etc.By these contactless energy exposure methods, implement friction treatment on the surface of alignment films in advance and after carrying out liquid crystal aligning control, can not contact the surface of alignment films, directly carry out the removal or the modification of alignment films, thereby can obtain to carry out the alignment films of liquid crystal aligning control with comparalive ease.In addition, these contactless energy exposure methods may be used alone, used in two or more.
In addition, as only for needing the configuration isolation particle position to cover the method for alignment films, there is no particular limitation, for example can enumerate, disposal routes such as the evaporation by carrying out across mask, sputter, CVD (Chemical Vapour Deposition) method, plasma polymerization method form the method for heterogeneous membrane on the surface of alignment films.These disposal routes may be used alone, used in two or more.
Only for not needing the configuration isolation particle position to form the method for alignment films, for example can enumerate, have on the substrate on surface that contact angle with respect to spacer particle dispersio is θ a, evenly the coating photosensitive polyimide is that resin precursor or photosensitive polyimide are resin, and expose and develop across mask, thereby needing on the configuration isolation particle position substrate surface in addition, forming by polyimide with pattern-like is the alignment films that resin constitutes, and making the contact angle with respect to spacer particle dispersio of described alignment layer surface is the method for θ b.The manufacture method of this present invention's 2 base plate for liquid crystal display device also is one of the present invention.
The advantage of the manufacture method of this base plate for liquid crystal display device of the present invention is, on substrate, form after the alignment films of pattern-like, need on substrate, implement in full friction treatment, but, even, do not have problems such as high polarity film peels off appearance being to carry out friction treatment again after covering other high polarity films on the alignment films that constitutes of resin by polyimide yet.In addition, can also form by polyimide by the following method is the alignment films that resin constitutes.Promptly, across forming figuratum mask, wherein, this pattern has the hole that forms the part of alignment films corresponding to the needs on the substrate, by disposal routes such as evaporation, sputter, CVD method, plasma polymerization methods, with polyimide is that the part that needs to dispose alignment films on the substrate is only separated out and be deposited on to resin precursor, is the alignment films that resin constitutes thereby form by polyimide.
Below, also be one of the present invention.Promptly, a kind of manufacture method of liquid crystal indicator, be to use the present invention's 2 base plate for liquid crystal display device to make the method for liquid crystal indicator, wherein, the contact angle with respect to spacer particle dispersio at described base plate for liquid crystal display device is the part of θ a, ejection spacer particle dispersio, and configuration isolation particle thus.
As the jet method of the spacer particle that here uses and spacer particle dispersio, spacer particle dispersio, play the drying means of the drop on substrate etc., all have no particular limits, can use known in the past material or method, but, material or the method used in preferred the present invention's 1 the LCD device preparation method.
According to this method, after spacer particle optionally being configured on the present invention's 2 the base plate for liquid crystal display device, by it being added thermo-compressed with relative to the substrate in this substrate with perimeter seal, and at the substrate gap filling liquid crystal that forms, the liquid crystal indicator that obtains expecting.
The present invention's 2 base plate for liquid crystal display device is applicable to the liquid crystal indicator of STN mode or any one in the TFT mode liquid crystal indicator.
The liquid crystal indicator of described STN mode, subtend substrate by color filter substrate that is formed with color filter and relative configuration with it constitutes, and described any substrate all has the transparency electrode that forms strip, and the present invention's 2 base plate for liquid crystal display device can be used for described any one substrate.
The liquid crystal indicator of described TFT mode is made of the subtend substrate of color filter substrate that is formed with color filter and relative configuration with it, and the subtend substrate generally has the array of TFT element etc., therefore is called as array base palte.In addition, generally be formed with contact shape transparency electrode on the colour filtering chip basic board, and be formed with element and transparency electrode on the array base palte, and the present invention's 2 base plate for liquid crystal display device can be used for described any one substrate.
Use under the present invention's the situation of 2 base plate for liquid crystal display device, can use ink discharge device, to the contact angle with respect to spacer particle dispersio is the part ejection spacer particle dispersio of θ a, therefore, can spacer particle is efficient, high precision and optionally be disposed at the non-displaypart of substrate, thereby can obtain the good liquid crystal indicator of display quality, the depolarized phenomenon that caused by spacer particle wherein can not take place or by lacking the contrast that luminous point causes or the decline of tone.
The present invention's 3 is, a kind of spacer particle dispersio, by inorganic be that spacer particle and the medium that combines vinyl based thermoplastic resin by graft polymerization on the surface of particulate and/or organic system particulate formed, and described spacer particle is scattered in the described medium with single-grain-shaped, wherein, the ethene base system monomer of the alkyl that this vinyl based thermoplastic resin is possess hydrophilic property functional group and/or carbon number 3~22 forms through free radical polymerization, and this medium is made up of water and/or organic solvent and 20 ℃ under surface tension be 25~50mN/m.
Use in 3 the spacer particle dispersio as the present invention described inorganic be particulate, there is no particular limitation, for example can enumerate silicon dioxide microparticle etc.These are inorganic to be that particulate may be used alone, used in two or more.In addition, there is no particular limitation for described organic system particulate, for example can enumerate resin particle etc.These organic system particulates may be used alone, used in two or more.In addition, described inorganic be that particle and organic system particulate can be distinguished separately and to use, also can both and use.Resin particle preferably wherein, this is because it has following advantage: hardness is suitable, can not damage the alignment films that is formed on the liquid crystal display base board; Adapt to the variation in thickness that causes by thermal expansion or thermal shrinkage easily; And then mobile fewer etc. at the spacer particle of inside, unit.
As the resin that constitutes described resin particle, for example, can use the same material of using in the present invention's the manufacture method of 1 liquid crystal indicator of spacer particle, and can obtain resin particle with same method.
Employed spacer particle in the present invention's 3 the spacer particle dispersio; be above-mentioned inorganic be on particulate or the organic system microparticle surfaces; combine the spacer particle of vinyl based thermoplastic resin by graft polymerization; this vinyl based thermoplastic resin is that the ethene base system monomer of the alkyl of possess hydrophilic property functional group and/or carbon number 3~22 forms through free radical polymerization.
As described hydrophilic functional group, there is no particular limitation, and preference is as being selected from least a in hydroxyl, carboxyl, sulfonyl, phosphono, amino, amide group, ether, mercapto and the thioether group.Wherein, consider with the interaction of liquid crystal few, more preferably hydroxyl, carboxyl and ether.These hydrophilic functional groups may be used alone, used in two or more.
As ethene base system monomer with described hydrophilic functional group, there is no particular limitation, for example can enumerate, 2-hydroxyethyl (methyl) acrylate, 1,4-hydroxyl butyl (methyl) acrylate, (gathering) caprolactone modification hydroxyethyl (methyl) acrylate, allyl alcohol, glycerine one allyl ether etc. have the ethene base system monomer of hydroxyl; Acrylic acid and their alpha-alkyl derivant or β-alkyl derivatives such as (methyl) acrylic acid, α-Yi Jibingxisuan, butenoic acid; Unsaturated dicarboxylic classes such as fumaric acid, maleic acid, citraconic acid, itaconic acid; Single 2-(methyl) acrylyl oxy-ethyl ester derivant of described unsaturated dicarboxylic etc. has the ethene base system monomer of carboxyl; T-butyl acrylamide sulfonic acid, styrene sulfonic acid, 2-acrylamide-2-ethyl propane sulfonic acid etc. have the ethene base system monomer of sulfonyl; Vinyl phosphate, 2-(methyl) acrylyl oxy-ethyl phosphate etc. have the ethene base system monomer of phosphoryl; Dimethyl aminoethyl methacrylate, diethylamino ethyl methacrylate etc. have amino ethene base system monomer; The end alkyl ether of the end alkyl ether of (gathering) ethylene glycol (methyl) acrylate, (gathering) propylene glycol (methyl) acrylate, tetrahydrofurfuryl (methyl) acrylate etc. have the ethene base system monomer of ether; (gathering) ethylene glycol (methyl) acrylate, (gathering) propylene glycol (methyl) acrylate etc. have the ethene base system monomer of hydroxyl and ether; (methyl) acrylamide, methylol (methyl) acrylamide, vinyl pyrrolidone etc. have the ethene base system monomer of amide group etc.Can use the ethene base system monomer of these possess hydrophilic property functional groups separately, also can two or more and usefulness.
There is no particular limitation as the alkyl of described carbon number 3~22, for example can enumerate n-propyl group, i-propyl group, n-butyl, i-butyl, t-butyl, n-amyl group, n-hexyl, cyclohexyl, 2-ethylhexyl, n-heptyl, n-octyl group, n-nonyl, decyl, undecyl, dodecyl, tridecyl, myristyl, pentadecyl, nonadecyl, eicosyl, heneicosyl, docosyl, isobornyl etc.The alkyl of these carbon numbers 3~22 may be used alone, used in two or more.
As the ethene base system monomer of the alkyl with described carbon number 3~22, there is no particular limitation, for example can enumerate the ester compounds that is made of the alkyl of (methyl) acrylic acid and described carbon number 3~22; The ester compounds that constitutes by the alkyl of vinyl alcohol and described carbon number 3~22; Ether ester compounds that constitutes by the alkyl of vinyl and described carbon number 3~22 etc.The ethene base system monomer that these have the alkyl of described carbon number 3~22 may be used alone, used in two or more.
The ethene base system monomer of described possess hydrophilic property functional group and have the ethene base system monomer of the alkyl of described carbon number 3~22 can be distinguished separately and use, also can both and use.Wherein, constitute the ethene base system monomer of vinyl based thermoplastic resin, preferably contain the described possess hydrophilic property of 30~80 weight % functional group base ethene base system monomer and, the described ethene base system monomer of 20~60 weight % with alkyl of carbon number 3~22.If in the ethene base system monomer, the content of the ethene base system monomer of described possess hydrophilic property functional group is less than 30 weight %, then the spacer particle that is obtained is difficult to be dispersed in the dispersion medium with the state of abundant single-particleization, thereby be easy to generate aggregated particle, and, be difficult in and stablize ejection in the ink discharge device, can't correctly form unit interval; If this content greater than 80 weight %, then in the unit that forms liquid crystal indicator, on the surface of the spacer particle that is extruded into display pixel, causes the anomalous orientation of liquid crystal easily, cause the decline of display quality.In addition, if in the ethene base system monomer, the content of the ethene base system monomer of described alkyl with carbon number 3~22 is less than 20%, then in the unit that forms liquid crystal indicator, surface at the spacer particle that is extruded into display pixel, the anomalous orientation that causes liquid crystal easily causes the decline of display quality.If this content is greater than 60 weight %, then the dispersion stabilization of the spacer particle that is obtained in medium might descend.
In addition, the vinyl based thermoplastic resin that forms through free radical polymerization in conjunction with ethene base system monomer by graft polymerization on the surface of particulate by the alkyl of above-mentioned possess hydrophilic property functional group and/or carbon number 3~22, thereby when forming the surface coating that constitutes by vinyl based thermoplastic resin, for the purpose of the thickness of thickening surface coating under the stacked situation with different multiple vinyl based thermoplastic resin beds of forming, the use of the desirable ethene base system monomer of the described alkyl with carbon number 3~22 that contains the ethene base system monomer of described possess hydrophilic property functional group base of 30~80 weight % and 20~60 weight % only limits to constitute the outermost vinyl based thermoplastic of surface coating resin and gets final product.This is because the dispersion of spacer particle or in the dispersiveness of the medium that is used for jetted ink or the functions such as inhibition of liquid crystal anomalous orientation is to embody by the state around the spacer particle surface.
Be used in the present invention's the spacer particle of 3 spacer particle dispersio, by at the described vinyl based thermoplastic of described microparticle surfaces graft polymerization resin, mode with chemical bond is fixed, thereby forms the surface coating that is made of vinyl based thermoplastic resin at microparticle surfaces.The surface coating that is formed by this method in jetted ink or in the unit of liquid crystal indicator, seldom has surface coating to peel off or problem such as elution takes place, thereby is desirable.Wherein, for example the spy opens in the flat 11-223821 communique and has put down in writing following method, promptly, the particulate and the oxygenant that have the reductibility base on the surface are reacted, generate free radical at microparticle surfaces, and, form the surface coating that constitutes by vinyl based thermoplastic resin at microparticle surfaces by being the graft polymerization of starting point with this free radical.Because it is high and have the surface coating of enough thick thickness to form density by this method, therefore preferably.
Described spacer particle content in the present invention's 3 the spacer particle dispersio is preferably 0.05~5 weight %.If less than 0.05 weight %, the probability that does not then comprise spacer particle in Pen Chu the drop can improve; And if greater than 5 weight %, then the nozzle of ink discharge device stops up easily, perhaps the spacer particle number that comprises in Dan Zhe the dispersant liquid drop can become too much, and spacer particle is not easy to move in dry run.More preferably 0.1~2 weight %.
Described spacer particle is dispersed in the present invention's 3 the spacer particle dispersio with the single-particle state.If there is condensation product in the spacer particle dispersio, then not only spraying precision can descend, and when serious, even can cause the obstruction of ink discharge device nozzle.
Constitute the medium of the present invention's 3 spacer particle dispersio, constitute by water and/or hydrophilic organic solvent.Generally, medium is under the situation of water or hydrophilic organic solvent, and ink discharge device has the tendency that can stablize ejection, and medium is when being the strong solvent of hydrophobicity, can the parts that erosion medium resistance constitutes shower nozzle take place easily, perhaps the situation of the bonding agent of a part of adhering part is fallen in elution.
As described water, there is no particular limitation, for example can enumerate ion exchange water, pure water, underground water, tap water, process water etc.These water may be used alone, used in two or more.
As described hydrophilic organic solvent, there is no particular limitation, for example can enumerate unary alcohols such as ethanol, n-propyl alcohol, 2-propyl alcohol, 1-butanols, 2-butanols, 1-methoxyl-2-propyl alcohol, furfuryl alcohol, tetrahydrofurfuryl alcohol; The polymer of ethylene glycol such as ethylene glycol, diglycol, triethylene glycol, tetraethylene glycol; The polymer of propylene glycol such as propylene glycol, dipropylene glycol, tripropylene glycol, four propylene glycol; Rudimentary monoalkyl ethers such as the monomethyl ether of the polymer of ethylene glycol or the polymer of propylene glycol, single ether, single isopropyl ether, single propyl ether, monobutyl ether; Lower dialkyl ethers such as the dimethyl ether of the polymer of ethylene glycol or the polymer of propylene glycol, diethyl ether, diisopropyl ether, dipropyl ether; Alkyl esters such as the monoacetate of the polymer of ethylene glycol or the polymer of propylene glycol, diacetate esters; 1, ammediol, 1,2-butylene glycol, 1,3 butylene glycol, 1,4-butylene glycol, 3-methyl isophthalic acid, 5-pentanediol, 3-hexene-2,5-glycol, 1,5-pentanediol, 2,4-pentanediol, 2-methyl-2,4-pentanediol, 2,5-hexanediol, 1, glycolss such as 6-hexanediol, neopentyl glycol; The ether derivant of glycols; The acetic ester derivative of glycols; Glycerine, 1,2,4-butantriol, 1,2,6-hexanetriol, 1,2, polyalcohols such as 5-penta triol, trimethylolpropane, trimethylolethane, pentaerythrite; The ether derivant of polyalcohols; The acetic ester derivative of polyalcohols etc.; Dimethyl sulfoxide (DMSO), sulfo-diglycol, N-N-methyl-2-2-pyrrolidone N-, N-vinyl-2-Pyrrolidone, gamma-butyrolacton, 1,3-dimethyl-2-imidazolidine, sulfolane, formamide, N, dinethylformamide, N, N-diethylformamide, N-NMF, acetamide, N-methylacetamide, α-terpilenol, ethylene carbonate, carbonic allyl ester, bis-beta-hydroxyethyl sulfone, bis-beta-hydroxyethyl urea, N, N-diethyl ethanolamine, abienol, diacetone alcohol, urea etc.These hydrophilic organic solvents may be used alone, used in two or more.In addition, water and hydrophilic organic solvent can be distinguished use separately, also can both and usefulness.
The surface tension of medium under 20 ℃ of the present invention's 3 spacer particle dispersio is 25~50mN/m.If exceed this scope, ejection then the present invention's 3 spacer particle dispersio, that carry out with ink discharge device and ejection precision will be insufficient.
The boiling point that preferably contains under 1 atmospheric pressure in the medium of the present invention's 3 spacer particle dispersio is lower than 100 ℃ liquid.This liquid carries out volatilizing under lower temperature in the drying after spacer particle dispersio is sprayed substrate, therefore, low baking temperature can be set.By setting baking temperature lower, medium pollution alignment films in the time of can preventing drying and the situation that influences the demonstration image quality of liquid crystal indicator takes place.More preferably contain boiling point more than 70 ℃ and be lower than 100 ℃ organic solvent.Can enumerate as this organic solvent, for example, low-grade monobasic alcohol classes such as ethanol, n-propyl alcohol, 2-propyl alcohol, perhaps ketone etc.
Described boiling point is lower than 100 ℃ liquid, 20 ℃ surface tension preferably below 25mN/m.Generally when the surface tension of the liquid that sprays was 25~50mN/m, ink discharge device can show good ejection precision.On the other hand, be ejected to the surface tension of the dispersant liquid drop on the substrate when big, easier mobile spacer particle in dry run.If boiling point is lower than 100 ℃ the surface tension of liquid below 25mN/m, then can the surface tension of spacer particle dispersio be reduced to smaller value in when ejection, thereby obtain good ejection precision, and on the other hand, owing to after being played on the substrate, can earlier evaporate than other compositions, therefore, the tension force on dispersion liquid surface can uprise, and the mobile meeting of spacer particle becomes easy.
In the medium of the present invention's 3 spacer particle dispersio, the content that above-mentioned boiling point is lower than 100 ℃ liquid is preferably 10-80 weight %.If less than 10 weight %, then under lower baking temperature, the rate of drying of dispersion liquid will be slack-off, cause the decline of production efficiency, if and above 80 weight %, then near the spacer particle dispersio the nozzle of ink discharge device is dry easily, can influence ink-jet ejection property, perhaps dry easily when making spacer particle dispersio or in fluid box, the possibility that produces aggregated particle can become big.
Preferably contain boiling point under 1 atmospheric pressure in the medium of the present invention's 3 spacer particle dispersio at the liquid more than 150 ℃.This liquid can prevent from the generation that produces the situation of aggregated particle because of drying in the time of perhaps can suppressing to make spacer particle dispersio in fluid box takes place because of the situation that near the spacer particle dispersio overdrying ink discharge device nozzle causes spraying precise decreasing.More preferably contain boiling point at the liquid more than 150 ℃, below 200 ℃.Can enumerate as this organic solvent, for example, the lower alcohol ethers of ethylene glycol, glycol monoethyl ether, glycol dimethyl ether etc.
Above-mentioned boiling point is preferably more than the 30mN/m in the surface tension of the liquid more than 150 ℃ at 20 ℃.This value is if more than 30mN/m, after then the drop of spacer particle dispersio is played on substrate, boiling point is lower evaporate after, can keep the high surface tension of spacer particle dispersio, thereby make the mobile of spacer particle become easy.
In the medium of the present invention's 3 spacer particle dispersio, described boiling point is at the content of the liquid more than 150 ℃, preferably in 10~80 weight % scopes.If less than 10 weight %, then be easy to produce the problem that causes ejection precise decreasing or generation aggregated particle because of the drying of spacer particle dispersio; And if greater than 80 weight %, then not only because of drying time significant prolongation cause efficient to reduce, and, also cause the decline of the demonstration image quality of liquid crystal indicator easily because of the pollution of alignment films.
In the present invention's 3 the spacer particle dispersio, in not hindering the scope of finishing problem of the present invention, for example can contain as required, in the various adjuvants such as cementability imparting agent, viscous regulator, pH regulator agent, surfactant, defoamer, antioxidant, thermal stabilizer, light stabilizer, ultraviolet light absorber, colorant more than a kind or 2 kinds.
The present invention's 3 spacer particle dispersio goes for by ink-jetting style it being disposed in the operation on the optional position on the base plate for liquid crystal display device.As operable ink discharge device, there is no particular limitation, can use above-mentioned device.
If use the present invention's 3 spacer particle dispersio, then when using ink discharge device to be ejected in it on base plate for liquid crystal display device, can guarantee good ejection, therefore and the unit interval that can correctly keep liquid crystal indicator after drying can obtain to show the liquid crystal indicator of even display quality.In addition,, also be difficult for causing the lip-deep liquid crystal anomalous orientation of spacer particle, can obtain to show the liquid crystal indicator of good display quality even spacer particle is extruded in the pixel in liquid crystal display unit cell.
Embodiment by following illustrates in greater detail the present invention, but the present invention is not limited in these embodiment.
(embodiment 1)
(1) modulation of spacer particle
In separable flask, divinylbenzene, the different monooctyl ester of 5 parts by weight of acrylic at 15 weight portions, the benzoyl peroxide that evenly mixes 1.3 weight portions as polymerization initiator, then, drop into 3% aqueous solution, 20 weight portions, lauryl sodium sulfate 0.5 weight portion of polyvinyl alcohol (PVA) (the Network ラ レ system<GL-03 of society 〉), and after fully stirring, add ion exchange water 140 weight portions.Stir this solution on one side, under stream of nitrogen gas at 80 ℃ react 15 hour on one side.After hot water and the clean particulate that obtains of acetone, carry out the gradation operation, obtain spacer particle after the volatilization acetone.The mean grain size of gained particulate is 5 μ m, and the CV value is 3.0%.
(2) surface treatment of spacer particle
Gained particulate 5 weight portions are put in dimethyl sulfoxide (DMSO) (DMSO) 20 weight portions and hydroxyethyl methylacrylate 20 weight portions, and, evenly stirred with after ultrasonic processor (sonicate) dispersion.Then, nitrogen is directed in the reaction system, and continues down to stir 2 hours at 30 ℃.To wherein adding the ceric ammonium nitrate solution of 10 weight portions, continue reaction 5 hours with the 0.1mol/L of the aqueous solution of nitric acid modulation of 1N.
Finish after the polyreaction, take out reactant liquor, and with the membrane filter of 3 μ m, filtered particles is separated with reactant liquor.Behind ethanol and fully clean this particle of acetone, in vacuum dryer, carry out drying under reduced pressure, obtained surface treated spacer particle.
(3) modulation of spacer particle dispersio
Get the surface treated gained spacer particle of necessary amount,, then, be added at leisure in the spreading agent with the described composition of table 1, and fully stir with ultrasonic processor and to make it to disperse, modulated spacer particle dispersio 1 to reach the particle concentration of regulation.With width of mesh is that the Stainless Steel system sieve of 10 μ m filters the spacer particle dispersio 1 that is obtained, and removes condensation product, the evaluation that is provided in the ink discharge device to be carried out.
(4) configuration of the spacer particle on the substrate
It is the ink discharge device of the piezoelectricity mode of 30 μ m shower nozzles that bore has been carried in use, and described spacer particle dispersio is ejected on the substrate with the initial temperature shown in the table 2.
Used substrate as this substrate through processing as described below, promptly, possess on the surface on the color filter glass plate of ito transparent electrode, according to the even coating polyimide intermediate of whirl coating (eastern Li She System,<LP-64 〉), and after 150 ℃ of following dryings, burn till at 280 ℃ and to harden in 90 minutes, and form alignment films thus.
On colour filtering chip basic board owing to be formed with the black matrix that width is 20 μ m between the color filter pixel, therefore, with ink discharge device on this black matrix with the arranged spaced of 150 μ m spacer particle.In addition, the distribution density of spacer particle is adjusted into 100/mm during configuration 2
During ejection, with the heater heats operator's console that is installed on the operator's console.
For drying is ejected to the spacer particle dispersio of the substrate on the operator's console, the substrate of finishing ejection is moved to rapidly on the electric hot plate that is heated to set point of temperature as shown in table 2, and carry out drying.When the substrate temperature at ejection initial stage was different with dry usefulness electric plate temperature, the surface temperature of substrate will slowly rise.
Behind Visual Confirmation medium bone dry, placed 30 minutes under the temperature at this moment again.
Colour filtering chip basic board and its subtend substrate of spacer particle have been disposed by above method with peripheral encapsulant gummed, and 150 ℃ of heated sealant materials made it in 1 minute the sclerosis, the production unit gap is the dummy cell of 5 μ m, then, with vacuum method to filling liquid crystal wherein, with sealing compound inlet is sealed again afterwards, obtain liquid crystal display thus.
(5) estimate
Based on following index, estimated respectively: surface tension under 20 ℃ of spacer particle dispersio and impact diameter D dispersed, when on substrate, spraying spacer particle dispersio 1Adhere to diameter D with dried spacer particle 2, spacer particle configuration, as the display quality of liquid crystal indicator, the purity of liquid crystal.
It the results are shown in the table 2.
(the dispersiveness evaluation of spacer particle dispersio)
The dispersion again of the sieve pore blockade that produces when filtering spacer particle dispersio with the Stainless Steel system mesh screen of mesh 10 μ m and the spacer particle of sedimentation by visualization, and estimate its dispersiveness according to following criterion.
◎: sieve pore blockade does not appear in Stainless Steel system mesh screen substantially, and spacer particle dispersio can be unimpeded.And, the good dispersion again of spacer particle.
Zero: though spacer particle dispersio can some blocked parts occur on the Stainless Steel system mesh screen after filtering by Stainless Steel system mesh screen.The good dispersion again of spacer particle.
△: obstruction has appearred in a lot of sieve apertures on the Stainless Steel system mesh screen, and spacer particle dispersio is failed unimpeded, but by prolonging filtration time, still can finish filtration.And, even rock container, through the also not appearance dispersion again of spacer particle of a period of time sedimentation.
*: the sieve pore blockade of Stainless Steel system mesh screen is serious, and spacer particle dispersio can't pass through at all.And, even rock container, through the also not appearance dispersion again of spacer particle of a period of time sedimentation.
(the configuration evaluation of spacer particle)
Filter spacer particle dispersio with Stainless Steel system mesh screen (mesh 10 μ m), remove after the condensation product, use and be equipped with the ink discharge device that bore is the piezoelectricity mode of 30 μ m shower nozzles, be sprayed on the substrate.
Used substrate as this substrate through processing as described below, promptly, possess on the surface on the color filter glass substrate of ito transparent electrode, according to the even coating polyimide intermediate of whirl coating (eastern Li She System, trade name<LP-64 〉), and after 150 ℃ of following dryings, burn till at 280 ℃ and to harden in 90 minutes, and form alignment films thus.On above-mentioned color filter glass substrate, be formed with the black matrix that width is 20 μ m between the color filter pixel, and with ink discharge device on this black matrix with the arranged spaced of 150 μ m spacer particle.In addition, the distribution density of spacer particle is adjusted into 100/mm during configuration 2In the configuration of carrying out described spacer particle, the substrate of room temperature is placed on the operator's console, and the substrate that will finish ejection moves to rapidly on the electric hot plate that is heated to 90 ℃, carry out drying.Behind Visual Confirmation medium bone dry, placed 30 minutes under the temperature at this moment again.After being disposed at spacer particle on the substrate with described method, use the microscopic examination configuration state, and, estimate the configuration of spacer particle according to following criterion.
◎: each circuit that has disposed spacer particle is not observed scarce luminous point simultaneously for uniformly-spaced and straight yet.
Zero: each circuit that has disposed spacer particle has been observed a small amount of luminous point that lacks for uniformly-spaced and straight.
△: the interval that has disposed between each circuit of spacer particle is inconsistent, and has observed many places and lack luminous point.
*: owing to there is not the spacer particle ejection on the substrate basically, therefore fail to dispose, and observed the scarce luminous point in many places.
(the display quality evaluation (1) of liquid crystal indicator)
Zero: do not observe spacer particle in the viewing area fully, and also do not observe the pollution of alignment films.
△: observed a small amount of spacer particle in the viewing area, but do not observed the pollution of alignment films.
△ *: observed a small amount of spacer particle in the viewing area, and to have observed a little may be to result from the scarce luminous point of the stain shape that alignment films pollutes.
*: having observed a plurality of spacer particles in the viewing area, may be to result from the scarce luminous point of the stain shape that alignment films pollutes but do not observe.
Observed a plurality of spacer particles in * *: the viewing area, and to have observed may be to result from the bigger scarce luminous point of the stain shape that alignment films pollutes.
(the display quality evaluation (2) of liquid crystal indicator)
◎: do not observe spacer particle extruding to the viewing area.
Zero: the spacer particle of only observing minute quantity is to showing extruding of field.
△: observe spacer particle to showing extruding of field.
*: observe spacer particle to showing extruding of field, and observed consequent scarce luminous point.
(the purity evaluation of liquid crystal)
With spacer particle 0.1g, be distributed among liquid crystal (trade name<ZL1-4720-000 〉, the メ Le Network System of the society) 2mL, place after 200 hours down for 80 ℃ and reclaim liquid crystal, and measured liquid crystal purity according to the gas chromatography method.
(embodiment 2~6, comparative example 2~6)
Use the surface treated spacer particle of making among the embodiment 1, modulation has the spacer particle dispersio of the composition of table 1, and uses this dispersion liquid, under condition as table 2, configuration isolation particle on substrate, and estimate, in addition, other are identical with embodiment 1.
In addition, the medium volatility height of spacer particle dispersio 5 has produced the condensation product of spacer particle on the wall of container when carrying out dispersion treatment, in addition, when filtering with Stainless Steel system mesh screen, produced sieve pore blockade.
Table 1
Spacer particle dispersio
1 2 3 4 5
Form (weight %) Isopropyl alcohol 20 20 30 - 90
Ethylene glycol 60 60 - 70 -
Water 20 20 70 30 10
Spacer particle 0.5 6.0 0.5 0.5 0.5
Table 2
Spacer particle dispersio Surface tension (mN/m) Dispersed The initial stage substrate temperature (℃) Electric plate temperature (℃) Finish dry time substrate temperature (℃) Finish drying time (second) Impact diameter D 1(μm) Adhere to diameter D 2(μm) Spacer particle configuration property Display quality (1) Display quality (2) Liquid crystal purity (%)
Embodiment 1 1 35 45 45 45 13 80 16 100
Embodiment 2 1 35 45 70 60 8 80 19 100
Embodiment 3 1 35 20 20 20 1700 80 25 100
Embodiment 4 1 35 20 70 60 15 80 15 100
Embodiment 5 4 64 20 70 60 35 70 20 × 100
Embodiment 6 4 64 20 90 80 20 70 23 × 100
Comparative example 1 1 35 100 100 100 0.5 80 110 ×× × 100
Comparative example 2 1 35 80 80 80 1 80 95 × × 100
Comparative example 3 1 35 45 150 100 1 80 130 ×× × 100
Comparative example 4 2 35 20 70 60 13 100 70 × × 100
Comparative example 5 3 29 20 70 60 20 120 80 × × 100
Comparative example 6 5 29 20 70 60 1 - - × - - 100
(embodiment 7)
(1) modulation of spacer particle
In separable flask, divinylbenzene, the different monooctyl ester of 5 parts by weight of acrylic for 15 weight portions as polymerization initiator, drop into the benzoyl peroxide of 1.3 weight portions, and evenly mix.Then, drop into 3 weight % aqueous solution 20 weight portions and lauryl sodium sulfate 0.5 weight portion of polyvinyl alcohol (PVA) (trade name<Network ラ レ Port バ one Le GL-03 〉, Network ラ レ society system), and after evenly mixing, drop into ion exchange water 140 weight portions.Then, under stream of nitrogen gas,,, obtain particulate Yi Bian under 80 ℃, carry out 15 hours polyreaction Yi Bian stir this mixed aqueous solution.After hot water and the fully clean particulate that obtains of acetone, carry out the gradation operation, acetone is vapored away, obtain spacer particle.The mean grain size of the spacer particle that obtains is 5 μ m, and the CV value is 3.0%.
(2) surface treatment of spacer particle
Spacer particle 5 weight portions that obtain are put in the mixed aqueous solution that is made of ion exchange water 20 weight portions and hydroxyethyl methylacrylate 10 weight portions, and, evenly mixed with after the ultrasonic processor dispersion.Then, use the nitrogen replacement reaction system, and under 30 ℃, continue to stir 2 hours.Then, in reaction system, add the ammonium ceric nitrate aqueous solution of 10 weight portions, and carry out taking out reactant liquor after 5 hours polyreactions, and, particle and reactant liquor are passed through isolated by filtration with the film filter of 3 μ m with the 0.1mol/L of the aqueous solution of nitric acid of 1N modulation.After fully cleaning the particle that obtains with ethanol and acetone, in vacuum dryer, carry out drying under reduced pressure, the spacer particle of vinyl based thermoplastic resin that obtained surface grafting polymerization.
(3) modulation of spacer particle dispersio
Take by weighing the gained spacer particle of necessary amount, so that particle concentration reaches 0.3 weight %, then, be added at leisure in the medium that the mixed liquor by isopropyl alcohol 20 weight portions, ethylene glycol 60 weight portions, ion exchange water 20 weight portions constitutes, and with ultrasonic processor fully mix make it evenly to disperse after, with width of mesh is that the Stainless Steel steel mesh screen of 10 μ m filters, and removes condensation product, has modulated spacer particle dispersio.
(4) making of substrate
Use following substrate, promptly, after being formed with the black matrix of wide 15 μ m between the pixel of color filter and on dyed layer, applying external coating, form the substrate of the color filter of ITO transparent contact electrode (transparentcontact electrode) again, made following 3 kinds of substrates.
1. substrate A: on whole of the ITO of described colour filtering chip basic board transparent contact electrode, evenly forming by polyimide is the alignment films that resin constitutes.The black matrix part of the color filter on this alignment films as shown in Figure 2, is implemented the Laser Processing of the width 8 μ m of striated, removes the alignment films (polyimide is a resin) on surface, exposes the ITO of substrate, thereby has made substrate A.The ito surface that exposes of the substrate A that obtains is 25 ° with respect to the contact angle θ a of the spacer particle dispersio that is obtained by (3), and the alignment films on surface is 50 ° with respect to the contact angle θ b of the spacer particle dispersio that is obtained by (3).
2. substrate B: on whole of the ITO of described colour filtering chip basic board transparent contact electrode, the coating photosensitive polyimide is a resin precursor, expose and develop by mask, thereby black matrix part at color filter, as shown in Figure 2, not forming by polyimide is the alignment films that resin constitutes, and exposes the ITO of the substrate of wide 8 μ m with striated, thereby has made substrate B.The ito surface that exposes of the substrate B that obtains is 25 ° with respect to the contact angle θ a of the spacer particle dispersio that is obtained by (3), and the alignment films (polyimide is a resin) on surface is 45 ° with respect to the contact angle θ b of the spacer particle dispersio that is obtained by (3).
3. substrate C: except not implementing Laser Processing, other are with 1. identical, and on whole of ITO transparent contact electrode, forming by polyimide is the alignment films that resin constitutes, thereby has produced substrate C.The alignment films (polyimide is a resin) on the surface of the substrate B that obtains is 50 ° with respect to the contact angle θ b of the spacer particle dispersio that is obtained by (3).
(5) configuration of the spacer particle on the substrate
It is the ink discharge device of the piezoelectricity mode of 30 μ m shower nozzles that bore has been carried in use, implement on the striated ito surface that Laser Processing exposes (with respect to b:25 ° of the contact angle θ of spacer particle dispersio) passing through on the substrate A (colour filtering chip basic board), spray at interval after the spacer particle dispersio of each 35pL with 120 μ m, carry out drying, the configuration isolation particle, thus the substrate A (colour filtering chip basic board) that disposes spacer particle made.In addition, the configuration density of spacer particle is adjusted to 150/mm during configuration 2In addition, in the configuration isolation particle, the substrate of normal temperature placed spray spacer particle dispersio on the operator's console again, and will finish the substrate of ejection, and move to rapidly on the electric hot plate that is heated to 90 ℃, carry out drying again, then, after visual definite medium drying, under 90 ℃ atmosphere, placed 30 minutes, make it bone dry.
Then, dispose in order to fit the substrate A (colour filtering chip basic board) of spacer particle with it relative to array base palte, use stencil printing printed perimeter encapsulant, both sides are fitted, afterwards, made it in 90 minutes to solidify at 160 ℃ of heated sealant materials, the production unit gap is the dummy cell of 5 μ m.Then, use vacuum method in this dummy cell, to fill the TN type liquid crystal of ormal weight, afterwards, with sealing compound inlet is sealed again, and carry out 30 minutes heat treated, thereby make TFT type liquid crystal indicator at 120 ℃.
The result that the display quality of the TFT type liquid crystal indicator that obtained by described method is estimated is: do not observe the spacer particle that is present in pixel portion, and, do not observe the poor display phenomenons such as scarce luminous point that the anomalous orientation by near the liquid crystal the spacer particle causes fully.In addition, described evaluation is, adds 4.2 volts of voltages and amplifies with electron microscope that the back undertaken by the visualization image.
(embodiment 8)
Use the substrate B (colour filtering chip basic board) that in embodiment 7, makes as the substrate that disposes spacer particle, and by on the striated ito surface that exposes on the substrate B (colour filtering chip basic board) (with respect to b:25 ° of the contact angle θ of spacer particle dispersio), beyond the ejection spacer particle dispersio, other and embodiment 1 have made substrate B (colour filtering chip basic board) and the TFT type liquid crystal indicator that disposes spacer particle in the same manner.
Display quality evaluation for the TFT type liquid crystal indicator that obtains, carry out according to the method identical with embodiment 7, consequently: do not observe the spacer particle that is present in pixel portion, and, do not observe the poor display phenomenons such as scarce luminous point that the anomalous orientation by near the liquid crystal the spacer particle causes fully.
(comparative example 7)
Use the substrate C (colour filtering chip basic board) that in embodiment 7, makes as the substrate that disposes spacer particle, and by on the alignment films on the substrate C (colour filtering chip basic board) (polyimide is a resin) face (with respect to b:50 ° of the contact angle θ of spacer particle dispersio), beyond the ejection spacer particle dispersio, other and embodiment 7 have made substrate C (colour filtering chip basic board) and the TFT type liquid crystal indicator that disposes spacer particle in the same manner.
Display quality evaluation for the TFT type liquid crystal indicator that obtains, carry out according to the method identical, consequently: around pixel portion, observed some spacer particles with embodiment 7, and, also found the scarce luminous point that the anomalous orientation by near the liquid crystal the spacer particle causes.
Use and described same method, estimate the spacer particle dispersio in embodiment 7,8 and comparative example 7, made the surface tension 20 ℃ under, dispersiveness, when on substrate, spraying spacer particle dispersio spacer particle configuration, as the purity of the display quality and the liquid crystal of liquid crystal indicator.
The results are shown in the table 3.
Table 3
Surface tension (mN/m) Dispersed Spacer particle configuration property Display quality (1) Display quality (2) Liquid crystal purity (%)
Embodiment 7 35 100
Embodiment 8 35 100
Comparative example 7 35 100
(embodiment 9)
(1) modulation of transad particle
In separable flask, divinylbenzene, the different monooctyl ester of 5 parts by weight of acrylic for 15 weight portions as polymerization initiator, drop into the benzoyl peroxide of 1.3 weight portions, and evenly mix.Then, drop into 3 weight % aqueous solution 20 weight portions and lauryl sodium sulfate 0.5 weight portion of polyvinyl alcohol (PVA) (trade name<Network ラ レ Port バ one Le GL-03 〉, Network ラ レ society system), and after evenly mixing, drop into ion exchange water 140 weight portions.Then, under stream of nitrogen gas,,, obtain particulate Yi Bian under 80 ℃, carry out 15 hours polyreaction Yi Bian stir this aqueous solution.After hot water and the clean particulate that obtains of acetone, carry out the gradation operation, acetone is vapored away, obtain the transad particle.The mean grain size of the transad particle that obtains is 5 μ m, and the CV value is 3.0%.
(2) surface treatment of spacer particle
With spacer particle 5 weight portions that obtain, put in the mix monomer that constitutes by dimethyl sulfoxide (DMSO) 20 weight portions, hydroxyethyl methylacrylate 10 weight portions, isobutyl methacrylate 8 weight portions and methacrylic acid 2 weight portions, and, evenly mix with after the ultrasonic processor dispersion.Then, use the nitrogen replacement reaction system, and under 30 ℃, continue to stir 2 hours.Then, in reaction system, add the ammonium ceric nitrate aqueous solution of 10 weight portions with the 0.1mol/L of the aqueous solution of nitric acid modulation of 1N, and carry out after 5 hours polyreactions, take out reactant liquor, and, particle is separated by filtration with reactant liquor with the film filter of 3 μ m.After fully cleaning the particle that obtains with ethanol and acetone, in vacuum dryer, carry out drying under reduced pressure, the spacer particle (A) of vinyl based thermoplastic resin that obtained on the transad particle surface graft polymerization.
(3) modulation of medium
Evenly mix ethylene glycol 60 weight portions, isopropyl alcohol 20 weight portions, ion exchange water 20 weight portions, be modulated into medium (a).
(4) modulation of spacer particle dispersio
Spacer particle (A) 0.5 weight portion gently is added in the 100 weight portion media (a), and evenly mixes, be made into spacer particle dispersio with ultrasonic processor.
(5) estimate
Use and above-mentioned same method, estimate the spacer particle dispersio that in embodiment 9~13 and comparative example 8~10, obtains the surface tension 20 ℃ under, dispersiveness, when on substrate, spraying spacer particle dispersio spacer particle configuration, as the purity of the display quality and the liquid crystal of liquid crystal indicator.
The results are shown in the table 6.
(embodiment 10~13 and comparative example 8~10)
Except the composition of mix monomer has composition as described in Table 4, other and embodiment 9 have made on the transad particle surface graft polymerization in the same manner spacer particle (B) of vinyl based thermoplastic resin~spacer particle (D).
In addition, in ethyl acetate, after making the mix monomer that constitutes by hydroxyethyl methylacrylate 10 weight portions, isobutyl methacrylate 8 weight portions and methacrylic acid 2 weight portions carry out free radical solution polymerization, remove ethyl acetate by drying under reduced pressure, and pulverize the solid resin that obtain this moment, obtain the resin powder.Then, resin powder 2 weight portions that use to obtain and transad particle 5 weight portions that obtain at embodiment 9 are opened embodiment 1 that the 2000-347191 communique put down in writing with the spy and have been made in the same manner by ballistic method in the high velocity air and form tectal spacer particle (E) on the surface of transad particle.
On the other hand, the composition of medium is changed into beyond the composition shown in the table 5, other has made medium (b)~medium (d) same as described abovely.
Except the combination with spacer particle and medium changed the combination shown in the table 6 into, other and embodiment 9 had made spacer particle dispersio in the same manner, and estimate.
The results are shown in the table 6.
Table 4
Spacer particle
A B C D E
Transad particle (weight portion) 5 5 5 5 5
Mix monomer is formed (weight portion) Isobutyl methacrylate 8 14 2 4 0.8
Methacrylic acid dodecane ester - - - 4 -
Jia Jibingxisuanyizhi - - - - -
Hydroxyethyl methylacrylate 10 6 18 10 1
Methacrylic acid 2 - - 2 0.2
Dimethyl sulfoxide (DMSO) 20 20 20 20 -
Method for making Graft polymerization Graft polymerization Graft polymerization Graft polymerization Ballistic method in the high velocity air
Table 5
Medium
a b c d
Form (weight portion) Isobutyl alcohol 20 50 5 70
Ethylene glycol 60 - 40 -
Ion exchange water 20 50 55 30
Surface tension under 20 ℃ (mN/m) 35 27 53 23
Table 6
Spacer particle dispersio Estimate
Spacer particle Medium Surface tension (mN/m) Dispersed Spacer particle configuration property Liquid crystal display display quality (1) Liquid crystal display display quality (2) Liquid crystal purity (%)
Embodiment 9 A a 35 100
Embodiment 10 B a 35 100
Embodiment 11 C a 35 100
Embodiment 12 D a 35 100
Embodiment 13 A b 27 100
Comparative example 8 C c 53 × × 100
Comparative example 9 A d 23 × × × 100
Comparative example 10 E a 35 99.5
In table 4~table 6, can be clear that the spacer particle dispersio of embodiment 9~13 all has good or excellent dispersiveness, spacer particle configuration property, the display quality of liquid crystal display and the purity of liquid crystal.
Relative therewith, surpass the spacer particle dispersio of comparative example 8 of 50mN/m and the surface tension of medium under 20 ℃ in the surface tension under 20 ℃ less than with regard to the spacer particle dispersio of the comparative example 9 of 25mN/m with regard to medium, both spacer particle configuration property on substrate are all very poor, thereby fail to carry out the evaluation of liquid crystal display display quality.In addition, having used is not the comparative example 10 of the spacer particle made by meeting Zhi Juhe but by ballistic method in the high velocity air, its liquid crystal purity difference.
According to the present invention, can provide by ink-jetting style and spacer particle correctly can be disposed at manufacture method, the base plate for liquid crystal display device of the liquid crystal indicator on the optional position of substrate, the manufacture method and the spacer particle dispersio of base plate for liquid crystal display device.

Claims (2)

1. spacer particle dispersio, described spacer particle dispersio is used for by ink-jetting style ejection spacer particle dispersio this spacer particle being disposed at the manufacture method of the liquid crystal indicator on the optional position of substrate, it is characterized in that, described spacer particle dispersio contains spacer particle and medium at least, contains boiling point under 1 atmospheric pressure of 10~80 weight % in the described medium at the liquid more than 150 ℃.
2. spacer particle dispersio as claimed in claim 1, wherein, the boiling point under described 1 atmospheric pressure is to be selected from ethylene glycol, glycol monomethyl ether, glycol dimethyl ether at least a kind at the liquid more than 150 ℃.
CNA200710166707XA 2002-03-26 2003-03-26 Spacer particle dispersion liquid Pending CN101149538A (en)