CA1281511C - Sheets having improved stiffness from fiber, latex and coalescing agent - Google Patents
Sheets having improved stiffness from fiber, latex and coalescing agentInfo
- Publication number
- CA1281511C CA1281511C CA 551680 CA551680A CA1281511C CA 1281511 C CA1281511 C CA 1281511C CA 551680 CA551680 CA 551680 CA 551680 A CA551680 A CA 551680A CA 1281511 C CA1281511 C CA 1281511C
- Authority
- CA
- Canada
- Prior art keywords
- sheet
- latex
- coalescing agent
- fiber
- conditions
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Fee Related
Abstract
ABSTRACT
A process for preparing a sheet with improved stiffness by mixing a fiber, a latex having minimum film-forming conditions greater than the conditions the sheet reaches during drying and a fugitive coalescing agent. The mixture is collected and dried under condi-tions less than the minimum film-forming conditions of the latex. The process enables hard latexes to be employed which do not form films under the drying conditions of the sheet whereby the hard latexes can contribute to the stiffness of the final sheet. A
sheet prepared by the process is also provided.
A process for preparing a sheet with improved stiffness by mixing a fiber, a latex having minimum film-forming conditions greater than the conditions the sheet reaches during drying and a fugitive coalescing agent. The mixture is collected and dried under condi-tions less than the minimum film-forming conditions of the latex. The process enables hard latexes to be employed which do not form films under the drying conditions of the sheet whereby the hard latexes can contribute to the stiffness of the final sheet. A
sheet prepared by the process is also provided.
Description
12815~1 , SHEETS HAVING IMPROVED STIFFNESS FRO~I
FIBER, LATEX AN~ COALESCING AGE~T
The present invention generally relates to sheets prepared from fiber, latex and a coalescing agent. Further, the present invention provides for a sheet having improved stiffness by employing a hard latex and a fugitive coalescing agent.
A wide variety of sheets made from fibrous materials have been described in the art. Typical examples of such sheets incLude fine printing papers, cardboard papers, underlayment felt for vinyl floor coverings, gasket papers, roofing papers, sound-deadening papers, pipewrap, heat deflection papers and board products.
In an effort to improve the properties of these products, various latex compositions have been employed. While such practices have greatly contributed to the art, it is still desirable to have further improvements in their physical properties such as stiffness.
Stiffness is very important in printing grades of paper, especially in the lightweight grades.
30,110A-F -1-Methods to increase sheet stiffness are therefore desirable. One potential method for increasing stiffness would be to employ a latex having greater hardness; however, use of such a latex would be limited by its ability to coalesce or form a film under the sheet prepar~-tion conditions. That is, a latex with a minimum film-forming temperature greater than the temperature a sheet reaches during preparation ~.~ould not be a viable choice. Unfortunately, such latexes could provide the desired stiffness, but increasing the drying temperature would be harmful to the fiber and other organic components of the sheet system.
Therefore, it would be desirable to be able to employ a latex having minimum film-forming conditions greater than the sheet preparation conditions in order to take advantage of the latex's physical properties (i.e., hardness which could translate to increased stiffness when used in a sheet system).
U.S. Patent No. 4.225,383 generally teaches composite sheet preparation and suggests polymers which are made film-forming by the use of plasticizers can bi~
used. This reference is, however, limited to composite sheets contalning relatively high levels of filler or pigment from 60 to 95 percent based on the dried weight of the composite sheet. The subject invention, instead, focuses on sheets with no filler or medium filler levels The present invention provides a process for preparing a sheet with improved stiffness which comprises: (a) mi~ing in an aqueous medium a mixture comprising (i) a fiber, (ii) a latex having minimum film-forming conditions greater than the conditions the sheet reaches during drying, and (iii) a fugitive i 30,11OA-F -2-. ~ . .
lZ8~511 coalescing asent (b) forming the mixture into a sheet, and (c) drying said sheet under conditions less t'nan the minimum film-forming conditions required by the latex. Additionally, the process can include the step of mixing the latex with the fugitive coalescing agent prior to the addition of the fiber in the aqueous medium.
Further, the present invention may include the addition of a pisment or filler to the aqueous mixture of the process of up to 60 weisht percent based on the total dry weight of the sheet. Additionally, the latex can be destabilized by combining a chemical flocculant to form the sheet.
The present invention further provides for a sheet prepared from the aforementioned process. An advantage of the sheet is improved stiffness for various grades of paper, especially fine printing paper.
The process of the invention requires a fiber, a latex and a coalescing agent. More particularly, a fugitive coalescing agent is employed. The process can further comprise the incorporation of fillers from low to medium levels (0 to 60 weight percent based on the total weight of the dried sheet) which are generally known in the art of sheet preparatïon.
3 As a first component, the process of the invention requires a fiber material. The fiber can be a water-insoluble, natural or synthetic water-dispersible fiber or blend thereof. Either long or short fibers, or mixtures of both, are useful. The most common natural fibers are those made from wood .
30,110A-F -3-~Z81~
--4-- . .
pulp, cotton, wool and jute to name only a few.
Typically, synthetic fibers useful in the subject invention comprise rayon, nylon, glass fibers and polyester. More examples of other suitable fiber material are disclosed in U.S. Patent No. 4,225,383.
.
The fiber is present in a reinforcing amount.
That is, sufficient fiber ~ill be present to impart additional physical strength to the sheet, compared to a similar sheet prepared without a fiber. Generally, the sheet will contain from 1 to 99, preferably from 10 to 80, more preferably from 15 to 70 weight percent fiber based on the total weight of the dried sheet.
As a second component, the process of the invention requires a latex. By the term "latex" is meant a colloidally stable dispersion of discrete polymer particles in an aqueous medium. The latex employed in the subject invention is critical to imparting the desired stif~ness to the sheet. There-fore, the latexes are termed "hard latexes" which is meant to describe a latex havLng a relatively high minimum film-forming temperature. That is a higher temperature than the sheet normally reaches at drying or due to the higher minim-lm ~ilm-~orming temperature?
the latex does not have su~ficient residence time to adequately coalesce under normal sheet preparation conditions. More particularly, these so called "hard latexes" are non-film-forming under sheet process conditions. "Non-film-forming" is meant to indicate a degree of latex coalescence. Sheet preparation "conditions" is meant to indicate the various parameters which effect the ability of a latex to coalesce such as temperatu`re, residence time and moisture level. Because the hard latex would not I , 30,110A-F -~-128~511 generally form a film (i.e., coalesce) the third component of the subject invention is required which is a fugitive coalescing agent.
The latexes employed in the subject invention are water-insoluble, natural or synthetLc and may be homopolymers or copolymers of two or more ethylenically unsaturated monomers or a mixture of such polymers.
Monovinylidene aromatic compounds such as styrene and aliphatic conjugated dienes such as 1,3-butadiene are preferred latexes. Generally, the more preferred latexes comprise styrene/butadiene. Other suitable latexes generally known in the art of sheet preparation can also be advantageously employed as described herein. Suitable latexes are disclosed in U.S. Patent No. 4,225,383.
The latex will be present in an amount sufficient to maintain the ~inished sheet in the form of a generalLy unitary sheet having su~ficient body to enable it to be handled without crumbli.ng. Preferably, there is sufficient late~ pres,enk to al~ow the dried sheet to be put on rolls, coated, cut and printed without crumbllng or tearing. Gerlerally, the sheet will have from 1 to 30, preferabLy ~rom 1.-5 to 10, more preferably from 2 to 7, weight percent based on the total weight of the dried sheet.
As a third component, the subject process requires a coalescing agent. More particularly, the coalescing agent must be a fugitive coalescing agent.
Therefore, unless otherwise indicated the term "coalescing agent" is meant to indicate a fugitive coalescing agent. By "fugitive" is meant that the coalescing agent is sufficiently volatile such that 30,11OA-F -5-~81Sl~
under the conditions employed to form and dry the sheet, the coalescing agent will be substantially removed from the sheet. Useful coalescing agents include ~lycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, - ethylene ~lycol monobutyl ether, dietnylene glycol monobutyl ether, diethylene glycol diethyl ether, and propylene glycol phenol ether; glyo~l ether acetates such as diethylene glycol monoethyl ether acetate and ethylene glycol monomethyl ether acetate; and ketones such as acetone, methyl ethyl ketone, methyl propyl ketone, and diacetone alcohol.
The coalescing agent is present in an effective amount. That is, sufficient coalescing agent will be present to assist in the deformation of the latex particles such that the finished sheet has greater stiffness than a similar sheet made without the use of a coalescing agent. Generally, the coalescing agent will be present from 1 to 20, preferably from 2.5 to 15, more preferably from 5 to 10 weight percent based on the total weight of the latex solids.
The fu~itive coale~cin~ agent is preferentially present in the latex particle as opposed to the aqueous phase of the ~iYture. In the late~ particle the coalescing agent assists the hard latex to deform or coalesce on the fiber or pigments if present. In effect, the hard lateY is, thus, made film-formin~
under drying conditions less than the minimum film-forming conditions required by the hard latex.
Further, during the drying of the sheet, the fugitive coalescing agent is substantially removed whereby the hard latex reverts and contributes to the stiffness of 30,11OA-F -6-the final sheet. Trace amounts of fugitive coalescing agent may, however, remain in the final sheet.
The invention also includes "composite papers"
which are non-woven fabrics containing a binder, a fiber~ and a nonbindlng filler. These fillers are generally finely divided solids (i.e., powders) such as clay, magnesium hydroxide, or calcium carbonate.
Examples of other suitable fillers are disclosed in U.S. Patent No. 4,225?383.
For use in the subject invention, the filler level is from 0 to 60 weight percent based on the weight of the dried sheet. The preferred filler range is from 25 to ~5 weight percent. Lower filler levels can be advantageously employed due to the excellent physical properties contributed by the hard latex.
Generally, the fiber, latex, coalesc;ng agent and optional filler are combined in an aqueous medium prior to formation o~ the sheet. ~hile not critical to the practice of the invention, it i9 ~enerally convenient to premix the latex and coalescing agent, and add this mixture to a dispersion o~ the fiber and filler in water. In preparing the latex-coalescing agent mixture, it is desirable to provide a standing -period so that the coalescing agent may have time to diffuse into the latex particles. Normally, a period of about one hour is sufficient. If the latex ar;d coalescing agent are added separately to the fiber slurry, an extensi~/e waiting period (perhaps several days or more) may be needed unless very large amounts of coalescing agent are used.
30,110A-F -7-1;~81 After the fiber, latex and coalescing agent have been combined in the aqueous medium, the late~ is destabilized so as to precipitate it onto the fibers.
This is conveniently accomplished by means of a floccu-lating (coagulating) agent. As the flocculant,substances capable of destabilizing the latec dispersion can be used. ~amples of suitable flocculants include modified cationic polyacrylamide and diallyldie~hylammonium chlorid~ for anionic lat~xes and partially hydrolyzed ?olyacrylamide for cationic latexes.
After flocculation is completed, the aqueous slurry is formed into a sheet or web and dewatered.
This sheet forming and dewatering process may be accom-plished by any conventional paper-making apparatus such as a sheet mold, or a Fourdrinier or cylinder machine.
After the composite is formed into a dewatered sheet, it may be desirable to densify the sheet by pressing it with a ~lat press or by sending it through calendering rolls. Dryin~ of the sheet may be either by air drying at ambi0nt conditlons or by oven drying.
The drying temperature of a sheet is limited by the temperature at which the fiber or other organic component of the system can withstand ~ithout being damaged. Thus, heretobefore, a latex selection was generally limited by the minimum film-forming temperature of the latex. Therefore, an advantage of the present invention is that for a given drying temperature, a harder latex may be used or for a given latex, the composite may be dried at a-lower temperature.
.
30,11OA-F -8-1~8~511 Other general teachings of the use of latexes in the formation of fibrous sheets may be found, for example, in U.S. Patent Nos. 3,875,097 and 3,518,113, and r~est German issued patent 1 446 609.
A particularly useful and commercially signi-ficant embodiment of the in/ention includes a composite made with a latex, a high grade cellulose fiber, a filler, and a fugitive coalescing agent, wherein the finished composite is relatively thin (i.e., ~rom 0.002 to 0.01 inches (0.05 to 0.25 mm)). These composites generally will contain desirably 3 to 99, preferably 25 to 90, most preferably 35 to 70, weight percent fiber based on the total weight of the dried composite;
desirably O to 60, preferably from 25 to 45, weight percent filler based on the weight of the dried compos;te; and desirably from 0.5 to 30, preferably from o.8 to 10, more preferably ~rom 1 to 5, weight percent (based on solids) of the late~, based on the total weight of the dried composite. Such composites are useful as printing papers, and have unexpectedly superior ~tiff`ness compared to similar papers made without the fugitive coalescin3 a~ent.
The invention is further illustrated by the following examples. In the e~amples all parts and percentages are by weight unless otherwise specified.
30 Example 1 - Fine Printin~ Paper A. Pulp Preparation A mixture of 50 parts kraft hardwood and 50 parts kraft softwood was dispersed in water at 1.35 percent consistency and mechanically refined into pulp having 392 CSF (Canadian Standard Freeness). The pulp 30,11OA-F -9-'. :
' 12815~1 was then diluted to 0.51 percent consistency. On the following da-y, the pulp wa3 adjusted to a pH of about 4.1 with 0.1 N HCl.
B.Latex ~reDaration A relatively hard latex wa3 prepared from 80 parts styrene, 17 parts butadiene and 2 parts acrylic acid using co~ventional emuIsion polymerization tech-niques. The resultin~ latex was filtered to remo~/e anycoagulum, and had 48 percent solids. To 100 wet grams of latex (45 percent solids), 4.5 g of propylene glycol phenyl ether were added, and mixed for at least 1 hour.
C.Sheet Preparation In a large beaker, 444 wet grams (0.5 percent solids) of pulp were thoroughly mixed with 1.3 g of kaolin filler clay and 0.18 g of the above-prepared latex were added. A~ter stirring was complete (3 minutes), cationic polyacrylamide (flocculating agent) was added unti] water phase clarity occurred, and then an additional 0.5 pounds/ton (0.025 percent) of Betz 1260 thigh molecular weight polyacrylamide) was added. The dispersicn was then immediately poured into a Noble and Wood sheet mold (8 in ~ 8 in (203 mm x 203 mm)) having 5 liters of pH 4.0 water therein, and then additional water was added to bring ` the total volume in the mold to 10.5 liters. The mold was then drained, and the sheet pressed and removed from the screen. The sheet was drum dried at 160F
(71C) for 330 seconds. The moisture content of the dried sheet was 4 percent.
30,110A-F -10-~ .
~Z8~5~1 D. Evaluations After aging for 1 day at 50 percent RH and 73F
(22.8C) (TAPPI method T-402-05-70), the sheets were evaluated for riOidity on a Licence ~odak P~the tester using 0.5 in (12.7 mm) wide test strips. The results are shown in the Table which follows.
E.Compa~i 3 ons - - ~
10 For comparative purposes, two other papers, Samples 2 and 3, were made. Sample 2 was identical to the above-described paper, except that it was made without the propylene glycol ?henyl ether coalescing agent. Sample 3 did not contain a coalescing agent and was made from a softer latex which was a blend of 40 percent of an 81 percent styrene, 17 percent 1,3-butadiene, 2 percent acrylic acid latex, and 60 percent of a latex comprising 49 percent styrene, 50 percent 1,3-butadiene, and 1 percent itaconic acid. The results are also ~hown below.
FINE ~R N~ ~NG PAPER
Sample Late.~ Coalescin~ A~ent Ri~itv_ 1 hard yes 35 . 7 2* hard no 28.6 303* Soft/hard no 27.7 blend *Not an example of the invention .
30, 110A-F -11-
FIBER, LATEX AN~ COALESCING AGE~T
The present invention generally relates to sheets prepared from fiber, latex and a coalescing agent. Further, the present invention provides for a sheet having improved stiffness by employing a hard latex and a fugitive coalescing agent.
A wide variety of sheets made from fibrous materials have been described in the art. Typical examples of such sheets incLude fine printing papers, cardboard papers, underlayment felt for vinyl floor coverings, gasket papers, roofing papers, sound-deadening papers, pipewrap, heat deflection papers and board products.
In an effort to improve the properties of these products, various latex compositions have been employed. While such practices have greatly contributed to the art, it is still desirable to have further improvements in their physical properties such as stiffness.
Stiffness is very important in printing grades of paper, especially in the lightweight grades.
30,110A-F -1-Methods to increase sheet stiffness are therefore desirable. One potential method for increasing stiffness would be to employ a latex having greater hardness; however, use of such a latex would be limited by its ability to coalesce or form a film under the sheet prepar~-tion conditions. That is, a latex with a minimum film-forming temperature greater than the temperature a sheet reaches during preparation ~.~ould not be a viable choice. Unfortunately, such latexes could provide the desired stiffness, but increasing the drying temperature would be harmful to the fiber and other organic components of the sheet system.
Therefore, it would be desirable to be able to employ a latex having minimum film-forming conditions greater than the sheet preparation conditions in order to take advantage of the latex's physical properties (i.e., hardness which could translate to increased stiffness when used in a sheet system).
U.S. Patent No. 4.225,383 generally teaches composite sheet preparation and suggests polymers which are made film-forming by the use of plasticizers can bi~
used. This reference is, however, limited to composite sheets contalning relatively high levels of filler or pigment from 60 to 95 percent based on the dried weight of the composite sheet. The subject invention, instead, focuses on sheets with no filler or medium filler levels The present invention provides a process for preparing a sheet with improved stiffness which comprises: (a) mi~ing in an aqueous medium a mixture comprising (i) a fiber, (ii) a latex having minimum film-forming conditions greater than the conditions the sheet reaches during drying, and (iii) a fugitive i 30,11OA-F -2-. ~ . .
lZ8~511 coalescing asent (b) forming the mixture into a sheet, and (c) drying said sheet under conditions less t'nan the minimum film-forming conditions required by the latex. Additionally, the process can include the step of mixing the latex with the fugitive coalescing agent prior to the addition of the fiber in the aqueous medium.
Further, the present invention may include the addition of a pisment or filler to the aqueous mixture of the process of up to 60 weisht percent based on the total dry weight of the sheet. Additionally, the latex can be destabilized by combining a chemical flocculant to form the sheet.
The present invention further provides for a sheet prepared from the aforementioned process. An advantage of the sheet is improved stiffness for various grades of paper, especially fine printing paper.
The process of the invention requires a fiber, a latex and a coalescing agent. More particularly, a fugitive coalescing agent is employed. The process can further comprise the incorporation of fillers from low to medium levels (0 to 60 weight percent based on the total weight of the dried sheet) which are generally known in the art of sheet preparatïon.
3 As a first component, the process of the invention requires a fiber material. The fiber can be a water-insoluble, natural or synthetic water-dispersible fiber or blend thereof. Either long or short fibers, or mixtures of both, are useful. The most common natural fibers are those made from wood .
30,110A-F -3-~Z81~
--4-- . .
pulp, cotton, wool and jute to name only a few.
Typically, synthetic fibers useful in the subject invention comprise rayon, nylon, glass fibers and polyester. More examples of other suitable fiber material are disclosed in U.S. Patent No. 4,225,383.
.
The fiber is present in a reinforcing amount.
That is, sufficient fiber ~ill be present to impart additional physical strength to the sheet, compared to a similar sheet prepared without a fiber. Generally, the sheet will contain from 1 to 99, preferably from 10 to 80, more preferably from 15 to 70 weight percent fiber based on the total weight of the dried sheet.
As a second component, the process of the invention requires a latex. By the term "latex" is meant a colloidally stable dispersion of discrete polymer particles in an aqueous medium. The latex employed in the subject invention is critical to imparting the desired stif~ness to the sheet. There-fore, the latexes are termed "hard latexes" which is meant to describe a latex havLng a relatively high minimum film-forming temperature. That is a higher temperature than the sheet normally reaches at drying or due to the higher minim-lm ~ilm-~orming temperature?
the latex does not have su~ficient residence time to adequately coalesce under normal sheet preparation conditions. More particularly, these so called "hard latexes" are non-film-forming under sheet process conditions. "Non-film-forming" is meant to indicate a degree of latex coalescence. Sheet preparation "conditions" is meant to indicate the various parameters which effect the ability of a latex to coalesce such as temperatu`re, residence time and moisture level. Because the hard latex would not I , 30,110A-F -~-128~511 generally form a film (i.e., coalesce) the third component of the subject invention is required which is a fugitive coalescing agent.
The latexes employed in the subject invention are water-insoluble, natural or synthetLc and may be homopolymers or copolymers of two or more ethylenically unsaturated monomers or a mixture of such polymers.
Monovinylidene aromatic compounds such as styrene and aliphatic conjugated dienes such as 1,3-butadiene are preferred latexes. Generally, the more preferred latexes comprise styrene/butadiene. Other suitable latexes generally known in the art of sheet preparation can also be advantageously employed as described herein. Suitable latexes are disclosed in U.S. Patent No. 4,225,383.
The latex will be present in an amount sufficient to maintain the ~inished sheet in the form of a generalLy unitary sheet having su~ficient body to enable it to be handled without crumbli.ng. Preferably, there is sufficient late~ pres,enk to al~ow the dried sheet to be put on rolls, coated, cut and printed without crumbllng or tearing. Gerlerally, the sheet will have from 1 to 30, preferabLy ~rom 1.-5 to 10, more preferably from 2 to 7, weight percent based on the total weight of the dried sheet.
As a third component, the subject process requires a coalescing agent. More particularly, the coalescing agent must be a fugitive coalescing agent.
Therefore, unless otherwise indicated the term "coalescing agent" is meant to indicate a fugitive coalescing agent. By "fugitive" is meant that the coalescing agent is sufficiently volatile such that 30,11OA-F -5-~81Sl~
under the conditions employed to form and dry the sheet, the coalescing agent will be substantially removed from the sheet. Useful coalescing agents include ~lycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, - ethylene ~lycol monobutyl ether, dietnylene glycol monobutyl ether, diethylene glycol diethyl ether, and propylene glycol phenol ether; glyo~l ether acetates such as diethylene glycol monoethyl ether acetate and ethylene glycol monomethyl ether acetate; and ketones such as acetone, methyl ethyl ketone, methyl propyl ketone, and diacetone alcohol.
The coalescing agent is present in an effective amount. That is, sufficient coalescing agent will be present to assist in the deformation of the latex particles such that the finished sheet has greater stiffness than a similar sheet made without the use of a coalescing agent. Generally, the coalescing agent will be present from 1 to 20, preferably from 2.5 to 15, more preferably from 5 to 10 weight percent based on the total weight of the latex solids.
The fu~itive coale~cin~ agent is preferentially present in the latex particle as opposed to the aqueous phase of the ~iYture. In the late~ particle the coalescing agent assists the hard latex to deform or coalesce on the fiber or pigments if present. In effect, the hard lateY is, thus, made film-formin~
under drying conditions less than the minimum film-forming conditions required by the hard latex.
Further, during the drying of the sheet, the fugitive coalescing agent is substantially removed whereby the hard latex reverts and contributes to the stiffness of 30,11OA-F -6-the final sheet. Trace amounts of fugitive coalescing agent may, however, remain in the final sheet.
The invention also includes "composite papers"
which are non-woven fabrics containing a binder, a fiber~ and a nonbindlng filler. These fillers are generally finely divided solids (i.e., powders) such as clay, magnesium hydroxide, or calcium carbonate.
Examples of other suitable fillers are disclosed in U.S. Patent No. 4,225?383.
For use in the subject invention, the filler level is from 0 to 60 weight percent based on the weight of the dried sheet. The preferred filler range is from 25 to ~5 weight percent. Lower filler levels can be advantageously employed due to the excellent physical properties contributed by the hard latex.
Generally, the fiber, latex, coalesc;ng agent and optional filler are combined in an aqueous medium prior to formation o~ the sheet. ~hile not critical to the practice of the invention, it i9 ~enerally convenient to premix the latex and coalescing agent, and add this mixture to a dispersion o~ the fiber and filler in water. In preparing the latex-coalescing agent mixture, it is desirable to provide a standing -period so that the coalescing agent may have time to diffuse into the latex particles. Normally, a period of about one hour is sufficient. If the latex ar;d coalescing agent are added separately to the fiber slurry, an extensi~/e waiting period (perhaps several days or more) may be needed unless very large amounts of coalescing agent are used.
30,110A-F -7-1;~81 After the fiber, latex and coalescing agent have been combined in the aqueous medium, the late~ is destabilized so as to precipitate it onto the fibers.
This is conveniently accomplished by means of a floccu-lating (coagulating) agent. As the flocculant,substances capable of destabilizing the latec dispersion can be used. ~amples of suitable flocculants include modified cationic polyacrylamide and diallyldie~hylammonium chlorid~ for anionic lat~xes and partially hydrolyzed ?olyacrylamide for cationic latexes.
After flocculation is completed, the aqueous slurry is formed into a sheet or web and dewatered.
This sheet forming and dewatering process may be accom-plished by any conventional paper-making apparatus such as a sheet mold, or a Fourdrinier or cylinder machine.
After the composite is formed into a dewatered sheet, it may be desirable to densify the sheet by pressing it with a ~lat press or by sending it through calendering rolls. Dryin~ of the sheet may be either by air drying at ambi0nt conditlons or by oven drying.
The drying temperature of a sheet is limited by the temperature at which the fiber or other organic component of the system can withstand ~ithout being damaged. Thus, heretobefore, a latex selection was generally limited by the minimum film-forming temperature of the latex. Therefore, an advantage of the present invention is that for a given drying temperature, a harder latex may be used or for a given latex, the composite may be dried at a-lower temperature.
.
30,11OA-F -8-1~8~511 Other general teachings of the use of latexes in the formation of fibrous sheets may be found, for example, in U.S. Patent Nos. 3,875,097 and 3,518,113, and r~est German issued patent 1 446 609.
A particularly useful and commercially signi-ficant embodiment of the in/ention includes a composite made with a latex, a high grade cellulose fiber, a filler, and a fugitive coalescing agent, wherein the finished composite is relatively thin (i.e., ~rom 0.002 to 0.01 inches (0.05 to 0.25 mm)). These composites generally will contain desirably 3 to 99, preferably 25 to 90, most preferably 35 to 70, weight percent fiber based on the total weight of the dried composite;
desirably O to 60, preferably from 25 to 45, weight percent filler based on the weight of the dried compos;te; and desirably from 0.5 to 30, preferably from o.8 to 10, more preferably ~rom 1 to 5, weight percent (based on solids) of the late~, based on the total weight of the dried composite. Such composites are useful as printing papers, and have unexpectedly superior ~tiff`ness compared to similar papers made without the fugitive coalescin3 a~ent.
The invention is further illustrated by the following examples. In the e~amples all parts and percentages are by weight unless otherwise specified.
30 Example 1 - Fine Printin~ Paper A. Pulp Preparation A mixture of 50 parts kraft hardwood and 50 parts kraft softwood was dispersed in water at 1.35 percent consistency and mechanically refined into pulp having 392 CSF (Canadian Standard Freeness). The pulp 30,11OA-F -9-'. :
' 12815~1 was then diluted to 0.51 percent consistency. On the following da-y, the pulp wa3 adjusted to a pH of about 4.1 with 0.1 N HCl.
B.Latex ~reDaration A relatively hard latex wa3 prepared from 80 parts styrene, 17 parts butadiene and 2 parts acrylic acid using co~ventional emuIsion polymerization tech-niques. The resultin~ latex was filtered to remo~/e anycoagulum, and had 48 percent solids. To 100 wet grams of latex (45 percent solids), 4.5 g of propylene glycol phenyl ether were added, and mixed for at least 1 hour.
C.Sheet Preparation In a large beaker, 444 wet grams (0.5 percent solids) of pulp were thoroughly mixed with 1.3 g of kaolin filler clay and 0.18 g of the above-prepared latex were added. A~ter stirring was complete (3 minutes), cationic polyacrylamide (flocculating agent) was added unti] water phase clarity occurred, and then an additional 0.5 pounds/ton (0.025 percent) of Betz 1260 thigh molecular weight polyacrylamide) was added. The dispersicn was then immediately poured into a Noble and Wood sheet mold (8 in ~ 8 in (203 mm x 203 mm)) having 5 liters of pH 4.0 water therein, and then additional water was added to bring ` the total volume in the mold to 10.5 liters. The mold was then drained, and the sheet pressed and removed from the screen. The sheet was drum dried at 160F
(71C) for 330 seconds. The moisture content of the dried sheet was 4 percent.
30,110A-F -10-~ .
~Z8~5~1 D. Evaluations After aging for 1 day at 50 percent RH and 73F
(22.8C) (TAPPI method T-402-05-70), the sheets were evaluated for riOidity on a Licence ~odak P~the tester using 0.5 in (12.7 mm) wide test strips. The results are shown in the Table which follows.
E.Compa~i 3 ons - - ~
10 For comparative purposes, two other papers, Samples 2 and 3, were made. Sample 2 was identical to the above-described paper, except that it was made without the propylene glycol ?henyl ether coalescing agent. Sample 3 did not contain a coalescing agent and was made from a softer latex which was a blend of 40 percent of an 81 percent styrene, 17 percent 1,3-butadiene, 2 percent acrylic acid latex, and 60 percent of a latex comprising 49 percent styrene, 50 percent 1,3-butadiene, and 1 percent itaconic acid. The results are also ~hown below.
FINE ~R N~ ~NG PAPER
Sample Late.~ Coalescin~ A~ent Ri~itv_ 1 hard yes 35 . 7 2* hard no 28.6 303* Soft/hard no 27.7 blend *Not an example of the invention .
30, 110A-F -11-
Claims (5)
1. A process for preparing printing paper having improved stiffness which comprises: (a) mixing in an aqueous medium a mixture comprising:
(i) a fiber, (ii) a latex having minimum film-forming conditions greater than the conditions the sheet reaches during drying, and (iii) a fugitive coalescing agent; and (iv) from 25 to 45 weight percent of a filler or pigment, based on the weight of said printing paper;
(b) forming said mixture into a sheet; and (c) drying said sheet under conditions less than the minimum film-forming conditions required by said latex.
(i) a fiber, (ii) a latex having minimum film-forming conditions greater than the conditions the sheet reaches during drying, and (iii) a fugitive coalescing agent; and (iv) from 25 to 45 weight percent of a filler or pigment, based on the weight of said printing paper;
(b) forming said mixture into a sheet; and (c) drying said sheet under conditions less than the minimum film-forming conditions required by said latex.
2. The process of Claim 1 which additionally includes the step of mixing said latex with said 30,110A-F -12-fugitive coalescing agent prior to the addition of said fiber in said aqueous medium.
3. The process of Claim 1 wherein the sheet is formed by destabilizing said latex with a chemical flocculant.
4. The process of Claim 1 wherein the fugitive coalescing agent is a glycol ether.
5. A printing paper prepared from the process of any one of Claims 1, 2 and 3.
30,110A-F -13-
30,110A-F -13-