WO2024068662A1 - Procédé et appareil de traitement de fibres pour la préparation d'un additif de pulpe à partir d'un matériau de départ de betterave sucrière - Google Patents

Procédé et appareil de traitement de fibres pour la préparation d'un additif de pulpe à partir d'un matériau de départ de betterave sucrière Download PDF

Info

Publication number
WO2024068662A1
WO2024068662A1 PCT/EP2023/076593 EP2023076593W WO2024068662A1 WO 2024068662 A1 WO2024068662 A1 WO 2024068662A1 EP 2023076593 W EP2023076593 W EP 2023076593W WO 2024068662 A1 WO2024068662 A1 WO 2024068662A1
Authority
WO
WIPO (PCT)
Prior art keywords
fibre
elements
pulp
sugar beet
processing apparatus
Prior art date
Application number
PCT/EP2023/076593
Other languages
English (en)
Inventor
Wolfgang Wach
Stefan Frenzel
Richard DANDAR
Richard Scott HURDING
René ROBIN
Original Assignee
Südzucker AG
Zelfo Technology Gmbh
Simply By Nature Gmbh
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Südzucker AG, Zelfo Technology Gmbh, Simply By Nature Gmbh filed Critical Südzucker AG
Publication of WO2024068662A1 publication Critical patent/WO2024068662A1/fr

Abstract

L'invention concerne un procédé de production d'un additif de pulpe à partir d'un matériau de départ de betterave sucrière, un appareil de traitement de fibres étant approprié pour ledit procédé, en particulier pour la préparation d'un additif de pulpe à partir d'un matériau de départ de betterave sucrière, et en particulier pour la défibrillation et/ou le défibrage de fibres de cellulose dans le matériau de départ de betterave sucrière, un procédé pour la production d'un additif de pulpe à partir d'un matériau de départ de betterave sucrière à l'aide dudit appareil de traitement de fibres ainsi qu'un additif de pulpe pouvant être obtenu à partir dudit procédé et un matériau d'emballage comprenant ledit additif de pulpe.
PCT/EP2023/076593 2022-09-27 2023-09-26 Procédé et appareil de traitement de fibres pour la préparation d'un additif de pulpe à partir d'un matériau de départ de betterave sucrière WO2024068662A1 (fr)

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
GB2214098.2 2022-09-27
GBGB2214098.2A GB202214098D0 (en) 2022-09-27 2022-09-27 Apparatus and method for defibrillating and/or defibering cellulose fibres and/or ligno-cellulosic fibres

Publications (1)

Publication Number Publication Date
WO2024068662A1 true WO2024068662A1 (fr) 2024-04-04

Family

ID=83978784

Family Applications (2)

Application Number Title Priority Date Filing Date
PCT/EP2023/076584 WO2024068657A1 (fr) 2022-09-27 2023-09-26 Appareil et procédé de défibrillation et/ou défibrage de fibres de cellulose et/ou de fibres ligno-cellulosiques
PCT/EP2023/076593 WO2024068662A1 (fr) 2022-09-27 2023-09-26 Procédé et appareil de traitement de fibres pour la préparation d'un additif de pulpe à partir d'un matériau de départ de betterave sucrière

Family Applications Before (1)

Application Number Title Priority Date Filing Date
PCT/EP2023/076584 WO2024068657A1 (fr) 2022-09-27 2023-09-26 Appareil et procédé de défibrillation et/ou défibrage de fibres de cellulose et/ou de fibres ligno-cellulosiques

Country Status (2)

Country Link
GB (1) GB202214098D0 (fr)
WO (2) WO2024068657A1 (fr)

Citations (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0644293A1 (fr) 1993-09-21 1995-03-22 CARTIERA FAVINI S.p.A. Procédé de fabrication de papier à partir de pulpe de betterave à sucre, et papier obtenu
WO1997030215A1 (fr) 1996-02-13 1997-08-21 Eridania Beghin-Say Utilisation de pulpes de betterave a sucre dans la fabrication de papier ou de carton
US20070177451A1 (en) * 2006-02-02 2007-08-02 Benjamin Craig A Serrated kneading disk and kneading block

Family Cites Families (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
DE10149765B4 (de) * 2001-10-02 2004-03-18 Krauss-Maffei Kunststofftechnik Gmbh Kämmelement
DE102004052055B4 (de) * 2004-10-26 2014-11-20 Blach Verwaltung Gmbh & Co.Kg Extruder

Patent Citations (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0644293A1 (fr) 1993-09-21 1995-03-22 CARTIERA FAVINI S.p.A. Procédé de fabrication de papier à partir de pulpe de betterave à sucre, et papier obtenu
WO1997030215A1 (fr) 1996-02-13 1997-08-21 Eridania Beghin-Say Utilisation de pulpes de betterave a sucre dans la fabrication de papier ou de carton
US20070177451A1 (en) * 2006-02-02 2007-08-02 Benjamin Craig A Serrated kneading disk and kneading block

Non-Patent Citations (4)

* Cited by examiner, † Cited by third party
Title
FISEROVA ET AL., CELLULOSE CHEM. TECHNOL., vol. 41, 2007, pages 283 - 289
FISEROVA ET AL., WOOD RESEARCH, vol. 52, 2007, pages 59 - 74
GIGAC ET AL., INTERNATIONAL SUGAR JOURNAL, vol. 111, 2008, pages 20 - 26
ROUILLY A ET AL: "Thermo-mechanical processing of sugar beet pulp. I. Twin-screw extrusion process", CARBOHYDRATE POLYMERS, APPLIED SCIENCE PUBLISHERS , LTD BARKING, GB, vol. 66, no. 1, 5 October 2006 (2006-10-05), pages 81 - 87, XP027941408, ISSN: 0144-8617, [retrieved on 20061005] *

Also Published As

Publication number Publication date
GB202214098D0 (en) 2022-11-09
WO2024068657A1 (fr) 2024-04-04

Similar Documents

Publication Publication Date Title
US8608095B2 (en) Method for the disintegration of lignocellulose to fibers
CN103429815B (zh) 用于生产纳米纤维素的方法和设备
EP2997191B1 (fr) Procédé de fabrication de cellulose nanofibrillaire et de fabrication d'un produit en papier
US9416493B2 (en) Method, system and apparatus for processing fibril cellulose and fibril cellulose material
US20110105650A1 (en) Method and system for preparing densified lignocellulosic pulp for use in thermoplastic composite manufacturing processes
EP3974579B1 (fr) Procédé de fabrication de compact
Karunanithy et al. Thermo-mechanical pretreatment of feedstocks
US10196775B2 (en) Method for processing grass for manufacturing paper, paperboard and cardboard
CN103005658A (zh) 一种提高烟梗成浆质量的新工艺
CN102106599A (zh) 一种造纸法烟草薄片的烟草原料制浆疏解工艺
WO2024068662A1 (fr) Procédé et appareil de traitement de fibres pour la préparation d'un additif de pulpe à partir d'un matériau de départ de betterave sucrière
CN115889396B (zh) 一种基于工业化利用的田间农作物秸秆分级方法及装置
CN106436404A (zh) 一年生非木本生物质类纤维浆环保制浆系统及制浆方法
WO2015011066A1 (fr) Procédé de production de produits moulés
CN1256482C (zh) 棉秆造纸方法及设备
AT510785B1 (de) Mechanischer halbstoff sowie ein system und ein verfahren zur produktion mechanischen halbstoffes
JP2022171415A (ja) 循環粉砕処理装置、循環粉砕処理方法、アルコールの製造方法及びセルロースを含む組成物の製造方法
JP2008088594A (ja) パルプの処理装置および処理方法
EP2237935A1 (fr) Procédé et système pour la préparation d'une pâte lignocellulosique densifiée pour utilisation dans des procédés de fabrication de composites thermoplastiques
WO2023039642A1 (fr) Procédé et appareil pour la production d'un matériau fibreux cellulosique moulable
CN118265684A (en) Method and apparatus for producing moldable cellulose fiber material
EP4222311A1 (fr) Papier pour carton ondulé à haut rendement
SE436369B (sv) Forfarande for framstellning av for vidarebearbetning till absoptionsprodukter i konverteringsanleggningar lempligt utgangsmaterial
US20140008472A1 (en) Method and system for preparing densified lignocellulosic pulp for use in thermoplastic composite manufacturing processes

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 23782810

Country of ref document: EP

Kind code of ref document: A1