WO2008156821A1 - Silicone resin composites for high temperature durable elastic composite applications and methods for fabricating same - Google Patents

Silicone resin composites for high temperature durable elastic composite applications and methods for fabricating same Download PDF

Info

Publication number
WO2008156821A1
WO2008156821A1 PCT/US2008/007667 US2008007667W WO2008156821A1 WO 2008156821 A1 WO2008156821 A1 WO 2008156821A1 US 2008007667 W US2008007667 W US 2008007667W WO 2008156821 A1 WO2008156821 A1 WO 2008156821A1
Authority
WO
WIPO (PCT)
Prior art keywords
composite
resin
blend
silica
boron oxide
Prior art date
Application number
PCT/US2008/007667
Other languages
French (fr)
Inventor
William A. Clarke
Original Assignee
Flexible Ceramics, Inc. A California Corporation
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Flexible Ceramics, Inc. A California Corporation filed Critical Flexible Ceramics, Inc. A California Corporation
Priority to CN200880102632.1A priority Critical patent/CN101903429B/en
Priority to EP08768638.2A priority patent/EP2162478B1/en
Priority to JP2010513247A priority patent/JP5307804B2/en
Priority to US12/665,715 priority patent/US8293830B2/en
Priority to ES08768638T priority patent/ES2862460T3/en
Publication of WO2008156821A1 publication Critical patent/WO2008156821A1/en

Abstract

This invention relates to composites for use in high temperature elastic composite applications. Most particularly, this invention relates to elastic composites formed with a silanol-silanol condensation reaction mixture of silsesquioxane silicone resins thermally stabilized by boron nitride, silica and boron oxide additives as their matrix.The polymer matrix composite comprise a matrix of cured high, intermediate and optionally low molecular weight silicone resins including boron nitride and silica additives and reinforcing material.

Description

Silicone Resin Composites for High Temperature Durable Elastic Composite Applications and Methods for Fabricating Same
Related Application Data
The present application claims benefit from commonly owned, co-pending United States Application for Provisional Patent, Application No. 60/936,472, filed June 19, 2007. The present application is related to commonly owned co-pending applications, "Red Heat" Exhaust System Silicone Composite O-Ring Gaskets and Method for Fabricating Same,
Application No. , and Internal Combustion (IC) Engine Head Assembly
Combustion Chamber Multiple Spark Ignition (MSI) Fuel Savings Device and Methods of Fabrication Thereof, Application No. , each filed on even day herewith.
Background of the Discovery
1. Field of the Discovery
This invention relates to composites for use in high temperature elastic composite applications. Most particularly, this invention relates to elastic composites formed with a silanol-silanol condensation reaction mixture of silsesquioxane silicone resins thermally stabilized by boron nitride, silica and boron oxide additives as their matrix. When the composites are heat cured from 200 to 1000 0C the % recovery from 15% compression fatigue cycle testing for 10,000,000 cycles drops off with increasing cure temperature as shown in Figure 1. Additionally, when these same porous composites are vacuum impregnated with the resin blend; they endure the same 10,000,000 fatigue cycles with greater than 95% recovery also shown in Figure 1. The composites have endured over 4 years internal combustion (IC) engine pressurized severe exhaust manifold temperatures without seal leakage or burn through from exhaust gas at sustained and spike temperatures approaching 1000 0C. The composites have passed FAA fire penetration, burn through, heat release (< 10 kW/m2), smoke density and Boeing toxicity testing per BSS 7239.
2. Description of the Previously Published Art
The Beckley patent, US 5,552,466 is specific to teach methods of producing processable resin blends that produce high density silica ceramics in the red heat zone. The preferred catalyst,
- I zinc hexanoic acid produces a high cross-link density polymer by the Beckley methods of processing that favor the formation of high yield ceramic composites compared the high temperature elastic silicone polymers produced by the Clarke methods of using boron nitride, silica and a preferred boron oxide catalyst. No mention is made of compression-recovery properties common to Clarke related composites.
The Boisvert, et al. patent, US 5,972,512 is specific to teach silanol-silanol condensation cured methylsilsesquioxane resins enabling the fabrication of non-burning composites with superior performance than organic laminates. No mention is made of producing a high temperature elastic silicone containing boron nitride and silica to produce the fire resistant elastic silicone laminate that slowly transforms into a flexible ceramic then ceramic with no burn through at 20000F after 15 minutes. Also, the fire resistance is specific to methyl resins overlooking the high thermal advantages of phenyl resins even when used sparingly. Also, elastic composites have dissimilar materials joining advantages not mentioned in the Boisvert patent.
The Clarke patent, US 6,093,763 is specific to teach the use of the zinc hexanoic acid catalyst for a specific ratio of 2:1 for two specific silicon resins with boron nitride as filler. The zinc hexanoic acid catalyst produces a different high cross-link density polymer than the preferred elastic composite produced from a reaction mixture of boron nitride, silica and boron oxide and controlled reaction methods. The amount of zinc catalyst required to enable the sealant to perform is also excessive in comparison to the boron oxide catalyst which is sparingly used to favor a slow reaction for producing elastic composites.
The Clarke patent, US 6,161,520 is specific to teach that the gasket materials derived from Clarke's copending US patent applications Ser. Nos. 08/962,782; 08/962,783 and 09/185,282, all teach the required use of boron nitride as the catalyst for condensation polymerization of the resin blend needed to produce the gaskets. Clarke has verified that boron nitride is not a catalyst as incorrectly claimed. Clarke verified the certainty that boron nitride is not a catalyst by attempting to repeat the 873 patent's Figure 1 "gel" curve at 177°C using the preferred CERAC, Inc. item #B-1084- 99.5% pure boron nitride. Other research associates have also confirmed the certainty that boron nitride is not a silicone condensation catalyst. Numerous possible contaminates would need to be investigated to find the actual catalyst or combination of catalysts including the possibility of humidity. No mention of using boron nitride, silica and boron oxide as a reaction mixture processed in a rotating cylinder at ambient temperature to favor the production of a high temperature elastic composite. Neither is boron oxide mentioned as catalyst with boron nitride cost advantage addressed when boron oxide is used as a residual from the chemical processing (Reference 1) of boron nitride.
The Clarke patent, US 6,183,873 Bl is specific to teach the use of boron nitride as the catalyst in producing polysiloxane resin formulations for hot melt or wet impregnation of ceramic reinforcements. As stated above, boron nitride is not a catalyst as incorrectly claimed. The more costly and toxic hot melt and wet processing methods of the above described '873 patent are eliminated with the superior ambient temperature methods addressed by the inventor. No resin formulations using boron oxide as the catalyst (Table 6) are mentioned. Additionally, the methods of producing "flexible ceramic" high temperature elastic laminates are not addressed. Also, the use of laser processing (up to 16,5000C) to increase the tensile strength by 25% and form ceramic sealed edges is not addressed. The economical advantage of using residual boron oxide contained in boron nitride as a source for the catalyst addition is not mentioned.
The Clarke SAE 2002-01-0332 paper (Reference 2) refers to high purity boron oxide as a Lewis acid catalyst with silica mentioned as an unobvious inhibitor for these silicone condensation polymerization catalysts. High cost boron nitride and boron oxide are added separately. No mention is made of producing resin formulations using boron nitride containing boron oxide residues as a source of boron oxide catalyst and cost savings advantage. Additionally, the methods of producing "flexible-ceramic" laminates capable of high-temperature elastic recovery (Figure 1) are not addressed. Also, the use of laser processing (up to 16,5000C) to increase the tensile strength by up to 25% and forming ceramic sealed edges is not addressed. The "self extinguishing" property of the elastic composite when heat is removed is also not mentioned. This is an essential requirement to prevent combustion pre-ignition in superior fuel saving flexible ceramic composite ignition devices.
References Cited
U.S. Patent Documents 5,552,466 09/03/1996 Beckley et al.
5,972,512 10/26/1999 Boisvert et al.
6,093,763 07/25/2000 Clarke
6,161,520 12/19/2000 Clarke
6,183,873 02/06/2001 Clarke
Published References
1. Lenonis, D.A.; Tereshko, J. and CM. Andersen, Boron Nitride Powder-A High- Performance Alternative for Solid Lubrication, Advanced Ceramics Corporation, A Sterling Publication (1994).
2. Clarke, W.A.; Azzazy, M and West, R., Reinventing the Internal Combustion Engine Head and Exhaust Gaskets, Clarke & Associates, SAE PAPER. 2002-01-0332. (March 4, 2002) pp.2-3.
3. Thompson, Raymond, The Chemistry of Metal Borides and Related Compounds, reprinted from PROGRESS IN BORON CHEMISTRY, Vol. 2, Pergamon Press, (1969) p.200.
4. Thompson, ibid, pp 212-213.
5. Sorenson W.R. and W. T. Campbell, Preparative Methods of Polymer Chemistry, John Wiley & Sons, (1968) p.387.
6. Rochow, E. G., Chemistry of the Silicones, Second Edition, Wiley, (1951).
7. Thompson, ibid, p.217.
SUMMARY OF THE DISCOVERY
Objectives of the Discovery The inventor has evaluated (Reference 2) ceramic oxide catalysts (see Table 1) and found boron and aluminum oxide to be Lewis acid catalysts for ambient temperature activating silicone reactions with the unexpected inhibiting capability of submicron silica. Also, boron oxide is a common contaminant of boron nitride commercial production requiring costly leaching stages to remove it. Because of this significant cost savings advantage, it is the objective of this discovery to exploit the use of lower cost boron nitride containing residual boron oxide for catalyzing the resin reaction mixtures.
Table 1
Silicone Resin "Gel" Times Taken at 1770C When Catalyzed By B2O3 or Al2O3 and Inhibited by SiO2.
Parts by Weight
Figure imgf000006_0001
Both B2O3 and Al2O3 behave as Lewis Acids in facilitating the condensation reaction of the selected silicone resin formulation. The Al2O3 is twice as effective on a weight basis.
It is the further objective of this discovery to exploit the multipurpose advantages of boron oxide throughout all phase transformations of the resin blend from initial condensation polymerization to cured, pyrolyzed and ceramitized composite articles. Where boron oxide initially is used for dehydrating the silanol-silanol condensation reactions. The boron nitride also serves as a source (Reference 3) for boron oxide when it forms a stable oxidation protective boron oxide film at approximately 500+500C which is stable at red heat (600 to 10000C) until the vapor pressure of boron oxide becomes appreciable (Reference 4) above 12000C. The rate controlling step is at most temperatures, the diffusion of oxygen through the boric oxide surface film (Reference 4).The hot surface is "self extinguishing" when heat is removed - a significant advantage in preventing combustion engine chamber preignition. Boron oxide is also used in combination with alumina which is a more effective catalyst on a weight basis and silica which inhibits both catalysts allowing them to be used in greater quantities than would otherwise be possible.
It is the further objective of this discovery to design and prepare flexible and resilient composite materials which will perform at 5000C temperatures, i.e., 200 0C higher than those encountered (Reference 5) in the past while still retaining low temperature elastic sealing advantages. These materials are at the same time "preceramic" capable of producing high yield ceramics upon being pyrolyzed to 10000C.
It is the further objective of this discovery to design and prepare "flexible ceramic" composite laminates from the above elastic composite structures, where "flexible ceramics" are flexible elastic composite structures heat processed in localized regions of the structure to create part ceramic and part flexible elastic "hybrid" composite structures.
This same approach is also achieved in reverse by vacuum filling the less elastic high temperature porous elastic composites (see Figure 1) with the elastic resin blend then heat curing the resin to 1500C to assure the formation of a highly elastic resin within the less elastic matrix producing a set of hybrid elastic matrices composites capable (as revealed in Figure 1) of making elastic composites with highly durable % recovery of the higher heat cured porous composites.
It is the further objective of this discovery to produce essentially nontoxic, solventless resin blends from silicone condensation polymerization carried out at ambient temperature in equipment designed to allow the polymerization to start in excess acetone (sufficient to dissolve the flake resin) while continuously co-mingling the solid additives (boron nitride, silica and boron oxide) within the polymerizing resin reaction mass, thereby producing a thermally stable elastic resin blend for producing high temperature cured elastic composites. It is the further objective of this discovery to provide a practical method of utilizing the cured polymer porosity (see Figure 3) for providing a secondary sealant application as the composite silicone polymer material is compressed up to 15% of its thickness releasing the sealant as required at the sealing surface. The method discovered for filling the porosity in one operation is a thermal quench reducing the porosity from up to 12% to less than 1% in one operation.
It is the further objective of this discovery to provide a matrix resin densification method (see Figure 4) for filling the porosity produced when the organic material the polysiloxane resins is pyrolyzed away at temperatures greater than 3000C. High temperature cured composites will typically have porosity from 10 to 20% when pyrolyzed from 300 to 1000 0C which provides an opportunity to form hybrid elastic matrices and produce elastic composites such as shown in Figure 1 with high elastic capability depending on the desired final composite required performance temperature.
It is the further objective of this discovery to provide elastic composites with different ceramic sealed edges by selecting different composite reinforcements for laser cutting fabrication of the preferred ceramic edge.
It is the further objective of this discovery to enable the fabrication of composite polysiloxane flexible ceramic gaskets that can complete up to 325,000 miles endurance testing (150,000 mile requirement) in cab fleets (all testing undertaken under confidentiality agreement).
It is the objective of this discovery to enable the fabrication of discontinuous chopped fiber filled high temperature (up to 5000C) "liquid" gaskets that can perform up to 6,640 hours (testing undertaken under confidentiality agreement) on 460 V8 truck engine dynamometer testing. Similarly, helical overlapping "O" rings as shown in Figure 5 can be made.
It is the further objective of this discovery to enable IC engine ignition devices to be prepared as flexible ceramic structures embedded with electric circuits that enable multiple spark ignition combustion per chamber with up to 33% fuel savings (testing under confidentiality agreement). This invention extends the elastic range of silicone composite materials from the typically -40 to 300 0C to temperatures within the "red heat", i.e., up to 600 to 1000 0C range of applications. The polymer matrix composite comprises a matrix of cured high, intermediate and optionally low molecular weight silicone resins including boron nitride and silica additives and reinforcing material. When the resin blend is combined with reinforcement to make composites and heat cured from 200 to 1000 0C the % recovery from 15% compression fatigue (ASTM-F-36 Rev. 95) cycle testing for 10,000,000 cycles, drops off with increasing cure temperature above 500 0C. Conversely, these same porous composites (heat cured up to 750 0C) when "densification" processed with the resin blend; unexpectedly endure the same 10,000,000 fatigue cycles with greater than 95% recovery (see Figure l).The composites have endured over 4 years internal combustion (IC) engine pressurized severe exhaust manifold temperatures without seal leakage or burn through from exhaust gas at sustained and spike temperatures approaching 10000C. The composites have passed FAA fire penetration, burn through, heat release (< 10 kW/m2), smoke density and Boeing toxicity testing per BSS 7239.
Boron oxide is a multipurpose additive. The boron oxide dehydrates the silanol-silanol condensation reaction to produce elastic polymers with high thermal properties, while simultaneously, the boron nitride part of the additive reaction mixture combined with silica, enables the formation of a superior flexible elastic matrix within the reinforced polysiloxane composites which is not possible with silica alone or boron nitride alone up to 10000C (see Figure 2). From 300 to 1000 C the burn off of the organic matter of the precursor silicone resins affords the opportunity to create new elastic composites with hybrid elastic matrices made by densification processing the 10 to 20% porosity of the high temperature cured composites with the resin blend as shown in Figure 4.
When the composites are heat treated in localized regions of their structures, the heated regions become high yield (>90%) ceramic while the nonheated areas remain flexible. The pyrolyzed preceramic and ceramic regions' porosity has been filled in a rapid thermal quench with the high temperature elastic matrix impregnant and cured to the desired elastic's performance temperature. Alternatively, laser cut ceramic or refractory fiber reinforced elastic laminates produce flexible composites with ceramic sealed edges, called Flexible Ceramics™. Varying the ceramic fibers produces different ceramic sealed edges. The multifunctional catalyst used throughout is boron oxide which can be supplied as a residual constituent of commercial reaction produced boron nitride. This approach provides a significant cost savings in eliminating the costly leaching operations needed to remove the boron oxide.
The resin blend's processing capabilities include ambient temperature solventless prepreg processing, heat barrier material enabling multiplaten press "book stack" laminated parts to be laser cut in multiple stacks in one multiple part cost advantaged operation, thermal quench impregnating, laser cutting formation of ceramic sealed laminate edges, and resin infusion mold processing of large structures, silk screening multiple parts with raised coatings and identification marking.
Additionally, the resin blend's products include "O" rings, micro-rod filled sealants that can be "pyroformed" into high-temperature viscoelastic engineering gaskets, adhesives, surface and subsurface wear protective coatings, oxidation protective coatings, porosity stored compliant coatings, pressure activated fastener thread high temperature adhesives, Pyrex™ glass adhesives, high temperature computer boards and fasteners, electrical and heat insulators, and affordable up to 33% fuel saving devices.
Many prototype parts have been made which demonstrate (under confidentiality agreement testing) that most engine components of diesel, internal combustion (IC) and turbine engines that operate up to 10000C can be made into fiber reinforced superior high temperature elastic composites made with the resin blend. Examples include engine blocks, cylinder heads, engine gaskets, push rods, valves, pistons, brakes, multiple ignition fuel saving devices, turbine engine combustion liners, compression blades, diesel engine head and exhaust gaskets and rocket motors, fire walls, and high-temperature viscoelastic exhaust manifold, pipe, catalytic converter gaskets and sealants.
BRIEF DESCRIPTION OF THE DRAWING
Fig. 1 is a graph of laminate thickness recovery as a function of cure temperature;
Fig. 2 is a thermogravimetric scan of glass fiber filled polysiloxane laminate; Fig. 3 is graph of percent porosity as a function of post cure temperature;
Fig. 4 is a process for a silicone resin densification cycle; and
Fig. 5 is a graph illustrating pressure decay curves for flexible ceramic and multilayer steel gaskets.
DESCRIPTION OF THE PREFERRED EMBODIMENTS
Durability testing (under confidentiality agreement) of "flexible ceramic" internal combustion engine exhaust manifold gaskets has revealed that they can perform up to and exceeding 350,000 miles cab fleet durability testing (typical automotive requirement is 150,000 miles) with "spike" temperatures up to 500°C (932°F). Figure 1 shows the percent compression recovery is approximately 87% at 2000C and 63% at 4000C which is the exhaust gasket's clamping surface performance temperature.
To accomplish the above product performance, the resin blend additive materials are selected with high flexible and thermal resistant properties. The unique resin blend is typically mixed from three silicone resins and two or more ceramic additives. To accomplish the elastic compression recovery performance (see Figure 1) of composites made from the resin blend's "prepreg" several different composite elements are utilized, the most important being the resin blend composition and methods of processing. The resin blend is formulated from a high-molecular-weight "flake resin" and intermediate liquid silicone resin precursor and optionally a lower molecular weight silicone resin. These resins are selected to have different functionality such as listed in Table 2.
Table 2 (Reference 6)
Organosilicon preferred functionalities ( where R=methyl or phenyl):
(RSJOJ/TV silsesquioxane polymers, e.g., methylphenylsesquisiloxane
R^Si1OH, silanol (hydroxyl) terminated, polydimethylsiloxane, e.g., HOSiMe2O-(SiMe2O)n-
SiMe2OH, and
Me^SiO-. trimethylsilyl terminated, e.g.,Me3SiO-(SiMe2O)n-SiMe3, or Dimethylpolysiloxane polymers containing methyl or phenyl silsesquioxanes, with optional methoxy-termination, e.g., CH3O-(SiMe2O)n-
A variety of polysiloxane oligomers are well known in the art that exhibit similar functionality; however, the discovery's most preferred organic groups are the methyl or phenyl because of their high thermal stability.
A typical resin blend with the preferred additive systems is given in Table 3.
Table 3
Typical Resin Blend
Parts by Weight
Resin Blend Formulation In General Preferred
(1) Dimethylsiloxane polymers 40-70 65 containing phenyl silsesquioxanes
(2) Dimethylsiloxane polymers 5-25 10 containing methyl silsesequioxanes.
(3) silanol terminated, poly- 5-25 25 dimethylsiloxane
(4) boron nitride & residual boron oxide 5-40 20
(5) boron oxide content of (4) 0.1-1.2 0.40
(6) silica 3-15 6 or other filler such as silica gel or 3-15 silicon carbide or 15-25 alumina or silica fiber 15-25 reinforced polysiloxane rods
In Table 4, the formulation using preferred commercially available resins is set forth.
Table 4 Preferred Commercially Available Resins
- i i Parts bv Weight
Formulations Using GE Silicones Dow Corning Commercial Resins In General Preferred In General Preferred
(1) Dimethyl polymers 40-70 65 (SR 355) 40-70 65 (233) w/ phenyl silsesqui- (or 249) oxanes, high MW
(2) Dimethyl polymers 5-25 10 (TPR- 179) 10-60 35 (3037) w/ methyl silsesqui- covers items oxanes, methoxy (2) and (3) terminated
(3) Silanol terminated 5-25 25 (TPR- 178) Polymethylsiloxane
ADDITIVES
The preferred resin blend additives are silica and boron nitride retaining 2+1.0 wt% residual boron oxide. These additives provide high thermal capabilities.
Silica/Boron Nitride:
Silica was discovered by Clarke (Reference 2) to slow down the time it takes for the silicone resin reaction mass catalyzed by boron oxide to reach "gel" at 177°C (Tablet). Using this capability, the silicone reaction mass is slowly polymerized at ambient temperature in excess acetone favoring the formation of high molecular weight silicone polymers with high elastic increased linear chain (Si-O-Si) growth. Additionally, a mixture of silica and boron nitride added to the silicone resin reaction mass produces a superior flexible elastic polymer with high-temperature elastic properties than can not be produced using silica or boron nitride alone.
Silica alone will increase the polymer modulus causing it to become nonelastic above 3000C. Boron nitride alone at the suggested 16 wt% will produce an excessively plasticized soft low modulus weak polymer that will fail in interlaminar shear loading as a gasket. But when boron nitride and silica are in a 10/6 to 20/6 parts by weight ratio with 100 parts resin blend (Table 5) the elastic polymer produced by the boron oxide processing will become a thermally stable high-temperature flexible elastic polymer up to 5000C because the silica is increasing the modulus to compensate for the plasticizing effect of the boron nitride which is thermally stable as a lubricant to 85O0C (Reference 4).
Boron Nitride and Residual Boron Oxide
Boron nitride retaining 2.0+1.0 wt.% boron oxide is available from the Momentive Performance Materials (grade SAM- 140) and ZYP Coating (grade ZPG- 18 and -19) Companies who can selectively provide this preferred residual boron oxide and within the boron nitride from their commercial synthesis and leaching production operations. This aggregate boron nitride retaining 2% residual boron oxide is superior to high purity boron nitride (requiring a separate catalyst addition) in processing efficiency and cost advantage.
The residual boron nitride containing the residual boron oxide is typically added up to 20 parts by weight for every 100 parts resin as shown in Table 3. The submicron boron nitride containing residual boron oxide is then about 16 wt. % of the resin blend and silica is added at 4.8 wt. %.
Boron nitride is subject to hydrolysis which is negligible (Reference 7) from ambient to less than 1000C, but when the temperature exceeds 1000C; particularly in autoclave processing, the hydrolysis of boron nitride readily produces noxious ammonia which was observed by the inventor.
The hydrolysis of boron nitride is controlled by the following processing procedures:
(1) The boron nitride containing the residual boron oxide is purchased free of moisture or ammonia and sealed in containers with appropriate desiccant, typically CaCl2.
(2) The polymer reaction is staged under vacuum soak, so the press heat is restricted to less than the boiling point of water until the evolution of water is negligible, then the temperature is allowed to rise to 1500C where full pressure is applied.
Additionally, silica and boron nitride have been observed to unobviously heat stabilize the elastic phase of the resin blend when used in formulations such as shown in Table 5.
Table 5 Heat Evaluation of Elastic Resin Blend Formulations
Figure imgf000015_0001
Unique blending method, mixing with acetone then stripping the acetone
A unique method of mixing the resin formulation has been discovered. The method incorporates the least amount of anhydrous acetone necessary to dissolve the flake resin which is typically 25 parts added to the preferred formulation shown in Table 4. The method uses additive co-mingling and acetone stripping equipment (capable of recovering the acetone) combined together to assure the initial polymerization of the resin precursors incorporates the solid submicron additives uniformly throughout as the resin blend is slowly produced at ambient temperature.
This specialized equipment assures that the boron oxide catalyst contained in the boron nitride particulate can uniformly activate the dehydration of the Si-OH groups to form long chain siloxane bonds, Si-O-Si as the acetone is stripped away. In this process, dehydration probably takes place between the Si-OH groups on the silanol-terminated polysiloxane and residual Si-OH groups on the silsequioxane polymer, leading to polycondensation and the formation of an interpenetrating network. The acetone at 16% of the mixture is removed during the mixing down to approximately 1%.
During the resin blend mixing and stripping of acetone, it is checked for the "gel" reaction time which generally ranges from 2 to 10 minutes at 1770C. Adjustments can be made by adding boron oxide or silica as required, generally this is not necessary.
Prepreg
It is common practice in the art to calculate the values given in Tables 7a and 7b before setting up an impregnation production run to assure the prepreg produced will have the necessary composition needed to mold the final parts accurately to the desired molded finish laminate thickness. Excel spread sheets are commonly used for producing the Table 8 calculations revealing the range of laminate properties. Tables 7a and 7b provide examples of the calculated prepreg and molded laminate properties for two different fiber glass and ceramic fabrics common to the automotive and aerospace industries.
Tables 7a and 7b accurately predict the fabric reinforced polysiloxane composite cure ply thicknesses, tu calculated for S-glass 6781 and E-glass 1583 reinforcement of the resin blend's polysiloxane cured laminates. These tables also predict the cured laminate cure ply thickness, tL, at different levels of reinforcement composition as well as the required prepreg composition and weight, Wp , necessary to produce each laminate thickness.
The entire impregnation is carried out cost effectively at ambient temperature not requiring solvents or heat. Standard metering blade "over-roll" or high speed "reverse roll" impregnating equipment are used to impregnate the fabric. The fabrics can be any of the glass (E-glass, S-glass, quartz or chemically altered variations of these), Nextel® or refractory (e.g., zirconia) high temperature fibers or advanced composite graphite or pitch fiber weaves or styles provided by the textile industry. When using graphite or pitch fabrics, electro-less metal (such as nickel or aluminum) coated fibers are preferred for producing these advance composite polysiloxane matrix composites with high performance mechanical properties. Nickel oxide activates the silicone resin blends just as aluminum oxide assuring increased bond strength.
Table 7a
Laminate and Prepreg Material Composition of S-Glass, 6781 8HS Fabric Reinforced Polysiloxane Composites
Figure imgf000017_0001
Nomenclature tL Cure Ply Thickness WF Fiber Weight
VF Fiber Volume wR+f Resin + Filler Weight vF+f Fiber + Filler Volume Wp Prepreg Fabric Weight of vR+f Resin + Filler Volume 4"x4"=16in2(103.23cm2) Test Sample
Figure imgf000018_0001
Table 7b
Laminate and Prepreg Material Composition of E-Glass, 1583 8 HS Fabric Reinforced Polysiloxane Composites
Figure imgf000019_0001
For Nomenclature, please see Table 7a.
Figure imgf000019_0002
Figure imgf000020_0001
Table 8
Volume and Mass Calculations Forecasting Table 8 Press Cured Laminate Properties from Prepreg Formulations
Nomenclature
tF Cure ply thickness of fabric WR Weight of resin tL Cure ply thickness of laminate wf Weight of filler
Aw Areal weight of fabric W8N Weight of boron nitride
AF Area of fabric W5102 Weight of silicon dioxide
AL Area of laminate wL Weight of laminate
Ap Area of prepreg WP Weight of fiber
VF Volume of fibers Wp Weight of prepreg vR+f Volume of resin + filler WF+f Weight of fiber + filler vf Volume of filler />BN Density of boron nitride
V0 Volume of voids Ps,O2 Density of silicon dioxide
VL Volume of laminate />R+f Density of resin + filler
Volume of fiber + filler /JP Density of fiber Procedure and Calculations:
Figure imgf000021_0001
(2) VF % = (tF/ tL> 100%, where VL% = 100% for VF= (tF/ tL)- VL from AF = AL (premise)
(3) VR+f % = (VL - VF - V0)* 100%, where VL%= 100% and Vo% = 1 %
(4) VF+f% = [(VF + Vr )/ VJ* 100%, where VR+f = (W, + Wf)/pR+f, then VL= VR+f/(VR+f%/ 100%), Vp = V1. - VR+f and Vf = Ψm/pw+ Ws,O2/psiO2
(5) WF% = (WF/WL)» 100%, where WF= VF • pF and WL= WF+ Wf + WR
(6) WF+f%= [(WF + Wf )/ WL)]« 100%, where Wf = WBN + WSl02
(7) Wp= WF/(WF%/ 100%), where WF = Aw « Ap
Nylon fabric thermo-vaporization heat barrier for multiple stack laser cutting
The prepreg is processed into stacks of laminates (called "books") separated by unobvious layers of nylon fabric (e.g., style P2220 made by Cramer Fabrics, Inc.) peel ply which the inventor discovered through extensive laser testing will provide a thermo-barrier for multiple stack laser cutting. This allows multiple parts to be cut in one laser cutting operation without thermo-vaporizing the flammable top and edge of each stacked laminate at significant cost advantage.
Lamination processing of stacked fiber reinforced polvsiloxane prepreg.
Each ply of each prepreg layer is typically molded in a balanced architecture, e.g., 4-ply laminates for gaskets lmm thick are molded with a (0 , +60 ,-60 , 90 ) balanced architecture (Reference 2), where the warp yarns are arbitrarily selected as the 0° primary reference.
A typical multiple platen stacked laminate press molding cycle consists of an ambient applied preload, followed by a 10 minute vacuum soak, followed by a 30 minute heat cycle to 95°C which is held until the loss of water from the condensation reaction is negligible, then the heat cycle is continued to 1500C where full pressure of 200 psi is applied, followed by a 19O0C cure for 2 hours. The laminates are cooled down under pressure to 37°C, and then the platen pressure is reduced to preload, then ambient. After sufficient cooling, the book stacks are removed for multiple part laser cutting.
It has been observed by the inventor that the thickness of the composite laminate is the major cost and performance driver in making such products as automotive or aerospace gaskets. The laminate uniform thickness is the most critical quality control capability requirement for assuring high durability sealing of exhaust manifold gaskets operating at "spike" exhaust gas temperatures of 927°C. Pressure decay testing (Table 9) of laminate gaskets reveals the maximum thickness standard deviation should not be greater than ± 0.45 x 10° inches to assure extended durability. Laminates made to Table 7a composition requirements and molded to the above thickness standard deviation limits have performed well over 4 years in cab fleet testing (under confidentiality agreement) up to 325,000 miles (exceeding 150,000 mile test requirement).
Table 9
Decay in Exhaust Gas Pressure from 30 psi (measured in minutes)
Figure imgf000022_0001
Laser cutting of cured laminate book stacks
The laser cutting procedure uses a carbon dioxide laser with nitrogen purge that produces a ceramic sealed cut edge depending upon which ceramic fiber is used for the laminate reinforcement and the laser cut parts have up to 25% higher tensile strength compared to mechanically sheared parts. The following preferred carbon dioxide power settings are used to cut multiple stack laminates with up to 16,5000C focus point to vaporize the laminate's cut edge. The typical power set up for laser cutting book stacks of multiple laminate is: Carbon dioxide production laser cutting set up:
Focal length 7 inches ( 17.78 cm)
Beam diameter 0.6 inches (1.52 cm)
Laser wavelength 10.6 micron
Focal point diameter 0.124 inches (0.0315 cm)
Laser power 3500 watt
Laser Power/Area 4.5x 109 watt/m2
Temperature at focus 16,785 K ( 16,5100C)
The multiple stack laminate laser cutting is achieved for significant cost advantage by using the following unobvious materials and processes:
(1) A heat barrier nylon fabric is initially placed between laminates molded together in "book stacks"enabling the multiple laminates to be protected from interface thermo- vaporization.
(2) A nitrogen purge is applied to cover the cutting focus point at a 1.5mm nozzle gap expelling nitrogen gas at 142 psi from a 2mm nozzle orifice, and
(3) the preferred carbon dioxide power settings (shown above) are used to cut multiple stack laminates with a up to 16,5000C focus point that vaporizes the laminate stack as it is cut, but not the laminate interface protected by the heat protected nylon fabric separator peel plies. The power set up enables book stacks of 10 to 20 laminates to be laser cut at a time with higher cutting capacity if needed.
Compression — Recovery Fatigue Testing
When the laminates made from the resin blend are compressed under standard gasket bolt torque requirements they will typically compress 10% of their initial thickness. When surface coatings are added, the compressed thickness will increase to 12 to 15% depending on the type of surface coating. Table 7a reveals for an uncompressed cure ply thickness, tL of 0.267mm, a 10% compression to a t^ of 0.241mm will change the cured laminate reinforcement volume, VF+f , from 52% to 56% realizing a higher composite fiber restraining capability for mechanically assisted elastic recovery. The change in volume is primarily due to the collapse of the matrix and surface coating porosity from the applied bolt torque compression causing the matrix thickness change. This compressed reinforcement is responsible for restraining the compression load until the applied load is released.
The following mechanical properties are found for Table 7a laminates cured at 315°C:
Figure imgf000024_0001
Figure 1 reveals the laminate thickness recovery after 15% compression and 10,000,000 compression recovery cycles at different temperatures, e.g., at 2000C there is 87% recovery and approximately 63% recovery at 4000C. Also, the hotter the steel bolted aluminum clamped laminate joint becomes, the greater the anisotropic thermal expansion sealing pressure exerted by the trapped polysiloxane matrix. In contrast, at the minimum automotive engine design operating temperature of -400C, the elastic recovery of the matrix prevents cold start blow outs. Deep thermo-shock testing under pressures higher than exhaust manifold pressures is utilized to verify the thermal cycling capability.
Porosity Advantages
An important consideration revealed by Figure 3 and Table 7 is the important role that porosity plays in the performance of the flexible laminates. When the gaskets are initially molded an allowance of 1% porosity provides a fiber volume %, VF%, of 50.2% for a cure ply thickness, tL, of .0095 inches. Since there are 4 plies in a standard gasket which is lmm or 0.039 inches thick, the desired as compressed thickness is 0.039/4 = 0.010 inches. Allowing for 10% compression, the initial as molded thickness needs to be 0.039/0.90 = 0.043 with a ti, = 0.043/4 = 0.011 inches.
Figure 3 reveals the porosity created when the gaskets are cured at different temperatures. When first molded the cure temperature is 177°C with approximately 1% porosity, but after post cure at 4000C, the porosity is approximately 11%. The fiber + filler volume is approximately constant because the compression at 10% is absorbed by the 11% porosity minimizing lateral displacement of the matrix. Also, the porosity is produced in the cured polymer matrix and surface coatings. Table 7 reveals that the fiber + filler volume % , VF+f % , at tL of 0.011 inches is 54.9%. Table 10 reveals the unobvious discovery of using the porosity to store sealing surface sealant until the laminate is compressed 10% reducing the porosity from 11% to 1%. The porosity also reduces the degree of lateral displacement that would occur in the matrix if the porosity were not free to absorb the compression (see Table 10).
The porosity is filled with the densification resin blend made with Dow Corning 233 flake resin at 65 parts by weight added to 35 parts Dow Corning 3037 intermediate liquid resin to make up the 100 parts resin to which 20 parts boron nitride and 6 parts silica are added and mixed with the 25 parts acetone. Figure 4 reveals how this deep penetrating resin blend is used for densification.
Table 10 Porosity Absorbed Compression
Comment Cure Temp.°C tL (inches) vF+f % vR % Porosity, V0 % as molded 150 0.011 54.9 44. 1 1 post cure 400 0.011 54.9 34. 1 11*
10% compression Ambient 0.010 54/ .90 = 61 38 1
The porosity of 11% is filled with resin blend by thermally quenching the hot laminate from 2000C to ambient in the presence of resin blend in one operation, reducing the porosity to 1%. When the laminate is compressed the resin blend is displaced as clamping surface sealant. See Table 8 for tL, VF+f> VR and V0 Nomenclature.
Thermo-Ouench Processing
Additionally, fast thermal quench heat treat processes are used to impregnate pyrolyzed porous polymer or ceramic products, e.g., 12% porosity can be brought to less than 1% in one operation. This same thermal quench process is used to fast impregnate braid and twisted yarn rolls in one operation for producing rod reinforcement for high temperature liquid sealants or "O" ring seals. Essentially all Table 6 resin formulations can be thermal quenched from the last laminate cure temperature. The exception is when using rod filled resins for making "pyroformed" viscoelastic gasket type products.
Prototype Parts
Many prototype parts have been made (under confidentiality agreement) which demonstrate that most engine components of diesel, internal combustion (IC) and turbine engines that operate from 500 to 10000C can be made with fiber reinforced composites made with the resin blend. Examples include engine gaskets, push rods, valves, pistons, brakes, multiple ignition fuel saving devices, turbine engine combustion liners, compression blades, diesel engine head and exhaust gaskets and rocket motors, fire walls, and liquid exhaust gaskets and high temperature sealants.
-2s - Testing
Testing (under confidentiality agreement) has been extensive on IC engine dynamometers including cab fleet testing and deep thermal shock, steam testing of head gaskets and multispark ignition prototypes. Automotive, coolant, oil and combustion gas sealing has been tested and reviewed with major automotive companies (under confidentiality agreement) including fleet testing. Liquid exhaust gaskets and multiple ignition composite devices are recent developments which solves current costly pollution and fuel burning efficiency automotive IC engine CAFE standards capability requirements.
Fire protective testing of the inventions under FAA typical tests has proven the superior performance of the discoveries to pass the FAA major testing requirements for aircraft interior, cargo container, fire blankets and fire wall requirements. The composites have passed FAA fire penetration, burn through, heat release (< 10 kW/m2), smoke density and Boeing toxicity testing per BSS 7239.
Ford Crown Victoria 4.6 liter V8 engine FC and MLS exhaust manifold gaskets were comparison tested (under confidentiality agreement) using pressure decay measured from an initial 30 psi applied pressure with the gaskets bolted between aluminum and iron sealing surfaces using standard studs and lock nuts and placed within an oven at 3500C. The pressure decay curves shown in Figure 5 reveal that FC gaskets had essentially no leakage compared to the MLS gaskets which leaked severely. The FC exhaust gasket matrix material when used as an exhaust manifold sealant was also evaluated for a year (under confidentiality agreement) on Jasper Engine Company Generators powered with Ford 460 V8 truck engines. All engines performed without a problem for 6640 hours which is equivalent to 400,000 miles of truck engine durability. Cab fleet testing has confirmed the durability in performing over 350,000 miles in Crown Victoria 4.6 liter V8 engine exhaust manifold composite gasket testing.

Claims

CLAIMSWhat is Claimed is:
1. A silicone resin blend consisting of: a high molecular-weight (MW) "flake silicone resin;" an intermediate MW liquid precursor and optionally, a low MW liquid resin, e.g., 5000MW; submicron boron oxide/nitride aggregates as catalyst in a resin to aggregate weight ratio of 20/1 to 2.5/1, where the resin may be anyone or combination of resins and where the boron oxide content of the boron oxide/boron nitride aggregate is 0.5 to 5 wt.% of the boron oxide/nitride aggregate content, and a submicron refractory filler, e.g., submicron silica or finely divided silica gel.
2. The blend of the preferred item 1 resins wherein the flake resin is dimethylsiloxane polymers containing phenyl silsesquioxane units,.
3. The blend of the preferred item 1 resins, wherein the liquid intermediate MW silicone resin is selected from a group consisting of dimethylsiloxane polymers' with methyl silsesquioxanes-methoxy terminated and the liquid low MW silicone resin is selected from silanol terminated, polydimethylsiloxanes and mixtures thereof.
4. The blend of the preferred item 1 resins wherein the said flake and intermediate MW silsesquioxanes and polydiorganosiloxanes are selected from precursors containing cage-like molecular structures.
5. The blend of the preferred item 1 resins wherein the refractory filler is selected from a group consisting of submicron boron oxide/nitride aggregates, boron oxide (or acids thereof), boron nitride, silica, fumed silica, silica gel, diatomaceous earth, silicon carbide, alumina, zirconia and mixtures thereof.
6. The blend of the preferred item 1 resins wherein the refractory filler is provided in the form of partially cured ID and 2D refractory and ceramic fibers (e.g., silica, alumina, zirconia, S or E-glass, Nextel® fibers) reinforced polysiloxane composite micro-rods retaining elastic recovery as shown in Figure 1.
7. The blend of the preferred item 1 resins wherein the specifics of the preferred items 2, 3, 4, 5 and 6 have been incorporated.
8. The blend of the preferred item's 2 and 3 resins comprising in approximate parts by weight,
(1) dimethylsiloxane polymers containing phenylsilsesquioxanes 40-70,
(2) dimethylsiloxane polymers containing methylsilsesquioxanes- 5-25, methoxy terminated
(3) silanol terminated, polydimethylsiloxane 5-25,
(4) catalyst submicron aggregate boron oxide/nitride 5-40,
(5) boron oxide catalyst content of (4) at 2+1.0 wt. % 0.08-1.0
(6) silica (submicron) and other preferred item's 5 fillers. 3-15
9. The blend of the preferred item's 2 and 3, comprising in approximate parts by weight,
(1) dimethylsiloxane polymers containing phenylsilsesquioxanes 65
(2) dimethylsiloxane polymers containing methylsilsesquioxanes 10 methoxy terminated
(3) silanol terminated polydimethylsiloxane 25
(4) catalyst submicron aggregate boron oxide/nitride 20
(5) boron oxide catalyst content of (4) at 2+1.0 wt.% 0.3-0.5
(6) silica (submicron) and other preferred item's 5 and 6 fillers 6-20
10. We claim also from the resin blend claims 1 to 9, wherein the prepreg has 30 to 80 weight % reinforcement (see Tables 7a and 7b) and 20 to 50 weight percent resin plus filler content. And, the prepreg resin blend formulation has a specific gravity of 1.27±0.25 gm/cc.
11. A prepreg of claim 10 which when heat and pressure ( 100 to 300 psi) cured transforms to composite properties where the reinforcement volume percentage is 30 to 70% and the resin plus filler additive volume percentage is 35 to 75%. And the cured resin plus filler additive polymer matrix has a specific gravity of 1.33+0.25 gm/cc.
12. A prepreg of claim 10 wherein the solvent is less than 3% by weight, impregnates thick (0.015 to 0.020 inches) reinforcement (e.g., E-Glass 1583 and 3783 woven fabrics) at ambient temperature, and is essentially odorless and non-toxic at ambient temperature.
13. A prepreg of claim 10, wherein the resin blend forms: a) an elastomeric film at 1500C ( which in turn can be used to film impregnate reinforcement at ambient temperature on high speed 100 to 400 ft./minute "reverse- roll" film" impregnating equipment,
14. A composite comprising
(a) a reinforcement material of claim 11 at 30 to 70 volume percent and
(b) and the resin plus filler additive volume percent at 35 to 75%.
15 A composite of claim 11 which has a heat cured resin and filler additives' matrix at a specific gravity of 1.33+0.25 gm/cc.
16. A porous composite of claim 11, wherein the composite laminate thickness % recovery after 15% compression for 10,000,000 compression cycles per ASTM-F-36; Rev. 95, Procedure: "A" for Table 7a composites cured at different temperatures reveals a 87% recovery typically at 2000C and 63% recovery at 400 0C (see Figure 1 for porous cured composites).
17. An elastic nonporous composite of claim 11, wherein the composite laminate thickness % recovery after 17+2 % compression is 95+2 % after completing 10,000,000 compression-recovery fatigue cycles (ASTM-F-36 Rev. 95, Procedure "A") for Table 7b composite test specimens heat cured at 200 to 7500C (see Figure 1 for elastic non-porous composites). After heat cure these test specimens were vacuum impregnated (see Figure 4) with the resin blend at 65 parts Dow Corning 233 and 35 parts Dow Corning 3037, 20 parts BN and 6 parts silica and post cured for 30 minutes at 15O 0C.
18. A composite of claim 17, wherein test specimens have 96± 2 % recovery from 17+ 2 % compression after heat cure at 850 and 9500C and vacuum impregnation, but not yet fatigue tested.
19. The composite of claim 16, wherein the composite laminate fabricated from Table 7b composite materials has successfully completed 350,000 miles (150,000 mile test requirement) cab fleet durability testing (under confidentiality agreement) as exhaust manifold elastic compression-recovery gaskets assembled on Desert Cab Company's cabs with Ford 4.6 liter V8 Crown-Victoria engines. The test was essentially four years sealing of combustion exhaust gas at sustained 871 0C and spike 982 0C temperatures.
20. The composite of claim 11 assembled as a "liquid exhaust manifold gasket" filled with discontinuous E-glass fibers has successfully completed nine months testing at Jasper Engine Rebuilders over 6000 hours (the equivalent of 400,000 miles) dynamometer testing (under confidentiality agreement) on Ford 460 truck V8 co- generator engines fired with methane gas that fires hotter than common fuel (see claim 19 temperatures).
21. The composite of claim 19 wherein the composite when laser cut at 165000C forms a protective ceramic sealed edge around an elastic composite. With S-glass fabric reinforced composite's sealing edge is alumina, i.e., the type of reinforcement determines the ceramic sealed edge material.
22. The composite at 10000C has a ceramic yield of greater than 90% when cured into porous composites, but the composites form "flexible ceramics" when vacuum impregnated as described in claim 17.
23. A method of fabricating a composite comprising:
1) mixing the resin blend and additives within a rotating chamber from which the solvent is extracted as the reaction mass advances at ambient temperature.
2) impregnating the reinforcement at ambient temperature with the solvent-less resin
3) curing the prepreg by staging the preform at 1000C followed by heat/pressure cure. 4) optionally add vacuum impregnation per claim 17 to provide elastic non-porous composite
5) cut with laser at 16500 0C to provide final composite parts with ceramic sealed edges.
24. The resin blend of claim 1, wherein the catalyst is a conventional organometallic such as Zinc hexanoic acid or metal oxide such as alumina or preferably an oxide of boron added independently with boron nitride free of excess oxides of boron oxide.
25. The resin blend of claim 11 wherein the additive is a lubricant material selected from a group consisting of liquids, solid lubricants, micro-spheres, Teflon, molybdenum sulfide or mixers thereof with a preference for boron nitride.
26. The composite of claim 11, where the composite has passed FAA testing for fire penetration, burn-through, heat release, smoke and Boeing's toxicity testing.
27. The prepreg of claim 10, wherein the reinforcing material is selected from the group consisting of fillers, hybrids, discontinuous fibers, continuous fibers, partially cured chopped, composite rods reinforced with braid, twisted yarn and combinations thereof.
28. The prepreg of claim 10 wherein the reinforcing material is selected from the group of continuous fibers consisting of glass, carbon, pitch, pre-ceramic (silicon carbide, nitride etc.) vapor grown carbon fiber whiskers.
29. The method of fabricating of claim 23, wherein the resin blend is wet impregnated via solvent impregnated into the reinforcement or the resin blend is heated to hot-melt the resin into the reinforcement.
30. The resin blend of claim 1, wherein the refractory additives is selected from the group consisting of silicates, silica, silicon boride, calcium silicates, fumed silicas, reactor produced ceramic particulates such as boron carbide.
PCT/US2008/007667 2007-06-19 2008-06-19 Silicone resin composites for high temperature durable elastic composite applications and methods for fabricating same WO2008156821A1 (en)