WO1997032821A1 - Method of increasing the initial transmittance of optical glass - Google Patents

Method of increasing the initial transmittance of optical glass Download PDF

Info

Publication number
WO1997032821A1
WO1997032821A1 PCT/US1997/003100 US9703100W WO9732821A1 WO 1997032821 A1 WO1997032821 A1 WO 1997032821A1 US 9703100 W US9703100 W US 9703100W WO 9732821 A1 WO9732821 A1 WO 9732821A1
Authority
WO
WIPO (PCT)
Prior art keywords
transmittance
glass
hydrogen
optical glass
deuterium
Prior art date
Application number
PCT/US1997/003100
Other languages
French (fr)
Inventor
Nicholas F. Borrelli
Daniel R. Sempolinski
Thomas P. Seward, Iii
Charlene Smith
Original Assignee
Corning Incorporated
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Corning Incorporated filed Critical Corning Incorporated
Priority to EP97907924A priority Critical patent/EP0885176A4/en
Priority to JP9531834A priority patent/JP2000506117A/en
Publication of WO1997032821A1 publication Critical patent/WO1997032821A1/en

Abstract

The invention relates to optical glass having improved initial transmittance, formed by subjecting the glass to a hydrogen and/or deuterium treatment at a temperature, and for a duration of time sufficient to diffuse the hydrogen and/or deuterium into the glass.

Description

METHOD OF INCREASING THE INITIAL TRANSMITTANCE
OF OPTICAL GLASS
FIELD OF THE INVENTION
The invention relates to optical glass having high initial transmittance in the ultraviolet spectral region. This inventive glass is particularly useful as an optical material for optical applications in the deep ultraviolet region.
BACKGROUND OF THE INVENTION
In the past, it has been suggested that the resistance of fused silica to laser damage can be improved by treating such glass with hydrogen.. The treatments of these previous reports are intended to cause impregnation of high concentrations of molecular hydrogen into the fused silica as the degree of laser damage resistance in such samples is said to be related to the amount of molecular hydrogen doped into the glass. The effect of high concentration of the molecular hydrogen on laser damage resistance in fused silica is reported in numerous publications for example, in JP - Hei 6[1994]-166552; JP-Hei6[ 1994]- 166528; JP-A- 1-201664; JP-A-6-48734; JP-A-6-24979; JP-A-6-53593; U.S. Pat. 5,410,428; U.S. Pat. 3,220,814; and in co-pending, co-assigned US serial no. 08/422,104.
If fused silica is to be used as an optical material in optical applications in the deep UV, the internal transmittance of the glass at the use wavelengths must be as high as possible. For example, in applications such as lenses for microlithography stepper cameras, where the total path length in glass may be in the 20-50 cm range, an increase in transmittance of 0.01 %/cm is significant. Accordingly, it is the object of the present invention to produce fused silica glass having improved initial transmittance, and to provide a method for producing such glass.
SUMMARY OF THE INVENTION Briefly, the invention relates to a method of producing glass, particularly fused silica glass, having improved initial transmittance in the UV wavelength region.
In one aspect, the inventive glass is produced by reacting such glass with hydrogen and/or deuterium.
In another aspect, the inventive glass is produced by treating glass with hydrogen at such temperature and for a duration sufficient to cause the hydrogen to diffuse into the glass.
BRIEF DESCRIPTION OF THE GLASS Figure 1 shows the subtraction spectra of the reference glass sample (untreated), from those of two deuterium-treated samples;
Figure 2 is a subtraction spectrum of the reference glass sample from a deuterium-treated sample;
Figure 3 a is a graph comparing the transmittance of an untreated synthetic fused silica glass, with the transmittance of samples of the same glass, treated with deuterium at 350 °C;
Figure 3 b is a graph comparing the absorbance spectra of the glasses of Figure la;
Figure 4 is a graph comparing the infrared spectra of untreated glass with those of two samples treated with deuterium; Figure 5 is a graph of the change in absorbance versus the parts per million
(ppm) by weight OD formed; and
Figures 6a and 6b compare the absorbance spectra of untreated glass with those of the same glass treated after treatment with hydrogen at 600 °C.
DETAILED DESCRIPTION OF THE INVENTION
We have observed that hydrogen treatment of optical glasses resulted in increased transmittance of the glass in the UV wavelengths. In order to better understand how initial transmittance can be affected by hydrogen, this work was then repeated using deuterium. Deuterium was used for the experiments to obtain spectroscopic evidence for the mode of action of hydrogen. Low UV transmittance of fused silicas can in many cases be related to the presence of impurity metal ions and their charge compensating non-bridging oxygen ions in the glass. In many cases, the transmittance is not as high as it could possibly be because of the presence of these metal ion impurities which may be present in the raw materials, or which may become entrapped in the glass from the environment during the manufacturing process In silica glass, these metal ion impurities do not enter the glass silicon-oxygen network, but their electric charge is compensated by the occurrence of non-bridging oxygen ions in the silicon-oxygen network. These non-bridging oxygen ions also contribute to absorption in the deep ultraviolet and vacuum ultraviolet spectral regions. Thus, the resulting structures give broad absoφtions in the UV spectral range, thereby decreasing the glass transmittance.
Although details of the reaction are not fully understood, without intending to be bound by theory, the following may be proposed. The decrease in UV transmittance may be associated with a charge transfer-type absoφtion between the impurity metal ions and their non-bridging oxygen ligands, with their energy level difference lying within the energy band gap of the glass. Thus, one method of improving the transmittance of the glass is by reducing the charge transfer absoφtion between the metal ion impurities and the non-bridging oxygen in the glass.
The resulting reaction with hydrogen reduces the oxidation state of the metal ion impurities and converts the non-bridging oxygen into SiOH groups as described by the following equations:
s Si - O- + 1/2H7 > = SiOH + e
M+n + e > M"-1
where e" is an electron and M+n is an impurity metal ion such as Fe and other transition metal ions for examples.
The increased transmittance results because either or both (a) the lowering of the energy level of the OH species relative to the O" and (b) the raising of the energy level of the reduced species of the metal impurity ion. The ability to reduce will depend on the specific ion in question; for example, common multi-valent ions such as Fe3+ will be easier to reduce than Na+.
The amount of hydrogen and/or deuterium that can be diffused into the glass is dictated by the concentration in the ambient. The uniform concentration throughout the sample was assured by using the results of the diffusion equation with the diffusion coefficient of H2 in SiO2 given by:
D = (5.65 x 10-4) exp[-10.4/RT] where, D= coefficient of diffusion
R= 1.987 x 10-3 kcal/mol °K
T= temp, °K The duration of the treatment with hydrogen and/or deuterium is calculated by the following equation: t = L74D where, L=thickness of the glass; and D is as defined above to assure that 90% of the ambient concentration was present at the midpoint of the sample. The required amount of hydrogen and/or deuterium will depend on the number of impurity ions and non-bridging oxygen ions present in the given glass. There is no requirement for excess molecular hydrogen and/or deuterium.
We have found that the benefits to be derived from the present invention are greater for those glasses having large numbers of impurity metal ions and non-bridging oxygen ions, than for glasses having relatively fewer impurity metal ions and non- bridging oxygen ions. Since the incremental improvement in transmittance is relatively less for the latter, the ability to observe improvements in the transmittance of glasses having very few non-bridging oxygen and metal ion impurity defects, will depend on the sensitivity of the measuring instrument. Some high purity fused silica glasses contain a high concentration of =SiOH as a result of the glass making process employed in the production of these glasses. This high initial concentration of ≡SiOH makes it difficult to follow, spectroscopically, the formation of new ≡SiOHs resulting from the hydrogen treatment. The use of deuterium, however, makes it possible to determine the amount of ≡SiOD formed through the process. Increases in ≡SiOD can then be correlated to improvements in UV transmittance.
In order to make the estimate of SiOD concentration as quantitative as the estimate of SiOH, the following procedure can be performed. The absoφtion peak assigned to molecular deuterium, D2 is located at 2975 cm'1. We have previously found that molecular hydrogen can be identified in the infrared when it is in sufficiently high concentrations, at 4136 cm- 1. Using a theoretical isotope substitution ratio of 1.39, D2 should come at 2975 cm-1. Referring to Figure 1, for example, Example 1, this peak is found. The extinction coefficient of D2 is estimated to be that of H2, ~ 0.26 liters/mole cm, giving a final concentration of D2 in Example 3 as approximately 2.3 x IO19 molecules / cc SiO2. From the previous work, hydrogen concentration at this loading pressure is calculated to be 2.8 XI 019 molecules / cc SiO2. This excellent agreement suggests that the use of the SiOH extinction coefficients for estimating SiOD concentration is justified.
A thermal scrambling of D for H by the reaction
=SiOH + D2 > =SiOD + HD
can be ruled out as the source of =SiOD formed. This is determined by subtracting the overtone band of =SiOH (4520 cm-1) in the reference sample from the same band in the deuterated samples. This is illustrated in Figure 2 . As shown, there is no change in ≡SiOH concentration with high pressure deuterium treatment. The ≡SiOD found in the
IR experiment can then be related to the reaction of D2 with non-bridging oxygens, the result of which is seen in increased UV transmittance.
We have found that increases in initial transmittance (T0) are observed, for the most part, only when the glass has relatively low transmittance to begin with. The following examples were carried out using essentially 100% hydrogen and deuterium gases. However, suitable mixtures of hydrogen and inert gases such as argon or nitrogen, for example, 4% hydrogen and 96 % nitrogen, may also be used. Other gaseous reducing agents such as carbon monoxide can also be used Hydrogen and deuterium have the advantage that they can more readily be diffused into the glass to produce the desired reactions.
EXAMPLES The examples below verify the improvement of transmittance by hydrogen treatment and also describe the mechanism by which this improvement is achieved.
Example 1: In order to verify the improvement of initial transmittance by high pressure hydrogen treatment, two pieces of 1 X 1.5 X 2 cm fused silica containing about 900 ppm of OH were deuterium treated at 90 atm, and 350 ° C, for 24 days. UV spectra, IR spectra and IR spectral subtractions were then obtained for the deuterium- treated samples (Tl and T2), and compared with those of the untreated sample (RI). Figure 3 a shows the UV transmittance spectra of untreated glass and for the two deuterium treated samples, Tl and T2, from 180 to 220 nm. The spectra were normalized to give 100% transmittance at 220 nm. The transmittance of each sample at 193 nm were 0.9262 for reference sample RI, 0.9363 for the first deuterium-treated sample Tl, and 0.9397 for the second deuterium-treated sample, T2. From the UV curves and from the transmittance numbers it is seen that there is a small but measurable improvement in transmittance in the UV after deuterium treatment. Figure 3b show the spectra for all three samples in absorbance. As shown, the initial absorbance of the reference sample RI was 0.0329, compared to 0.0284 and 0.0269 for deuterium-treated samples Tl and T2 respectively. Figure 4 shows the infrared spectra from 5000 to 2000 cm-1 of the two deuterated samples and a reference glass (RI). For all the samples, the peak at high wavenumbers (-4520 cm-1) can be attributed to an overtone of an OH and =SiOH combination band. The strong band at about 3600 cm-1 is the =SiOH stretch, typically used for determination of OH concentration. The band at 4520 cm-1 can also be used to calculate SiOH in thick samples or samples with high OH content. The subtractions of the untreated reference glass from the deuterium treated glasses from 3200 to 2500 cm-1 are shown in Figure 1. The subtraction spectra clearly show the presence of a peak at 2720 cm-1. This peak is attributed to SiOD which is the result from the deuterium treatment of the glasses, by the reaction described above. The shift, at 2720 cm-1, agrees well with what would be expected from isotopic substitution ofH for D.
It is seen that the sample that exhibits a greater increase in initial UV transmittance also has more SiOD (sample T2). A plot of =SiOD vs. change in absorbance for the three samples is presented in Figure 5. The line shows a modest agreement of SiOD formation with increased UV transmittance.
The results of the increased transmittance with formation of SiOD are in accordance with the observation that glass having poor initial transmittance benefits more from hydrogen treatment than does glass having high initial transmittance.
Example 2: Hydrogen/deuterium impregnation of fused silica samples was carried out, at 600° C, 1 atm, for 48 hours. This time was chosen in accordance with the diffusion equation for hydrogen in silica at 600° C for a 1 cm thick piece. Vacuum UV spectra (Figures 6a and 6b), recorded before and after the low pressure hydrogen treatment show a significant increase in initial transmittance as a result of the treatment. As in Example 1 and Figures 1 through 5, we have again shown that initial transmittance is improved by hydrogen treatment. This result shows that high pressure hydrogen treatment is not necessary in order to improve initial UV transmittance in fused silica.
Also, in this example, samples of Corning glass codes 7940 and 7980 were subjected to 600° C, 48 hours, 1 atm hydrogen treatment. Table 1 compares the transmittance/cm of the glasses at 210 nm and 248 nm before and after this hydrogen treatment. Table 1. Transmittance/cm before and after hydrogen
210 nm 248 nm
Sample Before/After Before/After
1 86 7/90.0 90.0/91.7
2 79.5/89.9 84.5/91.4
3 80.1/90.2 86.4/91.9
4 89.7/90.4 91.4/92.0 5 86.6/89.3 90.2/91.4
6 82.0/88.7 88.0/91.4
7 81.5/87.3 88.6/91.6
8 84.4/86.9 88.3/89.7
Example 3. In this example, silica was made by the densification of a powder precursor and subsequently treated in hydrogen at 600° C as above. The ultraviolet transmittance of the glass was measured before and after hydrogen treatment. Transmittance/cm and hydroxyl content, as determined by infrared, of the sample before and after hydrogen treatment are shown in Table 2 below.
Table 2. Transmittance and OH of powder process glass.
210 nm 248 nm OH (wt, ppm)
Before 70.9 82.1 <1
After 76.0 88.9 4
The present invention can be applied to any glass intended for use in the ultraviolet range to improve the initial transmittance. In our preferred embodiment, the method is applied to fused silica produced from silicon tetrachloride or a halide-free polymethylsiloxane. Preferred polymethylsiloxanes include, hexamethyldisiioxane, polymethylcyclosiloxane, and mixtures of these. In one particularly useful embodiment, the fused silica is made from a polymethylcyclosiloxane such as, octamethylcyclotetra- siloxane, decamethylcylcopentasiloxane, hexamethylcyclotrisiloxane, and mixtures of these.
In addition to the embodiments discussed above, it will be clear to persons skilled in the art that numerous modifications and changes can be made to the above invention without departing from its intended spirit and scope.

Claims

CLAIMS:
1. Method of improving the transmittance of optical glass by treating the optical glass with a gas selected from the group consisting of hydrogen and deuterium.
2. The method of claim 1, wherein the transmittance is improved by subjecting the optical glass to the gas at a temperature and for a duration sufficient to cause the gas to diffuse into the optical glass.
3. The method of claim 1 , wherein the gas is hydrogen.
4. The method of claim 3, wherein the optical glass is 1 cm in thickness and is subjected to hydrogen at a temperature of 600 °C, and for duration of 48 hours.
5. The method of claim 3, wherein the optical glass is subjected to hydrogen at a pressure of 90 atm and a temperature of 350 °C.
6. The method of claim 1, wherein the optical glass is fused silica.
7. The method of claim 6, wherein the fused silica is formed from SiCl4.
8. The method of claim 6, wherein the fused silica is formed from a halide-free polymethylsiloxane.
9. The method of claim 8, wherein the polymethylsiloxane is selected from hexamethyldisiloxane, polymethylcyclosiloxane, and mixtures of these.
10. The method of claim 9, wherein the polymethylcyclosiloxane is selected from the group consisting of octamethylcyclotetrasiloxane, decamethylcylcopentasiloxane, hexamethylcyclotrisiloxane, and mixtures of these.
1 1. The method of claim 1, wherein the optical glass comprises metal ion impurities and non-bridging oxygens.
12. The method of claim 11, wherein the metal ion impurities comprise transition metal ions.
13. The method of claim 12, wherein the transition metal is iron.
14. The method of claim 11, wherein the optical glass is further characterized by a charge transfer absoφtion between the metal ion impurities and the non-bridging oxygen.
15. The method of claim 14, wherein the transmittance is improved by reducing said charge transfer absoφtion.
PCT/US1997/003100 1996-03-05 1997-02-28 Method of increasing the initial transmittance of optical glass WO1997032821A1 (en)