WO1996006118A1 - Cationic polymerization in carbon dioxide - Google Patents
Cationic polymerization in carbon dioxide Download PDFInfo
- Publication number
- WO1996006118A1 WO1996006118A1 PCT/US1995/010607 US9510607W WO9606118A1 WO 1996006118 A1 WO1996006118 A1 WO 1996006118A1 US 9510607 W US9510607 W US 9510607W WO 9606118 A1 WO9606118 A1 WO 9606118A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- carbon dioxide
- cationic polymerization
- reaction mixture
- monomers
- monomer
- Prior art date
Abstract
Description
Claims