USRE35246E - Layed photosensitive material and electrophotography comprising selenium, arsenic and tellurium - Google Patents

Layed photosensitive material and electrophotography comprising selenium, arsenic and tellurium Download PDF

Info

Publication number
USRE35246E
USRE35246E US08/171,000 US17100093A USRE35246E US RE35246 E USRE35246 E US RE35246E US 17100093 A US17100093 A US 17100093A US RE35246 E USRE35246 E US RE35246E
Authority
US
United States
Prior art keywords
arsenic
photosensitive material
selenium
layer
alloy
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Lifetime
Application number
US08/171,000
Inventor
Mitsuru Narita
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Fuji Electric Co Ltd
Original Assignee
Fuji Electric Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Priority claimed from JP62152255A external-priority patent/JPS63316059A/en
Application filed by Fuji Electric Co Ltd filed Critical Fuji Electric Co Ltd
Priority to US08/171,000 priority Critical patent/USRE35246E/en
Assigned to FUJI ELECTRIC CO., LTD. reassignment FUJI ELECTRIC CO., LTD. ASSIGNMENT OF ASSIGNORS INTEREST (SEE DOCUMENT FOR DETAILS). Assignors: NARITA, MITSURU
Application granted granted Critical
Publication of USRE35246E publication Critical patent/USRE35246E/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Abstract

A photosensitive material for electrophotography is provided, which comprises in sequence an electroconductive substrate, a carrier transport layer composed of a selenium-arsenic alloy, a carrier generation layer composed of a selenium-tellurium alloy and a surface coating layer composed of a selenium-arsenic alloy. The present invention further relates to a photosensitive material having a carrier transport layer that is doped with iodine as well.

Description

.Iadd.This application is a continuation of application Ser. No. 07/830,471, filed on Feb. 3, 1992 now abandoned, which in turn is a continuation of Reissue application Ser. No. 07/571,186 filed on Aug. 21, 1990 now abandoned. .Iaddend.
BACKGROUND OF THE INVENTION
The present invention relates to photosensitive material for electrophotography having a surface coating layer on a function-separation type multi-layered photosensitive structure for use in printers, digital copiers, and the like.
Conventional photosensitive materials for electrophotography include selenium type, OPC type, and so forth, and among them, the selenium type is excellent with respect to resolution power, durability, electric properties and circumstantial resistance. However, the drawbacks of using selenium lie in that it has sensitivity only up to about 550 nm, except for crystalline selenium which is panchromatic. Further the surface of selenium photosensitive material crystallizes even at a slight temperature elevation which makes the material unusable. In light of the above, various elements have been added to the photosensitive material to overcome such drawbacks.
For example, tellurium has been used as an additive in photosensitive materials. Although the addition of tellurium can increase the spectral sensitivity as well contribute to the suppression of crystallization, if the photosensitive material is intended to be sensitive to semiconductor lasers (800 nm), the amount of tellurium required becomes excessive due to reduction in the residual potential and increase in fatigue. Consequently, a surface coating layer (OCL) is added for suppressing the electrical charges from the surface. However, most of the materials used in such a coating layer, such as pure Se, OPC and 4 wt % As-Se alloy, have extremely low hardness and are inferior in printing resistance.
In the case of adding arsenic to the coating layer in order to increase the spectral sensitivity, heat resistance and sensitivity are improved as the amount of arsenic is increased. However, since the effective sensitivity region is only up to 700 nm, a coating layer containing arsenic is not suitable for semiconductor laser light sources with wave lengths at 800 nm.
The object of the present invention is to provide a photosensitive material for electrophotography capable of overcoming the foregoing problems, having sensitivity at long wavelengths and also excellent heat stability and printing resistance.
SUMMARY OF THE INVENTION
In accordance with the present invention, a photosensitive material for electrophotography is provided, which comprises in sequence an electroconductive substrate, a carrier transport layer composed of a selenium-arsenic alloy, a carrier generation layer composed of a selenium-tellurium alloy and a surface coating layer composed of a selenium-arsenic alloy. The present invention further relates to a photosensitive material having a carrier transport layer that is doped with iodine as well.
The surface coating layer comprising a seleniumarsenic type alloy has increased hardness compared to a layer comprising only selenium. High printing resistance can therefore be obtained with a selenium-arsenic alloy layer. Furthermore, a carrier generation layer composed of a selenium-tellurium type alloy having a high tellurium concentration can be used, which increases the sensitivity of the carrier generation layer to the semiconductor layer. In addition, use of a selenium-arsenic type alloy in the carrier transport layer makes it possible to prevent cracking of the surface coating layer due to differences in the heat expansion coefficients of the surface coating layer, having a small heat expansion coefficient (e.g. 2×10-5 K-1), and the carrier generation layer.
BRIEF DESCRIPTION OF THE DRAWINGS
FIG. 1 is a cross sectional view illustrating the layer construction of one embodiment of the present invention.
DETAILED DESCRIPTION OF THE INVENTION
The present invention relates to a photosensitive material for electrophotography, which comprises in sequence an electroconductive substrate, a carrier transport layer composed of a selenium-arsenic alloy, a carrier generation layer composed of a selenium-tellurium alloy and a surface coating layer composed of a selenium-arsenic alloy.
Referring to FIG. 1, the photosensitive material of one embodiment of the present invention comprises a carrier transport layer 2 composed of selenium-arsenic or selenium-arsenic-iodine alloy, a carrier generation layer 3 composed of selenium-tellurium alloy and a surface coating layer 4 composed of selenium-arsenic alloy laminated disposed in sequence on an electroconductive substrate 1 which is usually made of aluminum. Intermediate layers can be added selectively for the improvement of electrical characteristics between the substrate 1 and the carrier transport layer 2, between the carrier transport layer 2 and the carrier generation layer 3, or between the carrier generation layer 3 and the surface coating layer 4. Examples of such layers are described in commonly owned U.S. patent application Ser. No. 07/192,469 and Ser. No. 07/192,470 filed concurrently herewith which are incorporated herein by reference.
The preferred thickness of the surface coating layer 4 is from 0.5 to 10 μm. Although the layer should be as thin as possible to allow maximum incidental light to pass through the layer, the printing resistance of the layer must also be maintained. The concentration of arsenic in the surface coating layer 4 is preferably 5 to 40 atomic %. Greater than 40 atomic % arsenic (As2 Se3) decreases the hardness of the layer, and less that 5 atomic % arsenic may involve decreases the printing resistance. At 5 atomic % arsenic the printing resistance of the surface coating layer 4 is maintained for about 300,000 sheets.
The preferred thickness of the carrier generation layer 3 is 0.05 to 5 μm. If it is less than 0.05 μm thick, high temperature stability of the photosensitive material decreases and the sensitivity is reduced at longer wavelengths. However, if the thickness of the carrier generation layer 3 exceeds 5 μm, dark decay increases. The composition of the carrier generation layer 3 is preferably from 5 to 40 atomic % tellurium. Greater than 40 atomic % tellurium causes an increase in dark decay and promotes crystallization of the layer.
The thickness of the carrier transport layer 2 is preferably from 30 to 80 μm in view of the surface potential or electric field. The arsenic concentration in the carrier transport layer 2 is preferably from 5 to 40 atomic % to maintain crystallization resistance and high temperature stability. If the arsenic concentration is increased to 40 atomic % in the surface coating layer 4 in order to increase the printing resistance, the arsenic concentration in the carrier transport layer 3 should be restricted to 30-40 atomic % arsenic to prevent cracking at high temperatures. However, if such photosensitive material is used for a high speed printer in which the time from exposure to development is approximately 100 μsec, since the running time in the film becomes more than 100 nsec, the effective sensitivity is reduced. In order to eliminate such a drawback, it is effective to dope the carrier transport layer 2 with iodine, thereby shortening the running time. If the amount of iodine exceeds 10,000 ppm, the dark decay is markedly increased and the surface charge density is decreased. If less than 100 ppm iodine is emplolyed, there is no substantial effect.
Each of the layers inevitably contains impurities that cannot be removed or need not be removed.
EXAMPLE 1
A photosensitive material for electrophotography was prepared in the following manner. First, an aluminum pipe of 242 mm diameter and 450 mm length was cleaned and fixed to a rotary support shaft of an evaporation device as the substrate, and maintained at a temperature of about 190° C. The evaporation device was evacuated down to a pressure of 1×10-5 torr. Then, an evaporation source incorporating (As2 Se3) alloy was heated to about 400° C. and a carrier transport layer was vapor deposited on the substrate having a film thickness of about 60 μm. Then, flash evaporation was used to vapor deposit Se/Te alloy of 34 atomic % Te as the carrier generation layer, so that the photosensitive material would have a spectral sensitivity at long wavelengths. The layer was vapor deposited to a thickness of about 0.5 μm while the temperature of the substrate axis was held at 60° C., the pressure in the evaporation device was held at 1×10-5 torr and the temperature of evaporazation source was 350° C. An intermediate layer of about 0.4 μm thickness with a graduated Te concentration was disposed between the carrier generation layer and the carrier transport layer so that carriers generated in the carrier generation layer would be smoothly transferred to the carrier transport layer. Then, As/Se alloy of 38 atomic % arsenic was vapor deposited to a thickness of about 2 μm of the carrier generation layer. This formed the surface coating layer.
EXAMPLE 2
A photosensitive material was prepared in the same manner as Example 1, except that the carrier transport layer was doped with 5000 ppm of iodine.
EXAMPLE 3
A photosensitive material was prepared in which just as As2 Se3 layer approximately 63 μm thick was formed on the aluminum substrate.
EXAMPLE 4
For comparison, a photosensitive material was prepared in the same manner as Example 1, except that the surface coating layer was composed of 4 atomic % arsenic with a thickness of approximately 2 mm.
The test results for the four photosensitive materials of Examples 1 through 4 are shown in Table 1, wherein o represents a good result, Δ represents some loss of quality and x an unacceptable result.
              TABLE 1                                                     
______________________________________                                    
                                  Printing                                
                         Spectral (Circum-                                
                                         Over-                            
Photo-  Layer    Hard-   sensitivity                                      
                                  ferential                               
                                         all                              
sensitive                                                                 
        constitu-                                                         
                 ness    (wavelength                                      
                                  speed 780                               
                                         estima-                          
material                                                                  
        tion     (HV)    (780 nm) mm/sec)                                 
                                         tion                             
______________________________________                                    
Example 1                                                                 
        Se/As-   150     ∘                                    
                                  Δ                                 
                                         Δ                          
        Se/Te-                                                            
        Se/As                                                             
        (38%)                                                             
Example 2                                                                 
        Se/As/I- 150     ∘                                    
                                  ∘                           
                                         ∘                    
        Se/Te-                                                            
        Se/As                                                             
        (38%)                                                             
Example 3                                                                 
        Se/As    150     ×  ×                                 
                                         ×                          
Example 4                                                                 
        Se/As-   60      ∘                                    
                                  Δ                                 
                                         ×                          
        Se/Te-                                                            
        Se/As                                                             
        (4%)                                                              
______________________________________                                    
As shown in Table 1, the photosensitive materials of Examples 1 and 2 according to the present invention and the photosensitive material of the comparative Example 4 has sufficient sensitivity at long wavelengths. The photosensitive materials of Examples 1 and 2 and the photosensitive material of the comparative Example 3 has high hardness and printing resistance. Furthermore, in the test using an actual printer of 100 msec from exposure to development corresponding to high speed response, the photosensitive materials of Examples 1 and 2 and the photosensitive material of Example 4 were satisfactory and they were particularly excellent with respect to the density contrast.

Claims (2)

    I claim: .[.1. A photosensitive material for electrophotography, which comprises in sequence
  1. coating layer is from 5 to 40 atopmic %..]. 6. .[.The.]. .Iadd.A .Iaddend.photosensitive material for electrophotography which comprises in sequence:
    (a) an electroconductive substrate;
    (b) a carrier transport layer composed of a selenium-arsenic .[.ally.]. .Iadd.alloy .Iaddend.comprising .[.5.]. .Iadd.30 .Iaddend.to 40 atomic % arsenic;
    (c) a carrier generation layer composed of a selenium-tellurium alloy comprising 20 to 40 atomic % tellurium; and
    (d) a surface coating layer composed of a selenium-arsenic alloy comprising .[.5 to.]. 40 atomic % arsenic.Iadd., wherein the composition of the selenium-arsenic alloy in the carrier transport layer prevents cracking of the surface coating layer due to differences in the heat expansion coefficients of the surface coating layer and the carrier generation
  2. layer.Iaddend.. .[.7. The photosensitive material according to claim 6, wherein the carrier transport layer also contains from 100 to 10,000 ppm iodine..]. .[.8. The photosensitive material according to claim 1, wherein the concentration of arsenic in the carrier transport layer is at such a level to maintain crystallization resistance and high temperature stability..]. .[.9. The photosensitive material according to claim 8, wherein the concentration of tellurium in the carrier generation layer is not so high as to cause an increase in dark decay and promote crystallization of the layer..]. .[.10. The photosensitive material according to claim 9, wherein the concentration of arsenic in the surface coating layer is not so high as to decrease the hardness of the layer..].
US08/171,000 1987-06-18 1993-12-21 Layed photosensitive material and electrophotography comprising selenium, arsenic and tellurium Expired - Lifetime USRE35246E (en)