TWI926552B - 隱形眼鏡保存溶液和隱形眼鏡的製作方法 - Google Patents

隱形眼鏡保存溶液和隱形眼鏡的製作方法

Info

Publication number
TWI926552B
TWI926552B TW113149200A TW113149200A TWI926552B TW I926552 B TWI926552 B TW I926552B TW 113149200 A TW113149200 A TW 113149200A TW 113149200 A TW113149200 A TW 113149200A TW I926552 B TWI926552 B TW I926552B
Authority
TW
Taiwan
Prior art keywords
polymer
lens
contact lens
contact
buffer
Prior art date
Application number
TW113149200A
Other languages
English (en)
Other versions
TW202626984A (zh
Inventor
許偉航
游主依
鄭堯聰
許惠雯
Original Assignee
望隼科技股份有限公司
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 望隼科技股份有限公司 filed Critical 望隼科技股份有限公司
Priority to TW113149200A priority Critical patent/TWI926552B/zh
Priority to CN202510178592.4A priority patent/CN120040899A/zh
Priority to JP2025060273A priority patent/JP2026106361A/ja
Priority to US19/172,272 priority patent/US20250270399A1/en
Priority to EP25204623.0A priority patent/EP4763234A1/en
Application granted granted Critical
Publication of TWI926552B publication Critical patent/TWI926552B/zh
Publication of TW202626984A publication Critical patent/TW202626984A/zh

Abstract

本發明提供一種隱形眼鏡保存溶液,適於讓鏡片核心本體浸泡,並於鏡片核心本體浸泡於隱形眼鏡保存溶液時進行滅菌步驟,隱形眼鏡保存溶液包含第一聚合物與第二聚合物,第一聚合物包括聚乙烯醇,第二聚合物包括聚乙烯吡咯烷酮。本發明另提供一種隱形眼鏡的製作方法。

Description

隱形眼鏡保存溶液和隱形眼鏡的製作方法
本發明是有關一種隱形眼鏡保存溶液和隱形眼鏡的製作方法。
軟性隱形眼鏡(Soft contact lens)材質從1960年代開始引入,由於材質柔軟解決了原本硬式隱形眼鏡(RGP Lens)在配戴上常有的不舒適感,原本不適應硬式隱形眼鏡的使用者可以轉為使用軟性隱形眼鏡,軟性隱形眼鏡因此成為現今隱形眼鏡使用者的主要選擇。
雖然軟式隱形眼鏡相比硬式隱形眼鏡已經柔軟舒適許多,但仍有許多使用者反應軟式隱形眼鏡配戴時感覺有東西在眼睛裡,這也促使這些使用者放棄使用隱形眼鏡。造成上述問題的主要原因是隱形眼鏡表面具有摩擦力,因此眨眼時鏡片在眼球上移動並且摩擦眼球,導致使用者感覺到有東西在眼睛裡。因此,增加鏡片表面潤滑度可以解決上述問題。
有許多研究投入在使鏡片表面被包覆聚丙烯酸(PAA),已達到表面潤滑的效果。然而,PAA屬於負電性質的聚合物(anionic polymer),本身傾向帶負電荷(negative charge),其性質容易被淚液中的酸鹼值影響,可能導致佩戴上有刺激性的問題。後續研究揭露了以帶有正電性質的聚合物(cationic polymer)去中和PAA的電性,目的在於改善上述的技術的穩定性,但這樣的方式在製程上需要投入大量的管控成本,且產品無法穩定保持長時間配戴的潤滑效果。
鑒於上述問題及技術發展,本發明提出一種可以有效增加隱形眼鏡表面潤滑度的方法,且該效果可以長期維持,同時具有成本競爭力的技術方案。
除非另有定義,本文中使用的所有技術和科學術語具有與本發明所屬技術領域具有通常知識者通常理解的相同含義。一般而言,本文所使用的命名法和實驗室程序是本領域眾所周知且普遍採用的。常規方法用於這些過程,例如本領域和各種一般參考文獻中提供的那些。當術語以單數形式提供時,發明者也考慮該術語的複數形式。本文所使用的命名法和下文所描述的實驗室程序是本領域眾所周知且普遍採用的。如本揭露全文所使用的,除非另有說明,否則以下術語應被理解為具有以下含義。
鏡片乾片(dry lens):指在生產隱形眼鏡過程中,已完成固化(curing),還未進行水化(hydration)的鏡片。
鏡片濕片(wet lens):指在生產隱形眼鏡過程中,已完成水化(hydration)的鏡片。
隱形眼鏡保存溶液:指在生產隱形眼鏡過程中,跟隨鏡片濕片一起經歷滅菌製程的水溶液,且經過滅菌製程形成的隱形眼鏡通常會繼續保存於該水溶液中,故該水溶液又稱之為隱形眼鏡保存溶液。此外,該水溶液通常具有緩衝功能(buffering function),即具有一定範圍內的酸鹼值(pH值)及滲透壓。因此,在本文中也用緩衝液指稱隱形眼鏡保存溶液。
鏡片核心本體(core lens body):指鏡片組成來自於鏡片配方(contact lens formulation)經過固化(curing)形成的部分。鏡片核心本體可以是鏡片乾片或鏡片濕片。本發明所列舉的部分實施樣品不具備外殼層(shell layer)。
外殼層(shell layer):指鏡片核心本體已經形成之後,才再固化以後的其他製程形成於鏡片核心本體的表面,但並非原本已形成之鏡片核心本體的結構,同時藉由形成類似互穿聚合物網路結構的穩定結構,外殼層可以穩定存在鏡片核心本體的表面。
互穿聚合物網路結構(interpenetrating polymer networks,IPNs):一般理論上定義互穿聚合物網路結構是包含兩種或多種聚合物,其中至少一種聚合物屬於交聯的聚合物網路結構,同時在聚合物尺度上至少兩種或多種聚合物有部分交錯但彼此之間並未形成共價鍵結(covalent bond)的聚合物網路。例如,聚合物A本身屬於交聯的聚合物網路結構,而聚合物B又與聚合物A有部分交錯,但聚合物A及聚合物B之間並未形成共價鍵結,則可稱聚合物A與聚合物B形成互穿聚合物網路結構。考量到聚合物及化學領域的複雜性,本發明中使用的互穿聚合物網路結構指稱的對象,不同的聚合物在形成互穿聚合物網路結構的過程及結果,允許發生共價鍵結。例如,在本發明揭露的案例,不排除有少量(少於0.1wt%)第一聚合物與鏡片核心本體的聚合物發生共價鍵結。為方便表達,發明人依然以互穿聚合物網路結構來描述於鏡片核心本體表面上第一聚合物與鏡片核心本體之聚合物所形成的部分交錯的聚合物網路。而外殼層中屬於第一聚合物與第二聚合物糾纏(entanglement)形成的聚合物結構,則以類似互穿聚合物網路結構的穩定結構稱呼,因為在該聚合物結構中,第一聚合物自己的聚合物鏈(polymeric chain)並未有明顯的交聯發生,第二聚合物自己也並未有明顯的交聯發生,只是第一聚合物在第一聚合物的聚合物鏈之間有很強的氫鍵(hydrogen bond),同時第一聚合物與第二聚合物的聚合物鏈之間也有很強的氫鍵,因此形成類似互穿聚合物網路結構的穩定結構,因此本發明不直接用互穿聚合物網路結構去描述第一聚合物跟第二聚合物在外殼層中形成的網路結構,以盡可能貼近一般理論上的定義。
半互穿聚合物網路結構(semi interpenetrating polymer network,Semi-IPN) :一般理論上定義特別指在互穿聚合物網路結構中,至少一種聚合物屬於線性聚合物。本發明所述之互穿聚合物網路結構可包含半互穿聚合物網路結構。
同步互穿聚合物網路結構(simultaneouslyinterpenetrating polymer network,Simultaneous-IPNs,SINs):一般理論上定義特別指互穿聚合物網路結構的形成來源於兩種或多種聚合物之組成單元在各自產生聚合反應時產生。例如一個互穿聚合物網路結構由聚合物A及聚合物B組成,聚合物A是由單體a經過聚合反應形成,聚合物B是由單體b經過聚合反應形成。若將單體a與單體b混合,再將該混合物進行聚合反應,則最終形成的聚合物A及聚合物B的互穿聚合物網路結構即可能是同步互穿聚合物網路結構。在本發明中涉及的互穿聚合物網路結構例如不包含同步互穿聚合物網路結構。
本發明提供一種隱形眼鏡保存溶液,適於讓鏡片核心本體浸泡,並於鏡片核心本體浸泡於隱形眼鏡保存溶液時進行滅菌步驟,隱形眼鏡保存溶液包含第一聚合物與第二聚合物,第一聚合物包括聚乙烯醇,第二聚合物包括聚乙烯吡咯烷酮。
本發明提供一種隱形眼鏡,包含一個鏡片核心本體(core lens body)與一個外殼層(shell layer),外殼層包覆鏡片核心本體。其中,外殼層包括至少兩種聚合物:第一聚合物及第二聚合物。
本發明使用的第一聚合物是包含聚乙烯醇(Polyvinyl alcohol)結構之聚合物。第一聚合物可以是聚乙烯醇,或是聚乙烯醇及聚醋酸乙烯酯的共聚物(PVA-PVAc copolymer),或是此兩者的混合物。其中,第一聚合物可以是可交聯的或不可交聯的。聚乙烯醇及聚醋酸乙烯酯的共聚物可以是嵌段共聚物(block copolymer),也可以是輪替共聚物(alternative copolymer),也可以是隨機共聚物(random copolymer),也可以是連枝共聚物(graft copolymer)。聚乙烯醇可以是可交聯的或不可交聯的。聚乙烯醇可以是完全水解的(fully hydrolyzed),即完全水解聚乙烯醇(fully hydrolyzed PVA),也可以是部分水解的(partially hydrolyzed),即部分水解聚乙烯醇(partially hydrolyzed PVA)。其中部分水解聚乙烯醇較佳。分類上來說,部分水解聚乙烯醇亦可以理解為是一種聚乙烯醇及聚醋酸乙烯酯的共聚物(PVA-PVAc copolymer),因為其聚合物鏈段上同時具有乙烯醇及醋酸乙烯酯兩種單元。進一步來說,完全水解聚乙烯醇即為組成上100%都是乙烯醇單元的聚乙烯醇;而部分水解聚乙烯醇,例如水解程度為80%的部分水解聚乙烯醇,代表含有80%的乙烯醇單元以及20%未水解的醋酸乙烯酯單元。在本發明的詞彙表達上,部分水解聚乙烯醇可與聚乙烯醇及聚醋酸乙烯酯的共聚物兩種詞彙可以指相同的對象,兩種詞彙可以互換使用。
在本發明中,第一聚合物以部分水解聚乙烯醇較佳。其中,部分水解聚乙烯醇的水解程度(degree of hydrolysis)較佳的範圍是70%~99%,更佳的範圍80%~98%,更佳的範圍是88%~95%。本發明發現適當的聚乙烯醇水解程度,可以增加其與鏡片核心本體表面的聚合物形成互穿聚合物網路結構(interpenetrating polymer network)的穩定性,同時也可以增加第一聚合物在外殼層中與第二聚合物形成互穿聚合物網路結構的穩定性。部分水解聚乙烯醇效果可以優於完全水解聚乙烯醇的原因在於:完全水解聚乙烯醇的分子內氫鍵較強,容易導致完全水解聚乙烯醇相對不容易進入到鏡片核心本體(聚合物)的表層結構中,不容易與鏡片核心本體(聚合物)形成互穿聚合物網路結構;同理,完全水解聚乙烯醇因為分子內氫鍵較強的緣故,較不容易與包含聚乙烯吡咯烷酮的第二聚合物形成分子間氫鍵。因此,與部分水解聚乙烯醇相比,完全水解聚乙烯醇較不容易與第二聚合物形成類似互穿聚合物網路結構。
第一聚合物的分子量(Mw)較佳的範圍是5,000~300,000Da,更佳的範圍是10,000~200,000Da,更佳的範圍是15,000~150,000Da,更佳的範圍是25,000~100,000Da。
本發明使用的第二聚合物是包含聚乙烯吡咯烷酮(Polyvinyl pyrrolidone)結構之聚合物。第二聚合物可以是聚乙烯吡咯烷酮,或是包含聚乙烯吡咯烷酮的共聚物,或是此兩者之混合物。其中,第二聚合物可以是可交聯的或不可交聯的。其中,包含聚乙烯吡咯烷酮的共聚物可以是乙烯基吡咯烷酮及甲基丙烯酸二甲胺基乙酯的共聚物(Poly(vinylpyrrolidone)-co-(dimethylaminoethylmethacrylate),具體的範例可以是Ashland Inc.販售的產品如Copolymer 845、Copolymer 937或Copolymer 958。上述乙烯基吡咯烷酮和甲基丙烯酸二甲胺基乙酯的共聚物的分子量例如大於或等於100,000Da,更優的上述乙烯基吡咯烷酮和甲基丙烯酸二甲胺基乙酯的共聚物的分子量例如大於或等於1,000,000Da。
第二聚合物的分子量(Mw)較佳的範圍是大於或等於8,000 Da,更佳的範圍是大於或等於100,000 Da,更佳的範圍是大於或等於160,000 Da,更佳的範圍是大於或等於360,000 Da。上述的第二聚合物分子量範圍可以形成較有效的外殼層。當第二聚合物分子量不夠大,很難與第一聚合物形成有效的外殼層,推測可能是第二聚合物分子量不夠大時,雖然仍能與第一聚合物形成類似互穿聚合物網路結構,但第二聚合物會因為分子量小容易在該結構中進行移動,導致外殼層穩定性不足。
在鏡片核心本體及外殼層交界處,有第一聚合物跟鏡片核心本體的聚合物結構形成互穿聚合物網路結構。在外殼層中的大部分區域,第一聚合物與第二聚合物之間形成類似互穿聚合物網路結構的穩定結構。
在鏡片核心本體及外殼層交界處,有第一聚合物跟鏡片核心本體的聚合物結構形成互穿聚合物網路結構,該互穿聚合物網路結構中,一部分的第一聚合物屬於可自由移動的聚合物,另一部分的第一聚合物之間則形成穩定的鍵結(bonding),該鍵結使上述互穿聚合物網路結構穩定。該鍵結的形成主要來自於隱形眼鏡在滅菌(autoclave)製程中,因為高溫高壓,使聚乙烯醇之間產生穩定的氫鍵鍵結(hydrogen bond)。因此在外殼層在跟鏡片核心本體接觸的部分,主要由第一聚合物構成,而外殼層在遠離鏡片核心本體的部分,主要由第二聚合物構成。在外殼層的大部分區域中,第一聚合物與第二聚合物之間形成類似互穿聚合物網路結構的穩定結構;其中,有部分的第一聚合物屬於可自由移動的聚合物,有部分的第二聚合物屬於可自由移動的聚合物,有部分的第一聚合物之間形成穩定的鍵結,該鍵結使該類似互穿聚合物網路結構穩定。該鍵結的形成主要來自於隱形眼鏡在滅菌製程中,聚乙烯醇及聚乙烯醇之間產生穩定的氫鍵(hydrogen bond);同時,聚乙烯醇也能與聚乙烯吡咯烷酮之間產生穩定的氫鍵,主要來自於聚乙烯醇上的羥基(hydroxyl group)與聚乙烯吡咯烷酮上的氧原子(oxygen atom),因此整個外殼層結構可以相對穩定,維持使用者配戴過程的舒適度。
更進一步說明,控制第一聚合物中醋酸乙烯酯的比例(亦即部分水解聚乙烯醇的水解程度)可以明顯影響形成外殼層的效果。聚乙烯醇結構本身帶有較強的結晶性,若第一聚合物的結晶性太強,則在形成外殼層之前,第一聚合物無法有效進入到鏡片核心本體的表層結構中,造成第一聚合物無法和鏡片核心本體的表層結構形成半互穿聚合物網路結構,自然也無法在後續的滅菌過程形成較穩定的互穿聚合物網路結構。同時,若第一聚合物的結晶性太強,第二聚合物中聚乙烯吡咯烷酮上的氧原子(oxygen atom)難以與第一聚合物中聚乙烯醇的羥基(hydroxyl group)形成氫鍵,因此不容易讓第一聚合物與第二聚合物產生足夠的糾纏(entanglement),也會影響第一聚合物與第二聚合物形成類似互穿聚合物網路結構的效果,並進一步影響外殼層的穩定性。同時,第一聚合物中部分的醋酸乙烯酯可在滅菌時與部分的乙烯醇產生反應,形成類似交聯反應的作用,可以進一步讓外殼層的結構穩定,同時幫助外殼層固定並包覆鏡片核心本體。
本發明提及的穩定外殼層的形成,其中一個重要原因是第一聚合物能與鏡片核心本體形成互穿聚合物網路結構,同時第一聚合物也能與第二聚合物形成互穿聚合物網路結構。其中,形成穩定的互穿聚合物網路結構的重要原因是滅菌製程。因為滅菌時的高溫高壓,使得第一聚合物中的聚乙烯醇之間產生穩定的氫鍵鍵結(hydrogen bond)。同時,第一聚合物中部分的醋酸乙烯酯可在滅菌時與部分的乙烯醇產生反應,形成類似交聯反應的作用。這使得原本第一聚合物與鏡片核心本體的表層結構從原本形成的半互穿聚合物網路結構,轉換成較穩定的互穿聚合物網路結構。同樣的,在外殼層中的第一聚合物跟第二聚合物原本僅是單純物理吸附或有少量糾纏(entanglement),在經過滅菌時的高溫高壓,第一聚合物之間形成氫鍵及類似交聯反應的作用,同時也加強了第一聚合物跟第二聚合物之間的氫鍵,進一步強化糾纏的強度(strength),因此滅菌過程不只幫助外殼層穩定包覆鏡片核心本體,也幫助加強外殼層本身的穩定度。
在本發明中使用的第一聚合物,可以不包含帶正電(cationic)的聚合物片段(polymeric segment),也可以不包含帶負電(anionic)的聚合物片段(polymeric segment)。
在本發明中使用的第一聚合物,可以包含帶正電的聚合物片段,但該帶正電的聚合物片段不應該對於第一聚合物與鏡片核心本體的聚合物形成互穿聚合物網路結構產生抑制效果,也不應該對第一聚合物與第二聚合物形成穩定的糾纏(entanglement)產生抑制效果。同樣地,在本發明中使用的第一聚合物,可以包含帶負電的聚合物片段,但該帶負電的聚合物片段不應該對於第一聚合物與鏡片核心本體的聚合物形成互穿聚合物網路結構產生抑制效果,也不應該對第一聚合物與第二聚合物形成穩定的糾纏(entanglement)產生抑制效果。
在本發明中使用的第二聚合物,可以不包含帶正電(cationic)的聚合物片段(polymeric segment),也可以不包含帶負電(anionic)的聚合物片段(polymeric segment)。
在本發明中使用的第二聚合物,可以包含帶正電的聚合物片段,但該有帶正電的聚合物片段不應該對於第一聚合物與鏡片核心本體的聚合物形成互穿聚合物網路結構產生抑制效果,也不應該對第二聚合物與第一聚合物形成穩定的糾纏(entanglement)產生抑制效果。同樣地,在本發明中使用的第二聚合物,可以包含帶負電的聚合物片段,但該帶負電的聚合物片段不應該對於第一聚合物與鏡片核心本體的聚合物形成互穿聚合物網路結構產生抑制效果,也不應該對第二聚合物與第一聚合物形成穩定的糾纏(entanglement)產生抑制效果。
本發明另提供一種隱形眼鏡的製作方法,使用上述的隱形眼鏡保存溶液。
本發明中,外殼層主要來自於隱形眼鏡保存溶液中第一聚合物與第二聚合物,在滅菌製程的過程中形成。
本發明中,第一聚合物與第二聚合物在隱形眼鏡保存溶液中重量百分比的相對比例可以為2:1~1:15,更優的為1:2~1:10,更優的為1:4~1:8。在選定的第一聚合物與第二聚合物相對比例範圍中,外殼層形成的較穩固,比較不會在形成後隨時間存放而消失。
本發明中,第一聚合物與第二聚合物在隱形眼鏡保存溶液中重量百分比的相對比例與第二聚合物的分子量有相關性,當兩者具有較佳的組合時可以形成更穩定的外殼層。較優的組合為第一聚合物與第二聚合物在隱形眼鏡保存溶液中重量百分比的相對比例為1:2~1:10,同時第二聚合物的分子量在160,000Da以上。更優的組合為第一聚合物與第二聚合物在隱形眼鏡保存溶液中重量百分比的相對比例為1:4~1:8,同時第二聚合物的分子量在360,000Da以上。
本發明中,第一聚合物與第二聚合物在隱形眼鏡保存溶液中重量百分比的相對比例與第一聚合物的水解程度有相關性,當兩者具有較佳的組合時可以形成更穩定的外殼層。較優的組合為第一聚合物與第二聚合物在隱形眼鏡保存溶液中重量百分比的相對比例為1:2~1:10,同時第一聚合物為水解程度80%~98%的部分水解聚乙烯醇。更優的組合為第一聚合物與第二聚合物在隱形眼鏡保存溶液中重量百分比的相對比例為1:4~1:8,同時第一聚合物為水解程度88%~95%的部分水解聚乙烯醇。
本發明中,隱形眼鏡保存溶液的酸鹼值(pH值)範圍在6.0~8.0,滲透壓範圍在200~400 mOsm/ (kg H2O)。
為了方便讀者閱讀理解,於此盡力以詳細的理論說明關於第一聚合物及鏡片核心本體之間的結構關係及原理,以及第一聚合物與第二聚合物之間的結構關係及原理,但理論說明不應被引申並進一步用作解讀成限制本發明申請之專利權範圍。
如實施例所示,本發明提供之隱形眼鏡,其鏡片核心本體可以是主要由HEMA(2-hydroxyethyl methacrylate)組成,即HEMA佔比在85%以上,或HEMA佔比在90%以上,或HEMA佔比在95%以上的隱形眼鏡。在此所述的組成及比例的計算不包含填充劑(diluent)。該類型隱形眼鏡一般也被稱為水膠隱形眼鏡(Hydrogel Contact Lens)。
如實施例所示,本發明提供之隱形眼鏡,其鏡片核心本體可以是包含含矽成分(silicone containing component)的隱形眼鏡。含矽成分可以是矽單體(silicone monomer)或矽巨分子(silicone macromer),也可以包含含矽交聯劑(silicone crosslinker)。該類型隱形眼鏡一般也被稱為矽水膠隱形眼鏡(Silicone Hydrogel Contact Lens)。
現在將詳細參考本發明的實施例,並闡述其一個或多個範例。提供每個實施例是為了解釋本發明,而非限制本發明。事實上,對於本發明所屬技術領域具有通常知識者來說顯而易見的是,在不脫離本發明的範圍或精神的情況下,可以對本發明進行各種修改和變化。例如,作為一個實施例的一部分揭露或描述的特徵,可以用於另一個實施例以再產生另一個新的實施例。因此,本發明旨在涵蓋落入所附申請專利範圍及其等同物的範圍內的此類修改和變化。本發明的其他目的、特徵和方向在以下詳細描述中公開或從以下詳細描述中顯而易見。本發明所屬技術領域具有通常知識者應理解,目前的討論僅是對示例性實施例的描述,並非旨在限制本發明的更廣泛的方面。
圖1為本發明一實施例的置於包裝內的隱形眼鏡的剖面示意圖。圖2為圖1中圓圈A的放大示意圖。圖3為本發明一實施例隱形眼鏡的製作方法的流程示意圖。請先參考圖1和圖3,本發明一實施例隱形眼鏡保存溶液200適於讓鏡片核心本體110浸泡,並於鏡片核心本體110浸泡於隱形眼鏡保存溶液200時,如圖3的步驟S100所示,進行滅菌步驟,如圖3的步驟S200所示,隱形眼鏡保存溶液200包含第一聚合物121與第二聚合物122,第一聚合物121包括聚乙烯醇,第二聚合物122包括聚乙烯吡咯烷酮。請參考圖2,本發明一實施例的隱形眼鏡100包含鏡片核心本體110與外殼層120,外殼層120包覆鏡片核心本體110;其中外殼層120包括第一聚合物121與第二聚合物122。第一聚合物121包括聚乙烯醇,第二聚合物122包括聚乙烯吡咯烷酮。第一聚合物121例如包覆鏡片核心本體110,第二聚合物122例如包覆第一聚合物121。
具體來說,本發明一實施例的隱形眼鏡100例如置於隱形眼鏡包裝300內,且隱形眼鏡包裝300盛裝有隱形眼鏡保存溶液200,使隱形眼鏡100浸泡於隱形眼鏡保存溶液200中。本實施例的隱形眼鏡包裝300例如包括鋁箔310和容器320,其中容器320具有適於盛裝隱形眼鏡100和隱形眼鏡保存溶液200的空腔,並例如以鋁箔310將容器320密封,但本發明不對此做具體限制。本實施例中,容器320例如是以聚丙烯(polypropylene,PP)為材料製成的容器(本文中亦以「pp杯」稱呼),但本實施例亦不以此為限。  
鏡片配方成分代號及化合物說明:  
鏡片配方成分縮寫 鏡片配方成分全名 鏡片配方成分代號
TRIS 3-[Tris(trimethylsilyloxy)silyl]propyl Methacrylate CAS 17096-07-0
MPDMS monoMethacryloxypropyl terminated Polydimethylsiloxane CAS 146632-07-0
NVP N-Vinylpyrrolidone CAS 88-12-0
HEMA 2-Hydroxyethyl Methacrylate CAS 868-77-9
MAA Methacrylic Acid CAS 79-41-4
EGDMA Ethylene Glycol Dimethacrylate CAS 97-90-5
Irgracure 819 Phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide CAS 162881-26-7
Glycerin CAS 56-81-5
1-Hexanol CAS 111-27-3
DEGBE Diethylene Glycol Monobutyl Ether CAS 112-34-5
 
實施樣品1-1(EX1-1):製作Hydrogel-1鏡片乾片,鏡片配方見表格1。從鏡片配方製作到鏡片乾片的過程為本領域習知技術,可選擇用鑄模方法進行製作。隱形眼鏡的固化方式可選擇光固化或熱固化,本次實施例選擇用光固化。將鏡片乾片以攝氏70±5度的熱水(使用逆滲透水(RO水))水化60分鐘,將鏡片乾片中經固化反應殘餘的單體、交聯劑、起始劑、填充劑洗淨,得到鏡片濕片。得到鏡片濕片後,再將該鏡片濕片浸泡在包含0.2g/L的PVA-PVAc copolymer水溶液中120分鐘,該浸泡過程目的是讓PVA-PVAc copolymer經質傳作用(Mass Transfer)進入鏡片核心本體的表層。在此使用的PVA-PVAc copolymer編號為PVA-PVAc-1,是分子量31,000Da且PVA佔整體比例88%的PVA-PVAc copolymer,亦即為水解程度88%的部分水解聚乙烯醇。完成上述步驟後,將鏡片濕片移出PVA-PVAc copolymer水溶液,放置到聚丙烯(polypropylene, pp)杯(pp cup)中,將緩衝液-1(Buffer-1)滴入pp杯中,緩衝液液面高度必須高過鏡片濕片,以保證所有緩衝液都包覆鏡片濕片。完成後以熱封方式將鋁箔與pp杯密合,並將之送入滅菌釜中進行滅菌(autoclave),滅菌條件為持續升溫至攝氏122度後,維持攝氏122度、2大氣壓並持續30分鐘,如此得到鏡片核心本體為HEMA作為主成分、含水量約在38%,外殼層為以PVA-PVAc copolymer及PVP為主,並以PVA-PVAc copolymer連結鏡片核心本體與PVP的隱形眼鏡。從鏡片濕片接觸緩衝液開始起算約12小時(包含滅菌過程)後,將鋁箔撕開,抽取其緩衝液並檢測酸鹼值(pH值)為7.2,滲透壓範圍在313 mOsm/ (kg H2O),同時取出隱形眼鏡,放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分。Buffer-1與Standard buffer的配方比例(又簡稱為「配比」)記錄在表格2。  表格1  
Contact Lens Formulation
Hydrogel-1 Hydrogel-2 Silicone Hydrogel
TRIS 22.0%
MPDMS 20.0%
NVP 41.0%
HEMA 98.5% 96.7% 14.0%
MAA 0.1% 2.0%
EGDMA 1.0% 1.0% 2.0%
Irgracure 819 0.4% 0.3% 1.0%
SUM (excluding diluent) 100.0% 100.0% 100.0%
Glycerin 15.0% 15.0%
1-Hexanol 10.0%
DEGBE 10.0%
附註: 表格1中diluent (包含Glycerin, 1-Hexanol, DEGBE)不在鏡片配方總和(SUM)的計算中。而是根據100%的SUM為分母再額外添加的。例如: Hydrogel-1配方中若為HEMA 98.5g、MAA 0.1g、EGDMA 1.0g、Irgracure 819 0.4g,總和重量為100g,則在另外添加Glycerin 15.0g作為diluent。 表格2  
Buffer Formulation
Buffer-1 Buffer-2 Buffer-3 Buffer-4 Buffer-5 Buffer-6 Standard Buffer
DI-Water 1000.000 1000.000 1000.000 1000.000 1000.000 1000.000 1000.000
NaCl 8.300 8.300 8.300 8.300 8.300 8.300 8.300
NaH2PO4.2H2O 0.530 0.530 0.530 0.530 0.530 0.530 0.530
Na2HPO4 2.380 2.380 2.380 2.380 2.380 2.380 2.380
PVP360K 0.600 0.600 0.600 0.600
PVP8K 0.600
PVA-PVAc-1 0.200 0.200
PVA-PVAc-2 0.200 0.200
PVA-PVAc-3 0.200
附註: 表格2中數值單位為克重(g)。PVP360K是分子量360,000Da的PVP、PVP8K是分子量8,000Da的PVP、PVA-PVAc-1是分子量31,000Da且PVA佔整體比例88%的PVA-PVAc copolymer、PVA-PVAc-2是分子量205,000Da且PVA佔整體比例88%的PVA-PVAc copolymer、PVA-PVAc-3是分子量27,000Da且PVA佔整體比例98%的PVA-PVAc copolymer。
實施樣品1-2(EX1-2):仿照實施樣品1-1的做法,但在完成熱封將鋁箔與pp杯密合之後,不送入滅菌釜中進行滅菌(autoclave),只讓鏡片濕片在熱封完鋁箔的pp杯中與Buffer-1浸泡。從鏡片濕片接觸緩衝液開始起算約12小時(包含滅菌過程)後,將鋁箔撕開,抽取其緩衝液並檢測酸鹼值(pH值)為7.2,滲透壓範圍在318 mOsm/ (kg H2O),同時取出隱形眼鏡,放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後量測隱形眼鏡的表面潤滑度。
實施樣品2-1(EX2-1):製作Hydrogel-2鏡片乾片,鏡片配方見表格1。從鏡片配方製作到鏡片乾片的過程為本領域習知技術,可選擇用鑄模方法進行製作。隱形眼鏡的固化方式可選擇光固化或熱固化,本次實施例選擇用光固化。將鏡片乾片以含有0.5 wt%的碳酸鈉水溶液浸泡20分鐘,目的是讓鏡片乾片中MAA能快速離子化,使鏡片乾片膨脹以增加清洗效率,再用室溫(攝氏20~30度)的RO水水化40分鐘,將鏡片乾片中經固化反應殘餘的單體、交聯劑、起始劑、填充劑洗淨,得到鏡片濕片。得到鏡片濕片後,再將該鏡片濕片浸泡在包含0.2g/L的PVA-PVAc copolymer水溶液中120分鐘,該浸泡過程目的是讓PVA-PVAc copolymer經質傳作用(Mass Transfer)進入鏡片核心本體的表層。在此使用的PVA-PVAc copolymer編號為PVA-PVAc-1,是分子量31,000Da且PVA佔整體比例88%的PVA-PVAc copolymer,亦即為水解程度88%的部分水解聚乙烯醇。完成上述步驟後,將鏡片濕片移出PVA-PVAc copolymer水溶液,放置到pp杯中,將緩衝液-1(Buffer-1)滴入pp杯中,緩衝液液面高度必須高過鏡片濕片,以保證所有緩衝液都包覆鏡片濕片。完成後以熱封方式將鋁箔與pp杯密合,並將之送入滅菌釜中進行滅菌(autoclave),滅菌條件為持續升溫至攝氏122度後,維持攝氏122度、2大氣壓並持續30分鐘。如此得到鏡片核心本體為HEMA作為主成分、含水量約在55%,外殼層為以PVA-PVAc copolymer及PVP為主,並以PVA-PVAc copolymer連結鏡片核心本體與PVP的隱形眼鏡。從鏡片濕片接觸緩衝液開始起算約12小時(包含滅菌過程)後,將鋁箔撕開,取出隱形眼鏡放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分。  
實施樣品2-2(EX2-2):仿照實施樣品2-1的做法,但在完成熱封將鋁箔與pp杯密合之後,不送入滅菌釜中進行滅菌(autoclave),只讓鏡片濕片在熱封完鋁箔的pp杯中與Buffer-1浸泡。從鏡片濕片接觸緩衝液開始起算約12小時(包含滅菌過程)後,將鋁箔撕開,取出隱形眼鏡,放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分。
實施樣品3-1(EX3-1):製作Silicone Hydrogel鏡片乾片,鏡片配方見表格1。從鏡片配方製作到鏡片乾片的過程為本領域習知技術,可選擇用鑄模方法進行製作。隱形眼鏡的固化方式可選擇光固化或熱固化,本次實施例選擇用光固化。先將鏡片乾片以含有50 wt% 異丙醇(isopropanol,IPA)的水溶液浸泡60分鐘,目的是讓鏡片乾片快速膨脹以增加清洗效率,同時利用IPA與含矽成分TRIS及MPDMS相容性較高的原理,以保證清洗掉未在固化階段反應完的TRIS跟MPDMS,同時也清洗掉殘留的其他單體、交聯劑、起始劑、填充劑,之後再用室溫(攝氏20~30度)的RO水浸泡4次,每次30分鐘,每次更換新鮮的RO水,保證將IPA清洗乾淨,得到鏡片濕片。得到鏡片濕片後,再將該鏡片濕片浸泡在包含0.2g/L的PVA-PVAc copolymer水溶液中120分鐘,該浸泡過程目的是讓PVA-PVAc copolymer經質傳作用(Mass Transfer)進入鏡片核心本體的表層。在此使用的PVA-PVAc copolymer編號為PVA-PVAc-1,是分子量31,000Da且PVA佔整體比例88%的PVA-PVAc copolymer,亦即為水解程度88%的部分水解聚乙烯醇。完成上述步驟後,將鏡片濕片移出PVA-PVAc copolymer水溶液,放置到pp杯中,將緩衝液-1(Buffer-1)滴入pp杯中,緩衝液液面高度必須高過鏡片濕片,以保證所有緩衝液都包覆鏡片濕片。完成後以熱封方式將鋁箔與pp杯密合,並將之送入滅菌釜中進行滅菌(autoclave),滅菌條件為持續升溫至攝氏122度後,維持攝氏122度、2大氣壓並持續30分鐘。如此得到鏡片核心本體為矽水膠(silicone hydrogel),外殼層為以PVA-PVAc copolymer及PVP為主,並以PVA-PVAc copolymer連結鏡片核心本體與PVP的隱形眼鏡。從鏡片濕片接觸緩衝液開始起算約12小時(包含滅菌過程)後,將鋁箔撕開,抽取其緩衝液並檢測酸鹼值(pH值)為7.2,滲透壓範圍在307mOsm/ (kg H2O),同時取出隱形眼鏡放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分。
實施樣品3-2(EX3-2):仿照實施樣品3-1的做法,但在完成熱封將鋁箔與pp杯密合之後,不送入滅菌釜中進行滅菌(autoclave),只讓鏡片濕片在熱封完鋁箔的pp杯中與Buffer-1浸泡。從鏡片濕片接觸緩衝液開始起算約12小時(包含滅菌過程)後,將鋁箔撕開,取出隱形眼鏡,放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分。
實施樣品4-1(EX4-1):製作Hydrogel-2鏡片乾片,鏡片配方見表格1。從鏡片配方製作到鏡片乾片的過程為本領域習知技術,可選擇用鑄模方法進行製作。隱形眼鏡的固化方式可選擇光固化或熱固化,本次實施例選擇用光固化。將鏡片乾片以含有0.5 wt%的碳酸鈉水溶液浸泡20分鐘,目的是讓鏡片乾片中MAA能快速離子化,使鏡片乾片膨脹以增加清洗效率,再用室溫(攝氏20~30度)的RO水水化40分鐘,將鏡片乾片中經固化反應殘餘的單體、交聯劑、起始劑、填充劑洗淨,得到鏡片濕片。得到鏡片濕片後,將鏡片濕片放置到pp杯中,將緩衝液-3(Buffer-3)滴入pp杯中,緩衝液液面高度必須高過鏡片濕片,以保證所有緩衝液都包覆鏡片濕片。完成後以熱封方式將鋁箔與pp杯密合,並將之送入滅菌釜中進行滅菌(autoclave),滅菌條件為持續升溫至攝氏122度後,維持攝氏122度、2大氣壓並持續30分鐘。如此得到鏡片核心本體為HEMA作為主成分、含水量約在55%,外殼層為以PVA-PVAc copolymer及PVP為主,並以PVA-PVAc copolymer連結鏡片核心本體與PVP的隱形眼鏡。從鏡片濕片接觸緩衝液開始起算約12小時(包含滅菌過程)後,將鋁箔撕開,抽取其緩衝液並檢測酸鹼值(pH值)為7.3,滲透壓範圍在321mOsm/ (kg H2O),同時取出隱形眼鏡放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分。Buffer-3的配比記錄在表格2。  
實施樣品4-2(EX4-2):製作Hydrogel-2鏡片乾片,鏡片配方見表格1。從鏡片配方製作到鏡片乾片的過程為本領域習知技術,可選擇用鑄模方法進行製作。隱形眼鏡的固化方式可選擇光固化或熱固化,本次實施例選擇用光固化。將鏡片乾片以含有0.5 wt%的碳酸鈉水溶液浸泡20分鐘,目的是讓鏡片乾片中MAA能快速離子化,使鏡片乾片膨脹以增加清洗效率,再用室溫(攝氏20~30度)的RO水水化40分鐘,將鏡片乾片中經固化反應殘餘的單體、交聯劑、起始劑、填充劑洗淨,得到鏡片濕片。得到鏡片濕片後,再將該鏡片濕片浸泡在包含0.6g/L的PVP水溶液中120分鐘,該浸泡過程目的是讓PVP經質傳作用(Mass Transfer)進入鏡片核心本體的表層。在此使用的PVP編號為PVP360,是分子量360,000Da的PVP。完成上述步驟後,將鏡片濕片移出PVP水溶液,放置到pp杯中,將緩衝液-2(Buffer-2)滴入pp杯中,緩衝液液面高度必須高過鏡片濕片,以保證所有緩衝液都包覆鏡片濕片。完成後以熱封方式將鋁箔與pp杯密合,並將之送入滅菌釜中進行滅菌(autoclave),滅菌條件為持續升溫至攝氏122度後,維持攝氏122度、2大氣壓並持續30分鐘。從鏡片濕片接觸緩衝液開始起算約12小時(包含滅菌過程)後,將鋁箔撕開,抽取其緩衝液並檢測酸鹼值(pH值)為7.2,滲透壓範圍在320mOsm/ (kg H2O),同時取出隱形眼鏡放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分。Buffer-2的配比記錄在表格2。  
實施樣品5-1(EX5-1):仿照實施樣品4-1的做法,但將緩衝液中PVP更換成Copolymer 845 (該聚合物之分子量約為1,000,000Da)。從鏡片濕片接觸緩衝液開始起算約12小時(包含滅菌過程)後,將鋁箔撕開,抽取其緩衝液並檢測酸鹼值(pH值)為7.4,滲透壓範圍在288mOsm/ (kg H2O),同時取出隱形眼鏡,放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分。
實施樣品5-2(EX5-2):製作Hydrogel-2鏡片乾片,鏡片配方見表格1。從鏡片配方製作到鏡片乾片的過程為本領域習知技術,可選擇用鑄模方法進行製作。隱形眼鏡的固化方式可選擇光固化或熱固化,本次實施例選擇用光固化。將鏡片乾片以含有0.5 wt%的碳酸鈉水溶液浸泡20分鐘,目的是讓鏡片乾片中MAA能快速離子化,使鏡片乾片膨脹以增加清洗效率,再用室溫(攝氏20~30度)的RO水水化40分鐘,將鏡片乾片中經固化反應殘餘的單體、交聯劑、起始劑、填充劑洗淨,得到鏡片濕片。得到鏡片濕片後,將鏡片濕片放置到pp杯中,將緩衝液-2(Buffer-2)滴入pp杯中,緩衝液液面高度必須高過鏡片濕片,以保證所有緩衝液都包覆鏡片濕片。完成後以熱封方式將鋁箔與pp杯密合,並將之送入滅菌釜中進行滅菌(autoclave),滅菌條件為持續升溫至攝氏122度後,維持攝氏122度、2大氣壓並持續30分鐘。完成上述滅菌後,將鋁箔撕開,抽取其緩衝液並檢測酸鹼值(pH值)為7.2,滲透壓範圍在315mOsm/ (kg H2O),同時取出隱形眼鏡再放置到另一新的pp杯中,將緩衝液-1(Buffer-1)滴入pp杯中,緩衝液液面高度必須高過鏡片濕片,以保證所有緩衝液都包覆鏡片濕片。完成後以熱封方式將鋁箔與pp杯密合,並將之送入滅菌釜中進行第二次滅菌(autoclave),滅菌條件為持續升溫至攝氏122度後,維持攝氏122度、2大氣壓並持續30分鐘。完成之後,將鋁箔撕開,取出隱形眼鏡放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分。
實施樣品6-1(EX6-1):仿照實施樣品4-1的製作方法,但將緩衝液換成緩衝液-4(Buffer-4),Buffer-4的配比記錄在表格2。滅菌完成後,確認從鏡片濕片接觸緩衝液開始起算達到約12小時(包含滅菌過程),將鋁箔撕開,抽取其緩衝液並檢測酸鹼值(pH值)為7.2,滲透壓範圍在307mOsm/ (kg H2O),同時取出隱形眼鏡放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分。
實施樣品7-1(EX7-1):仿照實施樣品4-1的製作方法,但將緩衝液-3換成緩衝液-5(Buffer-5),Buffer-5的配比記錄在表格2。滅菌完成後,確認從鏡片濕片接觸緩衝液開始起算達到約12小時(包含滅菌過程),將鋁箔撕開,抽取其緩衝液並檢測酸鹼值(pH值)為7.3,滲透壓範圍在311mOsm/ (kg H2O),同時取出隱形眼鏡放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分。
實施樣品8-1(EX8-1):仿照實施樣品4-1的製作方法,但將緩衝液-3換成緩衝液-6(Buffer-6),Buffer-6的配比記錄在表格2。滅菌完成後,確認從鏡片濕片接觸緩衝液開始起算達到約12小時(包含滅菌過程),將鋁箔撕開,抽取其緩衝液並檢測酸鹼值(pH值)為7.2,滲透壓範圍在313mOsm/ (kg H2O),同時取出隱形眼鏡放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分。
實施樣品9-1(EX9-1):製作Hydrogel-2鏡片乾片,鏡片配方見表格1。從鏡片配方製作到鏡片乾片的過程為本領域習知技術,可選擇用鑄模方法進行製作。隱形眼鏡的固化方式可選擇光固化或熱固化,本次實施例選擇用光固化。將鏡片乾片以含有0.5 wt%的碳酸鈉水溶液浸泡20分鐘,目的是讓鏡片乾片中MAA能快速離子化,使鏡片乾片膨脹以增加清洗效率,再用室溫(攝氏20~30度)的RO水水化40分鐘,將鏡片乾片中經固化反應殘餘的單體、交聯劑、起始劑、填充劑洗淨,得到鏡片濕片。得到鏡片濕片後,再將該鏡片濕片浸泡在包含0.2g/L的PVA(分子量145,000Da,水解度99%)水溶液中以攝氏70±5度加熱120分鐘,再將該鏡片濕片浸泡在包含0.6g/L的PVP(分子量360,000Da)水溶液中以攝氏70±5度加熱120分鐘,得到鏡片濕片後,將鏡片濕片放置到pp杯中,將標準緩衝鹽溶液滴入pp杯中,緩衝液液面高度必須高過鏡片濕片,以保證所有緩衝液都包覆鏡片濕片。完成後以熱封方式將鋁箔與pp杯密合,並將之送入滅菌釜中進行滅菌(autoclave),滅菌條件為持續升溫至攝氏122度後,維持攝氏122度、2大氣壓並持續30分鐘。從鏡片濕片接觸緩衝液開始起算約12小時(包含滅菌過程)後,抽取其緩衝液並檢測酸鹼值(pH值)為7.4,滲透壓範圍在320mOsm/ (kg H2O),同時將鋁箔撕開,取出隱形眼鏡放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分。標準緩衝鹽溶液的配比記錄在表格2。
實施樣品6-2(EX6-2):仿照實施樣品9-1的製作方法,但在完成熱封將鋁箔與pp杯密合之後,不送入滅菌釜中進行滅菌(autoclave),只讓鏡片濕片在熱封完鋁箔的pp杯中與標準緩衝鹽溶液浸泡。從鏡片濕片接觸緩衝液開始起算約12小時(包含滅菌過程)後,將鋁箔撕開,抽取其緩衝液並檢測酸鹼值(pH值)為7.2,滲透壓範圍在310mOsm/ (kg H2O),同時取出隱形眼鏡,放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分。
實施樣品7-2(EX7-2):仿照實施樣品4-1的製作方法,但將緩衝液-3換成緩衝液-1(Buffer-1),Buffer-1的配比記錄在表格2。滅菌完成後,確認從鏡片濕片接觸緩衝液開始起算達到約12小時(包含滅菌過程) ,抽取其緩衝液並檢測酸鹼值(pH值)為7.2,滲透壓範圍在320mOsm/ (kg H2O),同時將鋁箔撕開,取出隱形眼鏡放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分。
實施樣品8-2(EX8-2):仿照實施樣品7-2的做法,但評價隱形眼鏡的表面潤滑度之前,先將鋁箔撕開,取出隱形眼鏡,放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後再對隱形眼鏡的表面潤滑度進行評分。
實施樣品9-2(EX9-2):仿照實施樣品4-1的製作方法,但將緩衝液-3換成緩衝液-2(Buffer-2),Buffer-2的配比記錄在表格2。滅菌完成後,確認從鏡片濕片接觸緩衝液開始起算達到約12小時(包含滅菌過程),將鋁箔撕開,取出隱形眼鏡放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分。
隱形眼鏡表面潤滑度評分(surface lubricity score)。將隱形眼鏡的表面潤滑度以1~4分區分,分數越高表示隱形眼鏡潤滑度越高。1分代表以手指搓揉感覺隱形眼鏡完全沒有潤滑感。2分代表以手指搓揉感覺隱形眼鏡有一點潤滑感,評分上與市售隱形眼鏡產品為Acuvue Oasys 1 day相當。3分代表隱形眼鏡有適度的潤滑感。4分代表隱形眼鏡非常潤滑,評分上與市售隱形眼鏡產品為Dailies Total 1相當。必須說明的是,部分佩戴隱形眼鏡的使用者評價Dailies Total 1的配戴感非常好,但因為隱形眼鏡太滑導致使用後要將隱形眼鏡自眼睛中取下非常困難,影響使用者繼續使用該品牌隱形眼鏡的意願。因此隱形眼鏡的潤滑度並非越高越好。本發明評價中最合適的潤滑度為3分。
表面潤滑度評分測試方式: 選5位測試者,每位測試者都會同步搓揉Acuvue Oasys 1 day及Dailies Total 1兩項產品,並以Acuvue Oasys 1 day的搓揉感覺的潤滑度標定為2分,以Dailies Total 1的搓揉感覺的潤滑度標定為4分,若5位測試者中有4位認為測試樣品的潤滑度明顯低於Acuvue Oasys 1 day,則測試樣品的潤滑度分數將紀錄為1分。若僅有3位認為測試樣品潤滑度低於Acuvue Oasys 1 day,2位認為與Acuvue Oasys 1 day差異不顯著,則記錄為1~2分。若有4位以上認為測試樣品的潤滑度與Acuvue Oasys 1 day相當,則記錄為2分。若有3位以上認為測試樣品的潤滑度明顯高於Acuvue Oasys 1 day,另外2位認為測試樣品潤滑度與Acuvue Oasys 1 day相當,則記錄為2~3。若有4位以上認為潤滑度明顯高於Acuvue Oasys 1 day,則記錄為3分。
本次實施樣品的表面潤滑度評分見表格3。 表格3
Example Surface Lubricity Score
EX1-1 3
EX2-1 3
EX3-1 3
EX1-2 1
EX2-2 1
EX3-2 1
EX4-1 3
EX5-1 3
EX4-2 2
EX5-2 2-3
EX6-1 2
EX7-1 3
EX8-1 2-3
EX9-1 2-3
EX6-2 1
EX7-2 2
EX8-2 1
EX9-2 1
從表格3中的數據可以看出,按照本發明提出的技術方案(實施樣品EX1-1、2-1、3-1、4-1、5-1、6-1、7-1、8-1和9-1),可以有效提升表面潤滑度,並控制表面潤滑度在合適範圍。實施樣品1-1(EX1-1)和實施樣品1-2(EX1-2)的主要差異之處在於是否有滅菌,有進行滅菌處理的實施樣品1-1具有較高的表面潤滑度,其分數為3分。同理可證,實施樣品2-1(EX2-1)的表面潤滑度分數也比實施樣品2-2(EX2-2)的表面潤滑度分數高。實施樣品3-1(EX3-1)的表面潤滑度分數也比實施樣品3-2(EX3-2)表面潤滑度分數高,理由與實施樣品1-1(EX1-1)類似,於此不再贅述。實施樣品4-1(EX4-1)和實施樣品4-2(EX4-2)類似,兩者的主要差異之處在於:將第一聚合物與第二聚合物接觸鏡片核心本體的時機不同。在實施樣品4-1(EX4-1)中,將鏡片核心本體浸泡於同時含有第一聚合物與第二聚合物的緩衝液中,使第一聚合物可以有效地跟鏡片核心本體的表面結構形成互穿聚合物網路結構,因此影響最終隱形眼鏡的表面潤滑度。實施樣品5-1(EX5-1)和實施樣品5-2(EX5-2)的主要差異則在於:實施樣品5-2分為兩次滅菌,先在浸泡含有PVA的buffer-2後進行第一次滅菌,再於浸泡含有PVP的buffer-1後進行第二次滅菌。從表面潤滑度分數來看,可知實施樣品5-1的分數較實施樣品5-2高。推究其原因可能是因為實施樣品5-2在第一次滅菌時,先有第一聚合物中的部分聚乙烯醇之間形成較強的氫鍵及交聯反應,阻礙了第二聚合物在第二次滅菌時與第一聚合物形成外殼層,可能因此使得外殼層較不穩定,造成表面潤滑度分數較低。實施樣品9-1(EX9-1)和實施樣品6-2(EX6-2)相比,因為實施樣品9-1經過滅菌,因此表面潤滑度分數較高。實施樣品4-1(EX4-1)和實施樣品7-2(EX7-2)類似,主要差異之處在於:實施樣品4-1浸泡的buffer-3中除了有第二聚合物之外,更具有第一聚合物,使得第二聚合物在第一聚合物的幫助下,能夠讓第二聚合物穩定存在於鏡片核心本體的表面,因此實施樣品4-1的表面潤滑度分數較高。同理,實施樣品4-1(EX4-1)的表面潤滑度分數比實施樣品8-2(EX8-2)的表面潤滑度分數高,於此不再贅述。實施樣品4-1(EX4-1)與實施樣品9-2(EX9-2)相比,實施樣品4-1浸泡的buffer-3中除了具有第一聚合物之外,更具有第二聚合物,有助於形成增加隱形眼鏡表面潤滑度的外殼層,因此具有比實施樣品9-2更高的表面潤滑度分數。
將實施樣品4-1及實施樣品7-2的隱形眼鏡以RO水潤洗3次,去除隱形眼鏡表面可被RO水去除之成分(包含緩衝鹽類NaCl、 NaH2PO4、 Na2HPO4),之後將隱形眼鏡以105°C烘乾至少8個小時,將隱形眼鏡水分去除得到乾鏡片,並以掃描式電子顯微鏡的元素分析(Energy-dispersive X-ray spectroscopy with Scanning Electron Microscope,SEM-EDX)功能分析乾鏡片之表面成分。元素分析數據顯示,實施樣品4-1處理後的乾鏡片表面有4.39%的氮元素,表示即使經過RO水潤洗,第二聚合物(PVP)仍穩定存在鏡片核心本體的表面。然而,實施樣品7-2處理後的乾鏡片表面無法測到氮元素,表示經過RO水潤洗,原本鏡片核心本體的表面的第二聚合物(PVP)已經被洗掉。因此,以SEM-EDX的分析方式可以進一步說明本發明一實施例隱形眼鏡的鏡片核心本體被包含第二聚合物(PVP)的外殼層包覆。
實施樣品10~15 (EX10~EX15):仿照實施樣品4-1的製作方法,但將緩衝液-3換成緩衝液-7~緩衝液-12(Buffer-7~Buffer-12),緩衝液的配比記錄在表格4。滅菌完成後,確認從鏡片濕片接觸緩衝液開始起算達到約12小時(包含滅菌過程),將鋁箔撕開,抽取其緩衝液並檢測酸鹼值(pH值)及滲透壓。實施樣品10~15的酸鹼值(pH值)範圍在6.9~7.6,滲透壓範圍在288~337mOsm/ (kg• H2O)。仿照實施樣品4-1評量表面潤滑度的方法,評價實施樣品10~15,表面潤滑度評分見表格5。 表格4  
Buffer Formulation
  Buffer-7 Buffer-8 Buffer-9 Buffer-10 Buffer-11 Buffer-12
DI-Water 1000.000 1000.000 1000.000 1000.000 1000.000 1000.000
NaCl 8.300 8.300 1.800 1.800 1.750 1.750
NaH2PO4.2H2O 0.530 0.530 4.200 4.200 4.400 4.400
Na2HPO4 2.380 2.380 16.000 16.000 16.800 16.800
PVP360K 0.200 0.600 0.800 0.640
PVP8K 1.500 1.500
PVA-PVAc-1 0.080
PVA-PVAc-2 0.400 0.100 0.300 0.150
PVA-PVAc-3         0.200  
附註: 表格4中數值單位為克重(g)。PVP360K是分子量360,000Da的PVP、PVP8K是分子量8,000Da的PVP、PVA-PVAc-1是分子量31,000Da且PVA佔整體比例88%的PVA-PVAc copolymer、PVA-PVAc-2是分子量205,000Da且PVA佔整體比例88%的PVA-PVAc copolymer、PVA-PVAc-3是分子量27,000Da且PVA佔整體比例98%的PVA-PVAc copolymer。 表格5
Example Surface Lubricity Score
EX10 2-3
EX11 2-3
EX12 3
EX13 2-3
EX14 3
EX15 3
實施樣品16(EX16):仿照實施樣品1-1的製作方法,但在將鏡片濕片移出PVA-PVAc copolymer水溶液後,先不將鏡片放入pp杯中與緩衝液接觸,而是再將鏡片濕片放入含有0.6g/L濃度的PVP360水溶液中,以溫度攝氏80度的溫度加熱2小時,再將鏡片濕片放入pp杯中,接著將標準緩衝液(standard buffer)滴入pp杯中,緩衝液液面高度必須高過鏡片濕片,以保證所有緩衝液都包覆鏡片濕片。完成後以熱封方式將鋁箔與pp杯密合,並將之送入滅菌釜中進行滅菌(autoclave),滅菌條件為持續升溫至攝氏122度後,維持攝氏122度、2大氣壓並持續30分鐘。
實施樣品17(EX17):仿照實施樣品2-1的製作方法,但在將鏡片濕片移出PVA-PVAc copolymer水溶液後,先不將鏡片放入pp杯中與緩衝液接觸,而是再將鏡片濕片放入含有0.6g/L濃度的PVP360水溶液中,以溫度攝氏80度的溫度加熱2小時,再將鏡片濕片放入pp杯中,接著將標準緩衝液(standard buffer)滴入pp杯中,緩衝液液面高度必須高過鏡片濕片,以保證所有緩衝液都包覆鏡片濕片。完成後以熱封方式將鋁箔與pp杯密合,並將之送入滅菌釜中進行滅菌(autoclave),滅菌條件為持續升溫至攝氏122度後,維持攝氏122度、2大氣壓並持續30分鐘。
實施樣品18(EX18):仿照實施樣品17的製作方法,但把水化製程中使用的碳酸鈉更換成四硼酸鈉,其餘生產過程不變。
實施樣品19(EX19):仿照實施樣品16的製作方法,但把緩衝液替換為Buffer-3,其餘生產過程不變。
實施樣品20(EX20):仿照實施樣品17的製作方法,但把緩衝液替換為Buffer-3,其餘生產過程不變。
實施樣品21(EX21):仿照實施樣品2-1的製作方法,但把緩衝液替換成Buffer-3,其餘生產過程不變。
評價實施樣品16~21的表面潤滑度:從鏡片濕片接觸緩衝液開始起算約12小時(包含滅菌過程)後,將鋁箔撕開,取出隱形眼鏡放在標準緩衝鹽溶液(Standard buffer)中平衡,一片隱形眼鏡使用10ml的標準緩衝鹽,並每1小時後更換一次緩衝液,重複3次,之後對隱形眼鏡的表面潤滑度進行評分,將評分總結於表格6。從比對EX16、EX17與EX1-1及EX2-1(見表格3)可以看出,隱形眼鏡僅在水化製程與第一聚合物及第二聚合物接觸時隱形眼鏡的表面潤滑度分數較低,推測是滅菌時的溫度(攝氏122度)比水化的溫度(攝氏20度~攝氏80度)更高,對於隱形眼鏡形成外殼層較有利。從EX19跟EX20的對比,EX20的表面潤滑度分數較高,推測是因為鏡片核心本體中MAA比例較高,對於第一聚合物吸附到鏡片濕片表面有利,因此外殼層形成的更完整。EX20相比EX4-1(見表格3)表面潤滑度分數更高,推測是因為除了滅菌時鏡片核心本體跟第一聚合物及第二聚合物接觸,同時在水化製程時也讓鏡片核心本體與第一聚合物及第二聚合物接觸。 表格6
Example Surface Lubricity Score
EX16 2-3
EX17 2-3
EX18 3
EX19 3
EX20 3-4
EX21 3
從上述數據分析及說明,可以證實本發明提出的技術方案可以有效使隱形眼鏡具有適度的表面潤滑度,有利於增加隱形眼鏡配戴時的舒適度。
雖然本發明已以實施例揭露如上,然其並非用以限定本發明,本發明所屬技術領域中具有通常知識者,在不脫離本發明之精神和範圍內,當可作些許之更動與潤飾,因此本發明之保護範圍當視後附之申請專利範圍所界定者為準。
100:隱形眼鏡 110:鏡片核心本體 120:外殼層 121:第一聚合物 122:第二聚合物 200:隱形眼鏡保存溶液 300:隱形眼鏡包裝 310:鋁箔 320:容器 S100、S200:步驟
圖1為本發明一實施例的置於包裝內的隱形眼鏡的剖面示意圖。 圖2為圖1中圓圈A的放大示意圖。 圖3為本發明一實施例隱形眼鏡的製作方法的流程示意圖。
100:隱形眼鏡
110:鏡片核心本體
120:外殼層
200:隱形眼鏡保存溶液
300:隱形眼鏡包裝
310:鋁箔
320:容器
A:圓圈

Claims (14)

  1. 一種隱形眼鏡保存溶液,適於讓一鏡片核心本體浸泡,並於該鏡片核心本體浸泡於該隱形眼鏡保存溶液時進行一滅菌步驟,該隱形眼鏡保存溶液包含一第一聚合物與一第二聚合物,該第一聚合物包括聚乙烯醇,該第二聚合物包括聚乙烯吡咯烷酮;  其中該第一聚合物與該第二聚合物的重量百分比的相對比例為1:4~1:15。  
  2. 如請求項1所述之隱形眼鏡保存溶液,其中該第一聚合物為水解程度70%~99%的部分水解聚乙烯醇。  
  3. 如請求項1所述之隱形眼鏡保存溶液,其中該第一聚合物為水解程度80%~98%的部分水解聚乙烯醇。  
  4. 如請求項1所述之隱形眼鏡保存溶液,其中該第一聚合物為水解程度88%~95%的部分水解聚乙烯醇。  
  5. 如請求項1所述之隱形眼鏡保存溶液,其中該第二聚合物的分子量大於或等於8,000Da。
  6. 如請求項1所述之隱形眼鏡保存溶液,其中該第二聚合物的分子量大於或等於160,000Da。
  7. 如請求項1所述之隱形眼鏡保存溶液,其中該第二聚合物的分子量大於或等於360,000Da。
  8. 如請求項1所述之隱形眼鏡保存溶液,其中該第二聚合物為包含聚乙烯吡咯烷酮的共聚物。
  9. 如請求項8所述之隱形眼鏡保存溶液,其中該第二聚合物為乙烯基吡咯烷酮和甲基丙烯酸二甲胺基乙酯的共聚物。
  10. 如請求項9所述之隱形眼鏡保存溶液,其中該第二聚合物的分子量大於或等於100,000Da。
  11. 如請求項9所述之隱形眼鏡保存溶液,其中該第二聚合物的分子量大於或等於1,000,000Da。
  12. 如請求項1所述之隱形眼鏡保存溶液,其中該第一聚合物與該第二聚合物的重量百分比的相對比例為1:4~1:8。
  13. 如請求項1所述之隱形眼鏡保存溶液,其中該隱形眼鏡保存溶液的酸鹼值(pH值)範圍介於6.0~8.0,且該隱形眼鏡保存溶液的滲透壓範圍介於200~400 mOsm/ (kg H2O)。
  14. 一種隱形眼鏡的製作方法,包括: 將一鏡片核心本體浸泡於如請求項1~13任一項所述的隱形眼鏡保存溶液時; 進行一滅菌步驟後,得到一隱形眼鏡; 其中該隱形眼鏡包括該鏡片核心本體與一外殼層,該外殼層包覆該鏡片核心本體;其中,該外殼層包括該第一聚合物與該第二聚合物。
TW113149200A 2024-02-22 2024-12-17 隱形眼鏡保存溶液和隱形眼鏡的製作方法 TWI926552B (zh)