TWI646218B - Hot-dip galvanized steel sheet - Google Patents

Hot-dip galvanized steel sheet Download PDF

Info

Publication number
TWI646218B
TWI646218B TW106125688A TW106125688A TWI646218B TW I646218 B TWI646218 B TW I646218B TW 106125688 A TW106125688 A TW 106125688A TW 106125688 A TW106125688 A TW 106125688A TW I646218 B TWI646218 B TW I646218B
Authority
TW
Taiwan
Prior art keywords
steel sheet
hot
layer
iron
base material
Prior art date
Application number
TW106125688A
Other languages
Chinese (zh)
Other versions
TW201910535A (en
Inventor
森下敦司
金藤泰平
內田智史
中田達也
山口裕司
Original Assignee
日商新日鐵住金股份有限公司
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 日商新日鐵住金股份有限公司 filed Critical 日商新日鐵住金股份有限公司
Priority to TW106125688A priority Critical patent/TWI646218B/en
Application granted granted Critical
Publication of TWI646218B publication Critical patent/TWI646218B/en
Publication of TW201910535A publication Critical patent/TW201910535A/en

Abstract

本發明之以母材鋼板表面起1/4厚度為中心之1/8厚度~3/8厚度範圍中,肥粒鐵相以體積分率計為50%以上且97%以下,由變韌鐵相、變韌肥粒鐵相、新生麻田散鐵相與回火麻田散鐵相中之1種以上所構成之硬質組織的合計以體積分率計為3%以上,殘留沃斯田鐵相以體積分率計為0%~8%,波來鐵相與粗大雪明碳鐵相之合計以體積分率計為0%~8%,於熔融鍍鋅層與前述母材鋼板之界面具有平均厚度為0.1μm~2.0μm之Fe-Al合金層,且其在鋼板寬度方向上之最大厚度與最小厚度的差為0.5μm以內;以與前述Fe-Al合金層直接接觸之微細化層來說,前述微細化層在鋼板寬度方向上之最大厚度與最小厚度的差在2.0μm以內。In the range of 1/8 thickness to 3/8 thickness centered on the surface of the base material steel plate with a thickness of 1/4 of the thickness of the base material, the ferrite grain iron phase is 50% or more and 97% or less by volume fraction, and the toughened iron is used. The sum of the hard structures composed of one or more of the phase, the toughened ferrite phase, the new Matian iron phase and the tempered Matian iron phase is 3% or more by volume fraction, and the remaining Worthite iron phase The volume fraction is 0% to 8%, and the total of the ferrite phase and the coarse snowy carbon phase is 0% to 8% by volume fraction, and has an average at the interface between the hot-dip galvanized layer and the parent metal plate. a Fe-Al alloy layer having a thickness of 0.1 μm to 2.0 μm, and a difference between a maximum thickness and a minimum thickness in a width direction of the steel sheet of 0.5 μm or less; and a micronized layer in direct contact with the Fe-Al alloy layer The difference between the maximum thickness and the minimum thickness of the micronized layer in the width direction of the steel sheet is within 2.0 μm.

Description

熔融鍍鋅鋼板Hot-dip galvanized steel sheet

本發明係有關於延性、彎曲性、擴孔性及彎曲變形時的鍍敷密著性優異,且耐連續彎曲疲勞特性優異之高強度熔融鍍鋅鋼板。The present invention relates to a high-strength hot-dip galvanized steel sheet which is excellent in plating adhesion at the time of ductility, bendability, hole expandability, and bending deformation, and is excellent in continuous bending fatigue resistance.

發明背景 對於主要用於汽車骨架構件之鋼板一直以來都要求高強度化。而該等高強度鋼板為了獲得高強度與優異之成形性,一般係含有有助於強度提升之以Si及Mn為代表的合金元素。然,以Si及Mn為代表之合金元素卻亦會降低鍍敷密著性。 又,對於汽車用鋼板因一般皆在屋外使用故通常會要求具優異耐蝕性。Background of the Invention High-strength has been demanded for steel sheets mainly used for automobile frame members. In order to obtain high strength and excellent formability, these high-strength steel sheets generally contain alloying elements represented by Si and Mn which contribute to strength improvement. However, alloying elements such as Si and Mn also reduce plating adhesion. Moreover, since the steel sheets for automobiles are generally used outdoors, they are usually required to have excellent corrosion resistance.

而關於汽車外板等之用途,會利用壓製加工對板周邊部施行嚴酷的彎曲加工(摺邊彎曲)。而且不僅汽車外板,其他用途上亦多利用壓製加工施行嚴酷的彎曲加工或擴孔加工等後作使用。可是對習知的熔融鍍鋅鋼板施行嚴酷的彎曲加工或擴孔加工等時,該加工部分會發生鍍敷層從母材鋼板剝離之情形。而像這樣若鍍敷層剝離的話,該處即會喪失耐蝕性,而有母材鋼板從早期即腐蝕而生鏽之問題。就算不至於鍍敷層剝離之程度,鍍敷層與母材鋼板之間亦會喪失密著性,導致該部分產生些微空隙,造成外部空氣或水分從該空隙侵入,使鍍敷層喪失防蝕機能。而造成如同前述,母材鋼板從早期即腐蝕而生鏽。 基於該等問題,施行嚴酷的彎曲加工等後作使用之高強度鋼板係強烈希望使用具備鍍敷層對母材鋼板具優異密著性之熔融鍍鋅層的鍍敷鋼板。Regarding the use of the outer panel of the automobile, the peripheral portion of the panel is subjected to severe bending processing (bending and bending) by press working. Moreover, not only the outer panel of the automobile but also other applications are often subjected to severe bending or reaming processing by press working. However, when the conventional hot-dip galvanized steel sheet is subjected to severe bending processing or hole expanding processing, the plating portion may be peeled off from the base material steel sheet in the processed portion. In this case, if the plating layer is peeled off, the corrosion resistance is lost at this point, and there is a problem that the base material steel plate is corroded and rusted from the early stage. Even if the plating layer is not peeled off, the adhesion between the plating layer and the base material steel plate may be lost, resulting in some micro-voids in the portion, causing external air or moisture to intrude from the space, causing the plating layer to lose the corrosion prevention function. . As a result, the base metal sheet is corroded and rusted from the early stage. Based on these problems, it is strongly desired to use a plated steel sheet having a hot-dip galvanized layer having a plating layer with excellent adhesion to the base material steel sheet, which is used for a high-strength steel sheet which is subjected to severe bending work or the like.

為了提高鍍敷層的密著性,例如以專利文獻1~3為代表,有提出一種使鋼板內部生成氧化物,來減少會造成鍍敷剝離之基鐵與鍍敷層之界面上的氧化物之方法。然,當使所述氧化物生成於鋼板表層時,鋼板表層的碳會與氧結合而氣體化。結果造成碳自鋼板脫離,故該碳脫離之區域會有強度顯著降低之情形。當鋼板表層的強度降低時,受表層部特性大力影響之耐疲勞特性即會變差,而有疲勞強度大幅降低之虞。In order to improve the adhesion of the plating layer, for example, as disclosed in Patent Documents 1 to 3, it has been proposed to form an oxide inside the steel sheet to reduce oxides at the interface between the base iron and the plating layer which cause plating peeling. The method. However, when the oxide is formed on the surface layer of the steel sheet, the carbon of the surface layer of the steel sheet is combined with oxygen to be gasified. As a result, the carbon is detached from the steel sheet, so that the region where the carbon is detached has a situation in which the strength is remarkably lowered. When the strength of the surface layer of the steel sheet is lowered, the fatigue resistance characteristic which is strongly influenced by the characteristics of the surface layer portion is deteriorated, and the fatigue strength is greatly lowered.

或是為了提高鍍敷層的密著性,專利文獻4中提出了一種在一般退火步驟前新增新的退火步驟及酸洗步驟來施行,使母材鋼板表面改質,提高鍍敷密著性之方法。不過,專利文獻4所記載之方法對一般高強度鍍敷鋼板之製造方法來說要增加步驟,而有成本方面之課題。Or in order to improve the adhesion of the plating layer, Patent Document 4 proposes a new annealing step and a pickling step to be performed before the general annealing step to modify the surface of the base metal sheet to improve the plating adhesion. The method of sex. However, the method described in Patent Document 4 requires an additional step for the production method of a general high-strength plated steel sheet, and has a problem in terms of cost.

此外,專利文獻5中,提出了一種自母材鋼板表層部除去碳來提高鍍敷密著性之方法。然,專利文獻5所記載之方法卻會使經除去碳之區域的強度顯著降低。因此,專利文獻5所記載之方法會使受表層部特性大力影響之耐疲勞特性變差,而有疲勞強度大幅降低之虞。Further, Patent Document 5 proposes a method of removing carbon from the surface layer portion of the base material steel sheet to improve plating adhesion. However, the method described in Patent Document 5 significantly reduces the strength of the carbon-removed region. Therefore, in the method described in Patent Document 5, the fatigue resistance which is strongly influenced by the characteristics of the surface layer portion is deteriorated, and the fatigue strength is largely lowered.

又,專利文獻6、7中,提出了一種將鍍敷層中的Mn、Al及Si量控制在適宜的範圍內來使鍍敷密著性提升之鋼板。但專利文獻6、7所記載之鋼板因需在製造時將鍍敷層中的元素量作高精度的控制,造成作業上負擔變大而有成本方面之課題。Further, in Patent Documents 6 and 7, a steel sheet in which the amount of Mn, Al, and Si in the plating layer is controlled within an appropriate range to improve plating adhesion is proposed. However, in the steel sheets described in Patent Documents 6 and 7, it is necessary to control the amount of the elements in the plating layer with high precision at the time of manufacture, which causes an increase in work load and a cost problem.

關於提高鍍敷密著性之手法,專利文獻8有提出一種鋼板的微觀組織僅由肥粒鐵構成之高強度鋼板。但,專利文獻8所記載之鋼板其微觀組織因僅為軟質的肥粒鐵故無法獲得充分高的強度。Regarding the method of improving the adhesion of plating, Patent Document 8 proposes a high-strength steel sheet in which the microstructure of the steel sheet is composed only of ferrite. However, the steel sheet described in Patent Document 8 has a microstructure which is only soft and ferrite, so that a sufficiently high strength cannot be obtained.

而現在,係廣泛使用經於熔融鍍鋅處理後施行合金化處理之合金化熔融鍍鋅鋼板。合金化處理係一種將鍍敷層加熱至Zn熔點以上的溫度,使大量的Fe原子從母材鋼板中擴散到鍍敷層中,將鍍敷層製成Zn-Fe合金主體的層之處理。例如,專利文獻9、10、11提出了一種鍍敷密著性優異之合金化熔融鍍鋅鋼板。但,為了將鍍敷層充分合金化,必須將鋼板加熱至高溫。若將鋼板加熱至高溫,鋼板內部的微觀組織即會變質,尤其易生成粗大的鐵系碳化物而有損鋼板特性,故而不佳。Nowadays, alloyed hot-dip galvanized steel sheets subjected to alloying treatment after hot-dip galvanizing treatment are widely used. The alloying treatment is a treatment in which a plating layer is heated to a temperature higher than a melting point of Zn, a large amount of Fe atoms are diffused from a base material steel sheet into a plating layer, and a plating layer is formed into a layer of a Zn-Fe alloy body. For example, Patent Documents 9, 10, and 11 propose an alloyed hot-dip galvanized steel sheet excellent in plating adhesion. However, in order to sufficiently alloy the plating layer, it is necessary to heat the steel sheet to a high temperature. When the steel sheet is heated to a high temperature, the microstructure inside the steel sheet is deteriorated, and in particular, coarse iron-based carbides are easily formed to impair the characteristics of the steel sheet, which is not preferable.

另一方面,例如以專利文獻12所記載之熔融鍍鋅鋼板來說,有鍍敷層在寬度方向上之Fe含量不均勻性造成之外觀不均的課題。On the other hand, for example, the hot-dip galvanized steel sheet described in Patent Document 12 has a problem that the plating layer has uneven appearance due to uneven Fe content in the width direction.

先前技術文獻 專利文獻 專利文獻1:日本特開2008-019465號公報 專利文獻2:日本特開2005-060742號公報 專利文獻3:日本特開平9-176815號公報 專利文獻4:日本特開2001-026853號公報 專利文獻5:日本特開2002-088459號公報 專利文獻6:日本特開2003-055751號公報 專利文獻7:日本特開2003-096541號公報 專利文獻8:日本特開2005-200750號公報 專利文獻9:日本特開平11-140587號公報 專利文獻10:日本特開2001-303226號公報 專利文獻11:日本特開2005-060743號公報 專利文獻12:國際公開第2016/072477號CITATION LIST Patent Literature Patent Literature 1: Japanese Laid-Open Patent Publication No. Hei. No. Hei. No. Hei. No. Hei. No. Hei. Japanese Patent Laid-Open Publication No. JP-A-2003-096751, Patent Document No. JP-A-2003-096751, Patent Document No. JP-A-2003-096541, Patent Document 8: JP-A-2005-200750 Japanese Patent Laid-Open Publication No. Hei No. Hei. No. Hei. No. Hei. No. Hei. No. Hei. No. Hei. No. Hei.

發明概要 發明欲解決之課題 鑒於以上現況,本發明係提供一種具優異之以延性、彎曲性及延伸凸緣成形性為代表之鋼板成形性,且鍍敷的外觀均勻性、耐疲勞特性、熔接性、耐蝕性及鍍敷密著性優異之高強度熔融鍍鋅鋼板。SUMMARY OF THE INVENTION Problems to be Solved by the Invention In view of the above circumstances, the present invention provides an excellent formability of a steel sheet which is represented by ductility, flexibility, and stretch flange formability, and uniformity of appearance, fatigue resistance, and fusion of plating. High-strength hot-dip galvanized steel sheet excellent in properties, corrosion resistance and plating adhesion.

用以解決課題之手段 本發明人等為了製得具優異之以延性、彎曲性及延伸凸緣成形性為代表之鋼板成形性,及耐疲勞特性、熔接性、耐蝕性及鍍敷密著性優異之高強度熔融鍍鋅鋼板而積極努力反覆檢討。結果,本發明人等藉由將鋼板的微觀組織控制成適當的組織分率改善了延性及擴孔性(延伸凸緣性)。而且,本發明人等藉由從鍍敷層與母材鋼板之境界控制母材鋼板側的硬質相的體積分率而改善了彎曲性與耐疲勞特性。並且,本發明人等發現,即便在將含有大量Si及Mn之鋼板用作鍍敷原板之情況下,藉由於形成於鍍敷層與母材鋼板之界面的Fe-Al合金層正下方形成由肥粒鐵相的極微細粒所構成之特定微細化層可抑制加工時產生及傳播裂痕,而可抑制以其為起點之鍍敷剝離。又,藉由將鋼板寬度方向上之微細化層及Fe-Al合金層的厚度控制在特定範圍內,可製得不僅鍍敷密著性優異,外觀均勻性亦優異之熔融鍍鋅鋼板。Means for Solving the Problems The inventors of the present invention have obtained excellent formability, ductility, and stretch flange formability, and have fatigue resistance, weldability, corrosion resistance, and plating adhesion. Excellent high-strength galvanized steel sheet and active efforts to review it. As a result, the present inventors improved ductility and hole expandability (extension flangeability) by controlling the microstructure of the steel sheet to an appropriate tissue fraction. Further, the inventors of the present invention improved the flexibility and the fatigue resistance by controlling the volume fraction of the hard phase on the side of the base material steel plate from the boundary between the plating layer and the base material steel sheet. Further, the present inventors have found that even when a steel sheet containing a large amount of Si and Mn is used as a plating original plate, it is formed directly under the Fe-Al alloy layer formed at the interface between the plating layer and the base material steel sheet. The specific micronized layer composed of the extremely fine particles of the ferrite-grained iron phase suppresses generation and propagation of cracks during processing, and can suppress plating peeling from the starting point. In addition, by controlling the thickness of the fine layer and the Fe-Al alloy layer in the width direction of the steel sheet within a specific range, it is possible to obtain a hot-dip galvanized steel sheet which is excellent not only in plating adhesion but also in excellent appearance uniformity.

本發明即為鑑於所述見解而完成者,其態様如下。The present invention has been completed in view of the above findings, and its state is as follows.

(1)一種熔融鍍鋅鋼板,係於母材鋼板之至少一側具有熔融鍍鋅層,且該熔融鍍鋅鋼板之特徵在於前述母材鋼板具有以下化學組成: 以質量%計, C:0.040%~0.280%、 Si:0.05%~2.00%、 Mn:0.50%~3.50%、 P:0.0001%~0.1000%、 S:0.0001%~0.0100%、 Al:0.001%~1.500%、 N:0.0001%~0.0100%、 O:0.0001%~0.0100%、 Ti:0%~0.150%、 Nb:0%~0.100%、 V:0%~0.300%、 Cr:0%~2.00%、 Ni:0%~2.00%、 Cu:0%~2.00%、 Mo:0%~2.00%、 B:0%~0.0100%、 W:0%~2.00%、及 Ca、Ce、Mg、Zr、La及REM:合計0%~0.0100%,且 剩餘部份由Fe及雜質所構成;並且具有以下微觀組織: 相對於前述母材鋼板的總厚度,以前述母材鋼板表面起1/4厚度為中心之1/8厚度~3/8厚度範圍中, 肥粒鐵相以體積分率計為50%以上且97%以下, 由變韌鐵相、變韌肥粒鐵相、新生麻田散鐵相與回火麻田散鐵相中之1種以上所構成之硬質組織的合計以體積分率計為3%以上, 殘留沃斯田鐵相以體積分率計為0%~8%, 波來鐵相與粗大雪明碳鐵相之合計以體積分率計為0%~8%, 自前述熔融鍍鋅層與母材鋼板之界面起至鋼板方向深度20μm為止之表層部中, 殘留沃斯田鐵以體積分率計為0%~3%, 將前述表層部中前述硬質組織的體積分率V1、與以鋼板表面起1/4厚度為中心之1/8厚度~3/8厚度之範圍中前述硬質組織的體積分率V2之比,V1/V2設為0.10以上且0.90以下之範圍; 前述熔融鍍鋅層中Fe含量大於0%且在3.0%以下,Al含量大於0%且在1.0%以下, 於前述熔融鍍鋅層與前述母材鋼板之界面具有平均厚度為0.1μm~2.0μm之Fe-Al合金層,且其在鋼板寬度方向上之最大厚度與最小厚度的差在0.5μm以內, 前述母材鋼板內具有與前述Fe-Al合金層直接接觸之微細化層,前述微細化層的平均厚度為0.1μm~5.0μm,前述微細化層內之肥粒鐵相的平均粒徑為0.1μm~3.0μm,前述微細化層中含有Si及Mn之1種或2種以上的氧化物,前述氧化物的最大徑為0.01μm~0.4μm,在鋼板寬度方向上之前述微細化層之最大厚度與最小厚度的差在2.0μm以內。 (2)如(1)之熔融鍍鋅鋼板,其中前述熔融鍍鋅層之每單面鍍敷附著量為10g/m 2以上且100g/m 2以下。 (3)如(1)或(2)之熔融鍍鋅鋼板,其中前述母材鋼板以質量%計更含有選自於由Ti:0.001%~0.150%、Nb:0.001%~0.100%、及V:0.001%~0.300%所構成群組中之1種或2種以上。 (4)如(1)~(3)中任一項之熔融鍍鋅鋼板,其中前述母材鋼板以質量%計更含有選自於由Cr:0.01%~2.00%、Ni:0.01%~2.00%、Cu:0.01%~2.00%、Mo:0.01%~2.00%、B:0.0001%~0.0100%、及W:0.01%~2.00%所構成群組中之1種或2種以上。 (5)如(1)~(4)中任一項之熔融鍍鋅鋼板,其中前述母材鋼板以質量%計更含有合計0.0001%~0.0100%之選自於由Ca、Ce、Mg、Zr、La及REM所構成群組中之1種或2種以上。 (1) A hot-dip galvanized steel sheet having a hot-dip galvanized layer on at least one side of a base material steel sheet, and the hot-dip galvanized steel sheet is characterized in that the base material steel sheet has the following chemical composition: % by mass, C: 0.040 %~0.280%, Si:0.05%~2.00%, Mn:0.50%~3.50%, P:0.0001%~0.1000%, S:0.0001%~0.0100%, Al:0.001%~1.500%, N:0.0001%~ 0.0100%, O: 0.0001% to 0.0100%, Ti: 0% to 0.150%, Nb: 0% to 0.100%, V: 0% to 0.300%, Cr: 0% to 2.00%, Ni: 0% to 2.00% Cu: 0% to 2.00%, Mo: 0% to 2.00%, B: 0% to 0.0100%, W: 0% to 2.00%, and Ca, Ce, Mg, Zr, La, and REM: 0% in total 0.0100%, and the remainder is composed of Fe and impurities; and has the following microstructure: 1/8 thickness ~3 centering on the surface of the base material steel sheet with a thickness of 1/4 of the total thickness of the base material steel sheet In the thickness range of /8, the ferrite iron phase is 50% or more and 97% or less in volume fraction, and is composed of a toughened iron phase, a toughened ferrite phase, a new Matian iron phase, and a tempered Matian iron phase. Total of hard tissues composed of one or more types The volume fraction is 3% or more, and the residual Worthfield iron phase is 0% to 8% by volume fraction, and the total of the Borne iron phase and the coarse snowy carbon iron phase is 0% by volume fraction. 8%, in the surface layer portion from the interface between the hot-dip galvanized layer and the base material steel sheet to the depth of the steel sheet of 20 μm, the remaining Worthite iron is 0% to 3% by volume fraction, and the surface layer portion is the aforementioned The ratio of the volume fraction V1 of the hard structure to the volume fraction V2 of the hard structure in the range of 1/8 thickness to 3/8 thickness centering on the 1/4 thickness of the steel sheet surface, and V1/V2 is set to 0.10 or more. And a range of 0.90 or less; the Fe content in the hot-dip galvanized layer is greater than 0% and less than 3.0%, and the Al content is greater than 0% and less than 1.0%, and has an average thickness at the interface between the hot-dip galvanized layer and the parent metal steel sheet. It is an Fe-Al alloy layer of 0.1 μm to 2.0 μm, and the difference between the maximum thickness and the minimum thickness in the width direction of the steel sheet is within 0.5 μm, and the base material steel sheet has fine contact with the Fe-Al alloy layer directly. The average thickness of the micronized layer is 0.1 μm to 5.0 μm, and the ferrite phase in the micronized layer The average particle diameter is 0.1 μm to 3.0 μm, and the fine layer has one or two or more kinds of oxides of Si and Mn, and the maximum diameter of the oxide is 0.01 μm to 0.4 μm in the width direction of the steel sheet. The difference between the maximum thickness and the minimum thickness of the aforementioned micronized layer is within 2.0 μm. (2) The hot-dip galvanized steel sheet according to (1), wherein the single-sided plating adhesion amount of the hot-dip galvanized layer is 10 g/m 2 or more and 100 g/m 2 or less. (3) The hot-dip galvanized steel sheet according to (1) or (2), wherein the base material steel sheet further contains, in mass%, from Ti: 0.001% to 0.150%, Nb: 0.001% to 0.100%, and V : 0.001% to 0.300% of one or more of the groups formed. (4) The hot-dip galvanized steel sheet according to any one of (1) to (3), wherein the base material steel sheet further contains, in mass%, from: 0.01% to 2.00%, and Ni: 0.01% to 2.00. %, Cu: 0.01% to 2.00%, Mo: 0.01% to 2.00%, B: 0.0001% to 0.0100%, and W: 0.01% to 2.00% of one or more of the groups. (5) The hot-dip galvanized steel sheet according to any one of (1) to (4), wherein the base material steel sheet further contains, in mass%, from 0.0001% to 0.0100%, selected from the group consisting of Ca, Ce, Mg, and Zr. One or two or more of the groups consisting of La and REM.

發明效果 根據本發明前述態様,可提供一種鍍敷的外觀均勻性、成形性、耐疲勞特性、熔接性、耐蝕性及鍍敷密著性優異之熔融鍍鋅鋼板。Advantageous Effects of Invention According to the aspect of the invention, it is possible to provide a hot-dip galvanized steel sheet which is excellent in appearance uniformity, moldability, fatigue resistance, weldability, corrosion resistance and plating adhesion of plating.

發明實施形態 本發明實施形態之熔融鍍鋅鋼板係於具有以下化學成分之母材鋼板(以下,僅記為鋼板)表面形成熔融鍍鋅層(以下,僅記為鍍敷層)而成者,該母材鋼板之化學成分以質量%計含有C:0.040%~0.280%、Si:0.01%~2.00%、Mn:0.50%~3.50%、P:0.0001%~0.100%、S:0.0001%~0.0100%、Al:0.001%~1.500%、O:0.0001%~0.0100%、N:0.0001%~0.0100%,且剩餘部份由Fe及雜質構成。 並且,母材鋼板之板厚宜為0.6mm以上且低於5.0mm。母材鋼板的板厚若低於0.6mm,則母材鋼板形狀難以保持平坦而不適宜。又,若母材鋼板的板厚為5.0mm以上,則難以控制製造過程中的冷卻,而有無法獲得預定的微觀組織造成成形性變差的情況。 鍍敷層之Fe含量大於0%且在3.0%以下,Al含量大於0%且在1.0%以下。EMBODIMENT OF THE INVENTION The hot-dip galvanized steel sheet according to the embodiment of the present invention is formed by forming a hot-dip galvanized layer (hereinafter, simply referred to as a plating layer) on the surface of a base material steel sheet (hereinafter, simply referred to as a steel sheet) having the following chemical composition. The chemical composition of the base material steel plate contains C: 0.040% to 0.280%, Si: 0.01% to 2.00%, Mn: 0.50% to 3.50%, P: 0.0001% to 0.100%, and S: 0.0001% to 0.0100, by mass%. %, Al: 0.001% to 1.500%, O: 0.0001% to 0.0100%, N: 0.0001% to 0.0100%, and the remainder is composed of Fe and impurities. Further, the thickness of the base material steel sheet is preferably 0.6 mm or more and less than 5.0 mm. When the thickness of the base material steel sheet is less than 0.6 mm, it is difficult to keep the shape of the base material steel sheet flat and unsuitable. In addition, when the thickness of the base material steel sheet is 5.0 mm or more, it is difficult to control the cooling during the production process, and the predetermined microstructure may not be obtained, and the formability may be deteriorated. The Fe content of the plating layer is more than 0% and less than 3.0%, and the Al content is more than 0% and less than 1.0%.

首先,就構成本發明實施形態之熔融鍍鋅鋼板的母材鋼板的化學成分(組成)進行說明。此外,以下說明中的[%]只要無特別說明即表示[質量%]。First, the chemical composition (composition) of the base material steel sheet constituting the hot-dip galvanized steel sheet according to the embodiment of the present invention will be described. In addition, [%] in the following description means [% by mass] unless otherwise specified.

[C:0.040%~0.280%] C係為提高母材鋼板強度而含有。然若C含量大於0.280%,點熔接性會變差,故設C含量為0.280%以下。此外,以點熔接性之觀點,C含量宜為0.250%以下,更宜為0.220%以下。另一方面,C含量低於0.040%時,強度會降低,而難以確保充分的拉伸最大強度,故將C含量設為0.040%以上。此外,為了獲得更高的強度,C含量宜為0.055%以上,更宜為0.070%以上。[C: 0.040% to 0.280%] The C system is contained to improve the strength of the base material steel plate. However, if the C content is more than 0.280%, the spot weldability may be deteriorated, so that the C content is 0.280% or less. Further, from the viewpoint of spot weldability, the C content is preferably 0.250% or less, more preferably 0.220% or less. On the other hand, when the C content is less than 0.040%, the strength is lowered, and it is difficult to ensure sufficient tensile maximum strength, so the C content is made 0.040% or more. Further, in order to obtain higher strength, the C content is preferably 0.055% or more, more preferably 0.070% or more.

[Si:0.05%~2.00%] Si係可抑制母材鋼板中鐵系碳化物之生成,提高強度與成形性之元素。但Si亦為會使鋼板脆化之元素,故Si含量大於2.00%時,易發生鑄造出的鋼胚龜裂等之問題。因此,設Si含量為2.00%以下。並且Si會於退火步驟時於母材鋼板表面形成氧化物,顯著破壞鍍敷的密著性。而由此觀點,Si含量宜為1.500%以下,更宜為1.200%以下。另一方面,Si含量小於0.05%時,於熔融鍍鋅鋼板之鍍敷步驟中會大量生成粗大的鐵系碳化物,使強度及成形性變差,故設Si含量為0.05%以上。而以抑制鐵系碳化物生成之觀點,Si含量宜為0.10%以上,更宜為0.25%以上。[Si: 0.05% to 2.00%] The Si system can suppress the formation of iron-based carbides in the base material steel plate and improve the strength and formability. However, Si is also an element which causes the steel plate to be embrittled. Therefore, when the Si content is more than 2.00%, problems such as cracking of the cast steel are likely to occur. Therefore, the Si content is made 2.00% or less. Further, Si forms an oxide on the surface of the base material steel sheet during the annealing step, which significantly impairs the adhesion of the plating. From this point of view, the Si content is preferably 1.500% or less, more preferably 1.200% or less. On the other hand, when the Si content is less than 0.05%, coarse iron-based carbides are formed in a large amount in the plating step of the hot-dip galvanized steel sheet, and the strength and moldability are deteriorated. Therefore, the Si content is 0.05% or more. From the viewpoint of suppressing the formation of iron-based carbides, the Si content is preferably 0.10% or more, more preferably 0.25% or more.

[Mn:0.50%~3.50%] Mn可為了藉由提高母材鋼板的淬火性來提高強度而含有。然,當Mn含量大於3.50%時,母材鋼板的板厚中央部會生成粗大的Mn濃化部分而易引起脆化,而易發生鑄造出的鋼胚龜裂等之問題。因此,設Mn含量為3.50%以下。又,若增加Mn的含量亦會使熔融鍍鋅鋼板的點熔接性變差。由此觀點,Mn含量宜為3.00%以下,更宜為2.80%以下。而Mn含量小於0.50%時,於退火後之冷卻中會大量形成軟質組織,而難以確保充分高的拉伸最大強度。因此,須設Mn含量為0.50%以上。為了可更提高熔融鍍鋅鋼板的強度,Mn含量宜為0.80%以上,更宜為1.00%以上。[Mn: 0.50% to 3.50%] Mn can be contained in order to increase the strength by improving the hardenability of the base material steel sheet. However, when the Mn content is more than 3.50%, a coarse Mn-concentrated portion is formed in the center portion of the base material of the base material steel sheet, which is liable to cause embrittlement, and is liable to cause problems such as cracking of the cast steel. Therefore, the Mn content is set to 3.50% or less. Further, if the content of Mn is increased, the spot weldability of the hot-dip galvanized steel sheet is deteriorated. From this point of view, the Mn content is preferably 3.00% or less, more preferably 2.80% or less. On the other hand, when the Mn content is less than 0.50%, a large amount of soft structure is formed during cooling after annealing, and it is difficult to ensure a sufficiently high tensile maximum strength. Therefore, the Mn content must be 0.50% or more. In order to further increase the strength of the hot-dip galvanized steel sheet, the Mn content is preferably 0.80% or more, more preferably 1.00% or more.

[P:0.0001%~0.1000%] P係會使鋼材脆化之元素,且當P含量大於0.1000%時,會變得易發生鑄造出的鋼胚龜裂、鋼胚於軋延中龜裂等問題,因此設P含量為0.1000%以下。又,P亦為會使透過點熔接而生成之熔融部脆化之元素,故為了獲得充分的熔接接合強度,P含量宜設為0.0400%以下,更宜設為0.0200%以下。而P含量小於0.0001%時,會伴隨製造成本大幅增加,因此設P含量下限值為0.0001%,宜設為0.0010%以上。[P: 0.0001% to 0.1000%] P is an element which causes embrittlement of steel, and when the P content is more than 0.1000%, it is likely to cause cracking of steel blanks during casting, cracking of steel blanks during rolling, etc. The problem is therefore that the P content is 0.1000% or less. Further, P is an element which embrittles the molten portion which is formed by welding the transmission point. Therefore, in order to obtain sufficient fusion bonding strength, the P content is preferably 0.0400% or less, more preferably 0.0200% or less. On the other hand, when the P content is less than 0.0001%, the manufacturing cost is greatly increased. Therefore, the lower limit of the P content is 0.0001%, preferably 0.0010% or more.

[S:0.0001%~0.0100%] S係會與Mn結合形成粗大的MnS,使延性、擴孔性(延伸凸緣性)及彎曲性等成形性降低之元素,故設S含量為0.0100%以下。又,S係會使點熔接性變差之元素。因此,S含量宜設為0.0060%以下,更宜設為0.0035%以下。另一方面,將S含量設為小於0.0001%時,會伴隨製造成本大幅增加。因此,設S含量之下限值為0.0001%,宜設為0.0005%以上,更宜設為0.0010%以上。[S: 0.0001% to 0.0100%] The S system combines with Mn to form coarse MnS, which reduces the formability such as ductility, hole expandability (extension flangeability) and flexibility. Therefore, the S content is 0.0100% or less. . Further, S is an element which deteriorates the spot weldability. Therefore, the S content is preferably set to 0.0060% or less, more preferably 0.0035% or less. On the other hand, when the S content is less than 0.0001%, the manufacturing cost is greatly increased. Therefore, the lower limit of the S content is 0.0001%, preferably 0.0005% or more, and more preferably 0.0010% or more.

[Al:0.001%~1.500%] Al係會使鋼材脆化之元素。則當Al含量大於1.500%時,會易發生鑄造出的鋼胚龜裂等問題,故設Al含量為1.500%以下。又,因若增加Al含量會使點熔接性變差,故Al含量宜設為1.200%以下,更宜設為1.000%以下。另一方面,不特別限定Al含量下限亦可發揮本實施形態之效果。而Al係微量存在於原料中之雜質,而設其含量小於0.001%時,會伴隨製造成本大幅增加。因此,設Al含量為0.001%以上。又,Al亦為可有效作為脫氧材之元素,而為了要更充分獲得脱氧效果,Al含量宜設為0.010%以上。[Al: 0.001% to 1.500%] Al is an element that makes the steel brittle. When the Al content is more than 1.500%, problems such as cracking of the cast steel preform are liable to occur, so that the Al content is 1.500% or less. Further, if the Al content is increased, the spot weldability is deteriorated, so the Al content is preferably 1.200% or less, more preferably 1.000% or less. On the other hand, the effect of the present embodiment can be exhibited without particularly limiting the lower limit of the Al content. On the other hand, Al is a trace amount of impurities present in the raw material, and when the content is less than 0.001%, the manufacturing cost is greatly increased. Therefore, the Al content is made 0.001% or more. Further, Al is also an element which can be effectively used as a deoxidizing material, and in order to more fully obtain a deoxidizing effect, the Al content is preferably set to 0.010% or more.

[N:0.0001%~0.0100%] N係會形成粗大的氮化物,使延性、擴孔性(延伸凸緣性)及彎曲性等成形性變差之元素,基於此必須抑制其含量。當N含量大於0.0100%時,會使成形性顯著變差,故設N含量上限為0.0100%。又,N過度含有時,會造成於熔接時產生氣孔,故其含量宜少。由該等觀點來看,N含量宜為0.0070%以下,更宜為0.0050%以下。另一方面,不特別限定N含量下限亦可發揮本實施形態之效果,但若設N含量低於0.0001%時會導致製造成本大幅增加。基於此,設N含量之下限為0.0001%以上。N含量宜為0.0003%以上,更宜為0.0005%以上。[N: 0.0001% to 0.0100%] N-forms form coarse nitrides, and elements which deteriorate formability such as ductility, hole expandability (extension flangeability) and flexibility are necessary to suppress the content thereof. When the N content is more than 0.0100%, the formability is remarkably deteriorated, so the upper limit of the N content is made 0.0100%. Further, when N is excessively contained, pores are generated at the time of welding, so the content thereof is preferably small. From these viewpoints, the N content is preferably 0.0070% or less, more preferably 0.0050% or less. On the other hand, the effect of the present embodiment can be exhibited without particularly limiting the lower limit of the N content. However, if the N content is less than 0.0001%, the manufacturing cost is greatly increased. Based on this, the lower limit of the N content is made 0.0001% or more. The N content is preferably 0.0003% or more, more preferably 0.0005% or more.

[O:0.0001%~0.0100%] O會形成氧化物,使熔融鍍鋅鋼板之延性、擴孔性(延伸凸緣性)及彎曲性等成形性變差,故必須抑制O含量。當O含量大於0.0100%時,會使成形性顯著變差,故設O含量上限為0.0100%。並且O含量宜為0.0050%以下,更宜為0.0030%以下。不特別限定O含量下限亦可發揮本實施形態之效果,但若設O含量小於0.0001%時,會伴隨製造成本大幅增加,故設其下限為0.0001%。且O含量宜為0.0003%以上,更宜為0.0005%以上。[O: 0.0001% to 0.0100%] O forms an oxide and deteriorates the formability such as ductility, hole expandability (stretch flangeability) and flexibility of the hot-dip galvanized steel sheet. Therefore, it is necessary to suppress the O content. When the O content is more than 0.0100%, the formability is remarkably deteriorated, so the upper limit of the O content is set to 0.0100%. Further, the O content is preferably 0.0050% or less, more preferably 0.0030% or less. The effect of the present embodiment can be exhibited without particularly limiting the lower limit of the O content. However, when the O content is less than 0.0001%, the manufacturing cost is greatly increased, so the lower limit is made 0.0001%. Further, the O content is preferably 0.0003% or more, more preferably 0.0005% or more.

此外,本實施形態之熔融鍍鋅鋼板的母材鋼板中亦可因應需要含有以下元素。Further, the base material steel sheet of the hot-dip galvanized steel sheet according to the present embodiment may contain the following elements as needed.

首先,本實施形態之母材鋼板中,可更含有選自於由Ti:0.001%~0.150%、Nb:0.001%~0.100%及V:0.001%~0.300%所構成群組中之1種或2種以上。First, the base material steel sheet of the present embodiment may further contain one selected from the group consisting of Ti: 0.001% to 0.150%, Nb: 0.001% to 0.100%, and V: 0.001% to 0.300%. 2 or more types.

[Ti:0.001%~0.150%] Ti係可透過強化析出物、抑制肥粒鐵晶粒的成長使細粒強化、及抑制再結晶所行之差排強化而有助於提高熔融鍍鋅鋼板之強度的元素。然,Ti含量大於0.150%時,會使碳氮化物析出變多,造成成形性變差,故設Ti含量為0.150%以下。又,由成形性之觀點,Ti含量宜為0.080%以下。另一方面,不特別限定Ti含量下限亦可發揮本實施形態之效果,但為了利用Ti充分獲得提高強度之效果,Ti含量宜為0.001%以上。為了使熔融鍍鋅鋼板更高強度化,Ti含量更宜為0.010%以上。[Ti: 0.001% to 0.150%] The Ti-based system can enhance the growth of the galvanized steel sheet by strengthening the precipitates, suppressing the growth of the ferrite grains, and strengthening the fine particles and inhibiting the recrystallization. The element of strength. However, when the Ti content is more than 0.150%, the precipitation of carbonitrides is increased, and the formability is deteriorated. Therefore, the Ti content is made 0.150% or less. Further, from the viewpoint of moldability, the Ti content is preferably 0.080% or less. On the other hand, the effect of the present embodiment can be exhibited without particularly limiting the lower limit of the Ti content. However, in order to sufficiently obtain the effect of improving the strength by using Ti, the Ti content is preferably 0.001% or more. In order to increase the strength of the hot-dip galvanized steel sheet, the Ti content is more preferably 0.010% or more.

[Nb:0.001%~0.100%] Nb係可透過強化析出物、抑制肥粒鐵晶粒的成長使細粒強化、及抑制再結晶所行之差排強化而有助於提高熔融鍍鋅鋼板之強度的元素。然,Nb含量大於0.100%時,會使碳氮化物析出變多,造成熔融鍍鋅鋼板的成形性變差,故設Nb含量為0.100%以下。又,由成形性之觀點,Nb含量宜為0.060%以下。另一方面,不特別限定Nb含量下限亦可發揮本實施形態之效果,但為了利用Nb充分獲得提高強度之效果,Nb含量宜為0.001%以上。為了使熔融鍍鋅鋼板更高強度化,Nb含量更宜為0.005%以上。[Nb: 0.001% to 0.100%] Nb can enhance the precipitation of ferrite grains by inhibiting the growth of precipitates and suppressing the growth of ferrite grains, and inhibiting the recrystallization of the grains. The element of strength. However, when the Nb content is more than 0.100%, the precipitation of carbonitrides is increased, and the formability of the hot-dip galvanized steel sheet is deteriorated. Therefore, the Nb content is made 0.100% or less. Further, from the viewpoint of moldability, the Nb content is preferably 0.060% or less. On the other hand, the effect of the present embodiment can be exhibited without particularly limiting the lower limit of the Nb content. However, in order to sufficiently obtain the effect of improving the strength by using Nb, the Nb content is preferably 0.001% or more. In order to increase the strength of the hot-dip galvanized steel sheet, the Nb content is more preferably 0.005% or more.

[V:0.001%~0.300%] V係可透過強化析出物、抑制肥粒鐵晶粒的成長使細粒強化、及抑制再結晶所行之差排強化而有助於提高熔融鍍鋅鋼板之強度的元素。然,V含量大於0.300%時,會使碳氮化物析出變多,造成成形性變差。因此,設V含量為0.300%以下。且V含量宜為0.200%以下。另一方面,不特別限定V含量下限亦可發揮本實施形態之效果。而為了利用V充分獲得提高強度之效果,V含量宜為0.001%以上,更宜為0.010%以上。[V: 0.001% to 0.300%] The V-based system can enhance the growth of the galvanized steel sheet by strengthening the precipitates, suppressing the growth of the ferrite grains, and strengthening the fine particles and inhibiting the recrystallization. The element of strength. However, when the V content is more than 0.300%, precipitation of carbonitrides is increased, and formability is deteriorated. Therefore, the V content is set to 0.300% or less. And the V content is preferably 0.200% or less. On the other hand, the effect of the present embodiment can be exhibited without particularly limiting the lower limit of the V content. In order to sufficiently obtain the effect of improving the strength by using V, the V content is preferably 0.001% or more, more preferably 0.010% or more.

又,本實施形態之母材鋼板中更可含有選自於由Cr:0.01%~2.00%、Ni:0.01%~2.00%、Cu:0.01%~2.00%、Mo:0.01%~2.00%、B:0.0001%~0.0100%及W:0.01%~2.00%所構成群組中之1種或2種以上。Further, the base material steel sheet according to the present embodiment may further contain, from Cr: 0.01% to 2.00%, Ni: 0.01% to 2.00%, Cu: 0.01% to 2.00%, and Mo: 0.01% to 2.00%, B. One or two or more of the group consisting of 0.0001% to 0.0100% and W: 0.01% to 2.00%.

[Cr:0.01%~2.00%] Cr係可抑制在高溫下之相變態而對熔融鍍鋅鋼板的高強度化有效之元素,亦可取代一部份的C及/或Mn而含有之。然,Cr含量大於2.00%時,於熱處理之加工性會受損而導致生產性降低,因此,設Cr含量為2.00%以下。且Cr含量宜為1.20%以下。另一方面,不特別限定Cr含量下限亦可發揮本實施形態之效果,然為了利用Cr充分獲得高強度化之效果,Cr含量宜為0.01%以上,更宜為0.10%以上。[Cr: 0.01% to 2.00%] Cr is an element which is effective for suppressing the phase transformation at a high temperature and is effective for increasing the strength of the hot-dip galvanized steel sheet, and may be contained in place of a part of C and/or Mn. However, when the Cr content is more than 2.00%, the workability in the heat treatment is impaired and the productivity is lowered. Therefore, the Cr content is made 2.00% or less. And the Cr content is preferably 1.20% or less. On the other hand, the effect of the present embodiment is not particularly limited as long as the lower limit of the Cr content is exhibited. However, in order to sufficiently obtain the effect of increasing the strength by using Cr, the Cr content is preferably 0.01% or more, and more preferably 0.10% or more.

[Ni:0.01%~2.00%] Ni係可抑制在高溫下之相變態而對熔融鍍鋅鋼板的高強度化有效之元素,亦可取代一部份的C及/或Mn而含有之。然,Ni含量大於2.00%時,會有損熔接性,因此設Ni含量2.00%以下。且Ni含量宜為1.20%以下。另一方面,不特別限定Ni含量下限亦可發揮本實施形態之效果,然為了利用Ni充分獲得高強度化之效果,Ni含量宜為0.01%以上,更宜為0.10%以上。[Ni: 0.01% to 2.00%] The Ni-based element which suppresses the phase transformation at a high temperature and is effective for increasing the strength of the hot-dip galvanized steel sheet may be contained in place of a part of C and/or Mn. However, when the Ni content is more than 2.00%, the weldability is impaired, so that the Ni content is 2.00% or less. And the Ni content is preferably 1.20% or less. On the other hand, the effect of the present embodiment is not particularly limited, and the effect of the present embodiment is not particularly limited. However, in order to sufficiently obtain the effect of increasing the strength by using Ni, the Ni content is preferably 0.01% or more, and more preferably 0.10% or more.

[Cu:0.01%~2.00%] Cu係可作為微細粒子存在於鋼中來提高熔融鍍鋅鋼板的強度之元素,亦可取代一部份的C及/或Mn而含有之。然,Cu含量大於2.00%時,會有損熔接性,故設Cu含量為2.00%以下。且Cu含量宜為1.20%以下。不特別限定Cu含量下限亦可發揮本實施形態之效果,然為了利用Cu充分獲得提高熔融鍍鋅鋼板的強度之效果,Cu含量宜為0.01%以上,更宜為0.10%以上。[Cu: 0.01% to 2.00%] Cu may be used as an element in which fine particles are present in steel to increase the strength of the hot-dip galvanized steel sheet, and may be contained in place of a part of C and/or Mn. However, when the Cu content is more than 2.00%, the weldability is impaired, so that the Cu content is 2.00% or less. And the Cu content is preferably 1.20% or less. The effect of the present embodiment is not particularly limited, and the effect of the present embodiment can be exhibited. However, in order to sufficiently obtain the effect of improving the strength of the hot-dip galvanized steel sheet by using Cu, the Cu content is preferably 0.01% or more, and more preferably 0.10% or more.

[Mo:0.01%~2.00%] Mo係可抑制在高溫下之相變態而對熔融鍍鋅鋼板的高強度化有效之元素,因此,亦可取代一部份的C及/或Mn而含有之。然,Mo含量大於2.00%時,於熱處理之加工性會受損而導致生產性降低,因此設Mo含量為2.00%以下。且Mo含量宜為1.20%以下。另一方面,不特別限定Mo含量下限亦可發揮本實施形態之效果,然為了利用Mo充分獲得高強度化之效果,Mo含量宜為0.01%以上,更宜為0.05%以上。[Mo: 0.01% to 2.00%] Mo is an element which suppresses the phase transformation at a high temperature and is effective for increasing the strength of the hot-dip galvanized steel sheet. Therefore, it may be substituted for a part of C and/or Mn. . However, when the Mo content is more than 2.00%, the workability in the heat treatment is impaired and the productivity is lowered. Therefore, the Mo content is 2.00% or less. And the Mo content is preferably 1.20% or less. On the other hand, the effect of the present embodiment is not particularly limited, and the effect of the present embodiment is not particularly limited. However, in order to sufficiently obtain the effect of increasing the strength by Mo, the Mo content is preferably 0.01% or more, and more preferably 0.05% or more.

[B:0.0001%~0.0100%] B係可抑制在高溫下之相變態而對熔融鍍鋅鋼板的高強度化有效之元素,因此,亦可取代一部份的C及/或Mn而含有之。然,B含量大於0.0100%時,於熱處理之加工性會受損而導致生產性降低,因此設B含量為0.0100%以下。而由生產性之觀點,B含量宜為0.0050%以下。另一方面,不特別限定B含量下限亦可發揮本實施形態之效果,然為了利用B充分獲得高強度化之效果,B含量宜設為0.0001%以上。而為了進一步使熔融鍍鋅鋼板高強度化,B含量更宜為0.0005%以上。[B: 0.0001% to 0.0100%] B is an element which suppresses the phase transformation at a high temperature and is effective for increasing the strength of the hot-dip galvanized steel sheet. Therefore, it may be substituted for a part of C and/or Mn. . However, when the B content is more than 0.0100%, the workability in the heat treatment is impaired and the productivity is lowered. Therefore, the B content is made 0.0100% or less. From the viewpoint of productivity, the B content is preferably 0.0050% or less. On the other hand, the effect of the present embodiment is not particularly limited as long as the lower limit of the B content is exhibited. However, in order to sufficiently obtain the effect of increasing the strength by B, the B content is preferably made 0.0001% or more. Further, in order to further increase the strength of the hot-dip galvanized steel sheet, the B content is more preferably 0.0005% or more.

[W:0.01%~2.00%] W係可抑制在高溫下之相變態而對熔融鍍鋅鋼板的高強度化有效之元素,因此,亦可取代一部份的C及/或Mn而含有之。然,W含量大於2.00%時,於熱處理之加工性會受損而導致生產性降低,因此設W含量為2.00%以下。且W含量宜設為1.20%以下。另一方面,不特別限定W含量下限亦可發揮本實施形態之效果,然為了利用W充分獲得高強度化之效果,W含量宜為0.01%以上,更宜為0.10%以上。[W: 0.01% to 2.00%] W is an element which suppresses the phase transformation at a high temperature and is effective for increasing the strength of the hot-dip galvanized steel sheet. Therefore, it may be substituted for a part of C and/or Mn. . However, when the W content is more than 2.00%, the workability in the heat treatment is impaired and the productivity is lowered. Therefore, the W content is made 2.00% or less. Further, the W content is preferably set to 1.20% or less. On the other hand, the effect of the present embodiment is not particularly limited, and the effect of the present embodiment is not particularly limited. However, in order to sufficiently obtain the effect of increasing the strength by using W, the W content is preferably 0.01% or more, and more preferably 0.10% or more.

並且本實施形態之熔融鍍鋅鋼板的母材鋼板中亦可含有合計0.0001%~0.0100%之選自於由Ca、Ce、Mg、Zr、La及REM所構成群組中之1種或2種以上作為其他元素。含有該等元素的理由如下。其中,REM係Rare Earth Metal的簡稱,係指屬鑭系之元素。本發明實施形態中,REM及Ce大多以稀土金屬合金而含有,而除了La及Ce外還有複合含有鑭系元素之情形。含有該等La或Ce以外之鑭系元素作為雜質亦可發揮本實施形態之效果。又,含有金屬La或Ce亦可發揮本實施形態之效果。Further, the base material steel sheet of the hot-dip galvanized steel sheet according to the present embodiment may contain a total of 0.0001% to 0.0100% of one or two selected from the group consisting of Ca, Ce, Mg, Zr, La, and REM. Above as other elements. The reasons for containing these elements are as follows. Among them, REM is the abbreviation of Rare Earth Metal, which refers to the elements of the genus. In the embodiment of the present invention, REM and Ce are mostly contained in a rare earth metal alloy, and in addition to La and Ce, a lanthanoid compound is contained in combination. The effect of the present embodiment can also be exhibited by containing the lanthanoid elements other than such La or Ce as impurities. Further, the effect of the present embodiment can be exhibited by containing the metal La or Ce.

Ca、Ce、Mg、Zr、La及REM係可有效改善熔融鍍鋅鋼板的成形性之元素,因此亦可含有1種或2種以上。然選自於由Ca、Ce、Mg、Zr、La及REM所構成群組中之1種或2種以上之含量合計大於0.0100%時,會有損及延性之虞,故設各元素含量合計為0.0100%以下。且該等各元素含量合計宜為0.0070%以下。另一方面,不特別限定選自於由Ca、Ce、Mg、Zr、La及REM所構成群組中之1種或2種以上之含量下限亦可發揮本實施形態之效果,然為了充分獲得改善熔融鍍鋅鋼板的成形性之效果,該等各元素含量合計宜為0.0001%以上。而由成形性之觀點,選自於由Ca、Ce、Mg、Zr、La及REM所構成群組中之1種或2種以上之含量合計更宜為0.0010%以上。Ca, Ce, Mg, Zr, La, and REM are elements which can effectively improve the formability of the hot-dip galvanized steel sheet, and therefore may be contained in one type or two or more types. However, when the total content of one or more selected from the group consisting of Ca, Ce, Mg, Zr, La, and REM is more than 0.0100%, the ductility is impaired, so that the total content of each element is set. It is 0.0100% or less. Further, the total content of the respective elements is preferably 0.0070% or less. On the other hand, the lower limit of the content of one or more selected from the group consisting of Ca, Ce, Mg, Zr, La, and REM is not particularly limited, and the effect of the present embodiment can be exhibited. The effect of improving the formability of the hot-dip galvanized steel sheet is preferably 0.0001% or more in total of the respective elements. In view of the formability, the total content of one or more selected from the group consisting of Ca, Ce, Mg, Zr, La, and REM is preferably 0.0010% or more.

本實施形態之熔融鍍鋅鋼板的化學成分中,以上說明之各元素的剩餘部份為Fe及雜質。此外,前述Ti、Nb、V、Cr、Ni、Cu、Mo、B、W皆允許在低於各前述下限値的微量下含有作為雜質。又,Ca、Ce、Mg、Zr、La、REM亦允許在低於其合計量下限値的極微量下含有作為雜質。In the chemical composition of the hot-dip galvanized steel sheet according to the present embodiment, the remainder of each element described above is Fe and impurities. Further, the above Ti, Nb, V, Cr, Ni, Cu, Mo, B, and W are all allowed to be contained as impurities in a trace amount lower than each of the above lower limits. Further, Ca, Ce, Mg, Zr, La, and REM are also allowed to be contained as impurities in a very small amount below the lower limit of the total amount thereof.

所規定之本發明實施形態之熔融鍍鋅鋼板的母材鋼板組織的理由如下。The reason for the base material steel sheet structure of the hot-dip galvanized steel sheet according to the embodiment of the present invention is as follows.

(微觀組織) 說明本發明實施形態之熔融鍍鋅鋼板之母材鋼板的微觀組織。鋼板特性會隨微觀組織而改變,而要將微觀組織定量化時,以現實來說要將鋼板整個區域定量化來規定是不可能的。因此,本發明係將可表示鋼材代表性之微觀組織、即將以母材鋼板表面起1/4厚度為中心之1/8厚度~3/8厚度的微觀組織定量化來規定。板厚中央部之微觀組織會因強勁的凝固偏析而改變,故無法稱作可代表鋼板的微觀組織。而靠近鋼板表層的部位的微觀組織會因局部溫度變化或與外部氣體反應而改變,故無法稱作可代表鋼板的微觀組織。 本發明實施形態之熔融鍍鋅鋼板的母材鋼板的微觀組織,以母材鋼板表面起1/4厚度為中心之1/8厚度~3/8厚度範圍中,肥粒鐵相(以下稱肥粒鐵)以體積分率計在40%以上且97%以下,由變韌鐵相(以下稱變韌鐵)、變韌肥粒鐵相(以下稱變韌肥粒鐵)、新生麻田散鐵相(以下稱新生麻田散鐵)與回火麻田散鐵相(以下稱回火麻田散鐵)中之1種以上所構成之硬質組織合計以體積分率計為3%以上,殘留沃斯田鐵相(以下稱殘留沃斯田鐵)以體積分率計為0%~8%(包含0%),波來鐵相(以下稱波來鐵)與粗大雪明碳鐵相(以下稱雪明碳鐵)之合計以體積分率計為0%~8%(包含0%)。(Microstructure) The microstructure of the base material steel sheet of the hot-dip galvanized steel sheet according to the embodiment of the present invention will be described. The characteristics of the steel sheet change with the microstructure. When the microstructure is to be quantified, it is impossible to quantify the entire area of the steel sheet in reality. Therefore, the present invention is defined by quantifying a microstructure representative of a steel material, that is, a microstructure having a thickness of 1/8 to 3/8 centering on the surface of the base material steel sheet at a thickness of 1/4. The microstructure at the center of the plate thickness changes due to strong solidification segregation and cannot be called a microstructure representative of the steel sheet. The microstructure of the portion near the surface of the steel sheet may change due to local temperature changes or reaction with external gases, and therefore cannot be referred to as a microstructure representative of the steel sheet. The microstructure of the base material steel sheet of the hot-dip galvanized steel sheet according to the embodiment of the present invention is in the range of 1/8 thickness to 3/8 thickness centering on the surface of the base material steel sheet, and the ferrite grain phase (hereinafter referred to as fat) Granular iron) is 40% or more and 97% or less by volume fraction, and is composed of a toughened iron phase (hereinafter referred to as toughened iron), a toughened ferrite iron phase (hereinafter referred to as a toughened ferrite iron), and a new generation of Matian iron. The total number of hard structures consisting of one or more of the phase (hereinafter referred to as the nascent granulated iron) and the tempered granulated iron phase (hereinafter referred to as the tempered granulated iron) is 3% or more in terms of volume fraction, and the remaining Worthfield The iron phase (hereinafter referred to as residual Worthite iron) is 0% to 8% (including 0%) in terms of volume fraction, and the Borne iron phase (hereinafter referred to as Borne iron) and the coarse snowy carbon iron phase (hereinafter referred to as snow) The total amount of carbon iron is 0% to 8% (including 0%) in terms of volume fraction.

「肥粒鐵」 肥粒鐵係具有優異延性之組織。然,因肥粒鐵為軟質故強度低,而若設肥粒鐵的體積分率超過97%的話,無法獲得具充分拉伸最大強度的熔融鍍鋅鋼板。因此,肥粒鐵的體積分率設為97%以下。而為了提高熔融鍍鋅鋼板的拉伸最大強度,肥粒鐵的體積分率宜設為92%以下,更宜設為85%以下。進而,要獲得拉伸最大強度超過950MPa的熔融鍍鋅鋼板,肥粒鐵的體積分率設為80%以下更佳,又宜設為70%以下。另一方面,肥粒鐵的體積分率若低於50%則無法獲得充分的延性,故設肥粒鐵的體積分率為50%以上。肥粒鐵的體積分率宜設為55%以上,60%以上更佳。"Fat Grain Iron" A fermented iron system with excellent ductility. However, since the ferrite iron is soft, the strength is low, and if the volume fraction of the ferrite is more than 97%, the molten galvanized steel sheet having the maximum tensile strength can not be obtained. Therefore, the volume fraction of the ferrite iron is set to be 97% or less. In order to increase the maximum tensile strength of the hot-dip galvanized steel sheet, the volume fraction of the ferrite iron should be 92% or less, and more preferably 85% or less. Further, in order to obtain a hot-dip galvanized steel sheet having a tensile maximum strength of more than 950 MPa, the volume fraction of the ferrite iron is preferably 80% or less, and more preferably 70% or less. On the other hand, if the volume fraction of the ferrite iron is less than 50%, sufficient ductility cannot be obtained, so the volume fraction of the ferrite iron is set to 50% or more. The volume fraction of ferrite iron should be set to 55% or more, and more preferably 60% or more.

「殘留沃斯田鐵」 殘留沃斯田鐵係可提升熔融鍍鋅鋼板的強度-延性平衡之組織。另一方面,殘留沃斯田鐵會伴隨變形變態成硬質的麻田散鐵,而成為破壞的起點帶來影響,使延伸凸緣性變差,故設殘留沃斯田鐵的體積分率上限為8%。由熔融鍍鋅鋼板的成形性之觀點,殘留沃斯田鐵的體積分率宜小,而宜設為5%以下,設為0%~3%(包含0%)更佳。熔融鍍鋅鋼板的殘留沃斯田鐵的體積分率宜越小越好,0%亦無妨。"Residual Vostian Iron" Residual Worth Iron is a structure that enhances the strength-ductility balance of hot-dip galvanized steel sheets. On the other hand, the residual Worthite iron is deformed into a hard granulated loose iron, which has an influence on the starting point of the fracture, and the stretch flangeability is deteriorated. Therefore, the upper limit of the volume fraction of the remaining Worthite iron is 8%. From the viewpoint of moldability of the hot-dip galvanized steel sheet, the volume fraction of the remaining Worth iron is preferably small, and is preferably 5% or less, and more preferably 0% to 3% (including 0%). The volume fraction of the residual Worthite iron in the hot-dip galvanized steel sheet should be as small as possible, and 0% is also no problem.

「硬質組織」 為了提高熔融鍍鋅鋼板的拉伸最大強度,由變韌鐵、變韌肥粒鐵、新生麻田散鐵與回火麻田散鐵中之1種以上所構成之硬質組織的體積分率合計必須設為3%以上。為了提高熔融鍍鋅鋼板的拉伸最大強度,硬質組織的體積分率宜設為7%以上,設為15%以上更佳。另一方面,若過度提高硬質組織的體積分率會使熔融鍍鋅鋼板的延性變差,故將硬質組織的體積分率限制在60%以下。由該觀點,硬質組織的體積分率宜設為55%以下,50%以下更佳。"Hard tissue" In order to increase the maximum tensile strength of the hot-dip galvanized steel sheet, the volume fraction of the hard structure composed of one or more of the toughened iron, the toughened ferrite iron, the new Matian loose iron, and the tempered Matian loose iron The total ratio must be set to 3% or more. In order to increase the maximum tensile strength of the hot-dip galvanized steel sheet, the volume fraction of the hard structure is preferably 7% or more, and more preferably 15% or more. On the other hand, if the volume fraction of the hard structure is excessively increased, the ductility of the hot-dip galvanized steel sheet is deteriorated, so that the volume fraction of the hard structure is limited to 60% or less. From this point of view, the volume fraction of the hard tissue is preferably set to 55% or less, more preferably 50% or less.

「變韌肥粒鐵及變韌鐵」 變韌肥粒鐵及變韌鐵係熔融鍍鋅鋼板之強度與成形性之平衡優異的組織,而鋼板組織中亦可以體積分率計60%以下含有變韌肥粒鐵及/或變韌鐵。又,變韌肥粒鐵及變韌鐵係具有強度在軟質的肥粒鐵與硬質的麻田散鐵、回火麻田散鐵及殘留沃斯田鐵中間的微觀組織,而以延伸凸緣性之觀點含有5%以上更佳,且含有10%以上更佳。另一方面,變韌肥粒鐵及/或變韌鐵的體積分率若超過60%,則降伏應力會過度升高,而有形狀凍結性變差之虞,故而不適宜。"Toughened ferrite iron and toughened iron" The structure of the toughened ferrite and the toughened iron-based hot-dip galvanized steel sheet with excellent balance between strength and formability, and the steel sheet structure may contain 60% or less by volume fraction. Toughened ferrite iron and / or toughened iron. Moreover, the toughened ferrite iron and the toughened iron system have a strength in the middle of the soft ferrite iron and the hard Ma Tian loose iron, the tempered Ma Tian loose iron and the residual Worth iron, and the stretch flanged The viewpoint is more preferably 5% or more, and more preferably 10% or more. On the other hand, if the volume fraction of the toughened ferrite iron and/or the toughened iron exceeds 60%, the lodging stress is excessively increased, and the shape freezing property is deteriorated, which is not preferable.

「回火麻田散鐵」 回火麻田散鐵係可大幅提升熔融鍍鋅鋼板的拉伸強度之組織,而鋼板組織中亦可含有以體積分率計60%以下。由拉伸強度的觀點,回火麻田散鐵的體積分率宜設為5%以上。另一方面,鋼板組織所含回火麻田散鐵的體積分率若超過60%,降伏應力會過度升高,而有形狀凍結性變差之虞而不佳。"Returning to Ma Tian loose iron" The tempering Ma Tian loose iron system can greatly increase the tensile strength of the hot-dip galvanized steel sheet, and the steel sheet structure may also contain 60% or less by volume fraction. From the viewpoint of tensile strength, the volume fraction of the tempered granulated iron should be set to 5% or more. On the other hand, if the volume fraction of the tempered iron in the steel sheet structure exceeds 60%, the stress of the undulation will increase excessively, and the shape freezing property may be deteriorated.

「新生麻田散鐵」 新生麻田散鐵可大幅提升熔融鍍鋅鋼板的拉伸強度,但另一方面卻會成為破壞的起點使延伸凸緣性變差,因此鋼板組織中宜含有以體積分率計30%以下。尤其係為了提高擴孔性,新生麻田散鐵的體積分率更宜設為20%以下,設為10%以下更佳。"New Ma Tian San Shi" The new Ma Tian loose iron can greatly increase the tensile strength of the hot-dip galvanized steel sheet, but on the other hand, it will become the starting point of the damage and the stretch flangeability will be deteriorated. Therefore, the steel sheet structure should contain the volume fraction. It is less than 30%. In particular, in order to improve the hole expandability, the volume fraction of the new Ma Tian loose iron is more preferably set to 20% or less, and more preferably 10% or less.

「其他微觀組織」 本發明實施形態之熔融鍍鋅鋼板的鋼板組織中亦可含有波來鐵及/或粗大的雪明碳鐵等上述以外之組織。然,若熔融鍍鋅鋼板的鋼板組織中波來鐵及/或粗大的雪明碳鐵變多,會使延性變差。由此看來,設鋼板組織所含波來鐵及/或粗大的雪明碳鐵的體積分率合計為8%以下。此外,波來鐵及/或粗大的雪明碳鐵的體積分率合計宜為5%以下。"Other Microstructures" The steel sheet structure of the hot-dip galvanized steel sheet according to the embodiment of the present invention may contain a structure other than the above, such as a pulverized iron and/or a coarse stellite. However, if the amount of ferrite and/or coarse swarf carbon iron in the steel sheet structure of the hot-dip galvanized steel sheet increases, the ductility deteriorates. From this point of view, it is assumed that the volume fraction of the pulverized iron and/or the coarse swarf carbon iron contained in the steel sheet structure is 8% or less in total. Further, the volume fraction of the pulverized iron and/or the coarse swarf carbon iron is preferably 5% or less in total.

又,本發明實施形態之熔融鍍鋅鋼板的鋼板組織,以鍍敷層與母材鋼板(基鐵)之界面為起點之至鋼板方向深度20μm為止的表層部中,係將殘留沃斯田鐵的體積分率限制在3%以下,並且前述表層部中前述硬質組織的體積分率「V1」在以鋼板表面起1/4厚度為中心之1/8厚度~3/8厚度範圍中前述硬質組織的體積分率「V2」的0.10倍以上且0.90倍以下之範圍。In the steel sheet structure of the hot-dip galvanized steel sheet according to the embodiment of the present invention, the surface portion of the surface layer having a depth of 20 μm from the interface between the plating layer and the base material steel sheet (base iron) is retained, and the Worthite iron remains. The volume fraction is limited to 3% or less, and the volume fraction "V1" of the hard structure in the surface layer portion is in the range of 1/8 thickness to 3/8 thickness centering on the 1/4 thickness of the steel sheet surface. The volume fraction of the tissue "V2" is in the range of 0.10 times or more and 0.90 times or less.

「鍍敷層與基鐵之界面附近的殘留沃斯田鐵」 熔融鍍鋅鋼板之鍍敷層與母材鋼板之界面附近的殘留沃斯田鐵係一會伴隨變形變態成硬質的麻田散鐵,而在對熔融鍍鋅鋼板表面附近施加大的應變之彎曲變形時會成為破壞的起點帶來影響,造成彎曲性及耐疲勞特性變差的組織。由該觀點,以鍍敷層與母材鋼板之界面為起點之至鋼板方向深度20μm為止的表層部中,須將殘留沃斯田鐵的體積分率限制在0%~3%(包含0%)。並且,該表層部的殘留沃斯田鐵的體積分率宜越低越好,0%亦無妨。"Remaining Worthfield iron near the interface between the plating layer and the base iron" The residual Worthite iron near the interface between the plated layer of the hot-dip galvanized steel sheet and the base metal plate is deformed into a hard Ma Tian loose iron. On the other hand, when a large strain is applied to the vicinity of the surface of the hot-dip galvanized steel sheet, the deformation starts to be affected, and the bending property and the fatigue resistance are deteriorated. From this point of view, in the surface layer portion from the interface between the plating layer and the base material steel sheet to the depth of the steel sheet direction of 20 μm, the volume fraction of the residual Worthite iron must be limited to 0% to 3% (including 0%). ). Further, the volume fraction of the remaining Worthite iron in the surface layer portion is preferably as low as possible, and 0% is also not preferable.

「鍍敷層與基鐵之界面附近的硬質組織」 熔融鍍鋅鋼板之鍍敷層與母材鋼板(基鐵)之界面附近的硬質組織係可提高熔融鍍鋅鋼板表層部的強度,使疲勞極限強度大幅提升,而有助於耐疲勞特性改善的組織。由該觀點,將以鍍敷層與基鐵之界面為起點之至鋼板方向深度20μm為止的表層部中硬質組織的體積分率設為「V1」、且設以鋼板表面起1/4厚度為中心之1/8厚度~3/8厚度範圍的合計體積分率為「V2」時,必須令該等比V1/V2為0.10以上,來充分提高熔融鍍鋅鋼板表層部的強度。此外,為了充分提升耐疲勞特性,V1/V2宜為0.20以上,0.30以上更佳,且0.40以上更佳。另一方面,將以鍍敷層與基鐵之界面為起點之至鋼板方向深度20μm為止的表層部中硬質組織分率做某程度抑制,來降低熔融鍍鋅鋼板表面附近的強度以提升局部延性,亦可改善彎曲性。由該觀點,為了獲得良好的彎曲性,係將V1/V2設為0.90以下,且宜設為0.85以下,更宜設為0.80以下。"Hard structure near the interface between the plating layer and the base iron" The hard structure near the interface between the plating layer of the hot-dip galvanized steel sheet and the base material steel sheet (base iron) can improve the strength of the surface layer portion of the hot-dip galvanized steel sheet and cause fatigue. The ultimate strength is greatly improved, and the tissue contributes to the improvement of fatigue resistance. From this point of view, the volume fraction of the hard structure in the surface layer portion from the interface between the plating layer and the base iron to the depth in the steel sheet direction of 20 μm is "V1", and the thickness of the steel sheet is 1/4. When the total volume fraction of the 1/8 thickness to 3/8 thickness range of the center is "V2", the ratio V1/V2 must be 0.10 or more to sufficiently increase the strength of the surface layer portion of the hot-dip galvanized steel sheet. Further, in order to sufficiently improve the fatigue resistance, V1/V2 is preferably 0.20 or more, more preferably 0.30 or more, and more preferably 0.40 or more. On the other hand, the hard tissue fraction in the surface layer portion from the interface between the plating layer and the base iron to the depth of the steel sheet of 20 μm is suppressed to some extent, and the strength near the surface of the hot-dip galvanized steel sheet is lowered to improve the local ductility. It can also improve the flexibility. From this viewpoint, in order to obtain good bendability, V1/V2 is set to 0.90 or less, and is preferably set to 0.85 or less, and more preferably set to 0.80 or less.

並且,本實施形態之熔融鍍鋅鋼板中以鍍敷層與基鐵之界面為起點之至鋼板方向深度20μm為止的表層部中,亦可於鐵的BCC晶界及/或晶粒內具有含Si及/或Mn之微細的氧化物。藉由先於表層部之鋼板內部生成微細的氧化物,可抑制會成為鍍敷層剝離之起點之於鋼板表面、亦即於鍍敷層與母材鋼板之界面生成含Si及/或Mn的氧化物。Further, in the hot-dip galvanized steel sheet according to the present embodiment, the surface layer portion having a depth from the interface between the plating layer and the base iron to the depth of the steel sheet of 20 μm may be contained in the BCC grain boundary and/or the crystal grains of the iron. A fine oxide of Si and/or Mn. By forming a fine oxide in the steel sheet before the surface layer portion, it is possible to suppress the formation of Si and/or Mn at the interface of the steel sheet, that is, at the interface between the plating layer and the base material steel sheet, which is the starting point of the peeling of the plating layer. Oxide.

本發明實施形態之熔融鍍鋅鋼板的母材鋼板所含各組織的體積分率例如係依以下所示方法測定。The volume fraction of each structure contained in the base material steel sheet of the hot-dip galvanized steel sheet according to the embodiment of the present invention is measured, for example, by the method described below.

本發明熔融鍍鋅鋼板之鋼板組織所含肥粒鐵、變韌肥粒鐵、變韌鐵、回火麻田散鐵、新生麻田散鐵、波來鐵及粗大雪明碳鐵的體積分率可利用以下方法測定。首先,以與鋼板之軋延方向平行之板厚截面為觀察面採取試料後,研磨觀察面,並進行硝太蝕劑蝕刻。然後,分別將以板厚1/4為中心之1/8厚度~3/8厚度之範圍、或以鍍敷層與母材鋼板(基鐵)之界面為起點之至鋼板方向深度20μm為止的範圍,用場發射掃描型電子顯微鏡(FE-SEM:Field Emission Scanning Electron Microscope)觀察並測定面積分率,並將其視作體積分率。其中,鍍敷層被硝太蝕劑蝕刻去除時,亦可將試料表面視為鍍敷層與基鐵之界面。The volume fraction of the fermented iron, the toughened ferrite iron, the toughened iron, the tempering Ma Tian loose iron, the new Ma Tian loose iron, the Bora iron and the coarse snowy carbon iron may be included in the steel sheet structure of the hot-dip galvanized steel sheet of the present invention. It was measured by the following method. First, after taking a sample with a plate thickness section parallel to the rolling direction of the steel sheet as a viewing surface, the observation surface is polished and subjected to a nital etchant etching. Then, the thickness is 1/8 to 3/8 of the thickness of 1/4 of the thickness of the sheet, or the depth of the steel sheet is 20 μm from the interface between the plating layer and the base steel sheet (base iron). In the range, the area fraction was observed and measured by a field emission scanning electron microscope (FE-SEM: Field Emission Scanning Electron Microscope), and this was regarded as a volume fraction. When the plating layer is etched away by the oxidizing agent, the surface of the sample can also be regarded as the interface between the plating layer and the base iron.

本實施形態之熔融鍍鋅鋼板的鋼板組織所含殘留沃斯田鐵的體積分率,係用FE-SEM、及利用EBSD(Electron Bach-Scattering Diffraction)法進行高分解能晶體方向解析來評估。首先,將與軋延方向平行之板厚截面加工成鏡面,以母材鋼板表面起1/4厚度為中心之1/8厚度~3/8厚度範圍、或以鍍敷層與基鐵之界面為起點之至鋼板方向深度20μm為止的範圍,分別將測定間距設為0.15μm以下,在合計10000μm 2以上的區域中測定晶體方向。然後,判斷各測定點為BCC(體心立方結構)之鐵或為FCC(面心立方結構)之鐵,並以判斷為FCC鐵之點作為殘留沃斯田鐵,測定殘留沃斯田鐵的面積分率,而可將其作為體積分率。此外,若測定很廣的區域則面積分率會與體積分率等價,故在前述情況下藉由於合計10000μm 2以上之區域中測定晶體方向可將殘留沃斯田鐵的面積分率作為體積分率。 The volume fraction of the remaining Worthite iron contained in the steel sheet structure of the hot-dip galvanized steel sheet according to the present embodiment was evaluated by FE-SEM and analysis of the direction of the high decomposition energy crystal by the EBSD (Electron Bach-Scattering Diffraction) method. First, the plate thickness section parallel to the rolling direction is processed into a mirror surface, and the surface of the base material steel plate is 1/8 thickness to 3/8 thickness centered on the 1/4 thickness, or the interface between the plating layer and the base iron. In the range from the starting point to the depth of the steel sheet direction of 20 μm, the measurement pitch is 0.15 μm or less, and the crystal direction is measured in a total area of 10000 μm 2 or more. Then, it is judged that each measurement point is iron of BCC (body-centered cubic structure) or iron of FCC (face-centered cubic structure), and the point of FCC iron is judged as residual Worthite iron, and the residual Worthite iron is determined. Area fraction, which can be used as the volume fraction. In addition, if a wide area is measured, the area fraction will be equivalent to the volume fraction. Therefore, in the above case, the area fraction of the residual Worthite iron can be regarded as a volume by measuring the crystal direction in a total area of 10000 μm 2 or more. The rate.

如圖1所示,本實施形態之熔融鍍鋅鋼板係於熔融鍍鋅層10與母材鋼板20之界面具有Fe-Al合金層30,且於母材鋼板20內具有以下所示微細化層40及脫碳層50。 微細化層及脫碳層如後述,係在退火步驟中於特定溫度域下控制在特定氣體環境之條件下進行脫碳反應而生成之層。因此,微細化層及脫碳層內的結構相除了氧化物及介在物粒子外,實質上係以肥粒鐵相60為主體的組織。具體而言,係指肥粒鐵相的體積分率在70%以上,且剩餘部份組織為沃斯田鐵相、變韌鐵相、麻田散鐵相、波來鐵相中之1種或2種以上所佔之混合組織的層。 微細化層係定義為微細化層在母材鋼板最表部中肥粒鐵相的平均粒徑為脫碳層中肥粒鐵相的平均粒徑的1/2以下時存在。並將微細化層中肥粒鐵相的平均粒徑超過脫碳層中肥粒鐵相的平均粒徑1/2之境界定義為微細化層與脫碳層之境界。As shown in Fig. 1, the hot-dip galvanized steel sheet according to the present embodiment has an Fe-Al alloy layer 30 at the interface between the hot-dip galvanized layer 10 and the base material steel sheet 20, and has the following fine layer in the base material steel sheet 20. 40 and decarburization layer 50. The micronized layer and the decarburized layer are layers which are formed by performing a decarburization reaction under a specific gas atmosphere in a specific temperature range as described later in the annealing step. Therefore, in addition to the oxide and the intervening particles, the structure in the fine layer and the decarburized layer is substantially a structure mainly composed of the ferrite-grained iron phase 60. Specifically, it means that the volume fraction of the iron phase of the fertiliser is above 70%, and the remaining part of the structure is one of the Worthfield iron phase, the toughened iron phase, the Matian iron phase, and the Borne iron phase. Two or more layers of mixed tissue. The micronized layer is defined as a micronized layer which exists when the average particle diameter of the ferrite-grain phase in the outermost portion of the base material steel sheet is 1/2 or less of the average particle diameter of the ferrite-grain iron phase in the decarburized layer. The boundary between the average particle diameter of the ferrite iron phase in the micronized layer and the average particle diameter of the ferrite iron phase in the decarburized layer is defined as the boundary between the micronized layer and the decarburized layer.

微細化層係與前述Fe-Al合金層直接接觸。微細化層的平均厚度為0.1μm~5.0μm,微細化層內肥粒鐵相的平均粒徑為0.1μm~3.0μm,微細化層中含有Si及Mn之1種或2種以上氧化物,且其氧化物最大徑為0.01μm~0.4μm。The micronized layer is in direct contact with the aforementioned Fe-Al alloy layer. The average thickness of the fine layer is 0.1 μm to 5.0 μm, and the average particle diameter of the ferrite iron phase in the fine layer is 0.1 μm to 3.0 μm, and the fine layer contains one or more oxides of Si and Mn. Further, the maximum diameter of the oxide is from 0.01 μm to 0.4 μm.

微細化層的平均厚度為0.1μm~5.0μm。微細化層的平均厚度低於0.1μm時,則無法獲得抑制裂痕產生及延展的效果而無法獲得鍍敷密著性的改善效果。若大於5.0μm,則會促使鍍敷層合金化(生成Zn-Fe合金),使鍍敷層中的Fe含量變大,造成鍍敷密著性降低。較佳微細化層的平均厚度為0.2μm~4.0μm,更佳為0.3μm~3.0μm。The average thickness of the micronized layer is from 0.1 μm to 5.0 μm. When the average thickness of the micronized layer is less than 0.1 μm, the effect of suppressing the occurrence of cracks and stretching cannot be obtained, and the effect of improving the plating adhesion cannot be obtained. When it is more than 5.0 μm, the plating layer is promoted to be alloyed (the Zn-Fe alloy is formed), and the Fe content in the plating layer is increased to cause a decrease in plating adhesion. The average thickness of the finely refined layer is preferably 0.2 μm to 4.0 μm, more preferably 0.3 μm to 3.0 μm.

在鋼板寬度方向上之前述微細化層的最大厚度與最小厚度的差宜為2.0μm以內。在此,在鋼板寬度方向上之前述微細化層的最大厚度與最小厚度係指分別測定距離兩端50mm之位置與將其之間分成7等分之共計8處的微細化層的厚度,其中最大厚度與最小厚度。微細化層的厚度越厚,就越易使鍍敷層的合金化(生成Zn-Fe合金)進行,故在鋼板寬度方向上之微細化層的厚度差若大,其會造成合金化不均,而有對鍍敷密著性及鍍敷外觀均勻性造成不良影響之情形。故由鍍敷密著性及鍍敷外觀均勻性之觀點,在鋼板寬度方向上之前述微細化層的最大厚度與最小厚度的差宜為1.5μm以下,1.0μm以下更佳。The difference between the maximum thickness and the minimum thickness of the aforementioned fine layer in the width direction of the steel sheet is preferably within 2.0 μm. Here, the maximum thickness and the minimum thickness of the micronized layer in the width direction of the steel sheet mean the thickness of the micronized layer which is measured at a position of 50 mm from both ends and a total of 8 divisions which are divided into 7 equal parts. Maximum thickness and minimum thickness. The thicker the thickness of the fine layer, the easier the alloying of the plating layer (forming a Zn-Fe alloy) is. Therefore, if the thickness difference of the fine layer in the width direction of the steel sheet is large, uneven alloying may occur. There is a case where the plating adhesion and the uniformity of the plating appearance are adversely affected. Therefore, the difference between the maximum thickness and the minimum thickness of the fine layer in the width direction of the steel sheet is preferably 1.5 μm or less and 1.0 μm or less from the viewpoint of plating adhesion and uniformity of plating appearance.

微細化層內的肥粒鐵相的平均粒徑為0.1μm~3.0μm。肥粒鐵相的平均粒徑若低於0.1μm,則無法獲得抑制裂痕產生及延展的效果而無法獲得鍍敷密著性的改善效果。肥粒鐵相的平均粒徑若超過3.0μm,則無法獲得鍍敷密著性的改善效果。故較佳肥粒鐵相的平均粒徑為0.1μm~2.0μm。The average grain size of the ferrite iron phase in the micronized layer is from 0.1 μm to 3.0 μm. When the average particle diameter of the ferrite-particle iron phase is less than 0.1 μm, the effect of suppressing generation and elongation of cracks cannot be obtained, and the effect of improving plating adhesion cannot be obtained. When the average particle diameter of the ferrite-grained iron phase exceeds 3.0 μm, the effect of improving the plating adhesion cannot be obtained. Therefore, the preferred ferrite iron phase has an average particle diameter of 0.1 μm to 2.0 μm.

微細化層中所含Si及Mn的1種或2種以上氧化物,例如可舉選自於由SiO 2、Mn 2SiO 4、MnSiO 3、Fe 2SiO 4、FeSiO 3、MnO中之1種或2種以上。 微細化層中所含Si及Mn的1種或2種以上氧化物的最大徑為0.01μm~0.4μm。該氧化物如後述,會於退火時於特定溫度域下形成於母材鋼板內部,利用該氧化物粒子可抑制母材鋼板表層之肥粒鐵相結晶的成長,而形成微細化層。氧化物最大徑小於0.01μm時,微細化層會無法充分形成,而使鍍敷密著性變差。氧化物最大徑大於0.4μm時,肥粒鐵相會粗大化,使微細化層無法充分形成,且該氧化物本身會變成鍍敷剝離的起點,使鍍敷密著性變差。因此,氧化物最大徑的較佳範圍為0.05μm~0.2μm。 One or two or more kinds of oxides of Si and Mn contained in the fine layer are, for example, one selected from the group consisting of SiO 2 , Mn 2 SiO 4 , MnSiO 3 , Fe 2 SiO 4 , FeSiO 3 , and MnO. Or two or more. The maximum diameter of one or two or more kinds of oxides of Si and Mn contained in the fine layer is 0.01 μm to 0.4 μm. As will be described later, the oxide is formed inside the base material steel sheet at a specific temperature range during annealing, and the oxide particles can suppress the growth of the ferrite-grained iron phase crystal in the surface layer of the base material steel sheet to form a fine layer. When the maximum diameter of the oxide is less than 0.01 μm, the fine layer may not be sufficiently formed, and the plating adhesion may be deteriorated. When the maximum diameter of the oxide is larger than 0.4 μm, the ferrite-grained iron phase is coarsened, and the fine-grained layer is not sufficiently formed, and the oxide itself becomes a starting point of plating peeling, which deteriorates plating adhesion. Therefore, the preferred range of the maximum diameter of the oxide is from 0.05 μm to 0.2 μm.

微細化層的平均厚度及微細化層內肥粒鐵相的平均粒徑依以下所示方法測定。自熔融鍍鋅鋼板以與母材鋼板的軋延方向平行之板厚截面為觀察面採取試料。利用CP(Cross section polisher)裝置加工試料的觀察面,並用FE-SEM(Field Emission Scanning Electron Microscopy)中的反射電子像以5000倍觀察來測定。The average thickness of the fine layer and the average particle diameter of the ferrite iron phase in the fine layer were measured by the following methods. The sample was taken from the hot-dip galvanized steel sheet with a plate thickness section parallel to the rolling direction of the base material steel plate as an observation surface. The observation surface of the sample was processed by a CP (Cross section polisher) apparatus, and measured by a reflection electron image in FE-SEM (Field Emission Scanning Electron Microscopy) at 5000 times.

微細化層中所含Si及Mn之1種或2種以上氧化物的最大徑係利用以下所示方法測定。自熔融鍍鋅鋼板以與母材鋼板的軋延方向平行之板厚截面為觀察面採取試料。將試料觀察面用FIB(Focused Ion Beam)加工製成薄膜試料。之後,用FE-TEM(Field Emission Transmission Electr on Microscopy)以30000倍觀察薄膜試料。對各薄膜試料觀察5視野,將全視野計測所得之氧化物直徑的最大値作為該薄膜試料之氧化物的最大徑。The maximum diameter of one or two or more oxides of Si and Mn contained in the fine layer was measured by the following method. The sample was taken from the hot-dip galvanized steel sheet with a plate thickness section parallel to the rolling direction of the base material steel plate as an observation surface. The sample observation surface was processed by FIB (Focused Ion Beam) to prepare a film sample. Thereafter, the film sample was observed at 30,000 times by FE-TEM (Field Emission Transmission Electr on Microscopy). Five fields of view were observed for each film sample, and the maximum 値 of the oxide diameter obtained by the full-field measurement was taken as the maximum diameter of the oxide of the film sample.

(Fe-Al合金層) 本發明實施形態係於鍍敷層與鋼板之界面形成有Fe-Al合金層。藉由形成Fe-Al合金層可抑制鍍敷層合金化(Zn-Fe合金生成),而可抑制鍍敷密著性降低。並且,可抑制因合金化不均造成之外觀不均。相較於在熔融鍍鋅處理後施行了合金化處理的合金化熔融鍍鋅鋼板,未施行合金化處理的熔融鍍鋅鋼板更容易因合金化不均造成外觀不均。故設Fe-Al合金層的厚度為0.1μm~2.0μm。當少於0.1μm時,會有使鍍敷密著性及外觀變差之情形,而多於2.0μm時,會有使鍍敷密著性降低之情形。故較佳為0.1μm~1.0μm。(Fe-Al alloy layer) In the embodiment of the present invention, an Fe-Al alloy layer is formed at the interface between the plating layer and the steel sheet. By forming the Fe—Al alloy layer, it is possible to suppress the alloying of the plating layer (the formation of the Zn—Fe alloy), and it is possible to suppress the deterioration of the plating adhesion. Further, it is possible to suppress uneven appearance due to uneven alloying. Compared with the alloyed hot-dip galvanized steel sheet which has been alloyed after the hot-dip galvanizing treatment, the hot-dip galvanized steel sheet which has not been alloyed is more likely to be uneven in appearance due to uneven alloying. Therefore, the thickness of the Fe-Al alloy layer is set to be 0.1 μm to 2.0 μm. When it is less than 0.1 μm, the plating adhesion and the appearance may be deteriorated, and when it is more than 2.0 μm, the plating adhesion may be lowered. Therefore, it is preferably from 0.1 μm to 1.0 μm.

將在鋼板寬度方向上之前述Fe-Al合金層的最大厚度與最小厚度的差設為0.5μm以內。在此,在鋼板寬度方向上之前述Fe-Al合金層的最大厚度與最小厚度係指分別測定距離兩端50mm之位置與將其之間分成7等分之共計8處的Fe-Al合金層厚度,其中最大厚度與最小厚度。Fe-Al合金層的厚度越薄鍍敷層的合金化(Zn-Fe合金生成)越易進行,故在鋼板寬度方向上之Fe-Al合金層厚度差若大,其會造成合金化不均,而有對鍍敷密著性及鍍敷外觀均勻性造成不良影響之情形。故由鍍敷密著性及鍍敷外觀均勻性之觀點,在鋼板寬度方向上之前述Fe-Al合金層的最大厚度與最小厚度的差宜為0.4μm以下,且0.3μm以下更佳。The difference between the maximum thickness and the minimum thickness of the aforementioned Fe-Al alloy layer in the width direction of the steel sheet was set to be within 0.5 μm. Here, the maximum thickness and the minimum thickness of the aforementioned Fe-Al alloy layer in the width direction of the steel sheet refer to a position where the position of 50 mm from both ends is respectively measured and a total of 8 portions of Fe-Al alloy layer divided into 7 equal portions are formed. Thickness, where maximum thickness and minimum thickness. The thinner the thickness of the Fe-Al alloy layer, the easier the alloying of the plating layer (the formation of the Zn-Fe alloy) is. Therefore, if the thickness difference of the Fe-Al alloy layer in the width direction of the steel sheet is large, it may cause uneven alloying. There is a case where the plating adhesion and the uniformity of the plating appearance are adversely affected. Therefore, the difference between the maximum thickness and the minimum thickness of the Fe-Al alloy layer in the width direction of the steel sheet is preferably 0.4 μm or less and more preferably 0.3 μm or less from the viewpoint of plating adhesion and uniformity of plating appearance.

(鍍敷層) 本發明實施形態中,熔融鍍鋅層之Fe含量大於0%且在3.0%以下,Al含量大於0%且在1.0%以下。並且熔融鍍鋅層可含有或混入Ag、B、Be、Bi、Ca、Cd、Co、Cr、Cs、Cu、Ge、Hf、I、K、La、Li、Mg、Mn、Mo、Na、Nb、Ni、Pb、Rb、Sb、Si、Sn、Sr、Ta、Ti、V、W、Zr、REM之1種或2種以上。依上述,即便熔融鍍鋅層含有或混入上述元素之1種或2種以上,亦不損本發明效果,且亦有其含量可改善耐蝕性及加工性之較佳的情形。 又,本實施形態中,熔融鍍鋅層亦可含有由ζ相(FeZn 13)構成之柱狀晶,而由鍍敷密著性之觀點,鍍敷層與母材鋼板之整個界面的ζ相被覆比率宜低於20%。 並且,母材鋼板單面的熔融鍍鋅層的附著量宜為10g/m 2以上且100g/m 2以下。 (Placing layer) In the embodiment of the present invention, the Fe content of the hot-dip galvanized layer is more than 0% and not more than 3.0%, and the Al content is more than 0% and not more than 1.0%. And the molten galvanized layer may contain or mix with Ag, B, Be, Bi, Ca, Cd, Co, Cr, Cs, Cu, Ge, Hf, I, K, La, Li, Mg, Mn, Mo, Na, Nb One or more of Ni, Pb, Rb, Sb, Si, Sn, Sr, Ta, Ti, V, W, Zr, and REM. In the above, even if one or two or more kinds of the above-mentioned elements are contained or mixed in the hot-dip galvanized layer, the effects of the present invention are not impaired, and the content thereof is preferably improved in corrosion resistance and workability. Further, in the present embodiment, the hot-dip galvanized layer may contain columnar crystals composed of a ruthenium phase (FeZn 13 ), and the ruthenium phase of the entire interface between the plating layer and the base material steel sheet from the viewpoint of plating adhesion The coverage ratio should be less than 20%. Further, the amount of adhesion of the hot-dip galvanized layer on one side of the base material steel sheet is preferably 10 g/m 2 or more and 100 g/m 2 or less.

[熔融鍍鋅層之Fe含量:大於0%且在3.0%以下] 熔融鍍鋅層之Fe含量大於0%且在3.0%以下。實質上要製造Fe含量為0%係很困難的。若Fe含量超過3.0%會使鍍敷密著性降低。Fe含量若低於0.3%,因會有使鍍敷密著性降低之情況,故由確保鍍敷密著性之觀點,Fe含量較佳範圍為0.3%~2.5%,且以0.5%~2.0%更佳。[Fe content of the hot-dip galvanized layer: more than 0% and not more than 3.0%] The Fe content of the hot-dip galvanized layer is more than 0% and not more than 3.0%. It is difficult to produce a Fe content of 0% in practice. If the Fe content exceeds 3.0%, the plating adhesion is lowered. When the Fe content is less than 0.3%, the plating adhesion may be lowered. Therefore, the Fe content is preferably in the range of 0.3% to 2.5% and 0.5% to 2.0 from the viewpoint of ensuring plating adhesion. % is better.

[熔融鍍鋅層之Al含量:大於0%且在1.0%以下] 熔融鍍鋅層之Al含量大於0%且在1.0%以下。鍍敷浴中不含Al時、或含極少量時會使鍍敷層進行合金化,使鍍敷密著性降低,故鍍敷層中的Al含量宜設為0.1%以上。在此鍍敷層的合金化係指Fe原子擴散至鍍敷層中,生成Zn-Fe合金之意。Al含量若大於1.0%則會使鍍敷密著性降低。故由確保鍍敷密著性之觀點,Al含量較佳範圍為0.1%~0.8%,更佳為0.2%~0.5%。[Al content of the hot-dip galvanized layer: more than 0% and less than 1.0%] The Al content of the hot-dip galvanized layer is more than 0% and not more than 1.0%. When the plating bath does not contain Al or contains a very small amount, the plating layer is alloyed and the plating adhesion is lowered. Therefore, the Al content in the plating layer is preferably 0.1% or more. The alloying of the plating layer means that Fe atoms diffuse into the plating layer to form a Zn-Fe alloy. When the Al content is more than 1.0%, the plating adhesion is lowered. Therefore, from the viewpoint of ensuring plating adhesion, the Al content is preferably in the range of 0.1% to 0.8%, more preferably 0.2% to 0.5%.

[熔融鍍鋅的附著量:10g/m 2~100g/m 2] 熔融鍍鋅層鍍敷到母材鋼板單面之附著量若少則有無法獲得充分的耐蝕性之虞。由此看來,鍍敷層鍍敷到母材鋼板單面之附著量宜設為10g/m 2以上。而由耐蝕性之觀點,附著量以20g/m 2以上更佳,且30g/m 2以上更佳。另一方面,若鍍敷層的附著量一多,進行點熔接時電極損耗會變激烈,而有於連續進行熔接時熔融塊徑減少及熔接接合強度變差之虞。因此,鍍敷層的附著量宜設為100g/m 2以下。由連續熔接性之觀點,附著量以93g/m 2以下佳,且85g/m 2以下更佳。 [Amount of adhesion by hot-dip galvanizing: 10 g/m 2 to 100 g/m 2 ] If the amount of adhesion of the hot-dip galvanized layer to one side of the base material steel sheet is small, sufficient corrosion resistance cannot be obtained. From this point of view, the adhesion amount of the plating layer to the single side of the base material steel sheet is preferably set to 10 g/m 2 or more. On the other hand, from the viewpoint of corrosion resistance, the adhesion amount is more preferably 20 g/m 2 or more, and more preferably 30 g/m 2 or more. On the other hand, when the amount of adhesion of the plating layer is large, the electrode loss becomes intense when the spot welding is performed, and the melting block diameter decreases and the fusion bonding strength deteriorates when the welding is continuously performed. Therefore, the amount of adhesion of the plating layer is preferably set to 100 g/m 2 or less. The continuous weldability viewpoint, the adhesion amount of 93g / m 2 or less good, and 85g / m 2 or less more preferably.

(熔融鍍鋅鋼板之製造方法) 接著,就製造本發明實施形態之熔融鍍鋅鋼板的方法進行詳細說明。(Manufacturing Method of Hot-Dip Galvanized Steel Sheet) Next, a method of producing a hot-dip galvanized steel sheet according to an embodiment of the present invention will be described in detail.

本實施形態之熔融鍍鋅鋼板的製造方法具備以下步驟:將具有上述化學成分之鋼胚加熱至1080℃以上後,施行軋延結束溫度設為850℃~980℃之範圍內的熱軋延製成熱軋鋼板,之後捲成捲材之步驟,將自熱軋延後至300℃為止的冷卻過程中的熱軋鋼板溫度控制成滿足後述式(1)之熱軋步驟;接續熱軋步驟進行酸洗後,進行合計軋縮率設為85%以下之冷軋延之冷軋步驟;將冷軋步驟後的鋼板在600℃~750℃間之平均加熱速度設為1.0℃/s以上,最高加熱溫度設為(Ac1+25)℃以上且Ac3℃以下,且在750℃以上之溫度域內進行加熱,然後在760℃~700℃間之平均冷卻速度設為0.1℃/s~5.0℃/s,在650℃~500℃間之平均冷卻速度設為1.0℃/s以上進行冷卻之退火步驟;於退火步驟後,於將鍍敷浴溫度設為440℃~470℃、進入鍍敷浴時的鋼板溫度設為430℃~480℃、鍍敷浴中有效Al量設為0.180~0.250質量%的鍍敷條件下將鋼板浸漬於鍍敷浴,對鋼板表面施行熔融鍍鋅而形成鍍敷層之鍍敷步驟;及,於鍍敷步驟後,將鋼板冷卻至100℃以下後使用直徑50mm~800mm的輥進行彎折-折回變形合計2次以上之加工步驟。 以下,就各製造步驟進行詳細說明。The method for producing a hot-dip galvanized steel sheet according to the present embodiment includes the following steps: heating the steel slab having the chemical composition to 1080 ° C or higher, and then performing hot rolling at a rolling end temperature of 850 ° C to 980 ° C. The step of forming a hot-rolled steel sheet and then winding it into a coil, controlling the temperature of the hot-rolled steel sheet during the cooling process from the hot rolling to 300 ° C to a hot rolling step satisfying the following formula (1); continuing the hot rolling step After the pickling, a cold rolling step of a cold rolling reduction in which the total rolling reduction ratio is 85% or less is performed; and the average heating rate between the steel sheets after the cold rolling step is between 600 ° C and 750 ° C is 1.0 ° C / s or more, the highest The heating temperature is (Ac1+25) °C or higher and Ac3 °C or lower, and heating is performed in a temperature range of 750 ° C or higher, and then the average cooling rate between 760 ° C and 700 ° C is set to 0.1 ° C / s to 5.0 ° C / s, an annealing step of cooling at an average cooling rate between 650 ° C and 500 ° C of 1.0 ° C / s or more; after the annealing step, when the temperature of the plating bath is 440 ° C to 470 ° C, entering the plating bath The steel plate temperature is set to 430 ° C ~ 480 ° C, the effective Al amount in the plating bath is set to 0.180 a plating step of immersing a steel sheet in a plating bath under 0.250 mass% plating conditions, and performing a hot-dip galvanization on the surface of the steel sheet to form a plating layer; and, after the plating step, cooling the steel sheet to 100 ° C or lower and then using A roll having a diameter of 50 mm to 800 mm is subjected to a bending/returning deformation of a total of two or more processing steps. Hereinafter, each manufacturing step will be described in detail.

要製造本發明實施形態之熔融鍍鋅鋼板,首先要製造母材鋼板。 母材鋼板係鑄造因應特性含有之合金元素的鋼胚,並施行熱軋延後施行冷軋延來製造。 以下,就各製造步驟進行詳細說明。In order to manufacture the hot-dip galvanized steel sheet according to the embodiment of the present invention, first, a base material steel sheet is produced. The base material steel plate is produced by casting a steel embryo of the alloy element in accordance with the characteristics, and performing hot rolling and rolling to produce a cold rolling. Hereinafter, each manufacturing step will be described in detail.

「鑄造步驟」 首先,鑄造要供於熱軋延之鋼胚。鋼胚的化學成分(組成)宜為上述成分。要供於熱軋延之鋼胚可使用連續鑄造鋼胚或利用薄鋼胚連鑄機等所製出者。"Casting Step" First, the steel is to be cast for hot rolling. The chemical composition (composition) of the steel embryo is preferably the above component. Steel blanks to be used for hot rolling may be produced by continuously casting steel or by using a thin steel continuous casting machine or the like.

「熱軋步驟」 在熱軋步驟中,為了抑制鑄造所造成之晶體方向的各向異性,鋼胚的加熱溫度宜設為1080℃以上。鋼胚的加熱溫度更宜設為1150℃以上。另一方面,鋼胚的加熱溫度上限並無限定。在高於1300℃加熱鋼胚需投入大量能量,而會導致製造成本大幅增加。由此看來,鋼胚的加熱溫度宜設為1300℃以下。"Hot Rolling Step" In the hot rolling step, in order to suppress anisotropy in the crystal direction caused by casting, the heating temperature of the steel blank is preferably set to 1080 ° C or higher. The heating temperature of the steel embryo is more preferably set to be above 1150 °C. On the other hand, the upper limit of the heating temperature of the steel blank is not limited. Heating the steel embryo above 1300 °C requires a lot of energy, which leads to a substantial increase in manufacturing costs. From this point of view, the heating temperature of the steel blank should be set to 1300 ° C or less.

於加熱鋼胚後進行熱軋延。熱軋延的結束溫度(軋延結束溫度)若低於850℃,則會使軋延的反作用力變高,而難以穩定製得指定板厚。因此,熱軋延的結束溫度宜設為850℃以上,更宜設為870℃以上。另一方面,要將熱軋延的結束溫度設為高於980℃,於鋼胚加熱結束起至熱軋延結束為止之步驟中須使用加熱鋼板之裝置,而造成成本高騰。因此,熱軋延的結束溫度設為980℃以下,更宜設為950℃以下。Hot rolling is performed after heating the steel embryo. When the end temperature (rolling end temperature) of the hot rolling is lower than 850 ° C, the reaction force of the rolling is increased, and it is difficult to stably obtain the specified thickness. Therefore, the end temperature of the hot rolling is preferably set to 850 ° C or higher, and more preferably set to 870 ° C or higher. On the other hand, in order to set the end temperature of the hot rolling to be higher than 980 ° C, a device for heating the steel sheet is required in the step from the end of the heating of the steel bristles to the end of the hot rolling, which causes a high cost. Therefore, the end temperature of the hot rolling is set to 980 ° C or lower, and more preferably 950 ° C or lower.

接著,將熱軋延後的熱軋鋼板捲成捲材。此外,自熱軋延至捲取為止之冷卻過程中的平均冷卻速度宜設為10℃/秒以上。其係因藉由在更低溫下進行變態,可使熱軋鋼板的粒徑微細,使冷軋及退火後的母材鋼板的有效結晶粒徑微細。Next, the hot rolled steel sheet which has been subjected to hot rolling is wound into a coil. Further, the average cooling rate during the cooling from the hot rolling to the winding is preferably set to 10 ° C /sec or more. This is because the particle size of the hot-rolled steel sheet can be made fine by the transformation at a lower temperature, and the effective crystal grain size of the base material steel sheet after cold rolling and annealing can be made fine.

熱軋鋼板的捲取溫度宜設為450℃以上且650℃以下。其係因波來鐵及/或長徑1μm以上的粗大雪明碳鐵會分散並生成於熱軋鋼板的微觀組織中,使因冷軋延而導入熱軋鋼板的應變局域化之故。藉此可於退火步驟中使各種晶體方向的沃斯田鐵逆變態,將退火後的母材鋼板的有效晶粒微細化。捲取溫度若低於450℃,會有無法生成波來鐵及/或粗大雪明碳鐵之情況而不適宜。另一方面,捲取溫度若高於650℃,則波來鐵與肥粒鐵會分別沿軋延方向生成長帶狀。藉此,從肥粒鐵部分會有生成出在冷軋延及退火後生成之母材鋼板的有效晶粒沿軋延方向延展之粗大物的傾向,而不適宜。 而且,捲取熱軋鋼板後,會有於鏽皮層下發生內部氧化層形成地不均勻(中央部比端部厚)之情形。而捲取溫度若高於650℃則該現象越顯著。該內部氧化層在後述的後續步驟(酸洗、冷軋)中無法去除時,會影響微細化層及Fe-Al合金層形成地不均勻,而有給予鍍敷密著性及外觀均勻性不良影響的可能。因此,由鍍敷密著性及外觀均勻性之觀點宜將捲取溫度降低至650℃以下。The coiling temperature of the hot-rolled steel sheet is preferably set to 450 ° C or more and 650 ° C or less. This is because the ferrite and/or the coarse stellite having a long diameter of 1 μm or more are dispersed and formed in the microstructure of the hot-rolled steel sheet, and the strain introduced into the hot-rolled steel sheet due to the cold rolling is localized. Thereby, the Worstian iron inversion state in various crystal directions can be made in the annealing step, and the effective crystal grains of the annealed base material steel plate can be made fine. If the coiling temperature is lower than 450 ° C, it may not be possible to generate a wave of iron and/or a large snowy carbon. On the other hand, if the coiling temperature is higher than 650 ° C, the ferrite and the ferrite iron will form a long strip shape in the rolling direction. Therefore, it is not preferable to form a coarse material in which the effective crystal grains of the base material steel sheet which is formed after the cold rolling and annealing are formed in the rolling direction from the ferrite portion. Further, after the hot-rolled steel sheet is wound up, unevenness in formation of the internal oxide layer (the center portion is thicker than the end portion) may occur under the scale layer. This phenomenon is more pronounced if the coiling temperature is higher than 650 °C. When the internal oxide layer cannot be removed in the subsequent step (acid pickling or cold rolling) to be described later, the unevenness of the formation of the fine layer and the Fe-Al alloy layer is affected, and the plating adhesion and the uniformity of appearance are poor. The possibility of influence. Therefore, it is preferable to lower the coiling temperature to 650 ° C or less from the viewpoint of plating adhesion and appearance uniformity.

在此,於退火後的母材鋼板表面上,為了將硬質組織控制成預定體積分率,須於熱軋延步驟中適度從母材鋼板表面脫碳。從母材鋼板的脫碳行為雖可藉由控制氣體環境來控制,但須使用大規模的設備,而對成本方面負擔大。因此,本實施形態即係於自完工軋延結束(熱軋延結束)至達300℃為止期間,控制冷卻速度來控制鋼板溫度,藉此控制脫碳行為。  母材鋼板的溫度控制係在自完工軋延結束至達300℃為止期間中,在母材鋼板表面於以鐵的BCC相可穩定之溫度Ae3*℃以下的範圍下進行。其係因從鐵的BCC相脫碳比從在高溫下為穩定相的FCC相脫碳還快進行。此外本實施形態中,母材鋼板溫度若為低於300℃之溫度範圍時,氧的擴散速度會變很慢,而以脫碳的進行速度來說不會對脫碳行為造成影響,所以熱軋步驟中的母材鋼板的溫度控制的溫度範圍設為至300℃為止之間。 而Ae3*[℃]可利用下式求算。Here, in order to control the hard structure to a predetermined volume fraction on the surface of the base metal sheet after annealing, it is necessary to appropriately decarburize the surface of the base material steel sheet in the hot rolling step. Although the decarburization behavior from the base metal sheet can be controlled by controlling the gas environment, large-scale equipment must be used, which is burdensome in terms of cost. Therefore, in the present embodiment, the decarburization behavior is controlled by controlling the cooling rate to control the temperature of the steel sheet during the period from the completion of the completion rolling (end of hot rolling) to 300 °C. The temperature control of the base material steel sheet is performed in a range from the end of the completion rolling to 300 ° C, and the surface of the base material steel sheet is at a temperature at which the BCC phase of iron can be stabilized at a temperature of Ae3*° C. or lower. This is because the decarburization ratio of the BCC phase from iron is faster than the decarburization of the FCC phase which is a stable phase at a high temperature. Further, in the present embodiment, when the temperature of the base material steel sheet is lower than 300 ° C, the diffusion rate of oxygen becomes slow, and the decarburization progress does not affect the decarburization behavior, so heat The temperature range of the temperature control of the base material steel sheet in the rolling step is set to be between 300 °C. And Ae3*[°C] can be calculated by the following formula.

Ae3*[℃]=885+31.7Si-29.3Mn+123.2Al-18.2Cr-40.0Ni-21.0Cu+12.6MoAe3*[°C]=885+31.7Si-29.3Mn+123.2Al-18.2Cr-40.0Ni-21.0Cu+12.6Mo

上述式中,C、Si、Mn、Al、Cr、Ni、Cu、Mo分別為元素含量[質量%]。In the above formula, C, Si, Mn, Al, Cr, Ni, Cu, and Mo are each an element content [% by mass].

又,鋼板的脫碳行為係分成自完工軋延結束至捲成捲材為止之第1期、與捲成捲材後至到達室溫為止之第2期來控制。其係因在第1期係在大氣下進行脫碳,而第2期係捲成捲材來使鋼板彼此密著,在幾乎沒有外部氣體侵入之條件下進行脫碳,故兩者在脫碳進行速度上有很大的差異之故。Further, the decarburization behavior of the steel sheet is controlled from the first period from the completion of the rolling to the winding of the coil, and the second period from the winding of the coil to the arrival of the room temperature. This is because the first stage is decarburized in the atmosphere, and the second stage is wound into a coil to make the steel sheets adhere to each other, and decarburization is carried out under the condition that almost no external gas is invaded, so the two are decarburized. There is a big difference in speed.

具體而言,為了使鋼板表層部適度脫碳,係在自完工軋延結束至達300℃為止之冷卻過程中,將鋼板溫度控制在滿足下述式(1)之範圍。式(1)係關於脫碳行為之進行程度的算式,式(1)的値越大表示脫碳有在進行。  此外,有關式(1)中各項次,t[秒]係自完工軋延結束起之經過時間,t1[秒]係自完工軋延結束起至達Ae3*溫度為止之經過時間,t2[秒]係自完工軋延結束起至捲成捲材為止之經過時間,t3[秒]係自完工軋延結束起至鋼板溫度達300℃為止之經過時間。又,T(t)[℃]係鋼板溫度,W Si[質量%]及W Mn[質量%]分別係鋼板整體中Si、Mn各元素的平均含量。並且,α、β、γ、δ各項為常數項,分別為8.35×10 8、2.20×10 4、1.73×10 10、2.64×10 4Specifically, in order to appropriately decarburize the surface layer portion of the steel sheet, the steel sheet temperature is controlled to satisfy the following formula (1) during the cooling process from the end of the completion rolling to 300 ° C. Formula (1) is an equation for the degree of progress of the decarburization behavior, and the larger the enthalpy of the formula (1), indicates that decarburization is progressing. In addition, regarding the various times in the formula (1), t[sec] is the elapsed time from the end of the completion rolling, t1 [sec] is the elapsed time from the end of the rolling delay to the temperature of Ae3*, t2 [ Seconds] is the elapsed time from the end of the rolling process to the winding of the coil, and t3 [sec] is the elapsed time from the end of the completion rolling to the temperature of the steel sheet of 300 °C. Further, the T(t)[°C]-based steel sheet temperature, W Si [% by mass] and W Mn [% by mass] are the average contents of the respective elements of Si and Mn in the entire steel sheet. Further, α, β, γ, and δ are constant terms, and are 8.35 × 10 8 , 2.20 × 10 4 , 1.73 × 10 10 , and 2.64 × 10 4 , respectively .

[數1] [Number 1]

上述式(1)中,括弧內的第1積分項係關於第1期冷卻中脫碳進行程度的項次,第2積分項係關於第2期冷卻中脫碳進行程度的項次。不論哪一項,其脫碳皆為母材鋼板溫度越高且停留時間越長越有在進行。尤其係在第2期中,進行脫碳的元素氧幾乎不存在於氣體環境中,而係利用從表層的鏽皮層被鋼中的Si及Mn吸引而來的氧進行脫碳,故第2積分項中還包括Si及Mn含量的影響,而鋼中的Si及Mn量越多式(1)的値越大,表示有在進行脫碳。In the above formula (1), the first integral term in the parentheses is the term of the degree of decarburization in the first-stage cooling, and the second integral term is the term of the degree of decarburization in the second-stage cooling. In either case, the decarburization is performed on the base steel sheet at a higher temperature and a longer residence time. In particular, in the second phase, elemental oxygen which is decarburized is hardly present in a gas atmosphere, and is decarburized by oxygen which is attracted from Si and Mn in the steel layer of the surface layer, so the second integral term The influence of Si and Mn content is also included, and the larger the amount of Si and Mn in the steel, the larger the enthalpy of the formula (1), indicating that decarburization is being carried out.

完工軋延結束後的冷卻過程中,上述式(1)的値若低於0.8,則母材鋼板表層部幾乎不會脫碳,而表層部的硬質組織的體積率V1與以板厚表面起1/4厚度為中心之硬質組織的體積率V2之比V1/V2會大於0.90,使彎曲性變差,故以使上述式(1)的値成為0.8以上來進行冷卻。由該觀點,宜以使上述式(1)的値成為1.0以上來進行冷卻,且設成1.3以上更佳。另一方面,上述式(1)的値若超過20.0,則鋼板表層部會過度脫碳,使V1/V2小於0.30,造成鋼板的耐疲勞特性顯著變差,故宜以使上述式(1)的値成為20.0以下來進行冷卻。由該觀點,宜以使上述式(1)的値成為15.0以下來進行冷卻,設成10.0以下更佳。In the cooling process after the completion of the rolling and rolling, if the enthalpy of the above formula (1) is less than 0.8, the surface layer portion of the base material steel sheet is hardly decarburized, and the volume ratio V1 of the hard portion of the surface layer portion is from the surface of the plate thickness. The ratio V1/V2 of the volume ratio V2 of the hard structure centered at 1/4 thickness is more than 0.90, and the bendability is deteriorated. Therefore, the enthalpy of the above formula (1) is set to 0.8 or more to be cooled. From this viewpoint, it is preferable to set the enthalpy of the above formula (1) to 1.0 or more, and to set it to 1.3 or more. On the other hand, if the enthalpy of the above formula (1) exceeds 20.0, the surface layer portion of the steel sheet is excessively decarburized, and V1/V2 is less than 0.30, so that the fatigue resistance of the steel sheet is remarkably deteriorated, so that the above formula (1) is preferable. The crucible is cooled to 20.0 or less. From this viewpoint, it is preferable to set the enthalpy of the above formula (1) to 15.0 or less to be cooled, and it is more preferable to set it to 10.0 or less.

接著,酸洗依上述而製得之熱軋鋼板。酸洗可去除形成於熱軋鋼板表面之氧化物,對提升母材鋼板的鍍敷性係很重要的。酸洗可進行一次亦可分數次進行。由微細化層及Fe-Al合金層可均勻形成、且可確保其所達成之外觀均勻性之觀點,以強化酸洗來盡可能去除生成於鏽皮層下的內部氧化層為宜。酸洗條件只要可去除內部氧化層則無特別限定,例如由酸洗效率與經濟性之觀點,宜使用鹽酸。去除內部氧化層之條件,例如可舉鹽酸濃度係將氯化氫設為5質量%以上,酸洗溫度設為80℃以上,酸洗時間設為30秒以上之推薦條件。Next, the hot-rolled steel sheet obtained as described above is pickled. Pickling removes the oxide formed on the surface of the hot-rolled steel sheet and is important for improving the plating property of the base material steel sheet. Pickling can be carried out once or in fractions. From the viewpoint that the fine layer and the Fe-Al alloy layer can be uniformly formed and the appearance uniformity achieved can be ensured, it is preferable to strengthen the pickling to remove the internal oxide layer formed under the scale layer as much as possible. The pickling conditions are not particularly limited as long as the internal oxide layer can be removed. For example, hydrochloric acid is preferably used from the viewpoint of pickling efficiency and economy. The conditions for removing the internal oxide layer include, for example, a hydrogen chloride concentration of 5% by mass or more, a pickling temperature of 80° C. or more, and a pickling time of 30 seconds or more.

「冷軋步驟」 接著,對酸洗後的熱軋鋼板進行冷軋延而製得冷軋鋼板。 冷軋延中,軋縮率合計大於85%時,鋼板會喪失延性,而增加鋼板於冷軋延中斷裂的危險性。因此,軋縮率合計宜設為85%以下。由此觀點,軋縮率合計更宜設為75%以下,且設為70%以下更佳。冷軋延步驟中的軋縮率合計下限並無特別限定。然當軋縮率合計小於0.05%時,母材鋼板形狀會不均質,使鍍敷無法均勻附著,而損及外觀。因此,宜設為0.05%以上,更宜設為0.10%以上。此外,冷軋延宜多道次進行,然冷軋延的道次數及對各道次的軋縮率分配並無限制。"Cold rolling step" Next, the hot-rolled steel sheet after pickling is cold-rolled to obtain a cold-rolled steel sheet. In the case of cold rolling, when the rolling reduction ratio is more than 85%, the steel sheet loses ductility and increases the risk of the steel sheet breaking in the cold rolling. Therefore, the total reduction ratio is preferably 85% or less. From this point of view, the total reduction ratio is more preferably set to 75% or less, and more preferably 70% or less. The lower limit of the total reduction ratio in the cold rolling step is not particularly limited. However, when the total reduction ratio is less than 0.05%, the shape of the base material steel sheet may be uneven, so that the plating may not be uniformly adhered and the appearance may be impaired. Therefore, it is preferably set to 0.05% or more, and more preferably set to 0.10% or more. In addition, the cold rolling is preferably carried out in multiple passes, and there is no limitation on the number of passes of the cold rolling and the distribution of the rolling reduction of each pass.

又,冷軋延的軋縮率合計在大於10%且低於20%之範圍時,於其之後的退火步驟中會無法充分進行再結晶,於表層附近殘留因產生大量差排而失去延展性的粗大晶粒,而有使彎曲性及耐疲勞特性變差的情形。為避免該狀況,縮小軋縮率的合計,可有效減輕差排蓄積於晶粒而留住晶粒的延展性。或是增大軋縮率的合計,可於退火步驟中充分進行再結晶,而有效將加工組織製成內部的差排蓄積少之再結晶粒。由減輕差排蓄積於晶粒之觀點,冷軋步驟的軋縮率合計宜設為10%以下,更宜設為5.0%以下。另一方面,為了於退火步驟中使再結晶充分進行,軋縮率合計宜設為20%以上,更宜設為30%以上。Further, when the total rolling reduction ratio of the cold rolling is in the range of more than 10% and less than 20%, recrystallization may not be sufficiently performed in the subsequent annealing step, and the ductility may be lost in the vicinity of the surface layer due to generation of a large number of poor rows. The coarse crystal grains have a situation in which the bending property and the fatigue resistance are deteriorated. In order to avoid this, the total reduction of the rolling reduction ratio can be reduced, and the ductility of the crystal grains can be effectively reduced and accumulated in the crystal grains. Alternatively, by increasing the total reduction ratio, recrystallization can be sufficiently performed in the annealing step, and the processed structure can be effectively made into recrystallized grains having less internal discharge and less accumulation. The rolling reduction ratio in the cold rolling step is preferably 10% or less, and more preferably 5.0% or less, from the viewpoint of mitigating the difference in the accumulation of the crystal grains. On the other hand, in order to sufficiently carry out the recrystallization in the annealing step, the total reduction ratio is preferably 20% or more, and more preferably 30% or more.

「退火步驟」 本發明實施形態中係對冷軋鋼板施行退火。本發明實施形態中宜使用具有預熱帶、均熱帶與鍍敷帶之連續退火鍍敷生產線。而且,宜一邊進行退火步驟同時使其通過預熱帶與均熱帶,並在要到達鍍敷帶時結束退火步驟,於鍍敷帶進行鍍敷步驟。"Annealing step" In the embodiment of the present invention, the cold-rolled steel sheet is annealed. In the embodiment of the present invention, a continuous annealing plating line having a pre-tropical zone, a soaking zone and a plating zone is preferably used. Moreover, it is preferred to carry out the annealing step while passing it through the pre-tropical zone and the soaking zone, and to terminate the annealing step when the plating zone is to be reached, and to perform the plating step on the plating zone.

如上述,當於退火步驟及鍍敷步驟使用連續退火鍍敷生產線時,例如宜使用以下所示方法。 尤其係為了使微細化層及Fe-Al合金層適切且均勻生成,並確保鍍敷密著性及外觀均勻性,預熱帶的氣體環境、加熱方式的控制、以及控制均熱帶的氣體環境即很重要。As described above, when a continuous annealing plating line is used in the annealing step and the plating step, for example, the method shown below is preferably used. In particular, in order to make the fine layer and the Fe-Al alloy layer suitable and uniform, and to ensure plating adhesion and uniformity of appearance, the gas environment of the pre-tropical zone, the control of the heating method, and the gas environment for controlling the tropical zone are very important.

於預熱帶,係在水蒸氣分壓P(H 2O)與氫分壓P(H 2)之比的Log値Log(P(H 2O)/P(H 2))控制在-1.7~-0.2之氣體環境下,使用空氣比設為0.7~1.0之預熱燃燒器加熱至400℃~800℃的鋼板溫度,同時使鋼板通過。 於預熱帶調整水蒸氣分壓圧P(H 2O)與氫分壓P(H 2)之比,會對在後續熔融鍍鋅時於界面上使Fe-Al合金相於寬度方向均勻析出及對鍍敷前的鋼板的表面性狀帶來影響。 其係因於預熱帶調整空氣比可抑制Si等強脫氧元素的氧化膜生成於鋼板表面。而且調整水蒸氣分壓P(H 2O)與氫分壓P(H 2)之比,可抑制鋼板表面過度脫碳。藉此可於後續鍍敷步驟中,抑制鋼板表面晶界有過度的Fe-Zn合金反應,而能選擇性地進行Fe-Al合金反應。藉由選擇性地進行Fe-Al合金反應,可促使形成均勻的Fe-Al合金層,獲得優異的鍍敷密著性、外觀均勻化。當Log(P(H 2O)/P(H 2))大於-0.2時,易於後續鍍敷步驟中引起Fe-Zn合金化,使鍍敷中的Fe濃度變高。而造成鍍敷密著性降低,易發生外觀不均。另一方面,當Log(P(H 2O)/P(H 2))小於-1.7,鋼板表面會生成碳濃度高的部分,而無法於表面形成微細化層,使鍍敷密著性降低。 「空氣比」係指單位體積的混合氣體所含空氣體積、與為了使單位體積的混合氣體所含燃料氣體完全燃燒而理論上所需之空氣體積之比,可以下述式表示。 空氣比=[單位體積的混合氣體所含空氣體積(m 3)]/[為了使單位體積的混合氣體所含燃料氣體完全燃燒而理論上所需之空氣體積(m 3)] In the preheating zone, based Log Zhi water vapor partial pressure P (H 2 O) and the hydrogen partial pressure P (H 2) of the ratio of Log (P (H 2 O) / P (H 2)) in the control -1.7 ~ In a gas atmosphere of -0.2, use a preheating burner with an air ratio of 0.7 to 1.0 to heat the steel sheet to a temperature of 400 ° C to 800 ° C while passing the steel sheet. Adjusting the ratio of the water vapor partial pressure (P(H 2 O) to the hydrogen partial pressure P(H 2 ) in the pre-tropical zone, the Fe-Al alloy phase is uniformly deposited in the width direction at the interface in the subsequent hot-dip galvanizing and It affects the surface properties of the steel sheet before plating. This is because the pre-tropical air-adjusting ratio suppresses the formation of an oxide film of strong deoxidizing elements such as Si on the surface of the steel sheet. Further, by adjusting the ratio of the partial pressure of water vapor P (H 2 O) to the partial pressure of hydrogen P (H 2 ), excessive decarburization on the surface of the steel sheet can be suppressed. Thereby, in the subsequent plating step, the Fe-Al alloy reaction can be selectively performed by suppressing excessive Fe-Zn alloy reaction at the grain boundary of the steel sheet surface. By selectively performing the Fe-Al alloy reaction, formation of a uniform Fe-Al alloy layer can be promoted, and excellent plating adhesion and uniform appearance can be obtained. When Log(P(H 2 O)/P(H 2 )) is more than -0.2, it is easy to cause Fe-Zn alloying in the subsequent plating step, so that the Fe concentration in the plating becomes high. As a result, the adhesion of the plating is lowered, and uneven appearance is liable to occur. On the other hand, when Log(P(H 2 O)/P(H 2 )) is less than -1.7, a portion having a high carbon concentration is formed on the surface of the steel sheet, and a fine layer cannot be formed on the surface to lower the plating adhesion. . The "air ratio" is a ratio of the volume of the air contained in the mixed gas per unit volume to the theoretically required air volume for completely combusting the fuel gas contained in the mixed gas per unit volume, and can be expressed by the following formula. Air ratio = [air volume (m 3 ) contained in the mixed gas per unit volume] / [the theoretically required air volume (m 3 ) in order to completely burn the fuel gas contained in the mixed gas per unit volume]

上述空氣比大於1.0而過大時,會於鋼板表層部過度生成Fe氧化被膜,使退火後的脫碳層肥大化,且亦會過度生成微細化層。因此,鍍敷合金化會過度進行,使鍍敷密著性、碎裂性及粉碎性降低。所以,上述空氣比宜為1.0以下,更宜為0.9以下。當上述空氣比小於0.7而過小時,會無法形成微細化層,使鍍敷密著性降低。因此,將上述空氣比設為0.7以上,且宜設為0.8以上。 又,要通過預熱帶之鋼板溫度若低於400℃,則無法形成充分的微細化層。因此,要通過預熱帶之鋼板溫度設為400℃以上,且宜設為600℃以上。另一方面,要通過預熱帶之鋼板溫度若為高於800℃之高溫,則鋼板表面會生成含Si及/或Mn之粗大的氧化物,使鍍敷密著性降低。因此,要通過預熱帶之鋼板溫度設為800℃以下,且宜設為750℃以下。 預熱帶的加熱速度若慢則內部會氧化,而於鋼板內部生成粗大的氧化物。尤其係在600℃~750℃的加熱速度尤為重要,為了避免鋼板表層部過度脫碳、抑制生成粗大的氧化物,須將其之間的平均加熱速度設為1.0℃/秒以上。其之間的平均加熱速度若低於1.0℃/秒,則於微細化層中會形成粗大的氧化物,使鍍敷密著性及粉碎性降低。為了避免鋼板表層部過度脫碳、及生成粗大的氧化物,在600℃~750℃間之平均加熱速度宜設為1.5℃/秒以上,更宜設為2.0℃/秒以上。為了確保預熱帶的處理時間,在600℃~750℃的平均加熱速度宜設為50℃/秒以下。平均加熱速度若在50℃/秒以下,則易製得均勻的微細化層,而可製得鍍敷密著性及外觀均勻性優異之鍍敷層。When the air ratio is more than 1.0 and is too large, an Fe oxide film is excessively formed in the surface layer portion of the steel sheet, and the decarburized layer after annealing is enlarged, and the fine layer is excessively formed. Therefore, the plating alloying is excessively performed, and the plating adhesion, the chipping property, and the pulverization property are lowered. Therefore, the air ratio is preferably 1.0 or less, more preferably 0.9 or less. When the air ratio is less than 0.7 and is too small, the micronized layer cannot be formed, and the plating adhesion is lowered. Therefore, the air ratio is set to 0.7 or more, and is preferably set to 0.8 or more. Further, if the temperature of the steel sheet passing through the pretropical zone is lower than 400 ° C, a sufficient fine layer cannot be formed. Therefore, the temperature of the steel sheet passing through the pre-tropical zone is set to 400 ° C or higher, and is preferably set to 600 ° C or higher. On the other hand, if the temperature of the steel sheet passing through the pretropical zone is higher than 800 ° C, a coarse oxide containing Si and/or Mn is formed on the surface of the steel sheet to lower the plating adhesion. Therefore, the temperature of the steel sheet passing through the pre-tropical zone is set to 800 ° C or lower, and preferably set to 750 ° C or lower. If the heating rate of the pre-tropical zone is slow, the interior will oxidize and a coarse oxide will be formed inside the steel sheet. In particular, the heating rate of 600 ° C to 750 ° C is particularly important. In order to avoid excessive decarburization of the surface layer of the steel sheet and to suppress the formation of coarse oxides, the average heating rate between them must be 1.0 ° C / sec or more. When the average heating rate between them is less than 1.0 ° C / sec, a coarse oxide is formed in the fine layer, and the plating adhesion and the pulverizability are lowered. In order to avoid excessive decarburization of the surface layer portion of the steel sheet and formation of coarse oxides, the average heating rate between 600 ° C and 750 ° C is preferably 1.5 ° C / sec or more, more preferably 2.0 ° C / sec or more. In order to ensure the treatment time of the pre-tropical zone, the average heating rate at 600 ° C to 750 ° C is preferably set to 50 ° C / sec or less. When the average heating rate is 50 ° C /sec or less, it is easy to obtain a uniform fine layer, and a plating layer excellent in plating adhesion and appearance uniformity can be obtained.

要將與鋼板成形性相關之微觀組織分率控制在預定範圍,退火步驟的最高加熱溫度係很重要的因子。最高加熱溫度若低,則於鋼中會熔融殘留粗大的鐵系碳化物,使成形性變差。又,最高加熱溫度若低於750℃,則熱軋鋼板中粗大的鐵碳化物無法充分熔解,而殘存在製成製品的板中,有大幅損害延性之虞。為了使鐵系碳化物充分固溶,提高成形性,將最高加熱溫度設為(Ac1點+25)℃以上且750℃以上,且宜設為(Ac1點+50)℃以上。另一方面,最高加熱溫度若超過Ac3點,則鋼中的肥粒鐵分率會顯著減少,故將最高加熱溫度設為Ac3點以下。又,由鍍敷密著性之觀點,為了減少基鐵表面的氧化物,最高加熱溫度宜低。由該觀點最高加熱溫度宜設為850℃以下,更宜設為830℃以下。To control the microstructure fraction associated with the formability of the steel sheet to a predetermined range, the highest heating temperature of the annealing step is an important factor. When the maximum heating temperature is low, coarse iron-based carbides are melted in the steel to deteriorate the formability. Further, if the maximum heating temperature is lower than 750 ° C, the coarse iron carbide in the hot-rolled steel sheet cannot be sufficiently melted, and remains in the sheet of the product to be formed, and the ductility is greatly impaired. In order to sufficiently dissolve the iron-based carbide and improve the moldability, the maximum heating temperature is (Ac1 point + 25) ° C or more and 750 ° C or more, and is preferably set to (Ac1 point + 50) ° C or more. On the other hand, if the maximum heating temperature exceeds the Ac3 point, the iron content of the fertilizer in the steel is remarkably reduced, so the maximum heating temperature is set to be equal to or less than Ac3. Further, from the viewpoint of plating adhesion, in order to reduce the oxide on the surface of the base iron, the maximum heating temperature is preferably low. From this point of view, the maximum heating temperature is preferably 850 ° C or lower, and more preferably 830 ° C or lower.

鋼板的Ac1點及Ac3點分別為沃斯田鐵逆變態的開始點與結束點,具體而言,係自熱軋延後的鋼板切出小片後,以10℃/秒加熱至1200℃為止,並測定該期間之體積膨脹而得。The Ac1 point and the Ac3 point of the steel sheet are the starting point and the ending point of the inverted state of the Worstian iron, respectively. Specifically, the steel sheet after the hot rolling is cut into small pieces and heated to 1200 ° C at 10 ° C / sec. And measuring the volume expansion during this period.

退火步驟的最高加熱溫度(750℃以上)會在均熱帶達點。該均熱帶的氣體環境係將Log(P(H 2O)/P(H 2))控制在-1.7~-0.2。Log(P(H 2O)/P(H 2))小於-1.7時,會無法形成微細化層,使鍍敷密著性降低。Log(P(H 2O)/P(H 2))大於-0.2時,脫碳會過度進行,則不僅母材鋼板表層的硬質相會顯著減少,微細化層中還會形成粗大的氧化物,使鍍敷密著性及粉碎性降低。 The maximum heating temperature (above 750 °C) in the annealing step will reach the point in the tropics. The soaking tropical gas environment controls Log(P(H 2 O)/P(H 2 )) from -1.7 to -0.2. When Log(P(H 2 O)/P(H 2 )) is less than -1.7, the micronized layer cannot be formed, and the plating adhesion is lowered. When Log(P(H 2 O)/P(H 2 )) is greater than -0.2, the decarburization will be excessively performed, and not only the hard phase of the surface layer of the base metal sheet will be significantly reduced, but also the coarse oxide layer will be formed in the fine layer. The plating adhesion and pulverizability are lowered.

如上述,均熱帶的Log(P(H 2O)/P(H 2))為-1.7~-0.2時,會成為鍍敷剝離起點之Si及Mn氧化物不會形成於最表面層,而鋼板表層內部會形成最大徑為0.05μm~0.4μm之Si及/或Mn的微細氧化物。Si及/或Mn的微細氧化物可抑制退火中之Fe再結晶的成長。而且因退火氣體環境中的水蒸氣會使母材表層脫碳,故退火後的母材表層會變成肥粒鐵。結果而於退火後的母材表層形成平均厚度為0.1μm~5.0μm,肥粒鐵相的平均粒徑為0.1μm~3.0μm,且最大徑為0.01μm~0.4μm之含Si及/或Mn氧化物的微細化層。 As described above, when the log (P(H 2 O)/P(H 2 )) of the homogenous tropic is -1.7 to -0.2, Si and Mn oxide which are the starting points of the plating peeling are not formed on the outermost layer, and A fine oxide of Si and/or Mn having a maximum diameter of 0.05 μm to 0.4 μm is formed inside the surface layer of the steel sheet. The fine oxide of Si and/or Mn can suppress the growth of Fe recrystallization in annealing. Moreover, since the water vapor in the annealing gas environment decarburizes the surface layer of the base material, the surface layer of the base material after annealing becomes ferrite iron. As a result, the surface layer of the base material after annealing is formed to have an average thickness of 0.1 μm to 5.0 μm, the average particle diameter of the ferrite iron phase is 0.1 μm to 3.0 μm, and the maximum diameter is 0.01 μm to 0.4 μm containing Si and/or Mn. A fine layer of oxide.

退火步驟中,在到達最高加熱溫度後至到鍍敷浴為止之鍍敷前的冷卻(鍍敷前冷卻步驟)中,會分成760℃至700℃為止之溫度域、與650℃至500℃為止之溫度域2階段來控制鋼板溫度,藉此可製得預定微觀組織。首先,為了充分生成肥粒鐵,而規定從760℃至700℃為止之間的平均冷卻速度。從760℃至700℃為止之平均冷卻速度若超過5.0℃/秒,則會有無法充分生成肥粒鐵之情形,故將平均冷卻速度設為5.0℃/秒以下。為了充分生成肥粒鐵,平均冷卻速度宜設為3.5℃/秒以下,更宜設為2.5℃/秒以下。另一方面,從760℃至700℃為止之平均冷卻速度若低於0.3℃/秒則會有生成大量波來鐵之情形,故將平均冷卻速度設為0.3℃/秒以上。為了避免生成波來鐵,平均冷卻速度宜設為0.5℃/秒以上,更宜設為0.7℃/秒以上。In the annealing step, after the maximum heating temperature is reached and the plating before the plating bath is cooled (pre-plating cooling step), it is divided into a temperature range of 760 ° C to 700 ° C and 650 ° C to 500 ° C. The temperature domain 2 is controlled to control the temperature of the steel sheet, whereby a predetermined microstructure can be obtained. First, in order to sufficiently generate ferrite iron, an average cooling rate from 760 ° C to 700 ° C is specified. When the average cooling rate from 760 ° C to 700 ° C exceeds 5.0 ° C / sec, the ferrite iron may not be sufficiently formed, so the average cooling rate is set to 5.0 ° C / sec or less. In order to sufficiently form the ferrite iron, the average cooling rate is preferably set to 3.5 ° C / sec or less, more preferably 2.5 ° C / sec or less. On the other hand, when the average cooling rate from 760 ° C to 700 ° C is less than 0.3 ° C / sec, a large amount of ferrite is generated, so the average cooling rate is set to 0.3 ° C / sec or more. In order to avoid the generation of the wave iron, the average cooling rate is preferably set to 0.5 ° C / sec or more, more preferably set to 0.7 ° C / sec or more.

接著,為了變免過度生成波來鐵及/或粗大的雪明碳鐵,而規定在650℃至500℃為止之冷卻速度。在650℃至500℃為止之平均冷卻速度低於1.0℃/秒時,會大量生成波來鐵及/或粗大的雪明碳,故設平均冷卻速度為1.0℃/秒以上。因鋼中宜不含波來鐵及/或粗大的雪明碳鐵,故為了充分避免該等生成,平均冷卻速度宜設為2.0℃/秒以上,更宜設為3.0℃/秒以上。在650℃至500℃之溫度域的平均冷卻速度上限並無特別設定,然要獲得過大的平均冷卻速度,須使用特殊的冷卻設備或不會影響鍍敷步驟之冷媒,故而不適宜。由該觀點,在上述溫度域中之平均冷卻速度宜設為100℃/秒以下,更宜設為70℃/秒以下。Next, in order to avoid excessive generation of wave iron and/or coarse snowy carbon, the cooling rate at 650 ° C to 500 ° C is specified. When the average cooling rate at 650 ° C to 500 ° C is less than 1.0 ° C / sec, a large amount of ferrite and/or coarse snow carbon is generated, so that the average cooling rate is 1.0 ° C / sec or more. Since the steel preferably contains no pulverized iron and/or coarse swarf carbon iron, the average cooling rate is preferably 2.0 ° C / sec or more, and more preferably 3.0 ° C / sec or more, in order to sufficiently avoid such formation. The upper limit of the average cooling rate in the temperature range of 650 ° C to 500 ° C is not particularly set, but it is not suitable to obtain an excessive average cooling rate by using a special cooling device or a refrigerant which does not affect the plating step. From this viewpoint, the average cooling rate in the above temperature range is preferably 100 ° C / sec or less, and more preferably 70 ° C / sec or less.

接續鍍敷前冷卻步驟,為了獲得回火麻田散鐵,在鋼板溫度到達500℃後至到達鍍敷浴為止之期間,麻田散鐵變態處理亦可使鋼板在預定溫度域中停留一定時間。麻田散鐵變態處理溫度宜以麻田散鐵變態開始溫度Ms點為上限,且將上限設為(Ms點-20)℃更佳。麻田散鐵變態處理溫度宜以50℃為下限,且下限設為100℃更佳。又,麻田散鐵變態處理時間宜設為1秒鐘~100秒鐘,更宜設為10秒鐘~60秒鐘。此外,由麻田散鐵變態處理所製得之麻田散鐵,在鍍敷步驟中藉由進入高溫鍍敷浴會變成回火麻田散鐵。In order to obtain the tempering pre-plating cooling step, in order to obtain the tempered granulated iron, the metamorphic treatment of the granulated iron can also keep the steel sheet in a predetermined temperature range for a certain period of time after the steel sheet temperature reaches 500 ° C until the plating bath is reached. The metamorphic treatment temperature of the Ma Tian bulk iron should be based on the upper limit of the Ms point of the metamorphic iron metamorphosis of the Ma Tian, and the upper limit is set to be (Ms point -20) ° C. The metamorphic treatment temperature of the Ma Tian iron is preferably 50 ° C as the lower limit, and the lower limit is preferably 100 ° C. Moreover, the metamorphic treatment time of the Ma Tian loose iron should be set to 1 second to 100 seconds, and more preferably set to 10 seconds to 60 seconds. In addition, the methadrite iron produced by the metamorphic treatment of the granulated iron in the field will become tempered granulated iron by entering the high temperature plating bath in the plating step.

而Ms點係依下式計算。 Ms點[℃]=541-474C/(1-VF)-15Si-35Mn-17Cr-17Ni+19AlThe Ms point is calculated according to the following formula. Ms point [°C]=541-474C/(1-VF)-15Si-35Mn-17Cr-17Ni+19Al

上述式中,VF表示肥粒鐵的體積分率,C、Si、Mn、Cr、Ni、Al分別為元素含量[質量%]。 此外,要在製造中直接測定肥粒鐵的體積分率係很困難的。因此,本發明在決定Ms點時,係將冷軋鋼板在通過連續退火生產線前切出小片,並將該小片以同於通過連續退火生產線時之溫度歷程進行退火後,測定小片的肥粒鐵的體積變化,並將利用該結果算出之數値作為肥粒鐵的體積分率VF。In the above formula, VF represents the volume fraction of ferrite iron, and C, Si, Mn, Cr, Ni, and Al are elemental contents [% by mass], respectively. In addition, it is difficult to directly measure the volume fraction of ferrite in the manufacturing process. Therefore, in the determination of the Ms point, the present invention cuts the small piece before the cold-rolled steel sheet is passed through the continuous annealing line, and anneals the piece in the same temperature history as when passing through the continuous annealing line, and then determines the small piece of ferrite iron. The volume change, and the number calculated using the result is taken as the volume fraction VF of the ferrite iron.

並且,為了生成變韌鐵,在鋼板溫度到達500℃後至到鍍敷浴為止之間,變韌鐵變態處理亦可使鋼板停留在預定溫度域中一定時間。變韌鐵變態處理溫度若大於500℃則會生成波來鐵及/或粗大的雪明碳鐵,故將變韌鐵變態處理溫度設為500℃以下。又,變韌鐵變態處理溫度若低於350℃,則無法充分進行變態,故將變韌鐵變態處理溫度設為350℃以上。為了充分進行變態,而將變韌鐵變態處理時間設為10秒以上,為了抑制波來鐵及/或粗大的雪明碳鐵的生成,則設為500秒以下。此外,在鍍敷前冷卻步驟後,要進行變韌鐵變態處理與麻田散鐵變態處理兩者時,施行順序係設為變韌鐵變態處理與麻田散鐵變態處理。Further, in order to generate the toughened iron, the toughening iron metamorphic treatment may also cause the steel sheet to stay in the predetermined temperature range for a certain period of time after the steel sheet temperature reaches 500 ° C until the plating bath. If the toughening iron metamorphic treatment temperature is greater than 500 ° C, the ferrite and/or the coarse swarf carbon iron are generated, so the metamorphic iron metamorphic treatment temperature is set to 500 ° C or lower. Further, if the toughening iron metamorphic treatment temperature is lower than 350 ° C, the deformation cannot be sufficiently performed, so that the toughening iron transformation treatment temperature is set to 350 ° C or higher. In order to sufficiently perform the metamorphosis, the toughening iron metamorphic treatment time is set to 10 seconds or more, and in order to suppress the formation of the ferrite and/or the coarse ferritic carbon, it is set to 500 seconds or less. In addition, after the pre-plating cooling step, when both the toughening iron metamorphic treatment and the 麻田散铁 metamorphic treatment are performed, the execution sequence is set to the toughening iron metamorphic treatment and the granitic iron metamorphosis treatment.

「鍍敷步驟」 接著,將依上述製得之母材鋼板浸漬於鍍敷浴。 鍍敷浴具有以鋅為主體、且鍍敷浴中的總Al量減去總Fe量所得的値、即有效Al量為0.180%~0.250%之組成。鍍敷浴中的有效Al量小於0.180%時,Fe-Al合金層會無法充分形成,而Fe會進入鍍敷層中,損害鍍敷密著性,故須設為0.180%以上。而由此觀點,鍍敷浴中的有效Al量更宜設為0.185%以上,設為0.190%以上更佳。另一方面,鍍敷浴中的有效Al量若大於0.250%,母材鋼板與鍍敷層之Fe-Al合金層會過度生成,損害鍍敷密著性。由此觀點,鍍敷浴中的有效Al量須設為0.250%以下,且宜設為0.240%以下,設為0.230%以下更佳。"Plating Step" Next, the base material steel sheet obtained as described above was immersed in a plating bath. The plating bath has a composition mainly composed of zinc and having a total amount of Al in the plating bath minus the total amount of Fe, that is, an effective Al amount of 0.180% to 0.250%. When the amount of effective Al in the plating bath is less than 0.180%, the Fe-Al alloy layer may not be sufficiently formed, and Fe may enter the plating layer to impair the plating adhesion, so it is required to be 0.180% or more. From this point of view, the effective Al amount in the plating bath is more preferably 0.185% or more, and more preferably 0.190% or more. On the other hand, when the amount of effective Al in the plating bath is more than 0.250%, the Fe-Al alloy layer of the base material steel sheet and the plating layer is excessively formed to impair the plating adhesion. From this point of view, the effective Al amount in the plating bath must be 0.250% or less, and is preferably 0.240% or less, and more preferably 0.230% or less.

鍍敷浴中亦可混入Ag、B、Be、Bi、Ca、Cd、Co、Cr、Cs、Cu、Ge、Hf、I、K、La、Li、Mg、Mn、Mo、Na、Nb、Ni、Pb、Rb、Sb、Si、Sn、Sr、Ta、Ti、V、W、Zr、REM之1種或2種以上元素,且利用各元素的含量有可改善熔融鍍鋅層的耐蝕性及加工性等較佳的情況。Ag, B, Be, Bi, Ca, Cd, Co, Cr, Cs, Cu, Ge, Hf, I, K, La, Li, Mg, Mn, Mo, Na, Nb, Ni may also be mixed in the plating bath. One or two or more elements of Pb, Rb, Sb, Si, Sn, Sr, Ta, Ti, V, W, Zr, and REM, and the content of each element can improve the corrosion resistance of the hot-dip galvanized layer and A better case such as processability.

又,鍍敷浴溫度宜設為440℃~470℃。鍍敷浴溫度低於440℃時,鍍敷浴的黏度會過度升高,而難以控制鍍敷層的厚度,損及熔融鍍鋅鋼板的外觀。因此,鍍敷浴的溫度宜為440℃以上,更宜設為445℃以上。另一方面,鍍敷浴溫度高於470℃時會產生大量煙霧,而難以安全製造。因此,鍍敷浴溫度宜為470℃以下,更宜設為460℃以下。Further, the plating bath temperature should be set to 440 ° C to 470 ° C. When the temperature of the plating bath is lower than 440 ° C, the viscosity of the plating bath is excessively increased, and it is difficult to control the thickness of the plating layer, which impairs the appearance of the molten galvanized steel sheet. Therefore, the temperature of the plating bath is preferably 440 ° C or higher, more preferably 445 ° C or higher. On the other hand, when the plating bath temperature is higher than 470 ° C, a large amount of smoke is generated, which is difficult to manufacture safely. Therefore, the plating bath temperature is preferably 470 ° C or lower, more preferably 460 ° C or lower.

又,母材鋼板進入鍍敷浴時的鋼板溫度若低於430℃,為了使鍍敷浴溫度可在440℃以上穩定而須給予鍍敷浴大量熱量而不實用。另一方面,母材鋼板進入鍍敷浴時的鋼板溫度若高於480℃,則為了使鍍敷浴溫度可在470℃以下穩定,須導入可自鍍敷浴排出大量熱量的設備,而以製造成本方面來說不適宜。因此,為了穩定鍍敷浴的浴溫,母材鋼板進入鍍敷浴時的溫度宜設為430℃以上且480℃以下。並且,為了適切控制Fe-Al合金層,母材鋼板進入鍍敷浴時的溫度更宜設為440℃以上且470℃以下。Further, when the temperature of the steel sheet when the base material steel sheet enters the plating bath is lower than 430 ° C, in order to stabilize the temperature of the plating bath at 440 ° C or higher, it is necessary to give a large amount of heat to the plating bath without being practical. On the other hand, if the temperature of the steel sheet when the base material steel sheet enters the plating bath is higher than 480 ° C, in order to stabilize the temperature of the plating bath below 470 ° C, it is necessary to introduce a device capable of discharging a large amount of heat from the plating bath, and It is not suitable in terms of manufacturing cost. Therefore, in order to stabilize the bath temperature of the plating bath, the temperature at which the base material steel sheet enters the plating bath is preferably set to 430 ° C or more and 480 ° C or less. Further, in order to appropriately control the Fe-Al alloy layer, the temperature at which the base material steel sheet enters the plating bath is more preferably set to 440 ° C or more and 470 ° C or less.

鍍敷浴的溫度以可在440℃~470℃之範圍內的溫度穩定為佳。鍍敷浴的溫度若不穩定,Fe-Al合金層及鍍敷層中的Fe含量會不均勻,而使鍍敷層外觀及密著性不均勻。故為了使鍍敷浴溫度穩定,宜使進入鍍敷浴時的鋼板溫度與鍍敷浴溫度大略一致。具體而言,由實際製造設備的溫度控制性有限度來看,宜將進入鍍敷浴時的鋼板溫度設為鍍敷浴溫度±10℃以內,且設為鍍敷浴溫度±5℃以內更佳。The temperature of the plating bath is preferably stabilized at a temperature in the range of 440 ° C to 470 ° C. If the temperature of the plating bath is unstable, the Fe content in the Fe-Al alloy layer and the plating layer may be uneven, and the appearance and adhesion of the plating layer may be uneven. Therefore, in order to stabilize the temperature of the plating bath, it is preferable to make the temperature of the steel sheet entering the plating bath substantially coincide with the temperature of the plating bath. Specifically, from the viewpoint of limited temperature control of the actual manufacturing equipment, it is preferable to set the temperature of the steel sheet entering the plating bath to within ±10 ° C of the plating bath temperature, and to set the plating bath temperature to within ±5 ° C. good.

此外,於鍍敷浴浸漬後為了獲得適當的鍍敷附著量,宜對鋼板表面噴吹以氮為主體之高壓氣體來去除表層過多的鋅。之後冷卻至室溫。此時,Fe原子幾乎不會從母材鋼板往鍍敷層擴散,故以確保鍍敷密著性之觀點,至ζ相生成幾乎停止之溫度350℃為止宜確保冷卻速度為1℃/秒以上。Further, in order to obtain an appropriate amount of plating adhesion after immersion in the plating bath, it is preferable to spray a high-pressure gas mainly composed of nitrogen on the surface of the steel sheet to remove excessive zinc in the surface layer. It was then cooled to room temperature. In this case, since the Fe atoms hardly diffuse from the base material steel plate to the plating layer, it is preferable to ensure the cooling rate to be 1 ° C / sec or more from the viewpoint of ensuring the plating adhesion to a temperature at which the enthalpy phase is almost stopped at 350 ° C. .

又,冷卻至350℃後,為了獲得硬質組織,亦可以1.0℃/秒以上的平均冷卻速度冷卻至250℃以下。為了獲得新生麻田散鐵相及/或回火麻田散鐵相,平均冷卻速度宜設為3.0℃/秒以上,設為5.0℃/秒以上更佳。Further, after cooling to 350 ° C, in order to obtain a hard structure, it may be cooled to 250 ° C or lower at an average cooling rate of 1.0 ° C /sec or more. In order to obtain a new granulated iron phase and/or a tempered granule iron phase, the average cooling rate is preferably set to 3.0 ° C / sec or more, and more preferably 5.0 ° C / sec or more.

並且,冷卻至250℃以下之後,為了獲得回火麻田散鐵亦可施行再加熱處理。再加熱處理的處理溫度及處理時間可因應所欲特性適宜設定。惟,再加熱處理溫度低於250℃時無法獲得充分的效果,而高於350℃時,鍍敷層會變質,而有鍍敷密著性變差之虞,因此再加熱處理溫度宜設為250℃以上且350℃以下。又,再加熱處理時間若超過1000秒則處理效果會達飽和,故處理時間宜設為1000秒以下。Further, after cooling to 250 ° C or lower, reheating treatment may be performed in order to obtain tempered granulated iron. The treatment temperature and treatment time of the reheating treatment can be appropriately set according to the desired characteristics. However, when the reheating temperature is lower than 250 ° C, sufficient effect cannot be obtained, and when it is higher than 350 ° C, the plating layer is deteriorated, and the plating adhesion is deteriorated, so the reheating temperature should be set to be set. 250 ° C or more and 350 ° C or less. Further, if the reheating treatment time exceeds 1000 seconds, the treatment effect is saturated, so the treatment time should be set to 1000 seconds or less.

又,冷卻至350℃之後,為了獲得殘留沃斯田鐵,亦可進行停留在250℃~350℃之溫度範圍15秒~500秒的變韌鐵變態處理。變韌鐵變態處理溫度若低於250℃,則會生成麻田散鐵而無法充分獲得殘留沃斯田鐵。因此,變韌鐵變態處理溫度宜設為250℃以上,更宜設為300℃以上。而變韌鐵變態處理溫度若高於350℃,則Fe原子會從母材鋼板過度擴散到鍍敷層,使鍍敷密著性變差。因此,變韌鐵變態處理溫度宜設為350℃以下,更宜設為330℃以下。 變韌鐵變態處理時間若在15秒以上,即可充分獲得進行變韌鐵變態處理之效果。變韌鐵變態處理時間更宜為25秒以上。變韌鐵變態處理時間若在500秒以下,即可有效率進行變韌鐵變態處理。變韌鐵變態處理時間更宜為300秒以下。Further, after cooling to 350 ° C, in order to obtain the residual Worthite iron, a toughening iron metamorphosis treatment may be performed in a temperature range of from 250 ° C to 350 ° C for 15 seconds to 500 seconds. If the toughening iron metamorphic treatment temperature is lower than 250 ° C, the granulated iron is formed and the residual Worth iron is not sufficiently obtained. Therefore, the toughening iron metamorphic treatment temperature is preferably set to 250 ° C or higher, and more preferably set to 300 ° C or higher. When the toughening iron metamorphic treatment temperature is higher than 350 ° C, the Fe atoms are excessively diffused from the base material steel sheet to the plating layer, which deteriorates the plating adhesion. Therefore, the toughening iron metamorphic treatment temperature should be set to 350 ° C or lower, and more preferably set to 330 ° C or lower. If the toughening iron metamorphic treatment time is more than 15 seconds, the effect of the toughening iron metamorphosis treatment can be fully obtained. The toughening iron metamorphic treatment time is more preferably 25 seconds or more. If the toughening iron metamorphic treatment time is less than 500 seconds, the toughening iron metamorphosis treatment can be efficiently performed. The toughening iron metamorphic treatment time is preferably less than 300 seconds.

又,為了使殘留沃斯田鐵更穩定化,亦可冷卻至250℃以下後施行再加熱處理。再加熱處理的處理溫度及處理時間可因應所欲特性適宜設定。但,再加熱處理溫度若低於250℃則無法獲得充分的效果。因此,再加熱處理溫度宜設為250℃以上,更宜設為280℃以上。再加熱處理溫度若高於350℃,則Fe原子會從母材鋼板擴散到鍍敷層,使鍍敷密著性變差。因此,再加熱處理溫度宜設為350℃以下,更宜設為330℃以下。 又.再加熱處理時間若超過1000秒,則效果會達飽和,故再加熱處理時間宜設為1000秒以下。Further, in order to stabilize the residual Worthite iron, it may be cooled to 250 ° C or lower and then subjected to reheat treatment. The treatment temperature and treatment time of the reheating treatment can be appropriately set according to the desired characteristics. However, if the reheating treatment temperature is lower than 250 ° C, a sufficient effect cannot be obtained. Therefore, the reheating treatment temperature is preferably set to 250 ° C or higher, and more preferably set to 280 ° C or higher. When the reheating treatment temperature is higher than 350 ° C, Fe atoms diffuse from the base material steel sheet to the plating layer, and the plating adhesion is deteriorated. Therefore, the reheating treatment temperature is preferably set to 350 ° C or lower, and more preferably set to 330 ° C or lower. also. If the reheating treatment time exceeds 1000 seconds, the effect is saturated, so the reheat treatment time should be set to 1000 seconds or less.

「加工步驟」 接著,將鋼板溫度冷卻至100℃以下後,為了減少母材鋼板表層的殘留沃斯田鐵,對鍍敷鋼板施行彎折-折回變形。彎曲可使用直徑為50mm~800mm之輥來實施。輥徑小於50mm時,因彎曲變形會導致於母材鋼板表層導入大量應變,而損及鋼板成形性。而當輥徑大於800mm時,母材鋼板表層的應變量小,而無法充分減少殘留沃斯田鐵。彎折-折回變形為了減少母材鋼板表面背面各面的殘留沃斯田鐵,須各施行1次以上將表面背面各面彎成外側之變形,故而須施行合計2次以上彎折-折回變形。依上述,可將母材鋼板表面背面兩面的殘留沃斯田鐵控制在預定範圍。"Processing Step" Next, after the steel sheet temperature is cooled to 100 ° C or lower, the plated steel sheet is subjected to bending-folding deformation in order to reduce the residual Worth iron in the surface layer of the base material steel sheet. The bending can be carried out using a roller having a diameter of 50 mm to 800 mm. When the roll diameter is less than 50 mm, a large amount of strain is introduced into the surface layer of the base material steel sheet due to the bending deformation, and the formability of the steel sheet is impaired. When the roll diameter is larger than 800 mm, the strain amount of the surface layer of the base material steel plate is small, and the residual Worthite iron cannot be sufficiently reduced. Bending-folding deformation In order to reduce the residual Worthite iron on each surface of the back surface of the base material steel plate, it is necessary to perform one or more deformations of the front and back surfaces to the outside, so that a total of two or more bending-reversing deformations must be performed. . According to the above, the residual Worth iron on both sides of the front and back surfaces of the base material steel sheet can be controlled to a predetermined range.

本實施形態之熔融鍍鋅鋼板可依以上說明之製造方法製造,但本發明並不受限於上述實施形態。The hot-dip galvanized steel sheet according to the present embodiment can be produced by the above-described production method, but the present invention is not limited to the above embodiment.

例如本發明實施形態中,亦可對依上述方法製得之熔融鍍鋅鋼板的鍍鋅層表面賦予由磷氧化物及/或含磷之複合氧化物所構成之皮膜。 由磷氧化物及/或含磷之複合氧化物所構成之皮膜可在加工熔融鍍鋅鋼板時發揮潤滑劑的功能,而可保護形成於母材鋼板表面之鍍鋅層。For example, in the embodiment of the present invention, a film composed of a composite oxide of phosphorus oxide and/or phosphorus may be applied to the surface of the galvanized layer of the hot-dip galvanized steel sheet obtained by the above method. The film composed of the phosphorus oxide and/or the phosphorus-containing composite oxide functions as a lubricant when processing the hot-dip galvanized steel sheet, and can protect the galvanized layer formed on the surface of the base material steel sheet.

並且,本發明實施形態中,為了矯正形狀,亦可以軋縮率3.00%以下對已冷卻至室溫之熔融鍍鋅鋼板施行冷軋延。Further, in the embodiment of the present invention, in order to correct the shape, the hot-dip galvanized steel sheet which has been cooled to room temperature may be subjected to cold rolling at a rolling reduction ratio of 3.00% or less.

此外,以上所述本發明實施形態之熔融鍍鋅鋼板之製造方法宜適用母材鋼板板厚為0.6mm以上且小於5.0mm之熔融鍍鋅鋼板之製造。母材鋼板板厚小於0.6mm時,難以將母材鋼板形狀保持平坦,而有不適宜的情況發生。而母材鋼板板厚在5.0mm以上時,會有難以控制退火步驟及鍍敷步驟中之冷卻的情況。Further, the method for producing a hot-dip galvanized steel sheet according to the embodiment of the present invention described above is preferably applied to the production of a hot-dip galvanized steel sheet having a base material steel sheet thickness of 0.6 mm or more and less than 5.0 mm. When the thickness of the base material steel sheet is less than 0.6 mm, it is difficult to keep the shape of the base material steel sheet flat, and it is unfavorable. When the thickness of the base material steel plate is 5.0 mm or more, it may be difficult to control the cooling in the annealing step and the plating step.

實施例 針對本發明實施例進行說明。此外,本實施例中之條件係為確認本發明可實施性及效果而採用之一條件例。本發明並不受限於該一條件例。只要不脫離本發明要旨而可達成本發明之目的,本發明即可採用各種條件。EXAMPLES Examples of the invention will be described. Further, the conditions in the examples are those in which the conditions and effects of the present invention are confirmed. The present invention is not limited to this one conditional example. The present invention can be applied to various conditions without departing from the gist of the present invention for the purpose of the invention.

「實施例1」 鑄造具表1~表3所示A~BY的化學成分(組成)之鋼胚,並以表4~表7所示熱軋步驟條件(鋼胚加熱溫度、軋延結束溫度)進行熱軋延,且以表4~表7所示熱軋步驟條件(自熱軋結束至捲取為止之平均冷卻速度、捲取溫度、式(1))進行冷卻,而製得熱軋鋼板。 之後,對熱軋鋼板進行酸洗(浸漬於80℃的10%鹽酸,浸漬時間顯示於表4~表7),並施行表4~表7所示冷軋步驟條件(軋縮率)的冷軋延而製得冷軋鋼板。"Example 1" A steel preform having a chemical composition (composition) of A to BY shown in Tables 1 to 3 was cast, and the hot rolling step conditions (steel embryo heating temperature, rolling end temperature) shown in Tables 4 to 7 were cast. The hot rolling is performed, and the hot rolling step conditions (average cooling rate from the end of hot rolling to coiling, coiling temperature, and formula (1)) shown in Tables 4 to 7 are performed to obtain hot rolling. Steel plate. Thereafter, the hot-rolled steel sheet was pickled (immersed in 10% hydrochloric acid at 80 ° C, the immersion time is shown in Tables 4 to 7), and the cold rolling step conditions (rolling reduction ratio) shown in Tables 4 to 7 were performed. Cold rolled steel sheets were produced by rolling.

接著,對所製得之冷軋鋼板,以表8~表11所示退火步驟的加熱步驟條件(預熱帶的空氣比、預熱帶氣體環境中的Log(P(H 2O)/P(H 2))、均熱帶氣體環境中的Log(P(H 2O)/P(H 2))、在600℃~750℃之溫度域的平均加熱速度、最高加熱溫度)施行退火。將該鋼板以表8~表11所示條件(冷卻速度1(在760℃~700℃之溫度域的平均冷卻速度)、冷卻速度2(在650℃~500℃之溫度域的平均冷卻速度)、麻田散鐵變態處理條件(處理溫度、處理時間)、變韌鐵變態處理1的條件(處理溫度、處理時間))進行冷卻處理,而製得鍍敷處理用母材鋼板。 接著,以表12~表15所示條件(有效Al量、鍍敷浴溫度、鋼板進入溫度)浸漬於鍍鋅浴,並以表12~表15所示條件(冷卻速度3(至350℃為止之平均冷卻速度)、冷卻速度4(在350℃~250℃之溫度域的平均冷卻速度)、變韌鐵變態處理2的條件(處理溫度、處理時間)、再加熱處理條件(處理溫度、處理時間))進行鍍敷後冷卻處理。接著,以表12~表15所示條件(輥徑、加工次數)施行彎折-折回加工,並以表12~表15所示條件(軋縮率)施行冷軋延,而製得實驗例1~202的熔融鍍鋅鋼板(其中,一部份的實驗例中有中斷實驗者)。 Next, for the obtained cold-rolled steel sheet, the heating step conditions of the annealing step shown in Tables 8 to 11 (pre-tropical air ratio, Log(P(H 2 O)/P(H) in the pre-tropical gas environment) 2 )), Annealing is performed in Log (P(H 2 O)/P(H 2 )) in a tropical gas environment, an average heating rate in a temperature range of 600 ° C to 750 ° C, and a maximum heating temperature. The steel sheets have the conditions shown in Tables 8 to 11 (cooling rate 1 (average cooling rate in the temperature range of 760 ° C to 700 ° C) and cooling rate 2 (average cooling rate in the temperature range of 650 ° C to 500 ° C) The conditions (process temperature, treatment time) and the conditions of the toughened iron metamorphosis treatment 1 (treatment temperature, treatment time) of the granulated iron were subjected to a cooling treatment to obtain a base material steel sheet for plating treatment. Next, the conditions shown in Tables 12 to 15 (effective Al amount, plating bath temperature, and steel sheet entry temperature) were immersed in a galvanization bath, and the conditions shown in Tables 12 to 15 (cooling rate 3 (to 350 ° C) Average cooling rate), cooling rate 4 (average cooling rate in the temperature range of 350 ° C to 250 ° C), conditions of the toughened iron metamorphosis treatment 2 (treatment temperature, treatment time), reheating treatment conditions (treatment temperature, treatment) Time)) After the plating, it is cooled. Then, the bending-folding process was performed under the conditions shown in Tables 12 to 15 (roll diameter and number of times of processing), and cold rolling was performed under the conditions (rolling reduction ratio) shown in Tables 12 to 15 to obtain an experimental example. A hot-dip galvanized steel sheet of 1 to 202 (in which part of the experimental examples were interrupted).

接著,自各熔融鍍鋅鋼板以與母材鋼板之軋延方向平行之板厚截面為觀察面採取試料,並使用場發射掃描型電子顯微鏡(FE-SEM)進行微觀組織觀察及利用EBSD法進行高分解能晶體方向解析,分別測定以板厚1/4為中心之1/8厚度~3/8厚度範圍(1/4厚度)、及以鍍敷層與母材鋼板之界面為起點之至深度20μm為止的表層部(基鐵表層)的微觀組織的體積分率。此外,表16~表19中「麻田散鐵」表示新生麻田散鐵,表16~表19中微觀組織中之「其他」表示波來鐵及/或粗大的雪明碳鐵。且,「硬質相」係指由變韌鐵、變韌肥粒鐵、新生麻田散鐵與回火麻田散鐵之中1種以上所構成之硬質組織。Next, a sample was taken from each of the hot-dip galvanized steel sheets with a plate thickness section parallel to the rolling direction of the base material steel plate, and a microstructure was observed by a field emission scanning electron microscope (FE-SEM) and high by the EBSD method. Decomposition of crystal direction analysis, measuring 1/8 thickness to 3/8 thickness range (1/4 thickness) centered on 1/4 of the plate thickness, and starting from the interface between the plating layer and the base material steel plate to a depth of 20 μm The volume fraction of the microstructure of the surface layer portion (base iron surface layer). In addition, in Tables 16 to 19, "Mada's loose iron" means the new Ma Tian loose iron, and the "others" in the microstructures in Tables 16 to 19 indicate the Borne iron and/or the coarse swarf carbon iron. Further, the "hard phase" refers to a hard structure composed of one or more of toughened iron, toughened ferrite iron, new Matian loose iron, and tempered Matian loose iron.

鍍敷附著量係用摻有抑制劑之鹽酸來熔融鍍敷層,並比較熔融前後的重量而求得。同時用ICP定量Fe、Al來測定鍍敷層中的Fe濃度、Al濃度。The plating adhesion amount was obtained by melting the plating layer with hydrochloric acid doped with an inhibitor and comparing the weights before and after melting. At the same time, Fe and Al were quantitatively determined by ICP to determine the Fe concentration and the Al concentration in the plating layer.

然後,自鍍敷鋼板以與母材鋼板之軋延方向平行之板厚截面為觀察面採取試料,並用上述測定方法求出在母材鋼板與熔融鍍鋅層之界面的Fe-Al合金層的平均厚度與寬度方向的厚度差、以及與其直接相接之微細化層的平均厚度與寬度方向的厚度差、微細化層內之肥粒鐵相的平均粒徑(肥粒鐵相平均粒徑)、及微細化層中Si及Mn中之1種或2種以上氧化物的最大徑(氧化物最大徑)。並將該結果示於表20~表23。Then, a sample is taken from the plated steel sheet in a plate thickness section parallel to the rolling direction of the base material steel plate, and the Fe-Al alloy layer at the interface between the base material steel plate and the hot-dip galvanized layer is obtained by the above-described measurement method. The difference in thickness between the average thickness and the width direction, and the difference in thickness between the average thickness and the width direction of the micronized layer directly contacting the micro-thin layer, and the average particle diameter of the ferrite-grain iron phase in the micro-layer (fertilizer iron-phase average particle diameter) And the maximum diameter (maximum oxide diameter) of one or more oxides of Si and Mn in the micronized layer. The results are shown in Tables 20 to 23.

接著,為了調查鍍敷鋼板的特性,而進行了拉伸試驗、擴孔試驗、彎曲試驗、疲勞試驗、密著性評估試驗、點熔接試驗、腐蝕試驗、碎裂性試驗、粉碎性試驗及鍍敷外觀均勻性評估。並於表24~表31顯示各實驗例之特性。Next, in order to investigate the characteristics of the plated steel sheet, tensile test, hole expansion test, bending test, fatigue test, adhesion evaluation test, spot welding test, corrosion test, fragmentation test, pulverization test, and plating were performed. Appearance uniformity assessment. The characteristics of each experimental example are shown in Tables 24 to 31.

拉伸試驗係自鍍敷鋼板做出JIS Z 2201所記載之5號試驗片,並依JIS Z2241所記載之方法求出降伏強度YS、拉伸最大強度TS、總延伸率El。此外,拉伸特性係將拉伸最大強度TS為550MPa以上之情況評估為良好。 擴孔試驗係依JIS Z 2256所記載之方法進行。成形性中,延性(總延伸率)El及擴孔性λ雖會隨拉伸最大強度TS而變化,但於滿足下述式(2)時評估強度、延性及擴孔性為良好。 TS 1.5×El×λ 0.5≧ 2.0×10 6・・・式(2) In the tensile test, the test piece No. 5 described in JIS Z 2201 was prepared from the plated steel sheet, and the drop strength YS, the maximum tensile strength TS, and the total elongation El were determined according to the method described in JIS Z2241. Further, the tensile properties were evaluated as good when the maximum tensile strength TS was 550 MPa or more. The hole expansion test was carried out in accordance with the method described in JIS Z 2256. In the formability, the ductility (total elongation) El and the hole expandability λ vary depending on the maximum tensile strength TS, but the strength, ductility, and hole expandability are evaluated when the following formula (2) is satisfied. TS 1.5 × El × λ 0.5 ≧ 2.0 × 10 6・・・式(2)

彎曲試驗係自熔融鍍鋅鋼板做出JIS Z 2201所記載的5號試驗片,並依JIS Z 2248所記載之V型凹塊法進行90°V彎曲試驗。使V型凹塊底部之半徑以0.5mm刻度從1.0mm變到6.0mm為止,並以試驗片未產生龜裂之最小半徑作為最小彎曲半徑r[mm]。彎曲性係將最小彎曲半徑r以板厚t[mm]規格化之「r/t」作評估,將「r/t」在2.0以下之情況評估為良好的彎曲性。In the bending test, the No. 5 test piece described in JIS Z 2201 was prepared from the hot-dip galvanized steel sheet, and the 90° V bending test was carried out in accordance with the V-shaped concave block method described in JIS Z 2248. The radius of the bottom of the V-shaped concave block was changed from 1.0 mm to 6.0 mm on a scale of 0.5 mm, and the minimum radius at which the test piece was not cracked was taken as the minimum bending radius r [mm]. The bending property was evaluated by evaluating the minimum bending radius r as "r/t" normalized by the thickness t [mm], and evaluating "r/t" below 2.0 as good bending property.

疲勞試驗係從熔融鍍鋅鋼板做出JIS Z 2275所記載的1號試驗片,並依JIS Z 2273進行脈衝平面彎曲疲勞試驗。將最大反覆次數設為1000萬次來評估疲勞極限DL及疲勞極限比DL/TS,將疲勞極限比在0.30以上之情況評估為良好的耐疲勞特性。In the fatigue test, the No. 1 test piece described in JIS Z 2275 was prepared from the hot-dip galvanized steel sheet, and the pulse plane bending fatigue test was performed in accordance with JIS Z 2273. The fatigue limit DL and the fatigue limit ratio DL/TS were evaluated by setting the maximum number of repetitions to 10 million times, and the fatigue limit ratio was evaluated to be a good fatigue resistance characteristic with a fatigue limit ratio of 0.30 or more.

鍍敷密著性係對賦予了5%單軸拉伸應變之鍍敷鋼板施行杜邦衝撃試驗。於衝撃試驗後之鍍敷鋼板貼上黏著膠帶後剝除,將鍍敷未被剝離之情況評估為特別良好(◎),鍍敷有被剝離5%以上之情況評估為不良(×),鍍敷剝離小於5%之情況評估為良好(○)。杜邦衝撃試驗係使用前端的曲率半徑設為1/2吋的衝頭,使3kg的錘自1m高度落下來進行。The plating adhesion was performed on a plated steel sheet to which 5% uniaxial tensile strain was imparted. The plated steel sheet after the smashing test was peeled off with an adhesive tape, and the plating was not peeled off, and it was evaluated as particularly good (?), and the plating was evaluated as poor (×) when peeled by 5% or more, and plating was performed. The case where the peeling was less than 5% was evaluated as good (○). The DuPont Crushing Test uses a punch with a radius of curvature of 1/2 turn at the front end to allow a 3 kg hammer to fall from a height of 1 m.

點熔接性係進行連續打點試驗作評估。以熔融部直徑成為板厚平方根的5.3~5.7倍之熔接條件連續進行1000次點熔接。並以熔融部直徑之第1點d 1與第1000點d 1000作比較,d 1000/d 1在0.90以上之情況評估為合格(○),小於0.90之情況評估為不合格(×)。 The point weldability is evaluated by a continuous dot test. The spot welding was carried out 1,000 times in a welding condition in which the diameter of the molten portion became 5.3 to 5.7 times the square root of the plate thickness. Further, the first point d 1 of the diameter of the molten portion was compared with the 1000th point d 1000 , and the case where d 1000 /d 1 was 0.90 or more was evaluated as pass (○), and the case of less than 0.90 was evaluated as unacceptable (×).

耐蝕性評估係使用自鍍敷鋼板切出150mm×70mm之試驗片。對試驗片施行磷酸鋅系浸漬型化學轉化處理,接著施行20μm的陽離子電鍍塗裝、35μm的中間塗裝、35μm的表塗塗裝後,將背面與端部用絕緣膠帶密封。耐蝕性試驗係使用以SST 6hr→乾燥4hr→濕潤4hr→冷凍4hr為1循環之CCT。塗裝後耐蝕性評估係對塗裝面用切刀施行橫切到母材鋼板為止來測定CCT 60循環後的膨脹寬度。膨脹寬度在3.0mm以下之情況評估為合格(○),大於3.0mm之情況評估為不合格(×)。The corrosion resistance evaluation was performed by cutting a test piece of 150 mm × 70 mm from a plated steel plate. The test piece was subjected to a zinc phosphate-based immersion chemical conversion treatment, followed by a 20 μm cation plating coating, a 35 μm intermediate coating, and a 35 μm surface coating, and then the back surface and the end portion were sealed with an insulating tape. The corrosion resistance test used CCT with SST 6 hr → drying 4 hr → wet 4 hr → freezing 4 hr for 1 cycle. The evaluation of the corrosion resistance after coating was carried out by cutting the coated surface with a cutter to the base metal steel sheet to measure the expansion width after 60 cycles of CCT. The case where the expansion width was 3.0 mm or less was evaluated as pass (○), and the case where the expansion width was more than 3.0 mm was evaluated as unacceptable (×).

碎裂性係使用自鍍敷鋼板切出70mm×150mm的試驗片來進行評估。首先,對試驗片進行汽車用脫脂、形成化學轉化皮膜、及3層塗裝之各步驟。接著,於將試驗片冷卻保持在-20℃之狀態下,以2kgf/cm 2的空氣壓垂直照射10個碎石(0.3g~0.5g)。碎石的照射係對各試驗片反覆各進行5次來實施。之後,對各試驗片觀察合計50個碎裂痕,並就該剝離界面的位置依以下基準評估。剝離界面在比鍍敷層更上面(鍍敷層-化學轉化皮膜之界面、或電鍍塗裝-中間塗裝之界面)評估為合格(○),在鍍敷層-基鐵之界面有1處剝離評估為不合格(×)。 Fragmentation was carried out by using a test piece of 70 mm × 150 mm cut out from a plated steel plate. First, the test piece was subjected to steps of degreasing, forming a chemical conversion film, and three-layer coating for automobiles. Next, 10 pieces of gravel (0.3 g to 0.5 g) were vertically irradiated with an air pressure of 2 kgf/cm 2 while the test piece was cooled and maintained at -20 °C. The irradiation of the crushed stone was carried out five times for each test piece. Thereafter, a total of 50 cracks were observed for each test piece, and the position of the peeling interface was evaluated based on the following criteria. The peeling interface was evaluated to be more qualified than the plating layer (the interface of the plating layer-chemical conversion film or the interface of the plating coating-intermediate coating) (○), and there was one place at the interface of the plating layer-based iron. The peeling evaluation was unacceptable (×).

粉碎性為評估鍍敷層的加工性,係使用V彎曲加工(JIS Z 2248)進行評估。將鍍敷鋼板切成50×90mm,用1R-90°V字模具壓製機形成成型體作成試驗體。對各試驗體的谷部實施膠帶剝離。具體而言,係於試驗體的彎曲加工部上壓抵寬度為24mm的玻璃紙膠帶並撕起後,目視判斷玻璃紙膠帶長度90mm之部分。評估基準如下。鍍敷層的剝離相對於加工部面積小於5%評估為合格(○),鍍敷層的剝離相對於加工部面積大於5%評估為不合格(×)。The pulverizability was evaluated by evaluating the workability of the plating layer using V bending processing (JIS Z 2248). The plated steel sheet was cut into 50 × 90 mm, and a molded body was formed using a 1R-90°V-shaped mold press to prepare a test body. Tape peeling was performed on the valley of each test body. Specifically, after the cellophane tape having a width of 24 mm was pressed against the bent portion of the test piece and torn, the portion of the cellophane tape having a length of 90 mm was visually judged. The evaluation criteria are as follows. The peeling of the plating layer was evaluated as acceptable (○) with respect to the area of the processed portion of less than 5%, and the peeling of the plating layer was evaluated as unacceptable (×) with respect to the area of the processed portion of more than 5%.

外觀均勻性評估係測定鋼板寬度方向上距離其両端50mm之位置與將其之間分成7等分共計8處的明度(L*値),最大値減去最小値所得之差小於5評估為均勻(○), 5以上且小於10評估為稍不均勻(△),10以上評估為不均勻(×)。Appearance uniformity evaluation is to determine the position of the steel plate in the width direction of 50 mm from the 両 end and the brightness (L*値) of 8 points divided into 7 equal parts. The difference between the maximum 値 minus the minimum 小于 is less than 5 and is evaluated as uniform. (○), 5 or more and less than 10 were evaluated as slightly uneven (Δ), and 10 or more was evaluated as uneven (×).

[表1] [Table 1]

[表2] [Table 2]

[表3] [table 3]

[表4] [Table 4]

[表5] [table 5]

[表6] [Table 6]

[表7] [Table 7]

[表8] [Table 8]

[表9] [Table 9]

[表10] [Table 10]

[表11] [Table 11]

[表12] [Table 12]

[表13] [Table 13]

[表14] [Table 14]

[表15] [Table 15]

[表16] [Table 16]

[表17] [Table 17]

[表18] [Table 18]

[表19] [Table 19]

[表20] [Table 20]

[表21] [Table 21]

[表22] [Table 22]

[表23] [Table 23]

[表24] [Table 24]

[表25] [Table 25]

[表26] [Table 26]

[表27] [Table 27]

[表28] [Table 28]

[表29] [Table 29]

[表30] [Table 30]

[表31] [Table 31]

本發明實施例之實驗例30的有效Al量雖為0.180質量%,但Fe-Al合金有沿寬度方向均勻生成,故無專利文獻12所記載之鍍敷密著性降低,反而有改善。In the experimental example 30 of the embodiment of the present invention, the effective Al amount is 0.180% by mass, but the Fe-Al alloy is uniformly formed in the width direction. Therefore, the plating adhesion described in Patent Document 12 is not lowered, and the improvement is improved.

實驗例187係C含量小故硬質相的體積分率變小,而無法獲得充分的強度、延性及擴孔性之例。 實驗例188係C含量大故點熔接性變差之例。且其麻田散鐵的分率變大,而耐疲勞特性、延性、擴孔性及彎曲性較差。In Experimental Example 187, when the C content was small, the volume fraction of the hard phase became small, and sufficient strength, ductility, and hole expandability could not be obtained. Experimental Example 188 is an example in which the C content is large and the weldability of the spot is deteriorated. Moreover, the fraction of the granulated iron in the kenian becomes large, and the fatigue resistance, ductility, hole expandability, and bendability are inferior.

實驗例189係Si含量小,而在退火步驟及鍍敷步驟中生成大量波來鐵及粗大雪明碳鐵,無法充分獲得鋼板成形性之例。 實驗例190係Si含量大,而於熱軋步驟中鋼胚在加熱中龜裂,故中斷實驗之例。In Experimental Example 189, a large amount of Si was formed, and in the annealing step and the plating step, a large amount of ferrite and coarse swarf carbon iron were generated, and the formability of the steel sheet could not be sufficiently obtained. In Experimental Example 190, the Si content was large, and in the hot rolling step, the steel embryo was cracked during heating, so that the experiment was interrupted.

實驗例191係Mn含量小,而在退火步驟及鍍敷步驟中生成大量波來鐵及粗大雪明碳鐵,無法充分獲得鋼板成形性之例。 實驗例192係Mn含量大,而於熱軋步驟中鋼胚在加熱中龜裂,故中斷實驗之例。In Experimental Example 191, the Mn content was small, and a large amount of pulverized iron and coarse swarf carbon iron were generated in the annealing step and the plating step, and the formability of the steel sheet could not be sufficiently obtained. In Experimental Example 192, the Mn content was large, and in the hot rolling step, the steel embryo was cracked during heating, so that the experiment was interrupted.

實驗例193係P含量大,而在熱軋步驟中軋延鋼胚後發生龜裂,故中斷實驗之例。 實驗例194係S含量大,而生成大量粗大硫化物,故延性、擴孔性、彎曲性、點熔接性及耐疲勞特性變差之例。 實驗例195係Al含量大,而在熱軋步驟中鋼胚在運送中龜裂,故中斷實驗之例。In Experimental Example 193, the content of P was large, and cracking occurred after rolling the steel preform in the hot rolling step, so that the experiment was interrupted. In Experimental Example 194, the S content was large, and a large amount of coarse sulfide was formed, so that ductility, hole expandability, bendability, spot weldability, and fatigue resistance were deteriorated. In Experimental Example 195, the Al content was large, and in the hot rolling step, the steel blank was cracked during transportation, so that the experiment was interrupted.

實驗例196係N含量大,而生成大量的粗大氮化物,故延性、擴孔性、彎曲性、點熔接性及耐疲勞特性變差之例。 實驗例197係O含量大,而生成大量的粗大氧化物,故延性、擴孔性、彎曲性、點熔接性及耐疲勞特性變差之例。In Experimental Example 196, a large amount of N was formed, and a large amount of coarse nitride was formed, so that ductility, hole expandability, bendability, spot weldability, and fatigue resistance were deteriorated. In Experimental Example 197, a large amount of O was formed, and a large amount of coarse oxide was formed, so that ductility, hole expandability, bendability, spot weldability, and fatigue resistance were deteriorated.

實驗例28、131、155係在熱軋延步驟中式(1)的値小,故表層的硬質相分率(V1/V2)變大,而無法獲得充分的彎曲性之例。 實驗例51、114、165係在熱軋延步驟中式(1)的値大,而表層的脫碳過度進行,故硬質相分率(V1/V2)變小,無法獲得充分的耐疲勞特性之例。In Experimental Examples 28, 131, and 155, since the reduction of the formula (1) in the hot rolling step is small, the hard phase fraction (V1/V2) of the surface layer is increased, and sufficient flexibility cannot be obtained. In Experimental Examples 51, 114, and 165, in the hot rolling step, the formula (1) was large, and the decarburization of the surface layer was excessively performed. Therefore, the hard phase fraction (V1/V2) was small, and sufficient fatigue resistance could not be obtained. example.

實驗例84係在退火步驟中,在600℃~750℃間之溫度域的平均加熱速度小,故鋼板內部之氧化物成長過度進行,而生成會成為破壞起點的粗大氧化物,故彎曲性、耐疲勞特性變差之例。此外,伴隨彎曲性變差,在鍍敷密著性及粉碎性的評估試驗中發生因鋼板彎曲龜裂造成鍍敷剝離,故鍍敷密著性及粉碎性亦變差。 實驗例202在退火步驟中,於600℃~750℃間之溫度域的平均加熱速度過大,故鋼板寬度方向上之微細化層厚度之最大値與最小値的差大於2.0μm,而且鋼板寬度方向上之Fe-Al合金層厚度之最大値與最小値的差大於0.5μm。因此,鍍敷外觀稍不均勻。In the annealing example, in the annealing step, since the average heating rate in the temperature range between 600 ° C and 750 ° C is small, the oxide inside the steel sheet is excessively grown, and a coarse oxide which is a starting point of destruction is formed, so that the bending property is high. An example of deterioration of fatigue resistance. In addition, as the bending property is deteriorated, plating peeling occurs due to bending cracks of the steel sheet in the evaluation test of the plating adhesion and the pulverization property, so that the plating adhesion and the pulverizability are also deteriorated. In the annealing step, in the annealing step, the average heating rate in the temperature range between 600 ° C and 750 ° C is excessively large, so that the difference between the maximum 値 and the minimum 厚度 of the thickness of the fine layer in the width direction of the steel sheet is more than 2.0 μm, and the width direction of the steel sheet The difference between the maximum 値 and the minimum 厚度 of the thickness of the Fe-Al alloy layer is greater than 0.5 μm. Therefore, the plating appearance is slightly uneven.

實驗例67係在退火步驟中,最高加熱溫度(TM)比Ac3溫度高,故在1/4厚度的肥粒鐵相的體積分率變小,而延性及彎曲性變差之例。 實驗例183係在退火步驟中最高加熱溫度(TM)比(Ac1+20)℃低,故熔融殘留粗大的鐵系碳化物,而延性及擴孔性變差之例。 實驗例46係在退火步驟之加熱步驟中預熱帶的空氣比小,故鍍敷密著性變差之例。此外,因鍍敷密著性變差造成在彎曲變形時發生鍍敷剝離,故粉碎性亦變差。且,未鍍敷到亦造成外觀不良。In Experimental Example 67, in the annealing step, since the maximum heating temperature (TM) was higher than the Ac3 temperature, the volume fraction of the ferrite-grain iron phase at a thickness of 1/4 became small, and the ductility and the bendability were deteriorated. In Experimental Example 183, the maximum heating temperature (TM) was lower than (Ac1 + 20) °C in the annealing step, so that coarse iron-based carbides remained in the melt, and ductility and hole expandability were deteriorated. In Experimental Example 46, the air ratio of the pre-tropical zone was small in the heating step of the annealing step, so that the plating adhesion was deteriorated. Further, since plating adhesion occurs during bending deformation due to deterioration in plating adhesion, pulverizability is also deteriorated. Moreover, it is not plated and also causes poor appearance.

實驗例16係在退火步驟之加熱步驟中預熱帶的空氣比大,使表層的脫碳過度進行,故硬質相的分率(V1/V2)變小,而耐疲勞特性變差之例。並且,其為微細化層的平均厚度變厚,使鍍敷層的合金化(Zn-Fe合金生成)過度進行,造成鍍敷層中的Fe含量增加,而鍍敷密著性、碎裂性、粉碎性變差之例。In the experimental example 16, in the heating step of the annealing step, the air ratio of the pre-tropical zone is large, and the decarburization of the surface layer is excessively performed, so that the fraction (V1/V2) of the hard phase is small, and the fatigue resistance is deteriorated. In addition, the average thickness of the fine layer is increased, and the alloying of the plating layer (formation of Zn-Fe alloy) is excessively performed, resulting in an increase in Fe content in the plating layer, and plating adhesion and chipping property. An example of a smashing property.

實驗例181係在退火步驟之加熱步驟中預熱帶的Log(P(H 2O)/P(H 2))小,使表層未微細化,而鍍敷密著性變差之例。此外,表面的肥粒鐵的平均粒徑為3.2μm,在自表面起0.5μm之範圍的鋼板內部的氧化物最大徑低於0.01μm。而且,未鍍敷到亦造成外觀不良。 實驗例168係在退火步驟之加熱步驟中均熱帶的Log(P(H 2O)/P(H 2))小,使母材鋼板表層的粒徑無微細化,而鍍敷密著性變差之例。此外,母材鋼板表面的肥粒鐵的平均粒徑為3.4μm,在自表面起0.5μm之範圍的鋼板內部的氧化物最大徑低於0.01μm。 In Experimental Example 181, the Log (P(H 2 O)/P(H 2 )) of the pre-tropical zone was small in the heating step of the annealing step, and the surface layer was not refined, and the plating adhesion was deteriorated. Further, the average grain size of the ferrite iron on the surface was 3.2 μm, and the maximum diameter of the oxide inside the steel sheet in the range of 0.5 μm from the surface was less than 0.01 μm. Moreover, it is not plated and also causes poor appearance. In Experimental Example 168, the log (P(H 2 O)/P(H 2 )) in the tropical zone was small in the heating step of the annealing step, so that the particle size of the surface layer of the base material steel plate was not refined, and the plating adhesion was changed. Poor example. Further, the average particle diameter of the ferrite iron on the surface of the base material steel sheet was 3.4 μm, and the maximum diameter of the oxide inside the steel sheet in the range of 0.5 μm from the surface was less than 0.01 μm.

實驗例198係在退火步驟之加熱步驟中預熱帶的Log(P(H 2O)/P(H 2))大,故表層的微細化層過度變厚,使鍍敷層的合金化(生成Zn-Fe合金)過度進行,造成鍍敷層中的Fe含量增加,而鍍敷密著性變差之例。又,鋼板寬度方向上之Fe-Al合金層厚度之最大値與最小値的差大於0.5μm,故鍍敷外觀不均勻。 實驗例75係在退火步驟之加熱步驟中均熱帶的Log(P(H 2O)/P(H 2))特別大,表層的脫碳過度進行,使硬質相的分率(V1/V2)變小,故耐疲勞特性變差之例。並且,母材鋼板表層的微細化層過度變厚,使鍍敷層的合金化(生成Zn-Fe合金)過度進行,造成鍍敷層中的Fe含量增加,而鍍敷密著性、碎裂性、粉碎性變差之例。 In Experimental Example 198, the Log (P(H 2 O)/P(H 2 )) of the pre-tropical zone was large in the heating step of the annealing step, so that the surface layer of the fine layer was excessively thickened, and the plating layer was alloyed (generated). Excessive progress of the Zn-Fe alloy causes an increase in the Fe content in the plating layer and an example in which the plating adhesion is deteriorated. Further, the difference between the maximum 値 and the minimum 厚度 of the thickness of the Fe-Al alloy layer in the width direction of the steel sheet is more than 0.5 μm, so that the plating appearance is not uniform. In the experimental example 75, the log (P(H 2 O)/P(H 2 )) of the tropical zone was particularly large in the heating step of the annealing step, and the decarburization of the surface layer was excessively performed to make the fraction of the hard phase (V1/V2). As it becomes smaller, the fatigue resistance is deteriorated. Further, the fine layer of the surface layer of the base material steel sheet is excessively thick, and the alloying of the plating layer (formation of a Zn-Fe alloy) is excessively performed, resulting in an increase in the Fe content in the plating layer, and plating adhesion and chipping. Examples of poor sex and pulverization.

實驗例22係在退火步驟之加熱步驟中,在760℃~700℃間之平均冷卻速度(冷卻速度1)小,而生成大量的波來鐵,故延性及擴孔性變差之例。 實驗例49係在退火步驟之加熱步驟中,在760℃~700℃間之平均冷卻速度(冷卻速度1)大,使在1/4厚度的肥粒鐵相的體積分率變小,而無法獲得充分的延性之例。 實驗例137係在退火步驟之加熱步驟中,在650℃~500℃間之平均冷卻速度(冷卻速度2)小,而生成大量的波來鐵,故延性及擴孔性變差之例。In the heating step of the annealing step, in the heating step of the annealing step, the average cooling rate (cooling rate 1) between 760 ° C and 700 ° C is small, and a large amount of ferrite is generated, so that the ductility and the hole expandability are deteriorated. In Experimental Example 49, in the heating step of the annealing step, the average cooling rate (cooling rate 1) between 760 ° C and 700 ° C was large, and the volume fraction of the ferrite-grain iron phase at 1/4 thickness was small, and it was impossible to Obtain sufficient examples of ductility. In Experimental Example 137, in the heating step of the annealing step, the average cooling rate (cooling rate 2) between 650 ° C and 500 ° C was small, and a large amount of ferrite was generated, so that ductility and hole expandability were deteriorated.

實驗例2係在鍍敷步驟中,鍍敷浴中的有效Al濃度低,無法生成充分厚度的Fe-Al合金層,鍍敷層中的Fe含量變大,而無法獲得鍍敷密著性、碎裂性、粉碎性,鍍敷的外觀均勻性之例。 實驗例14係在鍍敷步驟中,鍍敷浴中的有效Al濃度極低,無法形成Fe-Al合金層,且鍍敷層中的Fe含量過度升高,而無法獲得充分的鍍敷密著性、碎裂性、粉碎性、鍍敷外觀均勻性之例。 實驗例148係在鍍敷步驟中,鍍敷浴中的有效Al濃度高,使鍍敷層中的Al含量過度升高,而無法獲得充分的鍍敷密著性、點熔接性之例。 實驗例180係在鍍敷步驟中鍍敷後冷卻速度小,鍍敷層中的Fe含量過度升高,而無法獲得充分的鍍敷密著性、碎裂性、粉碎性之例。In Experimental Example 2, in the plating step, the effective Al concentration in the plating bath was low, and a Fe-Al alloy layer having a sufficient thickness could not be formed, and the Fe content in the plating layer became large, and plating adhesion could not be obtained. Examples of fragmentation, pulverizability, and uniformity of appearance of plating. In Experimental Example 14, in the plating step, the effective Al concentration in the plating bath was extremely low, and the Fe-Al alloy layer could not be formed, and the Fe content in the plating layer was excessively increased, and sufficient plating adhesion could not be obtained. Examples of properties, fragmentation, pulverizability, and uniformity of plating appearance. In Experimental Example 148, in the plating step, the effective Al concentration in the plating bath was high, and the Al content in the plating layer was excessively increased, and sufficient plating adhesion and spot fusion properties could not be obtained. In Experimental Example 180, the cooling rate after plating in the plating step was small, and the Fe content in the plating layer was excessively increased, and sufficient plating adhesion, chipping property, and pulverizability could not be obtained.

實驗例8、17、31、81、179係在退火步驟之冷卻步驟中施行麻田散鐵變態處理之例,而製得成形性、鍍敷密著性、熔接性、耐蝕性及耐疲勞特性優異之高強度熔融鍍鋅鋼板。 實驗例37、45、66、89、102、104、108、142、149、162係在退火步驟之冷卻步驟中施行變韌鐵變態處理1之例,而製得成形性、鍍敷密著性、熔接性、耐蝕性及耐疲勞特性優異之高強度熔融鍍鋅鋼板。 實驗例43係在退火步驟之冷卻步驟中施行變韌鐵變態處理1之例,然其因處理溫度高,故生成波來鐵及粗大雪明碳鐵,而延性及擴孔性變差。 實驗例174係在退火步驟之冷卻步驟中施行變韌鐵變態處理1之例,然其因處理時間長,故生成波來鐵及粗大雪明碳鐵,而延性及擴孔性變差。Experimental Examples 8, 17, 31, 81, and 179 are examples in which the metamorphic treatment of the granulated iron is performed in the cooling step of the annealing step, and the formability, the plating adhesion, the weldability, the corrosion resistance, and the fatigue resistance are excellent. High strength hot-dip galvanized steel sheet. Experimental Examples 37, 45, 66, 89, 102, 104, 108, 142, 149, and 162 were subjected to the toughening iron metamorphosis treatment 1 in the cooling step of the annealing step to obtain formability and plating adhesion. High-strength hot-dip galvanized steel sheet with excellent weldability, corrosion resistance and fatigue resistance. In the experimental example 43, an example of the toughening iron metamorphosis treatment 1 was carried out in the cooling step of the annealing step. However, since the treatment temperature was high, the ferrite and the coarse snow-capped carbon iron were generated, and the ductility and the hole expandability were deteriorated. Experimental Example 174 was an example in which the toughening iron metamorphosis treatment 1 was carried out in the cooling step of the annealing step. However, since the treatment time was long, the ferrite and the coarse stellite carbon were generated, and the ductility and the hole expandability were deteriorated.

實驗例25、41、55、90、113、135、152、170、184係在鍍敷後冷卻步驟中施行變韌鐵變態處理2之例,而製得成形性、鍍敷密著性、熔接性、耐蝕性及耐疲勞特性優異之高強度熔融鍍鋅鋼板。 實驗例163係在鍍敷後冷卻步驟中施行變韌鐵變態處理2之例,然其因處理溫度高,故生成大量殘留沃斯田鐵,而為損及彎曲性之例。 實驗例5、20、48、53、62、73、76、87、94、112、129、186係在鍍敷後冷卻步驟中施行再加熱處理之例,而製得成形性、鍍敷密著性、熔接性、耐蝕性及耐疲勞特性優異之高強度熔融鍍鋅鋼板。Experimental Examples 25, 41, 55, 90, 113, 135, 152, 170, and 184 are examples in which the toughening iron metamorphosis treatment 2 is performed in the post-plating cooling step to obtain formability, plating adhesion, and fusion. High-strength hot-dip galvanized steel sheet excellent in properties, corrosion resistance and fatigue resistance. In Experimental Example 163, an example of the toughening iron metamorphosis treatment 2 was carried out in the post-plating cooling step. However, since the treatment temperature was high, a large amount of residual Worthite iron was generated, which was an example of the loss of flexibility. Experimental Examples 5, 20, 48, 53, 62, 73, 76, 87, 94, 112, 129, and 186 were subjected to reheating treatment in the post-plating cooling step to obtain formability and plating adhesion. High-strength hot-dip galvanized steel sheet excellent in properties, weldability, corrosion resistance and fatigue resistance.

實驗例18係在退火步驟之冷卻步驟中施行麻田散鐵變態處理及變韌鐵變態處理1之例,而製得成形性、鍍敷密著性、熔接性、耐蝕性及耐疲勞特性優異之高強度熔融鍍鋅鋼板。 實驗例9、110、132、138、154、169係在退火步驟之冷卻步驟中施行變韌鐵變態處理1後,於鍍敷後冷卻步驟中施行變韌鐵變態處理2之例,而製得成形性、鍍敷密著性、熔接性、耐蝕性及耐疲勞特性優異之高強度熔融鍍鋅鋼板。 實驗例24、34、96係在退火步驟之冷卻步驟中施行變韌鐵變態處理1後,於鍍敷後冷卻步驟中施行再加熱處理之例,而製得成形性、鍍敷密著性、熔接性、耐蝕性及耐疲勞特性優異之高強度熔融鍍鋅鋼板。In the experimental example 18, the Matian iron treatment and the toughening iron transformation treatment 1 were carried out in the cooling step of the annealing step, and the moldability, the plating adhesion, the weldability, the corrosion resistance and the fatigue resistance were excellent. High-strength galvanized steel sheet. In the experimental examples 9, 110, 132, 138, 154, and 169, after the toughening iron metamorphosis treatment 1 was performed in the cooling step of the annealing step, an example of the toughening iron metamorphosis treatment 2 was performed in the post-plating cooling step. High-strength hot-dip galvanized steel sheet excellent in formability, plating adhesion, weldability, corrosion resistance, and fatigue resistance. In the experimental examples 24, 34, and 96, after the toughening iron metamorphosis treatment 1 was performed in the cooling step of the annealing step, the reheating treatment was performed in the post-plating cooling step to obtain formability, plating adhesion, High-strength hot-dip galvanized steel sheet excellent in weldability, corrosion resistance and fatigue resistance.

實驗例11係在鍍敷後冷卻步驟中施行了變韌鐵變態處理2及再加熱處理之例,而有製得成形性、鍍敷密著性、熔接性、耐蝕性及耐疲勞特性優異之高強度熔融鍍鋅鋼板,但卻如後述鍍敷外觀稍不均勻。In the eleventh example, the toughened iron metamorphosis treatment 2 and the reheat treatment were carried out in the post-plating cooling step, and the moldability, the plating adhesion, the weldability, the corrosion resistance, and the fatigue resistance were excellent. The high-strength hot-dip galvanized steel sheet has a slightly uneven appearance as described later.

實驗例172係在退火步驟的冷卻步驟中施行了變韌鐵變態處理1後,於鍍敷後冷卻步驟中施行了變韌鐵變態處理2及再加熱處理之例,而製得了成形性、鍍敷密著性、熔接性、耐蝕性及耐疲勞特性優異之高強度熔融鍍鋅鋼板。In the experimental example 172, after the toughening iron metamorphosis treatment 1 was performed in the cooling step of the annealing step, the toughening iron metamorphosis treatment 2 and the reheating treatment were performed in the post-plating cooling step, and the formability and plating were obtained. A high-strength hot-dip galvanized steel sheet excellent in adhesion, weldability, corrosion resistance, and fatigue resistance.

實驗例79係在加工步驟的彎折-折回加工步驟中加工所用之輥的直徑小,而於鋼板表層部導入過度的應變,導致延性變差之例。 實驗例59係在加工步驟的彎折-折回加工步驟中加工所用之輥的直徑大,而無法於鋼板表層部充分導入應變,故鋼板表層部有大量殘留沃斯田鐵存在,而彎曲性變差之例。In the experimental example 79, the diameter of the roll used for the processing in the bending-folding processing step of the processing step was small, and excessive strain was introduced into the surface layer portion of the steel sheet, resulting in an example in which the ductility was deteriorated. In the experimental example 59, the diameter of the roll used for the processing in the bending-folding processing step of the processing step was large, and the strain was not sufficiently introduced into the surface layer portion of the steel sheet, so that a large amount of residual Worth iron was present in the surface layer portion of the steel sheet, and the bending property was changed. Poor example.

實驗例3、11、116在熱軋步驟中的捲取溫度為650℃以上,故在鋼板寬度方向上之微細化層厚度之最大値與最小値的差大於2.0μm,並且,在鋼板寬度方向上之Fe-Al合金層厚度之最大値與最小値的差大於0.5μm,鍍敷外觀稍不均勻。 另一方面,實驗例4、12如同上述,雖熱軋步驟的捲取溫度在650℃以上但藉由增長酸洗步驟的酸洗時間,在鋼板寬度方向上之微細化層厚度之最大値與最小値的差好轉至2.0μm以內,並且在鋼板寬度方向上之Fe-Al合金層厚度之最大値與最小値的差好轉至0.5μm以內,而獲得良好的鍍敷外觀均勻性。 實施例200之捲取溫度雖低於650℃但酸洗時間為15秒而時間較短,故無法完全去除生成地不均勻之內部氧化層,而在鋼板寬度方向上之微細化層厚度之最大値與最小値的差大於2.0μm,並且在鋼板寬度方向上之Fe-Al合金層厚度之最大値與最小値的差大於0.5μm,鍍敷外觀稍不均勻。In the experimental examples 3, 11, and 116, the coiling temperature in the hot rolling step was 650 ° C or more, so that the difference between the maximum 値 and the minimum 微 of the thickness of the micronized layer in the width direction of the steel sheet was more than 2.0 μm, and in the width direction of the steel sheet. The difference between the maximum 値 and the minimum 厚度 of the thickness of the Fe-Al alloy layer is greater than 0.5 μm, and the plating appearance is slightly uneven. On the other hand, in Experimental Examples 4 and 12, as described above, although the coiling temperature of the hot rolling step was 650 ° C or higher, the maximum thickness of the micronized layer in the width direction of the steel sheet was increased by increasing the pickling time of the pickling step. The difference of the minimum enthalpy was improved to within 2.0 μm, and the difference between the maximum 値 and the minimum 厚度 of the thickness of the Fe-Al alloy layer in the width direction of the steel sheet was improved to within 0.5 μm, and good plating appearance uniformity was obtained. In the embodiment 200, the coiling temperature is lower than 650 ° C, but the pickling time is 15 seconds and the time is short, so that the internal oxide layer which is uneven in formation cannot be completely removed, and the thickness of the micronized layer in the width direction of the steel sheet is the largest. The difference between 値 and the minimum 大于 is more than 2.0 μm, and the difference between the maximum 値 and the minimum 厚度 of the thickness of the Fe—Al alloy layer in the width direction of the steel sheet is more than 0.5 μm, and the plating appearance is slightly uneven.

以上,已就本發明各實施形態進行了詳細說明,但上述實施形態皆僅為為了實施本發明而具體化之例。本發明之技術範圍並不受限於該等實施形態。亦即,只要不脫離本發明技術思想、或其主要特徴則可以各種形態實施本發明。The embodiments of the present invention have been described in detail above, but the above embodiments are merely examples for carrying out the invention. The technical scope of the present invention is not limited to the embodiments. That is, the present invention can be implemented in various forms without departing from the technical idea of the present invention or its main features.

產業上之可利用性 本發明係一可有效用於鍍敷的外觀均勻性、成形性、耐疲勞特性、熔接性、耐蝕性及鍍敷密著性優異之高強度熔融鍍鋅鋼板及其製造方法之技術。而且,依據本發明實施形態,可提供延性、擴孔性及彎曲性優異,並且成形後之鍍敷密著性優異,具高疲勞極限,且具優異點熔接性及耐蝕性之高強度熔融鍍鋅鋼板及其製造方法。INDUSTRIAL APPLICABILITY The present invention is a high-strength hot-dip galvanized steel sheet which can be effectively used for plating uniformity of appearance, formability, fatigue resistance, weldability, corrosion resistance and plating adhesion, and its production Method of technology. Further, according to the embodiment of the present invention, it is possible to provide high-strength hot-dip plating which is excellent in ductility, hole expandability, and bendability, and has excellent plating adhesion after molding, has a high fatigue limit, and has excellent spot weldability and corrosion resistance. Zinc steel plate and its manufacturing method.

10‧‧‧熔融鍍鋅層10‧‧‧Metal galvanized layer

20‧‧‧母材鋼板20‧‧‧Basic steel plate

30‧‧‧Fe-Al合金層30‧‧‧Fe-Al alloy layer

40‧‧‧微細化層40‧‧‧Microlayer

50‧‧‧脫碳層50‧‧‧Decarburized layer

60‧‧‧肥粒鐵相60‧‧‧Fat iron phase

圖式簡單說明 圖1係顯示本發明熔融鍍鋅鋼板之截面結構的示意圖。BRIEF DESCRIPTION OF THE DRAWINGS Fig. 1 is a schematic view showing a sectional structure of a hot-dip galvanized steel sheet according to the present invention.

Claims (9)

一種熔融鍍鋅鋼板,係於母材鋼板之至少一側具有熔融鍍鋅層,且該熔融鍍鋅鋼板之特徵在於前述母材鋼板具有以下化學組成:以質量%計,C:0.040%~0.280%、Si:0.05%~2.00%、Mn:0.50%~3.50%、P:0.0001%~0.1000%、S:0.0001%~0.0100%、Al:0.001%~1.500%、N:0.0001%~0.0100%、O:0.0001%~0.0100%、Ti:0%~0.150%、Nb:0%~0.100%、V:0%~0.300%、Cr:0%~2.00%、Ni:0%~2.00%、Cu:0%~2.00%、Mo:0%~2.00%、B:0%~0.0100%、W:0%~2.00%、及Ca、Ce、Mg、Zr、La及REM:合計0%~0.0100%,且 剩餘部份由Fe及雜質所構成;並且具有以下微觀組織:相對於前述母材鋼板的總厚度,以前述母材鋼板表面起1/4厚度為中心之1/8厚度~3/8厚度範圍中,肥粒鐵相以體積分率計為50%以上且97%以下,由變韌鐵相、變韌肥粒鐵相、新生麻田散鐵相與回火麻田散鐵相中之1種以上所構成之硬質組織的合計以體積分率計為3%以上,殘留沃斯田鐵相以體積分率計為0%~8%,波來鐵相與粗大雪明碳鐵相之合計以體積分率計為0%~8%,自前述熔融鍍鋅層與母材鋼板之界面起至母材鋼板方向深度20μm為止之表層部中,殘留沃斯田鐵以體積分率計為0~3%,前述表層部中前述硬質組織的體積分率V1、與以母材鋼板表面起1/4厚度為中心之1/8厚度~3/8厚度範圍中前述硬質組織的體積分率V2之比,V1/V2設為0.10以上且0.90以下之範圍;前述熔融鍍鋅層中Fe含量以質量%計大於0%且在3.0%以下,Al含量以質量%計大於0%且在1.0%以下,於前述熔融鍍鋅層與前述母材鋼板之界面具有平均厚度為0.1μm~2.0μm之Fe-Al合金層,且其在母材鋼板寬度方向上之最大厚度與最小厚度的差在0.5μm以內,前述母材鋼板內具有與前述Fe-Al合金層直接接觸之 微細化層,前述微細化層的平均厚度為0.1μm~5.0μm,前述微細化層內之肥粒鐵相的平均粒徑為0.1μm~3.0μm,前述微細化層中含有Si及Mn之1種或2種以上的氧化物,前述氧化物的最大徑為0.01μm~0.4μm,在母材鋼板寬度方向上之前述微細化層之最大厚度與最小厚度的差在2.0μm以內。 A hot-dip galvanized steel sheet having a hot-dip galvanized layer on at least one side of a base material steel sheet, and the hot-dip galvanized steel sheet is characterized in that the base material steel sheet has the following chemical composition: in mass%, C: 0.040% to 0.280 %, Si: 0.05% to 2.00%, Mn: 0.50% to 3.50%, P: 0.0001% to 0.1000%, S: 0.0001% to 0.0100%, Al: 0.001% to 1.500%, N: 0.0001% to 0.0100%, O: 0.0001% to 0.0100%, Ti: 0% to 0.150%, Nb: 0% to 0.100%, V: 0% to 0.300%, Cr: 0% to 2.00%, Ni: 0% to 2.00%, Cu: 0%~2.00%, Mo: 0%~2.00%, B: 0%~0.0100%, W: 0%~2.00%, and Ca, Ce, Mg, Zr, La, and REM: total 0%~0.0100%, And The remaining portion is composed of Fe and impurities; and has a microstructure in which a thickness of 1/8 to 3/8 is centered on the surface of the base material steel sheet with respect to the total thickness of the base material steel sheet; In the middle, the ferrite grain iron phase is 50% or more and 97% or less by volume fraction, and one or more of the toughened iron phase, the toughened ferrite iron phase, the newly formed Matian iron phase, and the tempered Matian iron phase The total amount of the hard structures formed is 3% or more in terms of volume fraction, and the residual Worstian iron phase is 0% to 8% by volume fraction, and the total volume of the Borne iron phase and the coarse snowy carbon iron phase is in volume. The fractional rate is 0% to 8%. From the interface between the hot-dip galvanized layer and the base material steel plate to the depth of the base metal plate in the direction of 20 μm, the remaining Worthite iron is 0 to 3 by volume fraction. %, the ratio of the volume fraction V1 of the hard structure in the surface layer portion to the volume fraction V2 of the hard tissue in the thickness range of 1/8 thickness to 3/8 centering on the surface of the base material steel sheet by 1/4 thickness , V1/V2 is set to a range of 0.10 or more and 0.90 or less; the Fe content in the above-mentioned hot-dip galvanized layer is more than 0% by mass% and 3.0% or less, and the Al content is The amount % is more than 0% and is 1.0% or less, and has an Fe-Al alloy layer having an average thickness of 0.1 μm to 2.0 μm at the interface between the hot-dip galvanized layer and the base material steel sheet, and is in the width direction of the base material steel sheet. The difference between the maximum thickness and the minimum thickness is within 0.5 μm, and the base material steel sheet has direct contact with the aforementioned Fe-Al alloy layer. In the micronized layer, the average thickness of the fine layer is 0.1 μm to 5.0 μm, and the average grain size of the ferrite phase in the fine layer is 0.1 μm to 3.0 μm, and the fine layer contains Si and Mn 1 The oxide or the two or more kinds of oxides have a maximum diameter of 0.01 μm to 0.4 μm, and the difference between the maximum thickness and the minimum thickness of the fine layer in the width direction of the base material steel sheet is within 2.0 μm. 如請求項1之熔融鍍鋅鋼板,其中前述熔融鍍鋅層之每單面鍍敷附著量為10g/m2以上且100g/m2以下。 The hot-dip galvanized steel sheet according to claim 1, wherein the single-sided plating adhesion amount of the hot-dip galvanized layer is 10 g/m 2 or more and 100 g/m 2 or less. 如請求項1或2之熔融鍍鋅鋼板,其中前述母材鋼板以質量%計含有選自於由Ti:0.001%~0.150%、Nb:0.001%~0.100%、及V:0.001%~0.300%所構成群組中之1種或2種以上。 The hot-dip galvanized steel sheet according to claim 1 or 2, wherein the base material steel sheet is selected from the group consisting of Ti: 0.001% to 0.150%, Nb: 0.001% to 0.100%, and V: 0.001% to 0.300% by mass%. One or two or more of the groups formed. 如請求項1或2之熔融鍍鋅鋼板,其中前述母材鋼板以質量%計含有選自於由Cr:0.01%~2.00%、Ni:0.01%~2.00%、Cu:0.01%~2.00%、Mo:0.01%~2.00%、B:0.0001%~0.0100%、及W:0.01%~2.00%所構成群組中之1種或2種以上。 The hot-dip galvanized steel sheet according to claim 1 or 2, wherein the base material steel sheet contains, by mass%, selected from the group consisting of Cr: 0.01% to 2.00%, Ni: 0.01% to 2.00%, Cu: 0.01% to 2.00%, Mo: one or more of the group consisting of 0.01% to 2.00%, B: 0.0001% to 0.0100%, and W: 0.01% to 2.00%. 如請求項3之熔融鍍鋅鋼板,其中前述母材鋼板以質量%計含有選自於由Cr:0.01%~2.00%、Ni:0.01%~2.00%、Cu:0.01%~2.00%、Mo:0.01%~2.00%、B:0.0001%~0.0100%、及W:0.01%~2.00%所構成群組中之1種或2種以上。 The hot-dip galvanized steel sheet according to claim 3, wherein the base material steel sheet is selected from the group consisting of Cr: 0.01% to 2.00%, Ni: 0.01% to 2.00%, Cu: 0.01% to 2.00%, and Mo: 0.01% to 2.00%, B: 0.0001% to 0.0100%, and W: 0.01% to 2.00% of one or more of the groups. 如請求項1或2之熔融鍍鋅鋼板,其中前述 母材鋼板以質量%計含有合計0.0001%~0.0100%之選自於由Ca、Ce、Mg、Zr、La及REM所構成群組中之1種或2種以上。 A molten galvanized steel sheet according to claim 1 or 2, wherein the aforementioned The base material steel plate is contained in a total of 0.0001% to 0.0100% by mass, and one or more selected from the group consisting of Ca, Ce, Mg, Zr, La, and REM. 如請求項3之熔融鍍鋅鋼板,其中前述母材鋼板以質量%計含有合計0.0001%~0.0100%之選自於由Ca、Ce、Mg、Zr、La及REM所構成群組中之1種或2種以上。 The hot-dip galvanized steel sheet according to claim 3, wherein the base material steel sheet contains 0.0001% to 0.0100% by mass in total of one selected from the group consisting of Ca, Ce, Mg, Zr, La, and REM. Or two or more. 如請求項4之熔融鍍鋅鋼板,其中前述母材鋼板以質量%計含有合計0.0001%~0.0100%之選自於由Ca、Ce、Mg、Zr、La及REM所構成群組中之1種或2種以上。 The hot-dip galvanized steel sheet according to claim 4, wherein the base material steel sheet contains 0.0001% to 0.0100% by mass in total of one selected from the group consisting of Ca, Ce, Mg, Zr, La, and REM. Or two or more. 如請求項5之熔融鍍鋅鋼板,其中前述母材鋼板以質量%計含有合計0.0001%~0.0100%之選自於由Ca、Ce、Mg、Zr、La及REM所構成群組之中1種或2種以上。The hot-dip galvanized steel sheet according to claim 5, wherein the base material steel sheet contains 0.0001% to 0.0100% by mass in total of one selected from the group consisting of Ca, Ce, Mg, Zr, La, and REM. Or two or more.
TW106125688A 2017-07-31 2017-07-31 Hot-dip galvanized steel sheet TWI646218B (en)