KR101947240B1 - Coating composition - Google Patents

Coating composition Download PDF

Info

Publication number
KR101947240B1
KR101947240B1 KR1020160154666A KR20160154666A KR101947240B1 KR 101947240 B1 KR101947240 B1 KR 101947240B1 KR 1020160154666 A KR1020160154666 A KR 1020160154666A KR 20160154666 A KR20160154666 A KR 20160154666A KR 101947240 B1 KR101947240 B1 KR 101947240B1
Authority
KR
South Korea
Prior art keywords
weight
parts
acrylic polyol
polyol resin
coating composition
Prior art date
Application number
KR1020160154666A
Other languages
Korean (ko)
Other versions
KR20180056839A (en
Inventor
강필수
김준엽
박영희
Original Assignee
주식회사 케이씨씨
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 주식회사 케이씨씨 filed Critical 주식회사 케이씨씨
Priority to KR1020160154666A priority Critical patent/KR101947240B1/en
Publication of KR20180056839A publication Critical patent/KR20180056839A/en
Application granted granted Critical
Publication of KR101947240B1 publication Critical patent/KR101947240B1/en

Abstract

본 발명은 플라스틱 소재 상에 적용되는 도료 조성물에 관한 것이다.The present invention relates to a coating composition applied on a plastic material.

Description

도료 조성물{COATING COMPOSITION}[0001] COATING COMPOSITION [0002]

본 발명은 플라스틱 기재에 도포되는 도료 조성물에 관한 것이다.The present invention relates to a coating composition applied to a plastic substrate.

플라스틱 소재로 성형된 성형품에 심미감을 부여하는 방법 중 하나로 크롬(Cr)을 도금하는 방법을 들 수 있다. 이때, 크롬으로는 유해물질의 유발이 적고 어두운(dark) 거울상을 구현할 수 있는 3가의 크롬이 사용되고 있다.As a method of imparting a sense of beauty to a molded article formed of a plastic material, there is a method of plating chromium (Cr). At this time, trivalent chromium, which can generate a dark mirror image with less occurrence of harmful substances, is used as chromium.

그런데 크롬 도금층은 시간이 경과할수록 산화되어 그 기능이 저하되는 문제점이 있다. 이에 따라 크롬 도금층 상에 도료를 도포하여 그 기능을 유지시킬 수 있는데, 이때, 사용되는 도료는 크롬 도금층과 충분한 부착성을 가져야 하며 내습성, 내열성, 고휘도성 등의 물성을 요구되는 수준으로 얻을 수 있어야 한다.However, there is a problem that the chromium plating layer is oxidized and deteriorated in function over time. Accordingly, it is possible to apply the paint on the chromium plating layer to maintain its function. At this time, the paint used must have sufficient adhesion with the chromium plating layer, and the properties such as moisture resistance, heat resistance and high brightness can be obtained at a required level .

그러나 종래에는 크롬 도금층 상에 도료를 1-2회 도장할 경우 상기 물성을 만족할 만한 수준으로 얻을 수 없어 3회 이상 도장을 실시해야 하는 번거로움이 있었으며, 크롬 도금층과의 충분한 부착성을 얻는데도 한계가 있었다.However, conventionally, when the paint is applied 1-2 times on the chromium plated layer, the physical properties can not be obtained satisfactorily, so that the coating has to be carried out three times or more, and it is difficult to obtain sufficient adhesion with the chromium plating layer .

대한민국 공개특허공보 제1995-0018326호Korean Patent Publication No. 1995-0018326

본 발명은 부착성, 내습성, 내열성 등이 우수하고 휘도가 높은 도료 조성물을 제공하고자 한다.The present invention aims to provide a coating composition excellent in adhesion, moisture resistance, heat resistance and the like and having high brightness.

본 발명은, 제1 아크릴 폴리올 수지 5 내지 10 중량부, 제2 아크릴 폴리올 수지 25 내지 35 중량부, 금속계 안료 7 내지 9 중량부, 및 제1 용제 50 내지 60 중량부를 포함하는 주제부; 및 폴리이소시아네이트 30 내지 40 중량부, 및 제2 용제 60 내지 70 중량부를 포함하는 경화제부를 포함하는 도료 조성물을 제공한다.The present invention relates to a paint comprising: a main part comprising 5 to 10 parts by weight of a first acrylic polyol resin, 25 to 35 parts by weight of a second acrylic polyol resin, 7 to 9 parts by weight of a metallic pigment, and 50 to 60 parts by weight of a first solvent; And 30 to 40 parts by weight of a polyisocyanate and 60 to 70 parts by weight of a second solvent.

상기 제1 아크릴 폴리올 수지는 중량평균분자량(Mw)이 10,000 내지 23,000일 수 있다.The first acrylic polyol resin may have a weight average molecular weight (Mw) of 10,000 to 23,000.

상기 제1 아크릴 폴리올 수지는 수산기가(OH value)가 35 내지 60 mgKOH/g 일 수 있다.The first acrylic polyol resin may have an OH value of 35 to 60 mgKOH / g.

상기 제1 아크릴 폴리올 수지는 유리전이온도가 25 내지 50 ℃일 수 있다.The first acrylic polyol resin may have a glass transition temperature of 25 to 50 캜.

상기 주제부와 상기 경화제부의 혼합 비율이 100:13 내지 100:33의 중량비일 수 있다.The mixing ratio of the main portion and the curing agent portion may be a weight ratio of 100: 13 to 100: 33.

상기 주제부가 왁스, 침강방지제, 자외선 안정제, 소포제, 및 커플링제로 이루어진 군에서 선택된 1종 이상의 첨가제 0.8 내지 4 중량부를 더 포함할 수 있다.The subject matter may further include 0.8 to 4 parts by weight of at least one additive selected from the group consisting of waxes, anti-settling agents, ultraviolet stabilizers, defoaming agents, and coupling agents.

본 발명의 도료 조성물은 부착성, 내습성, 내열성 등의 물성이 우수하고 고휘도를 나타낼 수 있어, 이를 플라스틱 소재(특히, 크롬이 도장된 플라스틱 소재)에 도장할 경우 1-2회의 도장만으로도 물성이 우수한 도장면을 형성할 수 있다.The coating composition of the present invention is excellent in physical properties such as adhesiveness, moisture resistance and heat resistance and can exhibit high brightness, and when it is applied to a plastic material (in particular, a chromium-plated plastic material) An excellent coated surface can be formed.

이하, 본 발명을 설명한다.Hereinafter, the present invention will be described.

본 발명의 도료 조성물은 특정의 아크릴 폴리올 수지가 적용된 주제부를 포함하고, 각 성분의 함량을 최적화함에 따라 부착성, 내습성, 내열성이 우수하고 고휘도를 갖는 도막을 플라스틱 소재(구체적으로, 크롬이 도금된 플라스틱 소재) 상에 형성할 수 있는데, 이에 대해 구체적으로 설명하면 다음과 같다.The coating composition of the present invention contains a subject portion to which a specific acrylic polyol resin is applied and optimizes the content of each component so that the coating film having excellent adhesiveness, moisture resistance, heat resistance and high brightness is coated on a plastic material A plastic material), which will be described in detail as follows.

본 발명의 도료 조성물은 주제부와 경화제부를 포함한다.The coating composition of the present invention comprises a main portion and a curing agent portion.

상기 주제부는 주제부 100 중량부를 기준으로, 제1 아크릴 폴리올 수지 5 내지 10 중량부; 제2 아크릴 폴리올 수지 25 내지 35 중량부; 금속계 안료 7 내지 9 중량부; 및 제1 용제 50 내지 60 중량부를 포함한다.Wherein the main portion comprises, based on 100 parts by weight of the main portion, 5 to 10 parts by weight of the first acrylic polyol resin; 25 to 35 parts by weight of a second acrylic polyol resin; 7 to 9 parts by weight of a metallic pigment; And 50 to 60 parts by weight of the first solvent.

상기 제1 아크릴 폴리올 수지는 도막의 부착성, 내습성 등을 높이는 역할을 한다. 이러한 제1 아크릴 폴리올 수지는 유기산기를 갖는 단량체, 수산기를 갖는 단량체, 방향족계 비관능성 단량체, 지방족계 비관능성 단량체 등의 비닐형 이중결합을 갖는 단량체들과 열분해 개시제의 라디칼 용액 중합에 의해 얻어진 것일 수 있다.The first acrylic polyol resin serves to improve the adhesion of the coating film, moisture resistance, and the like. Such a first acrylic polyol resin may be obtained by radical solution polymerization of a monomer having a vinyl type double bond such as a monomer having an organic acid group, a monomer having a hydroxyl group, an aromatic non-functional monomer, an aliphatic non-functional monomer, etc. and a thermal decomposition initiator have.

상기 유기산기를 갖는 단량체로는 아크릴산, 메타크릴산, 말레인산, 또는 이의 무수물 등을 들 수 있으며, 이들은 단독 또는 혼합되어 사용될 수 있다. 상기 수산기를 갖는 단량체로는 2-하이드록시에틸아크릴레이트, 2-하이드록시에틸메타크릴레이트, 2-하이드록시부틸아크릴레이트, 하이드록시프로필메타크릴레이트, 카프로락톤아크릴레이트 등을 들 수 있으며, 이들은 단독 또는 혼합되어 사용될 수 있다.Examples of the monomer having an organic acid group include acrylic acid, methacrylic acid, maleic acid, and an anhydride thereof, which may be used alone or in combination. Examples of the monomer having a hydroxyl group include 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxybutyl acrylate, hydroxypropyl methacrylate and caprolactone acrylate, May be used alone or in combination.

상기 방향족계 비관능성 단량체로는 스티렌, 비닐톨루엔 등을 들 수 있으며, 이들은 단독 또는 혼합되어 사용될 수 있다.Examples of the aromatic non-functional monomer include styrene and vinyl toluene, which may be used alone or in combination.

상기 지방족계 비관능성 단량체로는 메틸메타크릴레이트, 에틸아크릴레이트, 에틸메타크릴레이트, 이소부틸아크릴레이트, 노르말부틸메타크릴레이트, 노르말부틸아크릴레이트, 이소프로필메타크릴레이트 등을 들 수 있고, 이들은 단독 또는 혼합되어 사용될 수 있다.Examples of the aliphatic non-functional monomer include methyl methacrylate, ethyl acrylate, ethyl methacrylate, isobutyl acrylate, n-butyl methacrylate, n-butyl acrylate and isopropyl methacrylate, May be used alone or in combination.

상기 라디칼 용액 중합에 사용되는 반응개시제로는 벤조일퍼옥사이드, 아조이소부티로니트릴, t-부틸퍼옥시-2-에틸헥사노에이트 등을 들 수 있으며, 이들은 단독 또는 혼합되어 사용될 수 있다.Examples of the reaction initiator used in the radical solution polymerization include benzoyl peroxide, azoisobutyronitrile, and t-butyl peroxy-2-ethylhexanoate, which may be used alone or in combination.

이와 같은 제1 아크릴 폴리올 수지는 중량평균분자량(Mw)이 10,000 내지 23,000일 수 있고, 수산기가(OH value)가 35 내지 60 mgKOH/g일 수 있고, 유리전이온도가 25 내지 50 ℃일 수 있다. 또한, 제1 아크릴 폴리올 수지의 고형분의 비율은 중량기준으로 50 내지 65 %일 수 있다.The first acrylic polyol resin may have a weight average molecular weight (Mw) of 10,000 to 23,000, an OH value of 35 to 60 mgKOH / g, and a glass transition temperature of 25 to 50 ° C . Further, the ratio of the solid content of the first acrylic polyol resin may be 50 to 65% by weight.

이와 같은 제1 아크릴 폴리올 수지의 함량은 주제부 100 중량부를 기준으로 5 내지 10 중량부이며, 이로 인해 도료 조성물의 부착성 등을 향상시킬 수 있다.The content of the first acrylic polyol resin is 5 to 10 parts by weight based on 100 parts by weight of the main portion, thereby improving the adhesion of the coating composition.

상기 제2 아크릴 폴리올 수지는 도막의 부착성, 내열성 등을 높이는 역할을 한다. 이러한 제2 아크릴 폴리올 수지는 중량평균분자량(Mw)이 10,000 내지 25,000일 수 있고, 수산기가(OH value)가 50 내지 80 mgKOH/g일 수 있고, 유리전이온도가 30 내지 45 ℃일 수 있다. 또한, 제2 아크릴 폴리올 수지의 고형분의 비율은 중량기준으로 50 내지 65 %일 수 있다.The second acrylic polyol resin plays a role of enhancing adhesion, heat resistance, etc. of the coating film. The second acrylic polyol resin may have a weight average molecular weight (Mw) of 10,000 to 25,000, an OH value of 50 to 80 mgKOH / g, and a glass transition temperature of 30 to 45 ° C. In addition, the ratio of the solid content of the second acrylic polyol resin may be 50 to 65% by weight.

이와 같은 제2 아크릴 폴리올 수지의 함량은 주제부 100 중량부를 기준으로 25 내지 35 중량부이며, 이로 인해 도료 조성물의 부착성, 내열성 등을 향상시킬 수 있다.The content of the second acrylic polyol resin is 25 to 35 parts by weight based on 100 parts by weight of the main portion, thereby improving the adhesion property and heat resistance of the coating composition.

상기 금속계 안료는 금속 재질의 느낌을 갖는 도막을 형성하면서 도막의 휘도를 높이는 역할을 한다. 이러한 금속계 안료로는 알루미늄 페이스트 등을 들 수 있다. 여기서, 알루미늄 페이스트는 분산성 등을 고려할 때, 알루미늄 입자의 크기가 9 내지 12.5 ㎛인 제1 알루미늄 페이스트와, 알루미늄 입자의 크기가 13 내지 20 ㎛인 제2 알루미늄 페이스트를 혼합하여 사용할 수 있다. 이때, 상기 제1 알루미늄 페이스트의 함량은 주제부 100 중량부를 기준으로 2 내지 3 중량부일 수 있고, 상기 제2 알루미늄 페이스트의 함량은 주제부 100 중량부를 기준으로 5 내지 6 중량부일 수 있다.The metallic pigment plays a role of enhancing the brightness of a coating film while forming a coating film having a metal-like feel. Examples of such metal-based pigments include aluminum paste and the like. Considering the dispersibility, the aluminum paste may be prepared by mixing a first aluminum paste having an aluminum particle size of 9 to 12.5 占 퐉 and a second aluminum paste having an aluminum particle size of 13 to 20 占 퐉. At this time, the content of the first aluminum paste may be 2 to 3 parts by weight based on 100 parts by weight of the main part, and the content of the second aluminum paste may be 5 to 6 parts by weight based on 100 parts by weight of the main part.

이와 같은 금속계 안료의 함량은 주제부 100 중량부를 기준으로 7 내지 9 중량부이며, 이로 인해 도료 조성물이 도장되었을 때 메탈릭한 질감을 나타내며, 도장된 표면의 심미감, 휘도 등을 향상시킬 수 있다.The content of the metal-based pigment is 7 to 9 parts by weight based on 100 parts by weight of the main portion, and when the coating composition is painted, it shows a metallic texture and can improve the aesthetics, brightness and the like of the painted surface.

상기 제1 용제는 주제부의 점도를 조절하는 역할을 한다. 이러한 제1 용제로는 메틸아세테이트, 에틸아세테이트, 부틸아세테이트, 프로필렌글리콜 모노메틸아세테이트, 또는 3-메톡시 부틸아세테이트와 같은 아세테이트류 용제; 디아세톤 알코올, 메틸에틸케톤, 시클로헥사논, 또는 이소포론과 같은 케톤류 용제; 글라이콜 에테르류 용제; 글라이콜 에테르 에스테르류 용제; 톨루엔, 자일렌 등과 같은 방향족 탄화수소계 용제; 또는 이들의 혼합물 등을 들 수 있다.The first solvent serves to adjust the viscosity of the main portion. Such a first solvent may be an acetate solvent such as methyl acetate, ethyl acetate, butyl acetate, propylene glycol monomethyl acetate, or 3-methoxybutyl acetate; Ketone solvents such as diacetone alcohol, methyl ethyl ketone, cyclohexanone, or isophorone; Glycol ether solvents; Glycol ether esters solvents; Aromatic hydrocarbon solvents such as toluene, xylene and the like; Or a mixture thereof and the like.

이와 같은 제1 용제의 함량은 주제부 100 중량부를 기준으로, 50 내지 60 중량부이며, 이로 인해 도료 조성물의 건조성, 작업성 등을 향상시킬 수 있다.The content of the first solvent is 50 to 60 parts by weight based on 100 parts by weight of the main portion, thereby improving the dryness and workability of the coating composition.

이러한 주제부에는 조성물의 물성을 높이기 위해 왁스, 침강방지제, 자외선 안정제, 소포제, 및 커플링제로 이루어진 군에서 선택된 1종 이상의 첨가제 0.8 내지 4 중량부를 더 포함할 수 있다.The subject part may further include 0.8 to 4 parts by weight of at least one additive selected from the group consisting of waxes, anti-settling agents, ultraviolet stabilizers, defoamers, and coupling agents to improve the physical properties of the composition.

상기 경화제부는 경화제부 100 중량부를 기준으로, 폴리이소시아네이트 30 내지 40 중량부; 및 제2 용제 60 내지 70 중량부를 포함한다.The curing agent part may contain, based on 100 parts by weight of the curing agent part, 30 to 40 parts by weight of a polyisocyanate; And 60 to 70 parts by weight of the second solvent.

상기 폴리이소시아네이트는 상기 제1 아크릴 폴리올 수지, 상기 제2 아크릴 폴리올 수지와 반응하여 우레탄 결합을 한다. 이러한 폴리이소시아네이트로는 헥사메틸렌 디이소시아네이트(HDI), 트리메틸-HDI(TMDI), 2-메틸펜탄-1,5-디이소시아네이트(MPDI), 이소포론 디이소시아네이트(IPDI), 1,4-비스(이소시아나토메틸)시클로헥산(H6XDI), 비스(이소시아나토메틸)노르보르난(NBDI), 3(4)-이소시아나토메틸-1-메틸-시클로헥실 이소시아네이트(IMCI), 4,4'-비스(이소시아나토시클로헥실)메탄(H12MDI), 또는 이들의 혼합물 등을 들 수 있다.The polyisocyanate reacts with the first acrylic polyol resin and the second acrylic polyol resin to form a urethane bond. Examples of such polyisocyanates include hexamethylene diisocyanate (HDI), trimethyl-HDI (TMDI), 2-methylpentane-1,5-diisocyanate (MPDI), isophorone diisocyanate (IPDI), 1,4- (Isocyanatomethyl) norbornane (NBDI), 3 (4) -isocyanatomethyl-1-methylcyclohexyl isocyanate (IMCI), 4,4'- Bis (isocyanatocyclohexyl) methane (H12MDI), or a mixture thereof.

이와 같은 폴리이소시아네이트의 함량은 경화제부 100 중량부를 기준으로 30 내지 40 중량부이며, 이로 인해 도료 조성물의 경화반응성을 향상시킬 수 있다.The content of the polyisocyanate is 30 to 40 parts by weight based on 100 parts by weight of the curing agent, thereby improving the curing reactivity of the coating composition.

상기 제2 용제는 경화제부의 점도를 조절하는 역할을 한다. 이러한 제2 용제로는 메틸아세테이트, 에틸아세테이트, 부틸아세테이트, 프로필렌글리콜 모노메틸아세테이트, 또는 3-메톡시 부틸아세테이트와 같은 아세테이트류 용제; 디아세톤 알코올, 메틸에틸케톤, 시클로헥사논, 또는 이소포론과 같은 케톤류 용제; 글라이콜 에테르류 용제; 글라이콜 에테르 에스테르류 용제; 톨루엔, 자일렌 등과 같은 방향족 탄화수소계 용제; 또는 이들의 혼합물 등을 들 수 있다.The second solvent serves to control the viscosity of the curing agent. Such a second solvent may be an acetate solvent such as methyl acetate, ethyl acetate, butyl acetate, propylene glycol monomethyl acetate, or 3-methoxybutyl acetate; Ketone solvents such as diacetone alcohol, methyl ethyl ketone, cyclohexanone, or isophorone; Glycol ether solvents; Glycol ether esters solvents; Aromatic hydrocarbon solvents such as toluene, xylene and the like; Or a mixture thereof and the like.

이와 같은 제2 용제의 함량은 경화제부 100 중량부를 기준으로, 60 내지 70 중량부이며, 이로 인해 도료 조성물의 건조성, 작업성 등을 향상시킬 수 있다.The content of the second solvent is 60 to 70 parts by weight based on 100 parts by weight of the curing agent, thereby improving the drying properties and workability of the coating composition.

본 발명의 메탈릭 도료 조성물은 상기 주제부와 상기 경화제부가 100:13 내지 100:33의 중량비로 혼합된 것일 수 있다. 주제부와 경화제부의 혼합비율이 상기 범위를 벗어날 경우, 도막의 부착성이 저하되거나 조성물의 경화 반응성이 저하될 수 있다.In the metallic coating composition of the present invention, the main portion and the curing agent may be mixed in a weight ratio of 100: 13 to 100: 33. If the mixing ratio of the main portion and the curing agent portion is out of the above range, the adhesion of the coating film may be lowered or the curing reactivity of the composition may be lowered.

상술한 본 발명의 도료 조성물은 부착성, 내습성, 내열성 등이 우수하고 고휘도를 나타낼 수 있기 때문에 이러한 물성이 요구되는 분야(예를 들어, TV와 같은 영상기기에서 크롬이 도금된 스탠드(stand)상에 도장)에 다양하게 적용될 수 있다. 또한, 본 발명의 도료 조성물은 부착성이 우수하기 때문에 1-2회의 도장 공정만으로도 소재와의 부착성이 우수한 도막을 형성할 수 있어, 도장 공정 효율을 높일 수 있다.The coating composition of the present invention is excellent in adhesion, moisture resistance, heat resistance, and can exhibit high brightness. Therefore, it is desirable to provide a chromium-plated stand in a field where such properties are required (for example, ), And the like. In addition, since the coating composition of the present invention is excellent in adhesion, it is possible to form a coating film excellent in adhesion to a workpiece only by one to two coating processes, and to improve the efficiency of the coating process.

이하 본 발명을 실시예를 통하여 상세히 설명하면 다음과 같다. 단, 하기 실시예는 본 발명을 예시하는 것일 뿐, 본 발명이 하기 실시예에 의해 한정되는 것은 아니다.Hereinafter, the present invention will be described in detail with reference to examples. However, the following examples are illustrative of the present invention, and the present invention is not limited by the following examples.

[[ 실시예Example 1 내지 6] 1 to 6]

1) One) 주제부Topic section 제조 Produce

하기 표 1의 조성을 갖는 주제부를 제조하였다.A subject portion having the composition shown in the following Table 1 was prepared.

2) 2) 경화제부Hardener part 제조 Produce

하기 표 2의 조성을 갖는 경화제부를 제조하였다.A curing agent part having the composition shown in the following Table 2 was prepared.

3) 도료 조성물 제조3) Preparation of Coating Composition

상기 주제부와 상기 경화제부를 100:13의 중량비로 혼합하여 도료 조성물을 제조하였다.The topical portion and the curing agent portion were mixed in a weight ratio of 100: 13 to prepare a coating composition.

항목Item 실시예 1Example 1 실시예2Example 2 실시예3Example 3 실시예4Example 4 실시예 5Example 5 실시예 6Example 6 제1 아크릴
폴리올 수지
The first acrylic
Polyol resin
수지1
(고형분: 60 중량%,
OH value: 45,
Tg: 32 ℃
Mw: 11,258)
Resin 1
(Solid content: 60% by weight,
OH value: 45,
Tg: 32 ° C
Mw: 11,258)
7.57.5 7.57.5 7.57.5 7.57.5 55 1010
수지2
(고형분: 60 중량%,
OH value: 66,
Tg: 20 ℃
Mw: 25,000)
Resin 2
(Solid content: 60% by weight,
OH value: 66,
Tg: 20 DEG C
Mw: 25,000)
-- -- -- -- -- --
제2 아크릴 폴리올 수지The second acrylic polyol resin 고형분: 60 중량%,
OH value: 66,
Tg: 37 ℃,
Mw: 12,360
Solid content: 60% by weight,
OH value: 66,
Tg: 37 DEG C,
Mw: 12,360
27.527.5 12.512.5 17.517.5 22.522.5 3030 2525
금속계 안료Metal-based pigment 알루미늄 페이스트
(Aliminum Paste)
Aluminum paste
(Aliminum Paste)
7.57.5 7.57.5 7.57.5 7.57.5 7.57.5 7.57.5
첨가제additive 디부틸주석 디라우레이트
(DIBUTYLTIN DILAURATE)
Dibutyltin dilaurate
(DIBUTYLTIN DILAURATE)
0.150.15 0.150.15 0.150.15 0.150.15 0.150.15 0.150.15
글리콜 디메르캅토프로피오네이트
(GLYCOL DIMERCAPTOPROPIONATE)
Glycol dimercaptopropionate
(GLYCOL DIMERCAPTOPROPIONATE)
0.150.15 0.150.15 0.150.15 0.150.15 0.150.15 0.150.15
합성왁스(침강 방지)Synthetic wax (anti-settling) 1One 1One 1One 1One 1One 1One 제1 용제The first solvent 부틸아세테이트(BA)Butyl acetate (BA) 16.216.2 31.231.2 26.226.2 21.221.2 16.216.2 16.216.2 자일렌(Xylene)Xylene 3030 3030 3030 3030 3030 3030 톨루엔(Toluene)Toluene 1010 1010 1010 1010 1010 1010 합계Sum 100100 100100 100100 100100 100100 100100

항목Item 실시예 1Example 1 실시예2Example 2 실시예3Example 3 실시예4Example 4 실시예5Example 5 실시예6Example 6 폴리이소
시아네이트
Polyiso
Cyanate
HDI/ HEXAMETHYLENE DIISOCYNATEHDI / HEXAMETHYLENE DIISOCYNATE 3737 3030 2525 2020 3737 3737
제2 용제The second solvent 자일렌(Xylene)Xylene 3333 4040 4545 5050 3333 3333 프로필렌 글리콜 모노 메틸 에테르 아세트산(PMA)Propylene glycol monomethyl ether acetic acid (PMA) 3030 3030 3030 3030 3030 3030 합계Sum 100100 100100 100100 100100 100100 100100

[[ 실시예Example 7 내지 9] 7 to 9]

1) One) 주제부Topic section 제조 Produce

하기 표 3의 조성을 갖는 주제부를 제조하였다.A subject portion having the composition shown in Table 3 below was prepared.

2) 2) 경화제부Hardener part 제조 Produce

하기 표 4의 조성을 갖는 경화제부를 제조하였다.A curing agent part having the composition shown in the following Table 4 was prepared.

3) 도료 조성물 제조3) Preparation of Coating Composition

상기 주제부와 상기 경화제부를 100:23의 중량비로 혼합하여 도료 조성물을 제조하였다.The main portion and the curing agent were mixed in a weight ratio of 100: 23 to prepare a coating composition.

항목Item 실시예 7Example 7 실시예 8Example 8 실시예 9Example 9 제1 아크릴
폴리올 수지
The first acrylic
Polyol resin
수지1
(고형분: 60 중량%,
OH value: 45,
Tg: 32 ℃
Mw: 11,258)
Resin 1
(Solid content: 60% by weight,
OH value: 45,
Tg: 32 ° C
Mw: 11,258)
7.57.5 55 1010
수지2
(고형분: 60 중량%,
OH value: 66,
Tg: 20 ℃
Mw: 25,000)
Resin 2
(Solid content: 60% by weight,
OH value: 66,
Tg: 20 DEG C
Mw: 25,000)
-- -- --
제2 아크릴 폴리올 수지The second acrylic polyol resin 고형분: 60 중량%,
OH value: 66,
Tg: 37 ℃,
Mw: 12,360
Solid content: 60% by weight,
OH value: 66,
Tg: 37 DEG C,
Mw: 12,360
27.527.5 3030 2525
금속계 안료Metal-based pigment 알루미늄 페이스트
(Aliminum Paste)
Aluminum paste
(Aliminum Paste)
7.57.5 7.57.5 7.57.5
첨가제additive 디부틸주석 디라우레이트
(DIBUTYLTIN DILAURATE)
Dibutyltin dilaurate
(DIBUTYLTIN DILAURATE)
0.150.15 0.150.15 0.150.15
글리콜 디메르캅토프로피오네이트
(GLYCOL DIMERCAPTOPROPIONATE)
Glycol dimercaptopropionate
(GLYCOL DIMERCAPTOPROPIONATE)
0.150.15 0.150.15 0.150.15
합성왁스(침강 방지)Synthetic wax (anti-settling) 1One 1One 1One 제1 용제The first solvent 부틸아세테이트(BA)Butyl acetate (BA) 16.216.2 16.216.2 16.216.2 자일렌(Xylene)Xylene 3030 3030 3030 톨루엔(Toluene)Toluene 1010 1010 1010 합계Sum 100100 100100 100100

항목Item 실시예 7Example 7 실시예 8Example 8 실시예 9Example 9 폴리이소
시아네이트
Polyiso
Cyanate
HDI/ HEXAMETHYLENE DIISOCYNATEHDI / HEXAMETHYLENE DIISOCYNATE 3737 3737 3737
제2 용제The second solvent 자일렌(Xylene)Xylene 3333 3333 3333 프로필렌 글리콜 모노 메틸 에테르 아세트산(PMA)Propylene glycol monomethyl ether acetic acid (PMA) 3030 3030 3030 합계Sum 100100 100100 100100

[[ 실시예Example 10] 10]

주제부와 경화제부를 100:33의 중량비로 혼합하여 도료 조성물을 제조한 것을 제외하고는, 실시예 7과 동일한 조성을 적용하였다.The same composition as in Example 7 was applied, except that the topical portion and the curing agent portion were mixed at a weight ratio of 100: 33 to prepare a coating composition.

[[ 실시예Example 11] 11]

주제부와 경화제부를 100:33의 중량비로 혼합하여 도료 조성물을 제조한 것을 제외하고는, 실시예 8과 동일한 조성을 적용하였다.The same composition as in Example 8 was applied, except that a paint composition was prepared by mixing the main part and the hardener in a weight ratio of 100: 33.

[[ 실시예Example 12] 12]

주제부와 경화제부를 100:33의 중량비로 혼합하여 도료 조성물을 제조한 것을 제외하고는, 실시예 9와 동일한 조성을 적용하였다.The same composition as in Example 9 was applied, except that a paint composition was prepared by mixing the main part and the hardener in a weight ratio of 100: 33.

[[ 비교예Comparative Example 1 내지 5] 1 to 5]

1) One) 주제부Topic section 제조 Produce

하기 표 5의 조성을 갖는 주제부를 제조하였다.A subject portion having the composition shown in Table 5 below was prepared.

2) 2) 경화제부Hardener part 제조 Produce

하기 표 6의 조성을 갖는 경화제부를 제조하였다.A curing agent part having the composition shown in the following Table 6 was prepared.

3) 도료 조성물 제조3) Preparation of Coating Composition

상기 주제부와 상기 경화제부를 100:13의 중량비로 혼합하여 도료 조성물을 제조하였다.The topical portion and the curing agent portion were mixed in a weight ratio of 100: 13 to prepare a coating composition.

항목Item 비교예 1Comparative Example 1 비교예 2Comparative Example 2 비교예 3Comparative Example 3 비교예 4Comparative Example 4 비교예 5Comparative Example 5 제1 아크릴
폴리올 수지
The first acrylic
Polyol resin
수지1
(고형분: 60 중량%,
OH value: 45,
Tg: 32 ℃
Mw: 11,258)
Resin 1
(Solid content: 60% by weight,
OH value: 45,
Tg: 32 ° C
Mw: 11,258)
7.57.5 7.57.5 -- 22 1515
수지2
(고형분: 60 중량%,
OH value: 66,
Tg: 20 ℃
Mw: 25,000)
Resin 2
(Solid content: 60% by weight,
OH value: 66,
Tg: 20 DEG C
Mw: 25,000)
7.57.5 -- 7.57.5 -- --
제2 아크릴 폴리올 수지The second acrylic polyol resin 고형분: 60 중량%,
OH value: 66,
Tg: 37 ℃,
Mw: 12,360
Solid content: 60% by weight,
OH value: 66,
Tg: 37 DEG C,
Mw: 12,360
-- 7.57.5 7.57.5 3535 2222
금속계 안료Metal-based pigment 알루미늄 페이스트
(Aliminum Paste)
Aluminum paste
(Aliminum Paste)
7.57.5 7.57.5 7.57.5 7.57.5 7.57.5
첨가제additive 디부틸주석 디라우레이트
(DIBUTYLTIN DILAURATE)
Dibutyltin dilaurate
(DIBUTYLTIN DILAURATE)
0.150.15 0.150.15 0.150.15 0.150.15 0.150.15
글리콜 디메르캅토프로피오네이트
(GLYCOL DIMERCAPTOPROPIONATE)
Glycol dimercaptopropionate
(GLYCOL DIMERCAPTOPROPIONATE)
0.150.15 0.150.15 0.150.15 0.150.15 0.150.15
합성왁스(침강 방지)Synthetic wax (anti-settling) 1One 1One 1One 1One 1One 제1
용제
1st
solvent
부틸아세테이트(BA)Butyl acetate (BA) 36.236.2 36.236.2 36.236.2 14.214.2 14.214.2
자일렌(Xylene)Xylene 3030 3030 3030 3030 3030 톨루엔(Toluene)Toluene 1010 1010 1010 1010 1010 합계Sum 100100 100100 100100 100100 100100

항목Item 비교예 1Comparative Example 1 비교예 2Comparative Example 2 비교예 3Comparative Example 3 비교예 4Comparative Example 4 비교예 5Comparative Example 5 폴리이소
시아네이트
Polyiso
Cyanate
HDI/ HEXAMETHYLENE DIISOCYNATEHDI / HEXAMETHYLENE DIISOCYNATE 3030 2525 2020 3737 3737
제2 용제The second solvent 자일렌(Xylene)Xylene 4040 4545 5050 3333 3333 프로필렌 글리콜 모노 메틸 에테르 아세트산(PMA)Propylene glycol monomethyl ether acetic acid (PMA) 3030 3030 3030 3030 3030 합계Sum 100100 100100 100100 100100 100100

[[ 비교예Comparative Example 6] 6]

주제부와 경화제부를 100:23의 중량비로 혼합하여 도료 조성물을 제조한 것을 제외하고는, 비교예 4와 동일한 조성을 적용하였다.The same composition as in Comparative Example 4 was applied, except that the topical portion and the curing agent portion were mixed in a weight ratio of 100: 23 to prepare a coating composition.

[[ 비교예Comparative Example 7] 7]

주제부와 경화제부를 100:23의 중량비로 혼합하여 도료 조성물을 제조한 것을 제외하고는, 비교예 5와 동일한 조성을 적용하였다.The same composition as in Comparative Example 5 was applied, except that the topical portion and the hardener portion were mixed in a weight ratio of 100: 23 to prepare a coating composition.

[[ 비교예Comparative Example 8] 8]

주제부와 경화제부를 100:33의 중량비로 혼합하여 도료 조성물을 제조한 것을 제외하고는, 비교예 4와 동일한 조성을 적용하였다.The same composition as in Comparative Example 4 was applied, except that the topical portion and the curing agent portion were mixed in a weight ratio of 100: 33 to prepare a coating composition.

[[ 비교예Comparative Example 9] 9]

주제부와 경화제부를 100:33의 중량비로 혼합하여 도료 조성물을 제조한 것을 제외하고는, 비교예 5와 동일한 조성을 적용하였다.The same composition as in Comparative Example 5 was applied, except that the topical portion and the curing agent portion were mixed in a weight ratio of 100: 33 to prepare a coating composition.

[[ 제조예Manufacturing example 1 내지 12 및  1 to 12 and 비교제조예Comparative Manufacturing Example 1 내지 9] 1 to 9]

실시예 1 내지 12 및 비교예 1 내지 9에서 제조된 각각의 조성물을 120 ℃(소재표면 온도 기준)에서 50 분 동안 강제 건조시켜 도막을 형성하였다.Each of the compositions prepared in Examples 1 to 12 and Comparative Examples 1 to 9 was forcibly dried at 120 캜 (based on the material surface temperature) for 50 minutes to form a film.

[[ 실험예Experimental Example ]]

제조된 도막의 물성을 하기와 같이 평가하였으며, 그 결과를 하기 표 7 내지 표 10에 나타내었다.Physical properties of the prepared coating films were evaluated as follows, and the results are shown in Tables 7 to 10 below.

1. 색상: 측색기로 측정하였다(DE≤0.5: ◎, 0.5∠DE≤1: ○, 1∠DE≤1.5: △, DE>1.5: ×).1. Color: Measured with a colorimeter (DE? 0.5:?, 0.5? DE? 1:?, 1? DE? 1.5:?, DE> 1.5:

2. 저장안정성: 조성물을 40 ℃의 오븐에서 4주 동안 방치한 후 평가하였다(조성물 총 부피 중 5 부피% 이내가 침전된 경우: ◎ / 조성물 총 부피 중 5-10 부피%가 침전된 경우: ○ / 조성물 총 부피 중 10-15 부피%가 침전된 경우: △ / 조성물 총 부피 중 15 부피% 이상이 침전된 경우: ×).2. Storage stability: The composition was evaluated after standing for 4 weeks in an oven at 40 占 폚 (when 5 volume% or less of the total volume of the composition was precipitated:? / 5 to 10 volume% ? / 10 to 15% by volume of the total volume of the composition was precipitated? / 15% or more of the total volume of the composition was precipitated.

3. 광택: 광택 측정기로 측정하였다(측정치≥90%인 경우: ◎ / 90%>측정치≥85% 인 경우: ○ / 85%>측정치≥80%인 경우: △ / 측정치<80%인 경우: ×).3. Gloss: Measured with a gloss meter (measured value ≥90%: ◎ / 90%> measured value ≥85%: ∘ / 85%> measured value ≥ 80%: △ / ×).

4. 내염수성: 제조된 도막에 30-40 ℃의 NaCl 5 % 용액을 8 시간 동안 분무한 후 16 시간 동안 방치하는 것을 1 cycle로 하여, 이를 3 cycle 연속 실시하였다. 이후 면포로 물기를 제거한 후 30 분 동안 방치하고 cross cutting test를 실시하였다(부착성 5B인 경우: ◎ / 부착성 4B인 경우: ○ / 부착성 3B인 경우: △ / 부착성 2B 미만인 경우: ×).4. Salt resistance: The coating film was sprayed with a 5% solution of NaCl at 30-40 ° C for 8 hours and allowed to stand for 16 hours. After the water was removed by a cotton swab, the mixture was allowed to stand for 30 minutes and subjected to a cross cutting test. (Adhesive 5B: ⊚ / Adhesive 4B: O / Adhesive 3B: ).

5. 내열탕성: 제조된 도막을 60 ℃의 항온항습조에 30 분 동안 침식시킨 후 2 시간 동안 방치하고 cross cutting test를 실시하였다(부착성 5B인 경우: ◎ / 부착성 4B인 경우: ○ / 부착성 3B인 경우: △ / 부착성 2B 미만인 경우: ×).5. Hot water resistance: The coated film was eroded for 30 minutes in a constant-temperature and constant-humidity chamber at 60 ° C, and then allowed to stand for 2 hours and subjected to a cross cutting test. (Adherence 5B: Attachment 3B:? / Attachment 2B:?).

제조예 1Production Example 1 제조예 2Production Example 2 제조예 3Production Example 3 제조예 4Production Example 4 제조예 5Production Example 5 제조예 6Production Example 6 색상color 저장안정성Storage stability 광택Polish 내염수성Saltwater 내열탕성My hot water castle ◎: 우수, ○: 양호, △: 보통, ×: 불량?: Excellent,?: Good,?: Fair, X: Bad

제조예 7Production Example 7 제조예 8Production Example 8 제조예 9Production Example 9 제조예 10Production Example 10 제조예 11Production Example 11 제조예 12Production Example 12 색상color 저장안정성Storage stability 광택Polish 내염수성Saltwater 내열탕성My hot water castle ◎: 우수, ○: 양호, △: 보통, ×: 불량?: Excellent,?: Good,?: Fair, X: Bad

비교
제조예 1
compare
Production Example 1
비교
제조예 2
compare
Production Example 2
비교
제조예 3
compare
Production Example 3
비교
제조예 4
compare
Production Example 4
비교
제조예 5
compare
Production Example 5
비교
제조예 6
compare
Production Example 6
비교
제조예 7
compare
Production Example 7
색상color ×× ×× ×× ×× ×× ×× ×× 저장안정성Storage stability 광택Polish ×× ×× ×× ×× ×× ×× ×× 내염수성Saltwater ×× ×× ×× ×× 내열탕성My hot water castle ×× ×× ×× ×× ◎: 우수, ○: 양호, △: 보통, ×: 불량?: Excellent,?: Good,?: Fair, X: Bad

비교
제조예 8
compare
Production Example 8
비교
제조예 9
compare
Production Example 9
색상color ×× ×× 저장안정성Storage stability 광택Polish ×× ×× 내염수성Saltwater ×× 내열탕성My hot water castle ×× ◎: 우수, ○: 양호, △: 보통, ×: 불량?: Excellent,?: Good,?: Fair, X: Bad

상기 표 7 내지 표 10을 참조하면, 본 발명의 도료 조성물은 전반적인 물성이 우수한 것을 확인할 수 있다.Referring to Tables 7 to 10, it can be confirmed that the coating composition of the present invention has excellent overall physical properties.

Claims (6)

제1 아크릴 폴리올 수지 5 중량부 이상 10 중량부 미만, 제2 아크릴 폴리올 수지 25 내지 35 중량부, 금속계 안료 7 내지 9 중량부, 및 제1 용제 50 내지 60 중량부를 포함하는 주제부; 및
폴리이소시아네이트 30 내지 40 중량부, 및 제2 용제 60 내지 70 중량부를 포함하는 경화제부를 포함하며,
제2 아크릴 폴리올 수지는 수산기가가 80 mgKOH/g 미만이고, 유리전이온도가 30℃ 초과인 것인 도료 조성물.
5 to 10 parts by weight of a first acrylic polyol resin, 25 to 35 parts by weight of a second acrylic polyol resin, 7 to 9 parts by weight of a metallic pigment, and 50 to 60 parts by weight of a first solvent; And
30 to 40 parts by weight of a polyisocyanate, and 60 to 70 parts by weight of a second solvent,
And the second acrylic polyol resin has a hydroxyl value of less than 80 mgKOH / g and a glass transition temperature of more than 30 ° C.
청구항 1에 있어서,
상기 제1 아크릴 폴리올 수지는 중량평균분자량(Mw)이 10,000 내지 23,000인 것인 도료 조성물.
The method according to claim 1,
Wherein the first acrylic polyol resin has a weight average molecular weight (Mw) of 10,000 to 23,000.
청구항 1에 있어서,
상기 제1 아크릴 폴리올 수지는 수산기가(OH value)가 35 내지 60 mgKOH/g 인 것인 도료 조성물.
The method according to claim 1,
Wherein the first acrylic polyol resin has an OH value of 35 to 60 mgKOH / g.
청구항 1에 있어서,
상기 제1 아크릴 폴리올 수지는 유리전이온도가 25 내지 50 ℃인 것인 도료 조성물.
The method according to claim 1,
Wherein the first acrylic polyol resin has a glass transition temperature of 25 to 50 占 폚.
청구항 1에 있어서,
상기 주제부와 상기 경화제부의 혼합 비율이 100:13 내지 100:33의 중량비인 것인 도료 조성물.
The method according to claim 1,
Wherein the mixing ratio of the main portion to the curing agent portion is 100: 13 to 100: 33.
청구항 1에 있어서,
상기 주제부가 왁스, 침강방지제, 자외선 안정제, 소포제, 및 커플링제로 이루어진 군에서 선택된 1종 이상의 첨가제 0.8 내지 4 중량부를 더 포함하는 것인 도료 조성물.
The method according to claim 1,
Further comprising 0.8 to 4 parts by weight of at least one additive selected from the group consisting of waxes, anti-settling agents, ultraviolet stabilizers, antifoaming agents and coupling agents.
KR1020160154666A 2016-11-21 2016-11-21 Coating composition KR101947240B1 (en)