JPH0871855A - Rolled material jointing device and jointing method - Google Patents

Rolled material jointing device and jointing method

Info

Publication number
JPH0871855A
JPH0871855A JP20641794A JP20641794A JPH0871855A JP H0871855 A JPH0871855 A JP H0871855A JP 20641794 A JP20641794 A JP 20641794A JP 20641794 A JP20641794 A JP 20641794A JP H0871855 A JPH0871855 A JP H0871855A
Authority
JP
Japan
Prior art keywords
rolled material
succeeding
moving
joining
horizontally
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP20641794A
Other languages
Japanese (ja)
Other versions
JP3491703B2 (en
Inventor
Nobuhiro Tazoe
信広 田添
Norio Iwanami
紀夫 岩波
Masami Oki
正海 沖
Koichi Sakamoto
浩一 坂本
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
IHI Corp
Nippon Steel Corp
Original Assignee
IHI Corp
Sumitomo Metal Industries Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by IHI Corp, Sumitomo Metal Industries Ltd filed Critical IHI Corp
Priority to JP20641794A priority Critical patent/JP3491703B2/en
Publication of JPH0871855A publication Critical patent/JPH0871855A/en
Application granted granted Critical
Publication of JP3491703B2 publication Critical patent/JP3491703B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

PURPOSE: To provide a rolled material jointing device and a jointing method which can joint the rear end part of preceding rolled material and the tip part of succeeding rolled material to each other in a short time with sufficient joint strength over the whole width of the rolled material and can roll the joint part almost uniformly with little unevenness at the joint part. CONSTITUTION: A rolled material jointing method is constituted of a processing process (A) of cutting the rear end part lower face of a preceding rolled material 1 and the tip part upper face of succeeding rolled material 2 by a surface processing device 18 while holding the machined face 1a or the like in the reduced state or nonoxidized state by reduction holding device 20, a positioning process (B) of overlapping the processed faces of the preceding rolled material and succeeding rolled material, a moving process (C) of moving the preceding rolled material and succeeding rolled material synchronously in the horizontal direction by moving devices 14, 16, with the processed faces as they are overlapped, and a jointing process (D) of compressing the overlapped part almost to the same thickness as the rolled material to joint by a pressure welding device 22.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は、熱間圧延設備において
先行圧延材の後端部と後続圧延材の先端部とを接合する
圧延材の接合装置と接合方法に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a rolling material joining apparatus and a joining method for joining a trailing end portion of a preceding rolled material and a leading end portion of a succeeding rolled material in a hot rolling facility.

【0002】[0002]

【従来の技術】従来の熱間圧延設備(ホットストリップ
ミル)では、粗圧延機で圧延されたバー材を、それぞれ
別々に仕上圧延機に供給し、所望の板厚のストリップ材
を得ていた。しかし、かかる手段では、圧延材全体を均
一に圧延できず、圧延材の端部(前端部と後端部)に欠
陥が生じやすく圧延材の歩留りを低下させ、かつ噛込み
/尻抜け等のため圧延速度を高速化しにくい問題点があ
った。
2. Description of the Related Art In a conventional hot rolling facility (hot strip mill), bar materials rolled by a rough rolling mill are separately supplied to a finishing rolling mill to obtain a strip material having a desired plate thickness. . However, with such means, the entire rolled material cannot be rolled uniformly, defects are likely to occur at the end portions (front end portion and rear end portion) of the rolled material, the yield of the rolled material is reduced, and biting / flanking etc. occur. Therefore, there is a problem that it is difficult to increase the rolling speed.

【0003】かかる問題点を解決するため、圧延材を連
続的に仕上圧延機に供給するために先行する圧延材の後
端と次の圧延材の前端とを接合する接合装置が従来から
提案されていた(例えば、特開昭62−252603号
公報、特開昭63−93408号公報、特公平5−13
9号公報)。
In order to solve such a problem, a joining device for joining the trailing end of the preceding rolled material and the leading end of the next rolled material in order to continuously feed the rolled material to the finish rolling mill has been conventionally proposed. (For example, JP-A-62-252603, JP-A-63-93408, JP-B-5-13).
No. 9).

【0004】[0004]

【発明が解決しようとする課題】しかし、特開昭62−
252603号の「板接合方法」は、接合すべき板の端
部相互間に、継手を打込んで接合するものであるが、圧
延材の幅全体にわたり十分な接合強度を確保するには多
数の継手を短時間で打込む必要があり、自動化(機械
化)が困難であり、かつ継手部を均一に圧延できない問
題点があった。
However, Japanese Patent Laid-Open No. 62-62
The "plate joining method" of No. 252603 is to insert a joint between the ends of the plates to be joined and join them, but in order to secure sufficient joining strength over the entire width of the rolled material, There is a problem that the joint needs to be driven in a short time, automation (mechanization) is difficult, and the joint cannot be uniformly rolled.

【0005】また、特開昭63−93408号の「バー
接合設備」は、圧延材にループを形成して、後端と先端
を圧接するものであるが、比較的厚いバー材をループに
形成するため、バー材に曲げ癖が付きやすくかつ十分な
接合時間を確保できず、また後端と先端を単に圧接して
も圧延材の幅全体にわたり十分な接合強度を確保できな
い問題点があった。
Further, the "bar joining equipment" of Japanese Patent Laid-Open No. 63-93408 forms a loop on a rolled material and press-contacts the rear end and the tip, but a relatively thick bar material is formed on the loop. Therefore, there is a problem that the bar material tends to have a bending tendency and sufficient bonding time cannot be secured, and even if the rear end and the tip are simply pressure-bonded, sufficient bonding strength cannot be secured over the entire width of the rolled material. .

【0006】更に、特公平5−139号の「帯板の走間
溶接装置」は、圧延材とともに走行しながら後端と先端
を溶接接合する装置であるが、幅広の圧延材を溶接する
には時間がかかるため設備全体が長くなりやすく、かつ
接合部に凸凹が生じやすく、接合部を均一に圧延するこ
とが困難である問題点があった。
[0006] Further, Japanese Patent Publication No. 5-139 "Bath strip welding device" is a device for welding and joining a rear end and a tip while traveling with a rolled material, but for welding a wide rolled material. Since it takes time, there is a problem that the entire equipment tends to be long, and unevenness is likely to occur at the joint, which makes it difficult to uniformly roll the joint.

【0007】本発明は上述した種々の問題点を解決する
ために創案されたものである。すなわち、本発明の目的
は、先行圧延材の後端部と後続圧延材の先端部とを短時
間に圧延材の幅全体にわたり十分な接合強度で接合する
ことができ、接合部の凸凹が少なく接合部をほぼ均一に
圧延できる圧延材接合装置と接合方法を提供することに
ある。
The present invention was created to solve the above-mentioned various problems. That is, the object of the present invention is to join the trailing end of the preceding rolled material and the leading end of the following rolled material with sufficient bonding strength over the entire width of the rolled material in a short time, and to reduce the unevenness of the bonded portion. It is an object of the present invention to provide a rolled material joining apparatus and a joining method capable of rolling a joined portion substantially uniformly.

【0008】[0008]

【課題を解決するための手段】本発明によれば、先行圧
延材の後端部下面と後続圧延材の先端部上面を切削加工
する面加工装置と、該加工面を還元状態又は非酸化状態
に保持する複数の還元保持装置と、先行圧延材の後端部
を水平に挟持したまま上下動及び水平移動可能な先行材
移動装置と、先行圧延材と後続圧延材の加工面を重ね合
わせたまま後続圧延材を先行圧延材と同期して水平移動
可能な後続材移動装置と、面加工装置の下流側に設けら
れ前記重ね合わせ部を圧延材とほぼ同一厚さまで圧縮し
て接合する圧接装置と、を備えたことを特徴とする圧延
材接合装置が提供される。
According to the present invention, a surface processing apparatus for cutting the lower surface of the trailing end of the preceding rolled material and the upper surface of the leading end of the succeeding rolled material, and the processed surface in a reduced state or a non-oxidized state. A plurality of reduction holding devices, a preceding material moving device that can move vertically and horizontally while holding the trailing end of the preceding rolled material horizontally, and the machined surfaces of the preceding rolled material and the succeeding rolled material are superimposed. The succeeding material moving device that can horizontally move the succeeding rolled material in synchronism with the preceding rolled material, and the pressure welding device that is provided on the downstream side of the surface processing device and that compresses and joins the overlapping portion to approximately the same thickness as the rolled material. And a rolled material joining device.

【0009】本発明の好ましい実施例によれば、前記還
元保持装置は、燃料を不完全燃焼させて還元状態を形成
する還元炎バーナであり、かつそのうち少なくとも1つ
が後続材移動装置に取付けられている。また、前記面加
工装置は、先行圧延材の下側に設けられ、幅方向の軸心
を中心に回転する円筒形下カッタと、後続圧延材の上側
に設けられ、幅方向の軸心を中心に回転し、かつ上下動
可能な円筒形上カッタと、からなる。
According to a preferred embodiment of the present invention, the reduction holding device is a reducing flame burner for incompletely burning fuel to form a reducing state, and at least one of them is attached to a succeeding material moving device. There is. Further, the surface processing device is provided on the lower side of the preceding rolled material and is provided on the upper side of the cylindrical lower cutter and the succeeding rolled material that rotate around the axis of the width direction. It consists of a cylindrical upper cutter that can rotate and move up and down.

【0010】更に本発明によれば、加工面を還元状態又
は非酸化状態に保持したまま、先行圧延材の後端部下面
と後続圧延材の先端部上面を切削加工し、先行圧延材と
後続圧延材の加工面を重ね合せ、加工面を重ね合せたま
ま先行圧延材と後続圧延材を同期して水平移動させ、重
ね合わせ部を圧延材とほぼ同一厚さまで圧縮して接合す
る、ことを特徴とする圧延材接合方法が提供される。
Further, according to the present invention, the lower surface of the trailing end portion of the preceding rolled material and the upper surface of the leading end portion of the succeeding rolled material are cut while the processed surface is kept in the reduced state or the non-oxidized state, and the preceding rolled material and the subsequent rolled material are processed. The processed surfaces of the rolled materials are overlapped, the preceding rolled material and the subsequent rolled material are horizontally moved in synchronization while the processed surfaces are overlapped, and the overlapping part is compressed to approximately the same thickness as the rolled material and joined. A characteristic rolling material joining method is provided.

【0011】[0011]

【作用】上記本発明の装置及び方法によれば、先行圧延
材の後端部下面と後続圧延材の先端部上面を切削加工す
る加工工程と、先行圧延材と後続圧延材の加工面を重ね
合せる位置決め工程と、加工面を重ね合せたまま先行圧
延材と後続圧延材を同期して水平移動させる移動工程
と、重ね合わせ部を圧延材とほぼ同一厚さまで圧縮して
接合する接合工程の4工程で圧延材の幅全体を接合でき
るため、接合時間を短縮することができ、圧延設備全長
を短くすることができる。また、先行材移動装置と後続
材移動装置により面加工装置と圧接装置を間隔を隔てる
ことができる。
According to the above-mentioned apparatus and method of the present invention, a processing step of cutting the lower surface of the trailing end of the preceding rolled material and the upper surface of the leading end of the succeeding rolled material, and the processed surface of the preceding rolled material and the succeeding rolled material are overlapped. 4 of the positioning process of combining, the moving process of synchronously moving the preceding rolled material and the succeeding rolled material horizontally while the processed surfaces are superposed, and the joining step of compressing and joining the superposed portion to the same thickness as the rolled material. Since the entire width of the rolled material can be joined in the process, the joining time can be shortened and the total length of rolling equipment can be shortened. Further, the surface processing device and the pressure welding device can be separated by the preceding material moving device and the succeeding material moving device.

【0012】更に、還元保持装置により加工面を還元状
態又は非酸化状態に保持したまま、面加工装置により後
端部下面と先端部上面を切削加工しかつ圧接装置により
加工面を圧延材とほぼ同一厚さまで圧縮するので、加工
面の酸化がほとんどなく圧接することができ、圧延材の
幅全体にわたり十分な接合強度で接合することができ
る。また、圧接装置により加工面を重ね合わせて圧延材
とほぼ同一厚さまで圧縮して接合するので、接合部の凸
凹がほとんどなく接合部をほぼ均一に圧延することがで
きる。
Further, while the machined surface is held in the reduced state or the non-oxidized state by the reducing and holding device, the rear surface of the rear end portion and the upper surface of the front end portion are cut by the surface processing apparatus, and the machined surface is made almost the same as the rolled material by the pressure welding apparatus. Since it is compressed to the same thickness, it is possible to perform pressure welding with almost no oxidation of the processed surface, and it is possible to join with sufficient joining strength over the entire width of the rolled material. Further, since the processed surfaces are superposed by the pressure welding device and compressed and bonded to the same thickness as the rolled material, there is almost no unevenness in the bonded portion and the bonded portion can be rolled substantially uniformly.

【0013】[0013]

【実施例】以下、本発明の好ましい実施例を図面を参照
して説明する。なお、各図において共通する部分には同
一の符号を付して重複した説明を省略する。図1は、本
発明による圧延材接合装置の全体構成図である。図1に
おいて、本発明の圧延材接合装置10は、先行圧延材1
の後端部下面と後続圧延材2の先端部上面を切削加工す
る面加工装置18と、加工面1a、2aを還元状態又は
非酸化状態に保持する複数の還元保持装置20と、先行
圧延材1の後端部を水平に挟持したまま上下動及び水平
移動可能な先行材移動装置14と、先行圧延材1と後続
圧延材2の加工面1a、2aを重ね合わせたまま後続圧
延材2を先行圧延材1と同期して水平移動可能な後続材
移動装置16と、面加工装置18の下流側に設けられ重
ね合わせ部3を圧延材1、2とほぼ同一厚さまで圧縮し
て接合する圧接装置22と、を備えている。
DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENT A preferred embodiment of the present invention will be described below with reference to the drawings. In addition, in each figure, the same parts are denoted by the same reference numerals, and the duplicated description will be omitted. FIG. 1 is an overall configuration diagram of a rolled material joining apparatus according to the present invention. In FIG. 1, a rolled material joining apparatus 10 of the present invention is provided with a preceding rolled material 1
A surface processing device 18 for cutting the lower surface of the rear end portion and the upper surface of the front end of the subsequent rolled material 2, a plurality of reduction holding devices 20 for holding the processing surfaces 1a, 2a in a reduced state or a non-oxidized state, and a preceding rolled material The leading material moving device 14 capable of vertically moving and horizontally moving while holding the rear end portion of 1 horizontally, and the trailing rolled material 2 with the machined surfaces 1a and 2a of the leading rolled material 1 and the trailing rolled material 2 superposed on each other. Pressure welding for compressing and joining the succeeding material moving device 16 capable of moving horizontally in synchronization with the preceding rolled material 1 and the overlapping portion 3 provided on the downstream side of the surface processing device 18 to approximately the same thickness as the rolled materials 1, 2. And a device 22.

【0014】面加工装置18は、先行圧延材1の下側に
設けられ、幅方向の軸心Zを中心に図示しない駆動装置
により回転する円筒形下カッタ19aと、後続圧延材2
の上側に設けられ、幅方向の軸心Zを中心に図示しない
駆動装置により回転し、かつ上下動可能な円筒形上カッ
タ19bと、からなる。カッタ19a、19bは、圧延
材1、2の全幅より長く、その外周部には複数の刃が同
径に設けられ、圧延材1、2の全幅にわたりそれぞれ単
一のカッタ19a、19bにより切削加工するようにな
っている。また、上カッタ19bは、後続圧延材2の先
端部上面を加工する加工位置Lと、その下を還元保持装
置20等が通過できるように図で斜め上方に移動した待
機位置Hとの間を、図示しない駆動装置(例えば液圧シ
リンダ)により上下動できるようになっている。かかる
構成により、カッタ19a、19bにより圧延材1の後
端部下面と後続圧延材2の先端部上面の両方を切削加工
し、次いで上カッタ19b及び下カッタ19aを待機位
置Hに移動させることができる。
The surface processing device 18 is provided on the lower side of the preceding rolled material 1, and has a cylindrical lower cutter 19a which is rotated by a driving device (not shown) about the axis Z in the width direction, and the succeeding rolled material 2
And a cylindrical upper cutter 19b which is provided on the upper side of, and which is rotatable by a drive device (not shown) about an axis Z in the width direction and is vertically movable. The cutters 19a and 19b are longer than the entire widths of the rolled materials 1 and 2, and have a plurality of blades with the same diameter on the outer peripheral portion thereof, and are cut by the single cutters 19a and 19b over the entire widths of the rolled materials 1 and 2, respectively. It is supposed to do. Further, the upper cutter 19b is provided between a processing position L for processing the upper surface of the leading end portion of the succeeding rolled material 2 and a standby position H which is moved obliquely upward in the drawing so that the reduction holding device 20 and the like can pass thereunder. It can be moved up and down by a driving device (not shown) (for example, a hydraulic cylinder). With this configuration, both the rear end lower surface of the rolled material 1 and the upper end surface of the succeeding rolled material 2 are cut by the cutters 19a and 19b, and then the upper cutter 19b and the lower cutter 19a can be moved to the standby position H. it can.

【0015】先行材移動装置14は、複数の支持ローラ
4の間に位置し先行圧延材1の後端部を水平に支持する
複数の支持部材15aと、支持部材15aとの間に先行
圧延材1の後端部を挟持するクランプローラ15bと、
先行圧延材1の後端部を水平に挟持したまま上下動させ
る昇降装置15cと、該昇降装置15cを水平に移動さ
せる移動装置15dとからなる。昇降装置15cと移動
装置15dはそれぞれ、昇降台又は移動台と液圧シリン
ダとの組み合わせであるのがよい。かかる構成により、
支持部材15aとクランプローラ15bにより先行圧延
材1の後端部を水平に支持したまま、下カッタ19aに
より圧延材1の後端部下面を切削加工し、次いで昇降装
置15cにより支持ローラ4(送りローラ)との干渉を
避けかつ少なくとも後続圧延材2の板厚以上に上昇さ
せ、更に移動装置15dにより圧接装置22の方向に水
平に移動させることができる。
The preceding material moving device 14 is provided between a plurality of supporting rollers 4 and horizontally supports the rear end portion of the preceding rolled material 1. A plurality of supporting members 15a are provided between the supporting members 15a. A clamp roller 15b for sandwiching the rear end of the first roller;
It is composed of an elevating device 15c for vertically moving while holding the rear end of the preceding rolled material 1 horizontally, and a moving device 15d for horizontally moving the elevating device 15c. The lifting device 15c and the moving device 15d are each preferably a combination of a lifting table or a moving table and a hydraulic cylinder. With this configuration,
While the rear end of the preceding rolled material 1 is horizontally supported by the supporting member 15a and the clamp roller 15b, the lower cutter 19a cuts the lower surface of the rear end of the rolled material 1, and then the lifting device 15c moves the supporting roller 4 (feeding roller 4). It is possible to avoid interference with the rollers, raise the thickness of the succeeding rolled material 2 to at least the plate thickness of the succeeding rolled material 2, and further move horizontally in the direction of the press contact device 22 by the moving device 15d.

【0016】後続材移動装置16は、後続圧延材1の先
端部を水平に支持する複数の支持ローラ17aと、支持
ローラ17aとの間に後続圧延材1の先端部を挟持する
クランプローラ17bと、後続圧延材2を先行圧延材1
と同期して水平移動させる移動装置17cとからなる。
かかる構成により、支持ローラ17aとクランプローラ
17bにより後続圧延材2の先端部を水平に支持したま
ま、上カッタ19bにより後続圧延材2の先端部上面を
切削加工し、次いで移動装置17cにより後続圧延材2
を先行圧延材1と同期して圧接装置22の方向に水平移
動することができる。
The subsequent material moving device 16 includes a plurality of support rollers 17a for horizontally supporting the leading end portion of the succeeding rolled material 1, and a clamp roller 17b for sandwiching the leading end portion of the succeeding rolled material 1 between the supporting rollers 17a. , Succeeding rolled material 2 to preceding rolled material 1
And a moving device 17c for horizontally moving in synchronism with.
With this structure, the upper cutter 19b cuts the upper surface of the leading end portion of the succeeding rolled material 2 while horizontally supporting the leading end portion of the succeeding rolled material 2 by the supporting roller 17a and the clamp roller 17b, and then the succeeding rolling operation is performed by the moving device 17c. Material 2
Can be horizontally moved in the direction of the pressure welding device 22 in synchronization with the preceding rolled material 1.

【0017】還元保持装置20は、COG(コークス炉
ガス)、LPG、LNG等の可燃性ガスを完全燃焼させ
る量よりも少ない酸素で燃焼させて、水素ラジカル、C
20ラジカル等還元性ラジカルを含有する還元炎にて
還元状態を形成する還元炎バーナであり、そのうち少な
くとも1つが後続材移動装置16に取付けられている。
かかる構成により、面加工装置18による切削加工工
程、後続材移動装置16による移動工程、及び圧接装置
22による圧接工程の間、加工面1a、2aを還元状態
又は非酸化状態に保持し、その酸化を防止し、高い接合
強度を確保することができる。
The reduction holding device 20 burns a combustible gas such as COG (coke oven gas), LPG, and LNG with less oxygen than the amount that completely burns it, thereby generating hydrogen radicals, C
A reducing flame burner that forms a reducing state in a reducing flame containing reducing radicals such as H 2 0 radicals, and at least one of them is attached to the subsequent material moving device 16.
With such a configuration, the machined surfaces 1a and 2a are held in the reduced state or the non-oxidized state during the cutting process by the surface processing device 18, the moving process by the subsequent material moving device 16, and the pressure welding process by the pressure welding device 22, and the oxidation thereof is performed. Can be prevented and a high bonding strength can be secured.

【0018】圧接装置22は、先行圧延材1の後端部上
面に接する上型23aと、後続圧延材2の先端部下面に
接する下型23bと、上型23a及び下型23bを挟持
して圧縮するプレス装置23cと、からなる。また、上
型23aはプレス装置23cのラム23eの下面に取付
られ、ラム23eとともに昇降するようになっている。
かかる構成により、先行圧延材1と後続圧延材2の加工
面1a、2aを移動工程後すぐさま圧縮することができ
る。また、この圧縮により重ね合わせ部分を圧延材1、
2とほぼ同一の厚さまで圧縮することにより、接合部の
凸凹がほとんどなく接合部をほぼ均一に圧延することが
できる。
The pressure welding device 22 sandwiches the upper die 23a which comes into contact with the upper surface of the rear end portion of the preceding rolled material 1, the lower die 23b which comes into contact with the lower surface of the leading end portion of the succeeding rolled material 2, and the upper die 23a and the lower die 23b. And a pressing device 23c for compressing. Further, the upper die 23a is attached to the lower surface of the ram 23e of the press device 23c so as to move up and down together with the ram 23e.
With such a configuration, the machined surfaces 1a, 2a of the preceding rolled material 1 and the succeeding rolled material 2 can be compressed immediately after the moving process. In addition, by this compression, the overlapped portion is rolled material 1,
By compressing to a thickness substantially the same as that of 2, the joint can be rolled substantially evenly with almost no irregularities in the joint.

【0019】図2は、本発明による圧延材接合方法の作
動説明図である。本発明の方法は、加工面を還元状態又
は非酸化状態に保持したまま、先行圧延材の後端部下面
と後続圧延材の先端部上面を切削加工する加工工程
(A)と、先行圧延材と後続圧延材の加工面を重ね合せ
る位置決め工程(B)と、加工面を重ね合せたまま先行
圧延材と後続圧延材を同期して水平移動させる移動工程
(C)と、重ね合わせ部を圧延材とほぼ同一厚さまで圧
縮して接合する接合工程(D)とからなる。
FIG. 2 is an explanatory view of the operation of the rolled material joining method according to the present invention. The method of the present invention comprises a processing step (A) of cutting a lower surface of a trailing end portion of a preceding rolled material and an upper surface of a leading end portion of a succeeding rolled material while maintaining the worked surface in a reduced state or a non-oxidized state, and a preceding rolled material. And a positioning step (B) for superimposing the processed surfaces of the subsequent rolled materials, a moving step (C) for synchronously moving the preceding rolled material and the subsequent rolled material while the processed surfaces are superposed, and a superposition part is rolled. A joining step (D) of joining the materials by compressing them to almost the same thickness.

【0020】図2(A)において、先行材移動装置14
の支持部材15aとクランプローラ15bにより先行圧
延材1の後端部を水平に支持したまま、下カッタ19a
により圧延材1の後端部下面を切削加工する。また、支
持ローラ17aとクランプローラ17bにより後続圧延
材2の先端部を水平に支持したまま、上カッタ19bに
より後続圧延材2の先端部上面を切削加工する。またこ
の加工工程中、還元保持装置20により加工面1a、2
aを還元状態又は非酸化状態に保持する。
In FIG. 2A, the preceding material moving device 14
While the rear end portion of the preceding rolled material 1 is horizontally supported by the supporting member 15a and the clamp roller 15b of the lower cutter 19a.
The lower surface of the rear end of the rolled material 1 is cut by. Further, the upper cutter 19b cuts the upper surface of the leading end portion of the subsequent rolled material 2 while the leading end portion of the trailing rolled material 2 is horizontally supported by the support roller 17a and the clamp roller 17b. Further, during this processing step, the reduction holding device 20 is used to process the processing surfaces 1a, 2
Hold a in the reduced or non-oxidized state.

【0021】次いで、図2(B)に示すように、先行材
移動装置14の昇降装置15cにより支持ローラ4との
干渉を避けかつ少なくとも後続圧延材2の板厚以上に先
行圧延材1を上昇させ、後続材移動装置16により後続
圧延材2を水平に移動して先行圧延材1と加工面1a、
2aを重ね合せる。またこの位置決め工程中、還元保持
装置20により加工面1a、2aを還元状態又は非酸化
状態に保持する。
Next, as shown in FIG. 2B, the elevating device 15c of the preceding material moving device 14 avoids interference with the supporting roller 4 and raises the preceding rolled material 1 to at least the plate thickness of the succeeding rolled material 2. Then, the subsequent rolled material 2 is moved horizontally by the subsequent rolled material moving device 16 to move the following rolled material 1 and the processed surface 1a,
Stack 2a. Further, during this positioning process, the reduction holding device 20 holds the machined surfaces 1a, 2a in a reduced state or a non-oxidized state.

【0022】次いで、図2(C)に示すように、先行材
移動装置14の移動装置15dにより圧接装置22の方
向に水平に移動させ、かつ後続材移動装置16の移動装
置17cにより後続圧延材2を先行圧延材1と同期して
圧接装置22の方向に水平移動させる。この移動工程中
も、後続材移動装置16に取付けられた還元保持装置2
0により加工面1a、2aを還元状態又は非酸化状態に
保持する。
Next, as shown in FIG. 2 (C), the moving device 15d of the preceding material moving device 14 horizontally moves it toward the pressure welding device 22, and the moving device 17c of the following material moving device 16 moves the succeeding rolled material. 2 is horizontally moved in the direction of the pressure welding device 22 in synchronization with the preceding rolled material 1. Even during this moving process, the reduction holding device 2 attached to the subsequent material moving device 16
0 holds the machined surfaces 1a, 2a in a reduced state or a non-oxidized state.

【0023】次いで、図2(D)に示すように、還元保
持装置20により加工面1a、2aを還元状態又は非酸
化状態に保持したまま、圧接装置22により先行圧延材
1と後続圧延材2の加工面1a、2aを圧縮し、重ね合
わせ部分を圧延材1、2とほぼ同一の厚さまで圧縮して
接合する。
Then, as shown in FIG. 2 (D), while the machined surfaces 1a, 2a are held in the reduced state or the non-oxidized state by the reduction holding device 20, the preceding rolling material 1 and the subsequent rolling material 2 are pressed by the pressure welding device 22. The machined surfaces 1a and 2a are compressed, and the overlapped portions are compressed to the same thickness as the rolled materials 1 and 2 and joined.

【0024】かかる接合方法により、加工工程、位置決
め工程、移動工程、及び接合工程の4工程で圧延材の幅
全体を接合でき、これにより接合時間を短縮することが
でき、かつ圧延設備全長を短くすることができる。ま
た、先行材移動装置と後続材移動装置により面加工装置
18と圧接装置22を間隔を隔てて配置することができ
る。
With this joining method, the entire width of the rolled material can be joined in the four steps of the working step, the positioning step, the moving step, and the joining step, whereby the joining time can be shortened and the total length of rolling equipment can be shortened. can do. Further, the surface processing device 18 and the pressure welding device 22 can be arranged at a distance by the preceding material moving device and the succeeding material moving device.

【0025】なお、本発明は上述した実施例に限定され
ず、本発明の要旨を逸脱しない範囲で種々変更できるこ
とは勿論である。
The present invention is not limited to the above-mentioned embodiments, and it goes without saying that various modifications can be made without departing from the gist of the present invention.

【0026】[0026]

【発明の効果】上述したように、本発明の装置及び方法
によれば、加工工程、位置決め工程、移動工程、及び接
合工程の4工程で圧延材の幅全体を接合できるため、接
合時間を短縮することができ、圧延設備全長を短くする
ことができる。また、先行材移動装置と後続材移動装置
により面加工装置と圧接装置を間隔を隔てることができ
る。
As described above, according to the apparatus and method of the present invention, the entire width of the rolled material can be joined in four steps including the working step, the positioning step, the moving step, and the joining step, so that the joining time can be shortened. Therefore, the total length of rolling equipment can be shortened. Further, the surface processing device and the pressure welding device can be separated by the preceding material moving device and the succeeding material moving device.

【0027】更に、還元保持装置により加工面を還元状
態又は非酸化状態に保持したまま、面加工装置により後
端部下面と先端部上面を切削加工しかつ圧接装置により
加工面を圧延材とほぼ同一厚さまで圧縮するので、加工
面の酸化がほとんどなく圧接することができ、圧延材の
幅全体にわたり十分な接合強度で接合することができ
る。また、圧接装置により加工面を重ね合わせて圧延材
とほぼ同一厚さまで圧縮して接合するので、接合部の凸
凹がほとんどなく接合部をほぼ均一に圧延することがで
きる。
Further, while the machined surface is held in the reduced state or the non-oxidized state by the reduction holding device, the rear end lower surface and the tip end upper surface are machined by the surface machining apparatus and the machined surface is made almost a rolled material by the pressure welding apparatus. Since it is compressed to the same thickness, it is possible to perform pressure welding with almost no oxidation of the processed surface, and it is possible to join with sufficient joining strength over the entire width of the rolled material. Further, since the processed surfaces are superposed by the pressure welding device and compressed and bonded to the same thickness as the rolled material, there is almost no unevenness in the bonded portion and the bonded portion can be rolled substantially uniformly.

【0028】従って、本発明の圧延材の接合装置と接合
方法は、先行する圧延材の後端と後続する圧延材の先端
と短時間に圧延材の幅全体にわたり十分な接合強度で接
合することができ、接合部の凸凹が少なく接合部をほぼ
均一に圧延できる、等の優れた効果を有する。
Therefore, according to the joining apparatus and joining method for rolled material of the present invention, it is possible to join the trailing end of the preceding rolled material and the leading end of the following rolled material with sufficient bonding strength over the entire width of the rolled material in a short time. It has an excellent effect such that there is little unevenness in the joint and the joint can be rolled substantially uniformly.

【図面の簡単な説明】[Brief description of drawings]

【図1】本発明による圧延材接合装置の全体構成図であ
る。
FIG. 1 is an overall configuration diagram of a rolled material joining device according to the present invention.

【図2】本発明による圧延材接合方法の作動説明図であ
る。
FIG. 2 is an operation explanatory view of a rolled material joining method according to the present invention.

【符号の説明】[Explanation of symbols]

1 先行圧延材 1a 加工面 2 後続圧延材 2a 加工面 3 重ね合わせ部 4 支持ローラ 10 圧延材接合装置 14 先行材移動装置 15a 支持部材 15b クランプローラ 15c 昇降装置 15d 移動装置 16 後続材移動装置 17a 支持ローラ 17b クランプローラ 17c 移動装置 18 面加工装置 19a 下カッタ 19b 上カッタ 20 還元保持装置 22 圧接装置 23a 上型 23b 下型 23c プレス装置 23e ラム H 上カッタの待機位置 L 上カッタの加工位置 1 Pre-rolled material 1a Processed surface 2 Subsequent rolled material 2a Processed surface 3 Stacking part 4 Support roller 10 Rolled material joining device 14 Preceding material moving device 15a Supporting member 15b Clamp roller 15c Lifting device 15d Moving device 16 Subsequent material moving device 17a Support Roller 17b Clamp roller 17c Moving device 18 Surface processing device 19a Lower cutter 19b Upper cutter 20 Reduction holding device 22 Pressing device 23a Upper mold 23b Lower mold 23c Press device 23e Ram H Standing position of upper cutter L Processing position of upper cutter

───────────────────────────────────────────────────── フロントページの続き (72)発明者 沖 正海 東京都千代田区大手町1丁目1番3号 住 友金属工業株式会社内 (72)発明者 坂本 浩一 茨城県鹿島郡鹿島町大字光3番地 住友金 属工業株式会社鹿島製鉄所内 ─────────────────────────────────────────────────── ─── Continuation of front page (72) Masami Oki, 1-3 1-3 Otemachi, Chiyoda-ku, Tokyo Sumitomo Metal Industries, Ltd. (72) Inventor, Koichi Sakamoto, Koujima-machi, Kashima-gun, Ibaraki Prefecture Sumitomo Metal Industries, Ltd. Kashima Steel Works

Claims (4)

【特許請求の範囲】[Claims] 【請求項1】 先行圧延材の後端部下面と後続圧延材の
先端部上面を切削加工する面加工装置と、該加工面を還
元状態又は非酸化状態に保持する複数の還元保持装置
と、先行圧延材の後端部を水平に挟持したまま上下動及
び水平移動可能な先行材移動装置と、先行圧延材と後続
圧延材の加工面を重ね合わせたまま後続圧延材を先行圧
延材と同期して水平移動可能な後続材移動装置と、面加
工装置の下流側に設けられ前記重ね合わせ部を圧延材と
ほぼ同一厚さまで圧縮して接合する圧接装置と、を備え
たことを特徴とする圧延材接合装置。
1. A surface processing device for cutting the lower surface of the trailing end of the preceding rolled material and the upper surface of the leading end of the subsequent rolled material, and a plurality of reduction holding devices for holding the processed surfaces in a reduced state or a non-oxidized state. Synchronize the trailing rolled material with the preceding rolled material with the leading material moving device that can move vertically and horizontally while holding the trailing end of the preceding rolled material horizontally And a horizontal movement device for moving the succeeding material, and a pressure welding device that is provided on the downstream side of the surface processing device and that compresses and joins the overlapping portion to approximately the same thickness as the rolled material. Rolled material joining device.
【請求項2】 前記還元保持装置は、燃料を不完全燃焼
させて還元状態を形成する還元炎バーナであり、かつそ
のうち少なくとも1つが後続材移動装置に取付けられて
いる、ことを特徴とする請求項1に記載の圧延材接合装
置。
2. The reduction holding device is a reducing flame burner that forms a reducing state by incompletely burning fuel, and at least one of them is attached to a succeeding material moving device. Item 1. A rolled material joining device according to item 1.
【請求項3】 前記面加工装置は、先行圧延材の下側に
設けられ、幅方向の軸心を中心に回転する円筒形下カッ
タと、後続圧延材の上側に設けられ、幅方向の軸心を中
心に回転し、かつ上下動可能な円筒形上カッタと、から
なることを特徴とする請求項1に記載の圧延材接合装
置。
3. The surface processing device is provided on the lower side of the preceding rolled material, and has a cylindrical lower cutter that rotates about an axis in the width direction. The rolled material joining device according to claim 1, comprising a cylindrical upper cutter that is rotatable about a center and is vertically movable.
【請求項4】 切削加工面を還元状態又は非酸化状態に
保持したまま、 先行圧延材の後端部下面と後続圧延材の先端部上面を切
削加工し、 先行圧延材と後続圧延材の加工面を重ね合せ、 加工面を重ね合せたまま先行圧延材と後続圧延材を同期
して水平移動させ、 重ね合わせ部を圧延材とほぼ同一厚さまで圧縮して接合
する、ことを特徴とする圧延材接合方法。
4. The machining of the preceding rolled material and the succeeding rolled material by cutting the lower surface of the trailing end portion of the preceding rolled material and the upper surface of the leading end of the succeeding rolled material with the cutting surface kept in a reduced state or a non-oxidized state. Rolling characterized by overlapping the surfaces, moving the preceding rolled material and the succeeding rolled material horizontally in synchronism while the processed surfaces are overlapped, and compressing and joining the overlapped part to approximately the same thickness as the rolled material. Material joining method.
JP20641794A 1994-08-31 1994-08-31 Rolled material joining equipment Expired - Fee Related JP3491703B2 (en)