JPH0742082A - Sheet material having nubuck-like visual appearance and its production - Google Patents

Sheet material having nubuck-like visual appearance and its production

Info

Publication number
JPH0742082A
JPH0742082A JP20467593A JP20467593A JPH0742082A JP H0742082 A JPH0742082 A JP H0742082A JP 20467593 A JP20467593 A JP 20467593A JP 20467593 A JP20467593 A JP 20467593A JP H0742082 A JPH0742082 A JP H0742082A
Authority
JP
Japan
Prior art keywords
polyurethane resin
sheet material
nubuck
impregnated
base material
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP20467593A
Other languages
Japanese (ja)
Inventor
Katsumi Osawa
克己 大沢
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Achilles Corp
Original Assignee
Achilles Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Achilles Corp filed Critical Achilles Corp
Priority to JP20467593A priority Critical patent/JPH0742082A/en
Publication of JPH0742082A publication Critical patent/JPH0742082A/en
Pending legal-status Critical Current

Abstract

PURPOSE:To produce a sheet material exhibiting a visual appearance like that of a nubuck having a soft touch by. preventing a polyurethane resin from penetrating to the back surface of a base fabric and to provide its production method. CONSTITUTION:The back surface of a base fabric is impregnated with an aqueous solution containing a penetrant and the right surface is subjected to raising treatment. This base fabric is coated and impregnated with a non-yellowing type polycarbonate-based polyurethane resin and the polyurethane resin is subsequently subjected to wet coagulation treatment to obtain a sheet material. The resultant sheet material is, as necessary, subjected to embossing finish to form a rugged surface and a raising treatment is subsequently applied thereto, thus producing the objective sheet material having a nubuck-like visual appearance. As the base fabric, a fabric in which the fibers constituting the raised part have <=1 denier single yarn fineness is preferably used.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は、家具、車輌等の素材用
として用いられるヌバック調の外観を有するシート材お
よびその製造方法に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a sheet material having a nubuck-like appearance used as a material for furniture, vehicles and the like, and a method for producing the sheet material.

【0002】[0002]

【従来の技術】ヌバック調の外観を有するシート材(以
下「ヌバック調シート材」と略記することがある)とし
ては、繊維基材の表面にポリウレタン系樹脂を塗布、含
浸し、湿式凝固させて多孔質層とした後、表面のスキン
層を研削除去して微細気孔の一部を露出したものや、起
毛処理または立毛処理(以下「起毛」または「起毛処
理」と略記することがある)させた繊維基材の表面にポ
リウレタン系樹脂を塗布、含浸し、湿式凝固して多孔質
層とした後、バフィングして繊維基材の起毛部を表面に
露出させたもの等が使用されていた。
2. Description of the Related Art As a sheet material having a nubuck-like appearance (hereinafter sometimes abbreviated as "nubuck-like sheet material"), a polyurethane resin is applied and impregnated on the surface of a fiber base material and wet-solidified. After forming a porous layer, the skin layer on the surface is removed by grinding to expose some of the fine pores, or a raised or napped treatment (hereinafter sometimes abbreviated as "raised" or "raised") A polyurethane resin was applied to the surface of the fiber substrate, impregnated, wet-coagulated to form a porous layer, and then buffed to expose the raised portion of the fiber substrate on the surface.

【0003】[0003]

【発明が解決しようとする課題】しかし、上記のような
ヌバック調シート材は、繊維基材の表面にポリウレタン
系樹脂を塗布、含浸し、湿式凝固して得られるため、ポ
リウレタン系樹脂が繊維基材の裏面側にまで浸透してし
まい、風合が硬くなるという問題があった。
However, since the nubuck-like sheet material as described above is obtained by coating, impregnating, and wet coagulating a polyurethane resin on the surface of a fiber base material, the polyurethane resin is a fiber base material. There has been a problem that the material feels hard because it penetrates into the back surface of the material.

【0004】本発明は、上記の課題を解決するためにな
されたものであって、ソフトな風合を有するヌバック調
の外観を有するシート材およびその製造方法を提供する
ことをその目的とする。
The present invention has been made to solve the above problems, and an object of the present invention is to provide a sheet material having a nubuck-like appearance having a soft texture and a method for producing the sheet material.

【0005】[0005]

【課題を解決するための手段】ヌバック調の外観を有す
るシート材は、繊維基材上に、無黄変タイプのポリカー
ボネート系ポリウレタン樹脂を塗布、含浸させた後、該
ポリウレタン樹脂を湿式凝固させることにより得られる
シート材の表面を起毛処理して得られるヌバック調の外
観を有するシート材であって、繊維基材が起毛処理され
た繊維基材で、且つ裏面に浸透剤を含有する水溶液を含
浸させたものであることを特徴とする。また、本発明の
ヌバック調の外観を有するシート材の製造方法は、起毛
処理され、かつ裏面に浸透剤を含浸させた繊維基材上に
無黄変タイプのポリカーボネート系ポリウレタン樹脂を
塗布、含浸させ、非溶剤中にてポリウレタン樹脂を湿式
凝固させて得られるシート材表面に、エンボス加工によ
り凹凸を形成させた後、起毛処理を施すことを特徴とす
るものである。
A sheet material having a nubuck-like appearance is obtained by applying a non-yellowing type polycarbonate-based polyurethane resin onto a fiber base material, impregnating the same, and then wet-coagulating the polyurethane resin. A sheet material having a nubuck-like appearance obtained by raising the surface of the sheet material obtained by the above, wherein the fiber base material is a raised fiber base material, and the back surface is impregnated with an aqueous solution containing a penetrant. It is characterized by being made. Further, the method for producing a sheet material having a nubuck-like appearance according to the present invention comprises applying and impregnating a non-yellowing type polycarbonate-based polyurethane resin on a fiber base material that is raised and impregnated with a penetrant on the back surface. It is characterized in that the surface of a sheet material obtained by wet-coagulating a polyurethane resin in a non-solvent is subjected to embossing to form irregularities and then raised.

【0006】本発明に使用される繊維基材としては、単
糸繊度が1デニール以下の繊維で作られた編布、織布あ
るいはポリウレタンや合成ゴム等の弾性重合体が付与さ
れた繊維絡合不織布などである。また、繊維基材を構成
する繊維としては、例えばポリエステル、ポリアミド、
ポリアクリロニトリル、ポリオレフィン、ポリビニルア
ルコールなどの合成繊維、再生セルロース等の化学繊
維、あるいは少なくとも一成分を溶解除去したり、二成
分を分割したりすることにより極細繊維に変成された多
成分繊維等を用いることができる。
The fiber base material used in the present invention is a knitted fabric, woven fabric made of fibers having a single yarn fineness of 1 denier or less, or fiber entanglement provided with an elastic polymer such as polyurethane or synthetic rubber. For example, non-woven fabric. Further, as the fiber constituting the fiber base material, for example, polyester, polyamide,
Synthetic fibers such as polyacrylonitrile, polyolefin, polyvinyl alcohol, etc., chemical fibers such as regenerated cellulose, or multi-component fibers modified into ultrafine fibers by dissolving and removing at least one component or dividing two components be able to.

【0007】上記の繊維基材は、サンドペーパー、サン
ドクロス、サンドネット、サンドロール、針布、砥石、
ブラシなどの公知の方法で起毛処理される。このときの
起毛の長さ、密度は特に限定されないが、一般的には起
毛が短く、かつ密度が多い程好ましいヌバック調シート
材を得ることができる。
The above-mentioned fiber base material is sandpaper, sand cloth, sand net, sand roll, needle cloth, grindstone,
Raising is performed by a known method such as a brush. The length and density of the naps at this time are not particularly limited, but generally, the shorter the naps and the higher the density, the more preferable the nubuck-like sheet material can be obtained.

【0008】本発明に使用される無黄変タイプのポリカ
ーボネート系ポリウレタン樹脂は、ポリカーボネートジ
オールと無黄変型ジイソシアネート、並びに必要に応じ
て鎖伸長剤とを反応させた重合物である。
The non-yellowing type polycarbonate-based polyurethane resin used in the present invention is a polymer obtained by reacting a polycarbonate diol with a non-yellowing type diisocyanate and, if necessary, a chain extender.

【0009】上記ポリカーボネートジオールとしては、
下記化1に示す一般式で表される、ポリアルキレンポリ
カーボネートジオールであり、特に1,6−ヘキサンポ
リカーボネートジオールが好ましく使用される。
As the above polycarbonate diol,
It is a polyalkylene polycarbonate diol represented by the general formula shown in the following chemical formula 1, and 1,6-hexane polycarbonate diol is particularly preferably used.

【化1】 (式中、p,rは2以上の整数、またmは5〜200の
整数を示す) また、必要に応じて上記のポリアルキレンポリカーボネ
ートジオールの一部をポリアルキレン変性カーボネート
で置換したものであってもよい。
[Chemical 1] (In the formula, p and r are integers of 2 or more, and m is an integer of 5 to 200.) Further, if necessary, a part of the above polyalkylene polycarbonate diol is substituted with a polyalkylene modified carbonate. May be.

【0010】上記のポリカーボネートジオールの水酸基
価から求めた平均分子量は、500〜5000、好まし
くは900〜3000の範囲のものを用いる。分子量が
500未満ではウレタン基濃度が大きくなり、ポリウレ
タン樹脂の柔軟性、溶剤溶解性が低下する。また分子量
5000を越えるとウレタン基濃度が低下し、ポリウレ
タン特有の強靱性、耐摩耗性等が悪化する。
The average molecular weight determined from the hydroxyl value of the above polycarbonate diol is in the range of 500 to 5,000, preferably 900 to 3,000. If the molecular weight is less than 500, the concentration of urethane groups will increase, and the flexibility and solvent solubility of the polyurethane resin will decrease. On the other hand, if the molecular weight exceeds 5,000, the urethane group concentration decreases, and the toughness and abrasion resistance peculiar to polyurethane deteriorate.

【0011】上記の無黄変型ジイソシアネートとして
は、例えばテトラメチレンジイソシアネート、1,6−
ヘキサンジイソシアネート、2,2,4−トリメチル−
1,6−ヘキサンジイソシアネート、1−メチルシクロ
ヘキサン−2,4−ジイソシアネート、3,3’−ジメ
チル−4,4’−ジイソシアネートジシクロヘキシルメ
タン、4,4’−ジシクロヘキシルメタンジイソシアネ
ート等の脂肪族もしくは脂環族のものが使用できる。こ
れらの有機ジイソシアネートは単独で使用してもよい
し、2種以上を混合して使用してもよい。
Examples of the non-yellowing type diisocyanate include tetramethylene diisocyanate and 1,6-
Hexane diisocyanate, 2,2,4-trimethyl-
Aliphatic or alicyclic compounds such as 1,6-hexanediisocyanate, 1-methylcyclohexane-2,4-diisocyanate, 3,3'-dimethyl-4,4'-diisocyanate dicyclohexylmethane and 4,4'-dicyclohexylmethane diisocyanate Can be used. These organic diisocyanates may be used alone or in combination of two or more.

【0012】また、鎖伸長剤としては、活性水素原子を
2個以上有する化合物、例えばエチレングリコール、プ
ロピレングリコール、ブタンジオール、ヘキサンジオー
ル、3−メチル−1,5−ペンタンジオール、1,4−
シクロヘキサンジオール、キシリレングリコールなどの
ジオール類、エチレンジアミン、プロピレンジアミン、
キシリレンジアミン、イソホロジアミン、ピペラジン、
フェニレンジアミン、トリレンジアミン等のジアミン
類、ヒドラジン、アジピン酸ジヒドラジド、イソフタル
酸ジヒドラジド等のヒドラジド類等が使用できる。これ
らの鎖伸長剤は単独で使用してもよいし、2種以上を混
合物して使用してもよい。
As the chain extender, a compound having two or more active hydrogen atoms, for example, ethylene glycol, propylene glycol, butanediol, hexanediol, 3-methyl-1,5-pentanediol, 1,4-
Cyclohexanediol, diols such as xylylene glycol, ethylenediamine, propylenediamine,
Xylylenediamine, isophorodiamine, piperazine,
Diamines such as phenylenediamine and tolylenediamine, hydrazides such as hydrazine, adipic acid dihydrazide, and isophthalic acid dihydrazide can be used. These chain extenders may be used alone or in combination of two or more.

【0013】本発明の無黄変タイプポリカーボネート系
ポリウレタン樹脂は、上記のポリカーボネートジオー
ル、無黄変型ジイソシアネート、および鎖伸長剤を所望
の割合で反応させることによって得られる。また、無黄
変タイプポリカーボネート系ポリウレタン樹脂は、ジメ
チルホルムアミドの20重量%溶液としたときの粘度
が、25℃において50〜150ポイズの範囲にあるも
のを使用するのが好ましい。更に、上記ポリウレタン系
樹脂は、100%モジュラスが10〜120kg/cm
2 のものが好ましい。100%モジュラスが10kg/
cm2 未満であると、機能的強度が低下し、100%モ
ジュラスが120kg/cm2 を越えると風合が硬くな
る。
The non-yellowing type polycarbonate polyurethane resin of the present invention is obtained by reacting the above-mentioned polycarbonate diol, non-yellowing type diisocyanate and chain extender in a desired ratio. As the non-yellowing type polycarbonate-based polyurethane resin, it is preferable to use one having a viscosity of a 20 wt% solution of dimethylformamide in the range of 50 to 150 poise at 25 ° C. Further, the polyurethane resin has a 100% modulus of 10 to 120 kg / cm.
2 is preferable. 100% modulus is 10kg /
When it is less than cm 2 , the functional strength decreases, and when 100% modulus exceeds 120 kg / cm 2 , the texture becomes hard.

【0014】本発明に使用できる無黄変タイプポリカー
ボネート系ポリウレタン樹脂は、耐加水分解性、耐光
性、耐熱性等の性能を低下させない範囲であれば、上記
の無黄変タイプポリカーボネート系ポリウレタン樹脂以
外のポリウレタン樹脂との共重合体や混合物であっても
使用できる。共重合体として具体的には、ポリカプロラ
クトン−ポリカーボネート共重合ポリウレタン樹脂、炭
素数6以上のジオールとジカルボン酸との縮合によって
得られるポリエステルジオール−ポリカーボネート共重
合ポリウレタン樹脂等が挙げられ、また、無黄変タイプ
ポリカーボネート系ポリウレタン樹脂と混合できるポリ
ウレタンとしては、ポリカプロラクトン系ポリウレタン
樹脂、ポリテトラメチレングリコール系ポリウレタン樹
脂、炭素数6以上のジオールとジカルボン酸との縮合に
よって得られるポリエステル系ポリウレタン樹脂等が挙
げられる。
The non-yellowing type polycarbonate polyurethane resin which can be used in the present invention is other than the above non-yellowing type polycarbonate polyurethane resin as long as it does not deteriorate the performance such as hydrolysis resistance, light resistance and heat resistance. It is possible to use even a copolymer or a mixture with the above polyurethane resin. Specific examples of the copolymer include a polycaprolactone-polycarbonate copolymer polyurethane resin, a polyester diol-polycarbonate copolymer polyurethane resin obtained by condensation of a diol having 6 or more carbon atoms and a dicarboxylic acid, and the like. Examples of the polyurethane that can be mixed with the modified polycarbonate polyurethane resin include polycaprolactone polyurethane resin, polytetramethylene glycol polyurethane resin, and polyester polyurethane resin obtained by condensation of diol having 6 or more carbon atoms and dicarboxylic acid. .

【0015】上記の無黄変タイプポリカーボネート系ポ
リウレタン樹脂は、必要に応じて凝固調節剤(界面活性
剤)、着色剤、充填剤、酸化防止剤、撥水、撥油剤等の
各種添加剤を混入し、ジメチルホルムアミド、ジメチル
アセトアミド、N−メチルピロリドン、ジメチルスルホ
キシド等の溶剤によって適宜の濃度のポリウレタン樹脂
溶液とされる。このときのポリウレタン樹脂含有割合
は、目的、用途によって異なるので一概には規定するこ
とができないが、一般には繊維基材に対し2〜30重量
%とされる。また、無黄変タイプポリカーボネート系ポ
リウレタン樹脂溶液には、必要に応じてコラーゲン粉末
等を添加してもよい。
The yellowing-free type polycarbonate polyurethane resin described above may be mixed with various additives such as a coagulation regulator (surfactant), a colorant, a filler, an antioxidant, a water repellent, and an oil repellent, if necessary. Then, a polyurethane resin solution having an appropriate concentration is prepared using a solvent such as dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and dimethylsulfoxide. The polyurethane resin content at this time cannot be unconditionally specified because it depends on the purpose and application, but is generally 2 to 30% by weight based on the fiber base material. Further, collagen powder or the like may be added to the non-yellowing type polycarbonate-based polyurethane resin solution, if necessary.

【0016】本発明に使用される浸透剤としては、エア
ロゾルOH型(すなわちスルホコハク酸ジ−2−エチル
ヘキシルエステルナトリウム塩)、ドデシルベンゼンス
ルホン酸ナトリウム、ラウリル硫酸エステルナトリウ
ム、オレイン酸ブチルエステル硫酸化物、アルキルナフ
タレンスルホン酸ナトリウム等のアニオン系、ノニルフ
ェノールエチレンオキサイド付加物、オクチルフェノー
ルエチレンオキサイド付加物、中級〜高級アルコールエ
チレンオキサイド付加物などがの非イオン系等が使用で
きる。
The penetrant used in the present invention includes aerosol OH type (ie, sodium salt of di-2-ethylhexyl sulfosuccinate), sodium dodecylbenzenesulfonate, sodium lauryl sulfate ester, butyl oleate sulfate ester, and alkyl ester. Anionic systems such as sodium naphthalene sulfonate, nonylphenol ethylene oxide adducts, octylphenol ethylene oxide adducts, non-ionic systems such as intermediate to higher alcohol ethylene oxide adducts and the like can be used.

【0017】上記の浸透剤は、0.1〜5%程度の水溶
液として上記の繊維基材の裏面に含浸される。このとき
の浸透剤水溶液の繊維基材に対する付着量としては、5
〜30重量%程度である。また、繊維基材の裏面への浸
透剤水溶液付与方法としては、スプレー法、メッシュロ
ールによるバックサイジング法等の公知の方法が採用さ
れ、特に限定はされない。
The penetrant is impregnated into the back surface of the fiber base material as an aqueous solution of about 0.1 to 5%. At this time, the amount of the penetrating agent aqueous solution attached to the fiber base material is 5
It is about 30% by weight. Further, as a method for applying the penetrant aqueous solution to the back surface of the fiber base material, a known method such as a spray method or a backsizing method using a mesh roll is adopted and is not particularly limited.

【0018】上記のポリカーボネート系ポリウレタン樹
脂溶液は、裏面に浸透剤水溶液を含浸させた繊維基材上
にドクターナイフ等の手段により塗布され、しかる後、
塗布部を水や前記ポリウレタン樹脂の溶剤の水溶液等の
非溶剤中に浸漬し、ポリウレタン系樹脂を凝固、脱溶媒
し、次いで水洗、乾燥してシート状物を得る。このとき
使用される非溶剤としては、ジメチルホルムアミドの0
〜20%水溶液が特に好ましい。また、ポリカーボネー
ト系ポリウレタン樹脂の凝固温度は、15〜40℃の範
囲で適宜選択すればよい。
The above-mentioned polycarbonate-based polyurethane resin solution is applied by a means such as a doctor knife onto a fiber substrate whose back surface is impregnated with an aqueous penetrant solution, and thereafter,
The coated part is immersed in water or a non-solvent such as an aqueous solution of the above-mentioned polyurethane resin solvent to coagulate and desolvate the polyurethane resin, then washed with water and dried to obtain a sheet. The non-solvent used at this time is 0 of dimethylformamide.
A ~ 20% aqueous solution is especially preferred. Further, the solidification temperature of the polycarbonate-based polyurethane resin may be appropriately selected within the range of 15 to 40 ° C.

【0019】ポリカーボネート系ポリウレタン樹脂層を
形成されたシート状物は、必要に応じて型押しロール等
によりエンボス加工を施し、表面に凹凸を付与された
後、起毛処理される。このときの起毛処理の方法として
は、前記した繊維基材の起毛処理方法と同様の方法で処
理することができるが、あまり強い条件ではなく、研削
作用の緩やかなサンドペーパーやブラシ等を用いて軽く
起毛処理するのが好ましい。
The sheet-like material on which the polycarbonate-based polyurethane resin layer is formed is embossed with a embossing roll or the like, if necessary, to have irregularities on the surface, and then raised. As a method for raising hair at this time, the same method as the above-described raising method for fiber base material can be used, but not so strong conditions, using sandpaper or a brush having a gentle grinding action. It is preferable to lightly brush the hair.

【0020】また、表面全体を均一に起毛処理せずに、
繊維起毛部を繊維起毛の殆どない部分とが混在した表
面、即ち、繊維起毛部と非繊維起毛部が明確に区分けさ
れておらず混然一体となって混じり合っている状態とす
ると、より天然皮革に類似したヌバック調シートを得る
ことができる。また、本発明のヌバック調シートは、上
記の工程の任意の段階において、通常の染色処理、揉み
処理を施すこともできる。
Further, without uniformly raising the entire surface,
If the fiber-raised part is a surface in which almost no fiber-raised part is mixed, that is, the fiber-raised part and the non-fiber-raised part are not clearly separated and are mixed together as a unit, they are more natural. A nubuck-like sheet similar to leather can be obtained. Further, the nubuck tone sheet of the present invention can be subjected to usual dyeing treatment and rubbing treatment at any stage of the above steps.

【0021】[0021]

【作用】本発明で得られるヌバック調シートは、繊維基
材の裏面に浸透剤水溶液を含浸させてなるので、ポリカ
ーボネート系ポリウレタン樹脂が繊維裏面側まで染み込
むのを防止するため、その結果として、風合の柔らかい
ヌバック調シートを得ることができる。また、繊維基材
の裏面側にポリウレタン樹脂が染み出すことがないの
で、得られたヌバック調シートの裏面側の美観も向上す
る。
The nubuck-like sheet obtained by the present invention has the back surface of the fiber base material impregnated with the penetrant aqueous solution, so that the polycarbonate polyurethane resin is prevented from seeping into the back surface side of the fiber. It is possible to obtain a soft nubuck-like sheet. Further, since the polyurethane resin does not seep out to the back surface side of the fiber base material, the appearance of the back surface side of the obtained nubuck tone sheet is improved.

【0022】[0022]

【実施例】以下に具体的な実施例を挙げ、本発明を更に
詳細に説明する。
EXAMPLES The present invention will be described in more detail with reference to specific examples.

【0023】・実施例1 フロントに単糸繊度が0.4デニールのハイマルチフィ
ラメントからなるポリエステル繊維、ミドルおよびバッ
クに単糸繊度が2デニールのマルチフィラメントからな
るポリエステル繊維とを縦編みに編成し、グレーに染色
した厚さ0.75mmの片面起毛を有する繊維基材の裏
面に、ドデシルベンゼンスルホン酸ナトリウムを0.5
重量%含有する水溶液を、60メッシュのメッシュロー
ルを用いて含浸させた後、繊維基材の起毛面上にナイフ
コーターにて表1に示す組成からなる無黄変タイプのポ
リカーボネート系ポリウレタン樹脂溶液を、ポリウレタ
ン固形分が30g/m2 (ポリウレタン付着量は、繊維
基材に対し約10.3%)となるように塗布し、次い
で、該繊維基材をジメチルホルムアミド13%水溶液
(液温20℃)中に浸漬して、ポリウレタン系樹脂を凝
固させた後、60℃の温水中で脱溶媒、洗浄し、乾燥し
て表面にポリウレタン系樹脂層を有するシート状物を得
た。得られたシート状物は、厚さ0.85mmで、ポリ
ウレタン系樹脂の裏抜け、染みだしもなく、風合もソフ
トで柔軟性に優れるものであった。
Example 1 A polyester fiber made of high multifilament having a single yarn fineness of 0.4 denier in the front and a polyester fiber made of multifilament having a single yarn fineness of 2 denier in the middle and back are knitted in a warp knit. 0.5% sodium dodecylbenzenesulfonate on the back side of the fiber substrate having a 0.75 mm thick single-sided brush dyed gray
After impregnating the aqueous solution containing 60% by weight with a 60-mesh mesh roll, a non-yellowing type polycarbonate-based polyurethane resin solution having the composition shown in Table 1 was formed on the raised surface of the fiber substrate with a knife coater. , Polyurethane solid content was 30 g / m 2 (polyurethane adhesion amount was about 10.3% with respect to the fiber substrate), and then the fiber substrate was coated with a 13% dimethylformamide aqueous solution (liquid temperature 20 ° C.). ), To solidify the polyurethane resin, and then to remove the solvent in warm water at 60 ° C., wash and dry to obtain a sheet-like product having a polyurethane resin layer on the surface. The obtained sheet-like material had a thickness of 0.85 mm, had no strike-through or exudation of the polyurethane resin, had a soft texture, and had excellent flexibility.

【0024】[0024]

【表1】 レザミン CNU650−20*1 100重量部 ジメチルホルムアミド 65重量部 着色剤 15重量部 凝固調節剤 2重量部 *1 大日精化社製(NV20%、100%モジュラス
60kg/m2
[Table 1] Resamine CNU650-20 * 1 100 parts by weight Dimethylformamide 65 parts by weight Colorant 15 parts by weight Coagulation regulator 2 parts by weight * 1 Dainichiseika Co., Ltd. (NV 20%, 100% modulus 60 kg / m 2 )

【0025】得られたシート状物の表面に、皮絞模様の
エンボスロールにて加熱加圧エンボス加工を行った後、
表面を240メッシュのサンドペーパーにて軽くバフィ
ングすることにより、厚さ0.65mmのヌバック調シ
ートを得た。得られたヌバック調シートは、風合がソフ
トで、柔軟性に優れ、しっとりとした触感と天然皮革に
類似のスムースで自然なタッチを有し、且つ天然皮革の
ヌバックの外観、タッチに非常に近似したものであっ
た。また、得られたヌバック調シートは、耐加水分解
性、耐光性、耐熱性に優れ、家具や車輌用のシートとし
て好適なものであった。
The surface of the obtained sheet-like material is subjected to heat and pressure embossing with an embossing roll having a leather pattern,
The surface was lightly buffed with a 240 mesh sandpaper to obtain a nubuck-like sheet having a thickness of 0.65 mm. The obtained nubuck-like sheet has a soft texture, excellent flexibility, a moist feel and a smooth and natural touch similar to natural leather, and the nubuck appearance and touch of natural leather is very high. It was an approximation. Further, the obtained nubuck-like sheet was excellent in hydrolysis resistance, light resistance and heat resistance, and was suitable as a sheet for furniture and vehicles.

【0026】・実施例2 フロントに単糸繊度が0.6デニールのマルチフィラメ
ントからなるポリエステル繊維、ミドルおよびバックに
単糸繊度が2デニールのマルチフィラメントからなるポ
リエステル繊維とを縦編みに編成し、茶色に染色した厚
さ0.85mmの片面起毛を有する繊維基材の裏面に、
スルホコハク酸ジ−2−エチルヘキシルエステルナトリ
ウムを1.0重量%含有する水溶液を、60メッシュの
メッシュロールを用いて含浸させた後、繊維基材の起毛
面上にナイフコーターにて表2に示す組成からなる無黄
変タイプのポリカーボネート系ポリウレタン樹脂溶液
を、ポリウレタン固形分が40g/m2 (ポリウレタン
付着量は、繊維基材に対し約12.9%)となるように
塗布し、次いで、該繊維基材をジメチルホルムアミド1
3%水溶液(液温20℃)中に浸漬して、ポリウレタン
系樹脂を凝固させた後、60℃の温水中で脱溶媒、洗浄
し、乾燥して表面にポリウレタン系樹脂層を有するシー
ト状物を得た。得られたシート状物は、厚さ0.9mm
で、ポリウレタン系樹脂の裏抜け、染みだしもなく、風
合もソフトで柔軟性に優れるものであった。
Example 2 A polyester fiber composed of a multifilament having a single yarn fineness of 0.6 denier in the front and a polyester fiber composed of a multifilament having a single yarn fineness of 2 denier in the middle and the back are knitted in a warp knit, On the back surface of the fiber substrate having a 0.85 mm thick single-sided brush dyed brown,
An aqueous solution containing 1.0% by weight of sodium di-2-ethylhexyl sulfosuccinate was impregnated with a mesh roll of 60 mesh, and then the composition shown in Table 2 with a knife coater on the raised surface of the fiber base material. A non-yellowing type polycarbonate-based polyurethane resin solution consisting of the above is applied so that the polyurethane solid content is 40 g / m 2 (the polyurethane adhesion amount is about 12.9% with respect to the fiber base material), and then the fiber is applied. Base material is dimethylformamide 1
A sheet material having a polyurethane resin layer on the surface after being immersed in a 3% aqueous solution (liquid temperature 20 ° C.) to solidify the polyurethane resin, desolvated in warm water at 60 ° C., washed and dried. Got The obtained sheet material has a thickness of 0.9 mm.
There was no strike-through or bleeding out of the polyurethane resin, the texture was soft and the flexibility was excellent.

【0027】[0027]

【表2】 クリスボン MP−303*2 100重量部 ジメチルホルムアミド 60重量部 着色剤 15重量部 凝固調節剤 2重量部 *2 大日本インキ社製(NV20%、100%モジュ
ラス45kg/m2
[Table 2] Crisbon MP-303 * 2 100 parts by weight Dimethylformamide 60 parts by weight Colorant 15 parts by weight Coagulation regulator 2 parts by weight * 2 Manufactured by Dainippon Ink and Chemicals (NV 20%, 100% modulus 45 kg / m 2 )

【0028】得られたシート状物の表面に、毛穴絞模様
のエンボスロールにて加熱加圧エンボス加工を行った
後、表面を240メッシュのサンドペーパーにて軽くバ
フィングすることにより、厚さ0.65mmのヌバック
調シートを得た。得られたヌバック調シートは、風合が
ソフトで、柔軟性に優れ、しっとりとした触感と天然皮
革に類似のスムースで自然なタッチを有し、且つ天然皮
革のヌバックの外観、タッチに非常に近似したものであ
った。また、得られたヌバック調シートは、耐加水分解
性、耐光性、耐熱性に優れ、家具や車輌用のシート材と
して好適なものであった。
The surface of the obtained sheet-like material was subjected to heat and pressure embossing with an embossing roll having a pore-drawing pattern, and then the surface was lightly buffed with 240 mesh sandpaper to obtain a thickness of 0. A 65 mm nubuck-like sheet was obtained. The obtained nubuck-like sheet has a soft texture, excellent flexibility, a moist feel and a smooth and natural touch similar to natural leather, and the nubuck appearance and touch of natural leather is very high. It was an approximation. The obtained nubuck-like sheet was excellent in hydrolysis resistance, light resistance, and heat resistance, and was suitable as a sheet material for furniture and vehicles.

【0029】・比較例1 ドデシルベンゼンスルホン酸ナトリウム水溶液を含浸さ
せない以外は、実施例1と同様にしてヌバック調シート
を得た。得られたシート材は基材の裏面全面にポリウレ
タン系樹脂が裏抜け、染みだしがあり、風合が硬く、柔
軟性に劣るものであった。
Comparative Example 1 A nubuck tone sheet was obtained in the same manner as in Example 1 except that the aqueous sodium dodecylbenzenesulfonate solution was not impregnated. The obtained sheet material had a polyurethane resin through the entire back surface of the substrate, had bleeding, had a hard texture, and was inferior in flexibility.

【0030】・比較例2 スルホコハク酸ジ−2−エチルヘキシルエステルナトリ
ウム水溶液を含浸させない以外は、実施例1と同様にし
てヌバック調シートを得た。得られたシート材は基材の
裏面全面にポリウレタン系樹脂が裏抜け、染みだしがあ
り、風合が硬く、柔軟性に劣るものであった。
Comparative Example 2 A nubuck tone sheet was obtained in the same manner as in Example 1 except that the aqueous sodium di-2-ethylhexyl sulfosuccinate solution was not impregnated. The obtained sheet material had a polyurethane resin through the entire back surface of the substrate, had bleeding, had a hard texture, and was inferior in flexibility.

【0031】・比較例3 ドデシルベンゼンスルホン酸ナトリウム含有しない水を
含浸させる以外は、実施例1と同様にしてヌバック調シ
ートを得た。得られたシート材は基材の裏面全面にポリ
ウレタン系樹脂が裏抜け、染みだしがあり、風合が硬
く、柔軟性に劣るものであった。
Comparative Example 3 A nubuck tone sheet was obtained in the same manner as in Example 1 except that water containing no sodium dodecylbenzenesulfonate was impregnated. The obtained sheet material had a polyurethane resin through the entire back surface of the substrate, had bleeding, had a hard texture, and was inferior in flexibility.

【0032】[0032]

【発明の効果】本発明で得られるヌバック調シートは、
風合の柔らかく、柔軟性に優れたものであって、繊維基
材の裏面側にポリウレタン系樹脂が染み出すことがない
美観に優れるものである。また、ポリウレタン系樹脂と
して無黄変タイプのポリカーボネート系ポリウレタン樹
脂を用いているので、耐加水分解性、耐光性、耐熱性に
優れ、家具や車輌用のシート材として好適に使用するこ
とができる。
The nubuck-like sheet obtained by the present invention is
It is soft to the touch and excellent in flexibility, and has an excellent aesthetic appearance in which the polyurethane resin does not seep out to the back surface side of the fiber base material. Further, since a non-yellowing type polycarbonate-based polyurethane resin is used as the polyurethane-based resin, it has excellent hydrolysis resistance, light resistance, and heat resistance, and can be suitably used as a seat material for furniture and vehicles.

Claims (4)

【特許請求の範囲】[Claims] 【請求項1】 繊維基材上に、無黄変タイプのポリカー
ボネート系ポリウレタン樹脂を塗布、含浸させた後、該
ポリウレタン樹脂を湿式凝固させることにより得られる
シート材の表面を起毛処理して得られるヌバック調の外
観を有するシート材であって、繊維基材が起毛処理され
た繊維基材で、且つ裏面に浸透剤を含有する水溶液を含
浸させたものであることを特徴とするヌバック調の外観
を有するシート材。
1. A non-yellowing type polycarbonate-based polyurethane resin is applied and impregnated on a fiber base material, and the surface of a sheet material obtained by wet coagulating the polyurethane resin is napped. A sheet material having a nubuck-like appearance, wherein the fibrous base material is a raised fibrous base material, and the back surface is impregnated with an aqueous solution containing a penetrant. Sheet material having.
【請求項2】 起毛処理を施された繊維基材の起毛部を
構成する繊維の繊度が、1デニール以下であることを特
徴とする請求項1記載のヌバック調の外観を有するシー
ト材。
2. The sheet material having a nubuck-like appearance according to claim 1, wherein the fiber constituting the raised portion of the fiber base material subjected to the raising treatment has a fineness of 1 denier or less.
【請求項3】 無黄変タイプのポリカーボネート系ポリ
ウレタン樹脂層の表面に起毛処理を施す前に、エンボス
加工によって表面凹凸を形成したことを特徴とする請求
項1記載のヌバック調外観を有するシート材。
3. A sheet material having a nubuck-like appearance according to claim 1, wherein surface irregularities are formed by embossing before the surface of the non-yellowing type polycarbonate-based polyurethane resin layer is raised. .
【請求項4】 起毛処理され、かつ裏面に浸透剤を含浸
させた繊維基材上に無黄変タイプのポリカーボネート系
ポリウレタン樹脂を塗布、含浸させ、非溶剤中にて無黄
変タイプのポリカーボネート系ポリウレタン樹脂を湿式
凝固させて得られるシート材表面に、エンボス加工によ
り凹凸を形成させた後、起毛処理を施すことを特徴とす
るヌバック調の外観を有するシート材の製造方法。
4. A non-yellowing type polycarbonate type resin is applied and impregnated on a fiber substrate which has been raised and has a back surface impregnated with a penetrant, which is impregnated and impregnated in a non-solvent. A method for producing a sheet material having a nubuck-like appearance, which comprises subjecting a surface of a sheet material obtained by wet-coagulating a polyurethane resin to embossing to form irregularities, and then performing a raising treatment.
JP20467593A 1993-07-27 1993-07-27 Sheet material having nubuck-like visual appearance and its production Pending JPH0742082A (en)