JPH0578634A - Rubber based pressure-sensitive adhesive and adhesive sheets therefrom - Google Patents

Rubber based pressure-sensitive adhesive and adhesive sheets therefrom

Info

Publication number
JPH0578634A
JPH0578634A JP3269007A JP26900791A JPH0578634A JP H0578634 A JPH0578634 A JP H0578634A JP 3269007 A JP3269007 A JP 3269007A JP 26900791 A JP26900791 A JP 26900791A JP H0578634 A JPH0578634 A JP H0578634A
Authority
JP
Japan
Prior art keywords
rubber
adhesive
parts
weight
molecular weight
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP3269007A
Other languages
Japanese (ja)
Other versions
JP3145742B2 (en
Inventor
Hirohito Onishi
啓仁 大西
Michio Umeda
道夫 梅田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nitto Denko Corp
Original Assignee
Nitto Denko Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nitto Denko Corp filed Critical Nitto Denko Corp
Priority to JP26900791A priority Critical patent/JP3145742B2/en
Publication of JPH0578634A publication Critical patent/JPH0578634A/en
Application granted granted Critical
Publication of JP3145742B2 publication Critical patent/JP3145742B2/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Abstract

PURPOSE:To obtain the subject adhesive consisting of specific ratio of each specific polyisobutylene, etc., rubber and tackiness-providing agent, etc., having prescribed gel fraction and having excellent adhesion strength without carrying out buffing or primer coating, and suitable as automotive members, etc. CONSTITUTION:The objective adhesive consisting essentially of (A) 100 pts.wt. polyisobutylene, butyl rubber or halogenated butyl rubber having 200000-1500000 weight-average molecular weight, (B) 30-300 pts.wt. liquid is semi-liquid rubber having < 10000-50000 weight-average molecular weight and (C) 30-300 pts.wt. tackiness-providing agent or/and softening agent having < 100000 weight-average molecular weight, and being 10-40% in gel fraction. Furthermore, layers of the adhesive are provided on both faces of a substrate to provide the adhesive sheets.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は、天然ゴム、クロロプレ
ンゴム、EPT(エチレン−プロピレンタ―ポリマ―)
ゴムなどからなる加硫ゴム成形品を接着するために用い
るゴム系感圧性接着剤とその接着シ―ト類に関する。
The present invention relates to natural rubber, chloroprene rubber, EPT (ethylene-propylene terpolymer).
The present invention relates to a rubber-based pressure-sensitive adhesive used for adhering a vulcanized rubber molded product made of rubber or the like and its adhesive sheets.

【0002】[0002]

【従来の技術】この種の加硫ゴム成形品は、自動車用部
材、家電、OA機器用部材のほか、各種の工業用製品と
して多用されている。
2. Description of the Related Art Vulcanized rubber moldings of this type are widely used as automobile parts, home electric appliances, OA equipment parts, and various industrial products.

【0003】しかし、これらのゴム成形品は、配合物と
して各種の充てん剤、加硫剤、油成分などの接着阻害物
質を数多く含み、かつゴム成形品を加硫する工程でプレ
ス金型からの型離れを良くするためにシリコ―ンオイル
などの離型剤を用いているため、成形品表面の接着性に
劣つている。
However, these rubber molded products contain a large number of various adhesion-inhibiting substances such as various fillers, vulcanizing agents, oil components, etc. as a compounded product, and in the process of vulcanizing the rubber molded product, they are molded from a press mold. Since a mold release agent such as silicone oil is used to improve the mold release, the adhesiveness of the surface of the molded product is poor.

【0004】しかも、これらの加硫ゴム成形品は、高い
弾性を有するため、これを曲面に貼り付ける場合などで
は、上記の弾性作用によつて応力が加えられた状態で接
着固定されることになり、これと前記成形品表面の接着
性の悪さから、接着固定後簡単に剥がれてしまう問題が
あつた。
Moreover, since these vulcanized rubber molded products have high elasticity, when they are attached to a curved surface, they are bonded and fixed in a state in which stress is applied by the elastic action. However, due to this and the poor adhesiveness of the surface of the molded product, there is a problem that the molded product is easily peeled off after being bonded and fixed.

【0005】このため、従来では、加硫ゴム成形品の被
着面を、まずバフ研磨し、ついで溶剤洗浄、プライマ―
塗布を施し、この上に感圧性の接着シ―ト類を貼り合わ
せて、他の被着体に接着固定するといつた方法がとられ
ていた。
For this reason, conventionally, the adhered surface of a vulcanized rubber molded product is first buffed, then solvent washed and primer-coated.
It has been a common practice to apply a coating, attach pressure-sensitive adhesive sheets to this, and fix it to another adherend.

【0006】[0006]

【発明が解決しようとする課題】しかるに、上記のバフ
研磨やプライマ―塗布などの処理は、工数がかさむうえ
に、バフ粉や溶剤が飛散して作業環境を悪化するおそれ
があり、またバフ研磨工程では、バフ加工の程度にばら
つきが生じやすく、これに伴い接着強度にもばらつきを
生じさせる問題があつた。
However, the above-mentioned treatments such as buffing and primer coating require a lot of man-hours, and buffing powder and solvent may scatter to deteriorate the working environment. In the process, there is a problem that the degree of buffing tends to vary, and the adhesive strength also varies accordingly.

【0007】本発明は、上記の事情に鑑み、加硫ゴム成
形品に対し、従来のようなバフ研磨やプライマ―塗布な
どの処理を施さなくとも、十分な接着強度を得ることの
できるゴム系感圧性接着剤とその接着シ―ト類を提供す
ることを目的としている。
In view of the above circumstances, the present invention is a rubber system capable of obtaining a sufficient adhesive strength without subjecting a vulcanized rubber molded product to conventional treatments such as buffing and primer coating. It is intended to provide a pressure sensitive adhesive and its adhesive sheet.

【0008】[0008]

【課題を解決するための手段】本発明者らは、上記の目
的を達成するために鋭意検討した結果、接着剤の必須成
分として、ゴム質ポリマ―をはじめとする特定分子量の
ポリマ―成分や粘着付与剤などを3種組み合わせ使用す
るとともに、これら成分を含む接着剤全体のゲル分率を
特定の範囲に設定することにより、加硫ゴム成形品を、
従来のようなバフ研磨やプライマ―塗布などの処理を施
すことなく、十分に接着できるものであることを知り、
本発明を完成するに至つた。
Means for Solving the Problems As a result of intensive studies to achieve the above object, the present inventors have found that as an essential component of an adhesive, a polymer component having a specific molecular weight such as a rubbery polymer or By using a combination of three types of tackifiers and setting the gel fraction of the entire adhesive containing these components within a specific range, a vulcanized rubber molded product can be obtained.
Knowing that it can be fully adhered without the need for conventional buffing or primer coating,
The present invention has been completed.

【0009】すなわち、本発明は、つぎのa〜c三成
分; a)重量平均分子量が20万〜150万のポリイソブチ
レン、ブチルゴムまたはハロゲン化ブチルゴム100重
量部 b)重量平均分子量が1万〜15万の液状ないし半液状
のゴム30〜300重量部 c)重量平均分子量が1万未満の粘着付与剤または/お
よび軟化剤30〜300重量部 を必須成分として含有するとともに、ゲル分率が10〜
40%の範囲にあることを特徴とするゴム系感圧性接着
剤に係るものである。また、本発明は、このゴム系感圧
性接着剤の層を基材の一面または両面に設けて、シ―ト
状やテ―プ状などの形態とした接着シ―ト類に係るもの
である。
That is, the present invention comprises the following three components a to c: a) 100 parts by weight of polyisobutylene, butyl rubber or halogenated butyl rubber having a weight average molecular weight of 200,000 to 1.5 million b) a weight average molecular weight of 10,000 to 15 30 to 300 parts by weight of liquid or semi-liquid rubber c) Contains 30 to 300 parts by weight of a tackifier or / and a softening agent having a weight average molecular weight of less than 10,000 as an essential component and a gel fraction of 10 to 10
The present invention relates to a rubber-based pressure-sensitive adhesive characterized by being in a range of 40%. The present invention also relates to an adhesive sheet in which a layer of the rubber-based pressure-sensitive adhesive is provided on one surface or both surfaces of a base material to form a sheet shape or a tape shape. ..

【0010】[0010]

【発明の構成・作用】本発明におけるa成分のゴム質ポ
リマ―は、加硫ゴム成形品との親和性が高く、表面層の
接着阻害物質を排除して選択的な濡れ性を発揮するポリ
マ―として、イソブチレンの単独重合体であるポリイソ
ブチレン、イソブチレンと1〜3重量%のイソプレンと
の共重合体であるブチルゴム、このブチルゴムを臭素化
または塩素化したハロゲン化ブチルゴムのいずれかがが
用いられる。
The rubber polymer of the component a in the present invention has a high affinity for a vulcanized rubber molded product and is a polymer which exhibits a selective wettability by eliminating the adhesion-inhibiting substance in the surface layer. As-, any one of polyisobutylene which is a homopolymer of isobutylene, butyl rubber which is a copolymer of isobutylene and 1 to 3% by weight of isoprene, and halogenated butyl rubber obtained by brominated or chlorinated this butyl rubber is used. ..

【0011】このゴム質ポリマ―の分子量は、重量平均
分子量で20万〜150万の範囲にあることが必要で、
特に好適には30万〜100万の範囲にあるのがよい。
20万より小さくなると、接着剤の凝集力が十分に得ら
れず、加硫ゴム成形品を曲面に貼り付ける場合などで
は、接着固定後に剥がれやすい。逆に、150万より大
きくなると、接着剤の凝集力が高くなりすぎて、加硫ゴ
ム成形品との濡れが十分に得られ難い。
The molecular weight of this rubbery polymer is required to be in the range of 200,000 to 1,500,000 in terms of weight average molecular weight,
Particularly preferably, it is in the range of 300,000 to 1,000,000.
When it is less than 200,000, the cohesive force of the adhesive cannot be sufficiently obtained, and when the vulcanized rubber molded product is attached to a curved surface, the adhesive is likely to be peeled off after being bonded and fixed. On the other hand, when it is more than 1.5 million, the cohesive force of the adhesive becomes too high, and it is difficult to obtain sufficient wetting with the vulcanized rubber molded product.

【0012】本発明におけるb成分の液状ないし半液状
のゴムとしては、たとえば、ポリイソブチレン、ポリブ
テン、エチレンプロピレンゴムなどが挙げられ、これら
の中でも、特にポリイソブチレンが最も好ましく用いら
れる。このb成分は、a成分のゴム質ポリマ―と良好に
相溶しこのポリマ―を適度に可塑化して、加硫ゴム成形
品に対する濡れ性を高めるためのものである。
Examples of the liquid or semi-liquid rubber of the component b in the present invention include polyisobutylene, polybutene, ethylene propylene rubber and the like. Among these, polyisobutylene is most preferably used. The component b is well compatible with the rubbery polymer of the component a and appropriately plasticizes the polymer to improve the wettability of the vulcanized rubber molded article.

【0013】なお、上記の液状ないし半液状とは、常温
(25℃)での状態を意味し、また半液状とは、非常に
ゆつくりではあるが、流動現象を示すような状態にある
ことを意味する。
The above-mentioned liquid or semi-liquid means a state at room temperature (25 ° C.), and semi-liquid means a state in which a fluid phenomenon is exhibited although it is very loose. Means

【0014】このような液状ないし半液状のゴムの分子
量は、重量平均分子量で1万〜15万の範囲にあること
が必要で、特に好適には2万〜12万の範囲にあるのが
よい。1万より小さくなると、接着剤の凝集力が十分に
得られず、加硫ゴム成形品を曲面に貼り付ける場合など
では、接着固定後に剥がれやすい。逆に、15万より大
きくなると、十分な可塑化効果が得られず、接着剤の凝
集力が高くなりすぎて、加硫ゴム成形品との濡れが十分
に得られ難い。
The molecular weight of such liquid or semi-liquid rubber is required to be in the range of 10,000 to 150,000 in terms of weight average molecular weight, and particularly preferably in the range of 20,000 to 120,000. .. If it is less than 10,000, the cohesive force of the adhesive cannot be sufficiently obtained, and in the case where a vulcanized rubber molded product is attached to a curved surface, the adhesive tends to be peeled off after adhesion and fixation. On the other hand, if it is more than 150,000, a sufficient plasticizing effect cannot be obtained, and the cohesive force of the adhesive becomes too high, so that it is difficult to obtain sufficient wetting with the vulcanized rubber molded product.

【0015】このb成分の液状ないし半液状のゴムの使
用量は、a成分のゴム質ポリマ―100重量部に対し、
30〜300重量部の範囲とすることが必要で、特に好
適には50〜150重量部の範囲とするのがよい。30
重量部より少ないと、十分な可塑化効果が得られず、接
着剤の凝集力が高くなりすぎて、加硫ゴム成形品との濡
れが十分に得られ難い。逆に、300重量部より多くな
ると、接着剤の凝集力が十分に得られず、加硫ゴム成形
品を曲面に貼り付ける場合などでは、接着固定後に剥が
れやすい。
The amount of the liquid or semi-liquid rubber of component b used is 100 parts by weight of the rubbery polymer of component a.
The amount is required to be in the range of 30 to 300 parts by weight, particularly preferably 50 to 150 parts by weight. Thirty
If the amount is less than the weight part, a sufficient plasticizing effect cannot be obtained, and the cohesive force of the adhesive becomes too high, and it is difficult to obtain sufficient wetting with the vulcanized rubber molded product. On the other hand, if the amount is more than 300 parts by weight, the cohesive force of the adhesive cannot be sufficiently obtained, and in the case where a vulcanized rubber molded product is attached to a curved surface, the adhesive is likely to be peeled off after the adhesive fixing.

【0016】本発明におけるc成分のひとつである粘着
付与剤としては、テルペン系樹脂、テルペン−フエノ―
ル系樹脂、石油系樹脂、スチレン系樹脂、クマロン−イ
ンデン樹脂、キシレン系樹脂、フエノ―ル系樹脂などの
室温で固形の粘着付与剤のほか、室温で液状の各種の粘
着付与剤を使用できる。また、c成分の他のひとつであ
る軟化剤としては、プロセスオイル、ポリエステル系可
塑剤、ポリブテンなどの低分子量の液状ゴムが挙げられ
る。
As the tackifier which is one of the component c in the present invention, a terpene resin, terpene-pheno-
In addition to solid tackifiers that are solid at room temperature, such as resin, petroleum resin, styrene resin, coumarone-indene resin, xylene resin, and phenol resin, various liquid tackifiers at room temperature can be used. .. Further, as the softening agent which is another one of the component c, a low molecular weight liquid rubber such as a process oil, a polyester type plasticizer and polybutene can be mentioned.

【0017】これらc成分の分子量は、重量平均分子量
で1万未満であることが必要で、特に好適には200〜
5,000であるのがよい。1万以上となると、接着剤
の凝集力が高くなりすぎて、加硫ゴム成形品との濡れが
十分に得られ難い。
The molecular weight of these c components is required to be less than 10,000 in terms of weight average molecular weight, and particularly preferably 200 to
It should be 5,000. If it is 10,000 or more, the cohesive force of the adhesive becomes too high, and it is difficult to obtain sufficient wetting with the vulcanized rubber molded product.

【0018】このようなc成分としての粘着付与剤また
は/および軟化剤の使用量は、a成分のゴム質ポリマ―
100重量部あたり、30〜300重量部の範囲とする
ことが必要で、特に好適には40〜150重量部の範囲
とするのがよい。30重量部より少ないと、接着剤の凝
集力が高くなりすぎて、加硫ゴム成形品との濡れが十分
に得られ難い。逆に、300重量部より多くなると、接
着剤の凝集力が十分に得られず、加硫ゴム成形品を曲面
に貼り付ける場合などでは、接着固定後に剥がれやす
い。
The amount of the tackifier or / and the softening agent used as the component c is such that the rubber polymer of the component a is used.
It is necessary to set the range of 30 to 300 parts by weight per 100 parts by weight, and it is particularly preferable to set the range of 40 to 150 parts by weight. If the amount is less than 30 parts by weight, the cohesive force of the adhesive becomes too high, and it is difficult to obtain sufficient wetting with the vulcanized rubber molded product. On the other hand, if the amount is more than 300 parts by weight, the cohesive force of the adhesive cannot be sufficiently obtained, and in the case where a vulcanized rubber molded product is attached to a curved surface, the adhesive is likely to be peeled off after the adhesive fixing.

【0019】本発明においては、上記のa〜c三成分の
ほかに、他のポリマ―成分や架橋剤を使用でき、また一
般の感圧性接着剤に用いられている各種の配合剤、たと
えば、酸化防止剤、紫外線吸収剤、充てん剤、顔料、増
量剤などを使用することもできる。ただし、これら任意
成分の使用量は、a成分のゴム質ポリマ―100重量部
あたり、100重量部以下とすることが必要で、特に好
適には80重量部以下の範囲とするのがよい。100重
量部を超えてしまうと、ゴム系感圧性接着剤としての特
徴が損なわれるなどの弊害がある。
In the present invention, in addition to the above three components a to c, other polymer components and crosslinking agents can be used, and various compounding agents used for general pressure sensitive adhesives, for example, Antioxidants, ultraviolet absorbers, fillers, pigments, extenders and the like can also be used. However, the amount of these optional components used is required to be 100 parts by weight or less, and particularly preferably 80 parts by weight or less, per 100 parts by weight of the rubber polymer of the component a. If the amount exceeds 100 parts by weight, there is an adverse effect such that the characteristics of the rubber-based pressure-sensitive adhesive are impaired.

【0020】本発明におけるゴム系感圧性接着剤は、上
記のa〜c三成分を必須成分とし、必要に応じて上述の
各種の任意成分を含有するとともに、そのゲル分率が1
0〜40%の範囲、特に好適には10〜30%の範囲に
あることを大きな特徴としたものである。
The rubber-based pressure-sensitive adhesive in the present invention contains the above-mentioned three components a to c as essential components, contains the above-mentioned various optional components as required, and has a gel fraction of 1
The major feature is that it is in the range of 0 to 40%, particularly preferably in the range of 10 to 30%.

【0021】すなわち、この種のゴム系感圧性接着剤に
おいては、そのゲル分率が10%より小さくなると、接
着剤の凝集力が十分に得られず、加硫ゴム成形品を曲面
に貼り付ける場合などでは、接着固定後に剥がれやす
い。逆に、40%より大きくなると、接着剤の凝集力が
高くなりすぎて、加硫ゴム成形品との濡れが十分に得ら
れ難い。
That is, in this type of rubber-based pressure-sensitive adhesive, if the gel fraction is less than 10%, sufficient cohesive force of the adhesive cannot be obtained, and the vulcanized rubber molded product is attached to a curved surface. In some cases, it easily peels off after adhesion and fixation. On the other hand, when it is more than 40%, the cohesive force of the adhesive becomes too high, and it is difficult to obtain sufficient wetting with the vulcanized rubber molded product.

【0022】ゲル分率を前記の如く設定するには、a〜
c三成分を含有するゴム系感圧性接着剤を適度に架橋す
る方法が有効である。この架橋方法としては、たとえ
ば、過酸化物を用いて架橋する方法、キノンジオキシム
と過酸化物などを用いて架橋する方法、酸化亜鉛と各種
の促進剤とを用いて架橋する方法などが挙げられ、その
他電子線で架橋する方法を用いてもよい。電子線で架橋
する方法は、a成分のゴム質ポリマ―がハロゲン化ブチ
ルゴムの場合に特に有効である。
To set the gel fraction as described above,
c A method of appropriately crosslinking a rubber-based pressure-sensitive adhesive containing three components is effective. Examples of this cross-linking method include a cross-linking method using a peroxide, a cross-linking method using a quinonedioxime and a peroxide, a cross-linking method using zinc oxide and various accelerators, and the like. Alternatively, a method of crosslinking with an electron beam may be used. The method of crosslinking with an electron beam is particularly effective when the rubber polymer of the component a is a halogenated butyl rubber.

【0023】このようにして調製される本発明のゴム系
感圧性接着剤は、通常はトルエン、ヘキサン、ヘプタン
などの適宜の有機溶剤を用いた溶液とされ、加硫ゴム成
形品用の感圧性接着剤として、種々の用途目的に使用さ
れる。
The rubber-based pressure-sensitive adhesive of the present invention thus prepared is usually prepared as a solution using an appropriate organic solvent such as toluene, hexane, heptane, and the like. Used as an adhesive for various purposes.

【0024】この使用に際し、上記の接着剤溶液を、加
硫ゴム成形品からなる被着体に対し直接塗布してもよい
が、通常は適宜の基材上に層形成した、シ―ト状、フイ
ルム状、テ―プ状などの接着シ―ト類として使用するの
がよい。また、この場合、基材の片面だけに層形成して
もよいが、加硫ゴム成形品を他の被着体に接着する目的
からして、基材の両面に層形成した、いわゆる両面接着
シ―ト類とするのが望ましい。
In this use, the above-mentioned adhesive solution may be directly applied to an adherend composed of a vulcanized rubber molded product, but it is usually a sheet-like sheet formed in a layer on an appropriate substrate. It is good to use as an adhesive sheet such as film, tape or tape. Further, in this case, the layer may be formed on only one side of the base material, but for the purpose of adhering the vulcanized rubber molded article to another adherend, so-called double-sided adhesion in which a layer is formed on both sides of the base material It is desirable to use sheets.

【0025】このような両面接着シ―ト類を得る場合、
たとえば、セパレ―タ上に一旦上記の接着剤溶液を塗布
乾燥して層形成し、このものを二つ用意して、これらを
基材の両面に貼り合わせればよい。
When obtaining such double-sided adhesive sheets,
For example, the above adhesive solution may be applied on a separator once and dried to form a layer, two of these may be prepared, and these may be attached to both surfaces of the base material.

【0026】基材としては、不織布、織布、紙などの多
孔性基材や、ポリエステルフイルム、ポリエチレンフイ
ルム、ポリプロピレンフイルム、ポリ塩化ビニルフイル
ムなどのプラスチツクフイルムからなる、厚さが通常5
〜200μm程度のものが用いられる。プラスチツクフ
イルムを用いると、接着使用後長期間放置する場合に、
フイルムの一面側から他面側への接着阻害成分の移行を
防げるため、接着力の経時的な低下が抑制される。な
お、これらの基材に対して、接着剤層を設ける前に、下
塗り処理を施すと、接着剤の投錨力が向上する。
As the substrate, a porous substrate such as a non-woven fabric, a woven fabric or paper, or a plastic film such as a polyester film, a polyethylene film, a polypropylene film or a polyvinyl chloride film, usually having a thickness of 5
The thickness of about 200 μm is used. If you use a plastic film, when you leave it for a long time after adhesive use,
Since the migration of the adhesion-inhibiting component from the one surface side to the other surface side of the film can be prevented, the decrease in the adhesive strength with time is suppressed. If an undercoating treatment is applied to these base materials before forming the adhesive layer, the anchoring force of the adhesive is improved.

【0027】この基材上に設けられる接着剤層、つまり
ゴム系感圧性接着剤の層としては、その厚さが片面で通
常10〜400μm程度であるのが望ましいが、これに
限定されることなく、使用目的に応じて適宜決定でき
る。
It is desirable that the thickness of the adhesive layer provided on the base material, that is, the layer of the rubber-based pressure-sensitive adhesive is usually about 10 to 400 μm on one side, but the thickness is not limited to this. However, it can be appropriately determined according to the purpose of use.

【0028】また、両面接着シ―ト類を得る場合に、基
材の一面にのみ上記のゴム系感圧性接着剤の層を設け、
他面に他の接着剤、特にアクリル系感圧性接着剤の層を
設けるといつた変更態様をとつてもよい。
When a double-sided adhesive sheet is obtained, a layer of the above-mentioned rubber-based pressure-sensitive adhesive is provided only on one surface of the substrate,
Modifications may be made by providing the other side with a layer of another adhesive, in particular an acrylic pressure sensitive adhesive.

【0029】この態様によると、加硫ゴム成形品に対す
る接着はゴム系感圧性接着剤の層を利用でき、他の被着
体への接着は上記のアクリル系感圧性接着剤などの層を
利用できるため、使用目的によつてはより望ましい接着
特性が得られることになる。なお、上記のアクリル系感
圧性接着剤の層には、ゴム系感圧性接着剤の層の場合と
同様に、着色顔料などの各種添加剤を適宜含ませること
ができる。
According to this aspect, a layer of a rubber-based pressure-sensitive adhesive can be used for adhesion to a vulcanized rubber molded article, and a layer of the acrylic pressure-sensitive adhesive or the like can be used for adhesion to other adherends. Therefore, more desirable adhesive properties can be obtained depending on the purpose of use. The acrylic pressure-sensitive adhesive layer may contain various additives such as coloring pigments, as in the case of the rubber pressure-sensitive adhesive layer.

【0030】[0030]

【発明の効果】以上のように、本発明では、接着剤の必
須成分として、ゴム質ポリマ―をはじめとする特定分子
量のポリマ―成分や粘着付与剤などを3種組み合わせ使
用するとともに、これら成分を含む接着剤全体のゲル分
率を特定の範囲に設定したことにより、加硫ゴム成形品
の接着に際し、特にこの成形品を曲面を有する被着体に
貼り付ける場合に、従来のようなバフ研磨やプライマ―
塗布などの処理を施さなくとも、十分な接着強度を発揮
するゴム系感圧性接着剤とその接着シ―ト類を得ること
ができる。
As described above, in the present invention, as the essential components of the adhesive, three types of polymer components such as rubbery polymers having a specific molecular weight and tackifiers are used in combination, and these components are used. By setting the gel fraction of the adhesive as a whole in a specific range, when bonding vulcanized rubber molded products, especially when bonding this molded product to an adherend with a curved surface Polishing and primer
It is possible to obtain a rubber-based pressure-sensitive adhesive that exhibits a sufficient adhesive strength and its adhesive sheet without applying treatment such as coating.

【0031】[0031]

【実施例】つぎに、本発明の実施例を比較例と対比して
具体的に説明する。なお以下、部とあるのは重量部を意
味するものとする。
EXAMPLES Next, examples of the present invention will be specifically described in comparison with comparative examples. In the following, "parts" means "parts by weight".

【0032】実施例1 臭素化ブチルゴム(重量平均分子量50万) 100部 ポリイソブチレン(重量平均分子量8万) 120部 石油系樹脂(重量平均分子量2,500) 100部 ロジン系液状樹脂(重量平均分子量630) 50部 酸化亜鉛 3部 塩化亜鉛 2部 イソブチルキサントゲン酸亜鉛 4部 N・N´−ジフエニル−p−フエニレンジアミン 1部Example 1 Brominated butyl rubber (weight average molecular weight 500,000) 100 parts Polyisobutylene (weight average molecular weight 80,000) 120 parts Petroleum resin (weight average molecular weight 2,500) 100 parts Rosin-based liquid resin (weight average molecular weight) 630) 50 parts Zinc oxide 3 parts Zinc chloride 2 parts Zinc isobutylxanthate 4 parts N.N'-diphenyl-p-phenylenediamine 1 part

【0033】上記の各成分をトルエン700部に溶解し
て、ゴム系感圧性接着剤の溶液を調製した。この溶液を
アプリケ―タを用いて、乾燥後の厚さが70μmとなる
ように、セパレ―タ上に塗布し、100℃で3分間乾燥
した。
The above components were dissolved in 700 parts of toluene to prepare a rubber-based pressure-sensitive adhesive solution. This solution was applied onto a separator using an applicator so that the thickness after drying would be 70 μm, and dried at 100 ° C. for 3 minutes.

【0034】つぎに、上記のセパレ―タ上に形成された
ゴム系感圧性接着剤の層を二つ用意して、これらを厚さ
が50μmの不織布の両面に貼り合わせたのち、60℃
で2日間放置して、両面接着シ―トを作製した。
Next, two layers of the rubber-based pressure-sensitive adhesive formed on the above separator were prepared, and these were laminated on both sides of a non-woven fabric having a thickness of 50 μm, and then at 60 ° C.
It was left for 2 days to prepare a double-sided adhesive sheet.

【0035】実施例2 ブチルゴム(重量平均分子量50万) 100部 ポリイソブチレン(重量平均分子量3万) 70部 石油系樹脂(重量平均分子量2,500) 100部 テルペン系液状樹脂(重量平均分子量680) 50部 p−ベンゾキノンジオキシム 2部 クメンハイドロパ―オキサイド 0.5部 ナフテン酸コバルト 0.05部Example 2 Butyl rubber (weight average molecular weight 500,000) 100 parts Polyisobutylene (weight average molecular weight 30,000) 70 parts Petroleum resin (weight average molecular weight 2,500) 100 parts Terpene liquid resin (weight average molecular weight 680) 50 parts p-benzoquinone dioxime 2 parts cumene hydroperoxide 0.5 parts cobalt naphthenate 0.05 parts

【0036】上記の各成分をトルエン590部に溶解し
て、ゴム系感圧性接着剤の溶液を調製した。この溶液を
用いて、以下実施例1と同様にして、両面接着シ―トを
作製した。
The above components were dissolved in 590 parts of toluene to prepare a rubber pressure-sensitive adhesive solution. Using this solution, a double-sided adhesive sheet was produced in the same manner as in Example 1 below.

【0037】実施例3 臭素化ブチルゴム(重量平均分子量45万) 50部 ポリイソブチレン(重量平均分子量100万) 50部 ポリイソブチレン(重量平均分子量3万) 70部 プロセスオイル(重量平均分子量200) 50部 酸化亜鉛 2部 塩化亜鉛 2部 イソプロピルキサントゲン酸亜鉛 4部 N・N´−ジフエニル−p−フエニレンジアミン 1部Example 3 Brominated butyl rubber (weight average molecular weight 450,000) 50 parts Polyisobutylene (weight average molecular weight 1,000,000) 50 parts Polyisobutylene (weight average molecular weight 30,000) 70 parts Process oil (weight average molecular weight 200) 50 parts Zinc oxide 2 parts Zinc chloride 2 parts Zinc isopropylxanthate 4 parts N.N'-diphenyl-p-phenylenediamine 1 part

【0038】上記の各成分をトルエン425部に溶解し
て、ゴム系感圧性接着剤の溶液を調製した。この溶液を
用いて、以下実施例1と同様にして、両面接着シ―トを
作製した。
The above components were dissolved in 425 parts of toluene to prepare a rubber-based pressure-sensitive adhesive solution. Using this solution, a double-sided adhesive sheet was produced in the same manner as in Example 1 below.

【0039】実施例4 アクリル酸n−ブチル80部、アクリル酸2−エチルヘ
キシル17部、アクリル酸3部および酢酸エチル233
部の単量体溶液を、常法によりラジカル重合して、重量
平均分子量が60万のアクリル系ポリマ―を含む重合体
溶液を得た。これに、アクリル系ポリマ―100部に対
し、3官能性の低分子量イソシアネ―ト化合物3部を添
加混合して、アクリル系感圧性接着剤の溶液を調製し
た。
Example 4 80 parts of n-butyl acrylate, 17 parts of 2-ethylhexyl acrylate, 3 parts of acrylic acid and ethyl acetate 233
Part of the monomer solution was radical-polymerized by a conventional method to obtain a polymer solution containing an acrylic polymer having a weight average molecular weight of 600,000. To this, 100 parts of the acrylic polymer and 3 parts of the trifunctional low molecular weight isocyanate compound were added and mixed to prepare a solution of the acrylic pressure-sensitive adhesive.

【0040】つぎに、厚さが12μmのポリエステルフ
イルムの一面に、実施例1のゴム系感圧性接着剤の溶液
を乾燥後の厚さが70μmとなるように塗布し、100
℃で3分間乾燥したのち、さらに60℃で2日間放置し
た。その後、このポリエステルフイルムの他面に、上記
のアクリル系感圧性接着剤の溶液を乾燥後の厚さが70
μmとなるように塗布し、100℃で3分間乾燥して、
両面接着シ―トを作製した。
Next, the solution of the rubber-based pressure-sensitive adhesive of Example 1 was applied onto one surface of a polyester film having a thickness of 12 μm so that the thickness after drying was 70 μm, and 100
After drying at ℃ for 3 minutes, it was left at 60 ℃ for 2 days. Then, a solution of the acrylic pressure-sensitive adhesive is dried on the other surface of the polyester film to a thickness of 70.
It is applied so that it becomes μm, and dried at 100 ° C. for 3 minutes,
A double-sided adhesive sheet was prepared.

【0041】比較例1 臭素化ブチルゴム(重量平均分子量50万) 100部 ポリイソブチレン(重量平均分子量10万) 80部 石油系樹脂(重量平均分子量2,500) 70部 テルペン系液状樹脂(重量平均分子量300) 50部 酸化亜鉛 2部 テトラメチルチウラムジスルフイド 4部Comparative Example 1 Brominated butyl rubber (weight average molecular weight 500,000) 100 parts Polyisobutylene (weight average molecular weight 100,000) 80 parts Petroleum resin (weight average molecular weight 2,500) 70 parts Terpene liquid resin (weight average molecular weight) 300) 50 parts Zinc oxide 2 parts Tetramethylthiuram disulfide 4 parts

【0042】上記の各成分をトルエン638部に溶解し
て、ゴム系感圧性接着剤の溶液を調製した。この溶液を
用いた以外は、実施例1と同様にして、両面接着シ―ト
を作製した。
The above components were dissolved in 638 parts of toluene to prepare a rubber-based pressure-sensitive adhesive solution. A double-sided adhesive sheet was produced in the same manner as in Example 1 except that this solution was used.

【0043】比較例2 臭素化ブチルゴム(重量平均分子量50万) 100部 ポリイソブチレン(重量平均分子量8万) 20部 石油系樹脂(重量平均分子量2,500) 50部 ロジン系液状樹脂(重量平均分子量630) 50部 酸化亜鉛 3部 塩化亜鉛 2部 イソブチルキサントゲン酸亜鉛 4部 N・N´−ジフエニル−p−フエニレンジアミン 1部Comparative Example 2 Brominated butyl rubber (weight average molecular weight 500,000) 100 parts Polyisobutylene (weight average molecular weight 80,000) 20 parts Petroleum resin (weight average molecular weight 2,500) 50 parts Rosin liquid resin (weight average molecular weight) 630) 50 parts Zinc oxide 3 parts Zinc chloride 2 parts Zinc isobutylxanthate 4 parts N.N'-diphenyl-p-phenylenediamine 1 part

【0044】上記の各成分をトルエン700部に溶解し
て、ゴム系感圧性接着剤の溶液を調製した。この溶液を
用いた以外は、実施例1と同様にして、両面接着シ―ト
を作製した。
The above components were dissolved in 700 parts of toluene to prepare a rubber pressure-sensitive adhesive solution. A double-sided adhesive sheet was produced in the same manner as in Example 1 except that this solution was used.

【0045】以上の実施例1〜4および比較例1,2で
得られた各両面接着シ―トにつき、ゴム系感圧性接着剤
のゲル分率と、接着力および曲面貼り付け特性を測定し
た。その結果は、後記の表1に示されるとおりであつ
た。なお、上記のゲル分率、接着力および曲面貼り付け
特性の測定試験は、下記の要領で行つた。
With respect to each of the double-sided adhesive sheets obtained in Examples 1 to 4 and Comparative Examples 1 and 2, the gel fraction of the rubber pressure-sensitive adhesive, the adhesive strength and the curved surface sticking property were measured. .. The results are as shown in Table 1 below. The above-mentioned measurement tests of the gel fraction, the adhesive force and the curved surface sticking property were carried out as follows.

【0046】<ゲル分率>ゴム系感圧性接着剤約0.1
gを多孔質テフロン膜(重量b)で包み秤量する。この
重量をaとする。これを常温で7日間50mlのトルエン
に浸漬し、取り出し、130℃で3時間乾燥させる。常
温にもどして、このときの重量を秤量する。この重量を
cとする。ゲル分率は、〔(c−b)/(a−b)〕×
100(%)として算出される。
<Gel Fraction> Rubber-based pressure-sensitive adhesive about 0.1
g is wrapped with a porous Teflon membrane (weight b) and weighed. Let this weight be a. This is immersed in 50 ml of toluene at room temperature for 7 days, taken out, and dried at 130 ° C. for 3 hours. Return to room temperature and weigh the weight. Let this weight be c. The gel fraction is [(c-b) / (a-b)] x
It is calculated as 100 (%).

【0047】<接着力>被着体として加硫ゴム板を用い
て、JIS Z−1528に準じて、接着力(g/20
mm幅)を測定した。
<Adhesive strength> Using a vulcanized rubber plate as an adherend, the adhesive strength (g / 20) was measured according to JIS Z-1528.
mm width) was measured.

【0048】<曲面貼り付け特性>10mm×100mmの
大きさの加硫ゴム板をウエスで乾拭きし、両面接着シ―
トの一面側を2kgロ―ル1往復で貼り合わせる。つぎ
に、剥離紙を剥がして、他面側を5kgロ―ルを用い、直
径200mmのステンレスの円筒に貼り合わせる。50℃
に2日間放置後、端面からの浮きの高さを測定した。
<Curved surface pasting characteristics> A vulcanized rubber plate of 10 mm x 100 mm size is wiped dry with a waste cloth and double-sided adhesive sheet is attached.
Attach one side of the toe with one round trip of a 2kg roll. Next, the release paper is peeled off, and the other side is attached to a stainless steel cylinder having a diameter of 200 mm using a 5 kg roll. 50 ° C
After standing for 2 days, the height of floating from the end face was measured.

【0049】なお、上記の測定試験において、加硫ゴム
板としては、厚さ3mmのクロロプレンゴム板(入間川ゴ
ム製のNeo−180)と、厚さ3mmのEPTゴム板
(入間川ゴム製のEP−5065)を使用した。また、
実施例4の両面接着シ―トは、ゴム系感圧性接着剤の層
が加硫ゴム板側に接するようにして測定した。
In the above measurement test, as the vulcanized rubber plate, a chloroprene rubber plate having a thickness of 3 mm (Neo-180 made by Irumagawa Rubber) and an EPT rubber plate having a thickness of 3 mm (EP-made by Irumagawa Rubber- 5065) was used. Also,
The double-sided adhesive sheet of Example 4 was measured such that the rubber pressure-sensitive adhesive layer was in contact with the vulcanized rubber plate side.

【0050】[0050]

【表1】 [Table 1]

【0051】上記の表1の結果から明らかなように、本
発明の両面接着シ―トによれば、加硫ゴム板に対し、従
来のようなバフ研磨やプライマ―塗布などの処理を施さ
なくとも、非常に良好な接着特性が得られるものである
ことがわかる。
As is clear from the results of Table 1 above, according to the double-sided adhesive sheet of the present invention, the vulcanized rubber plate is not subjected to the conventional treatment such as buffing or primer coating. In both cases, it can be seen that very good adhesive properties can be obtained.

Claims (4)

【特許請求の範囲】[Claims] 【請求項1】 つぎのa〜c三成分; a)重量平均分子量が20万〜150万のポリイソブチ
レン、ブチルゴムまたはハロゲン化ブチルゴム100重
量部 b)重量平均分子量が1万〜15万の液状ないし半液状
のゴム30〜300重量部 c)重量平均分子量が1万未満の粘着付与剤または/お
よび軟化剤30〜300重量部 を必須成分として含有するとともに、ゲル分率が10〜
40%の範囲にあることを特徴とするゴム系感圧性接着
剤。
1. The following a to c three components; a) 100 parts by weight of polyisobutylene, butyl rubber or halogenated butyl rubber having a weight average molecular weight of 200,000 to 1.5 million b) Liquid or having a weight average molecular weight of 10,000 to 150,000 30 to 300 parts by weight of semi-liquid rubber c) Contains 30 to 300 parts by weight of a tackifier or / and a softening agent having a weight average molecular weight of less than 10,000 as an essential component and a gel fraction of 10 to
A rubber-based pressure-sensitive adhesive characterized by being in the range of 40%.
【請求項2】 b成分の液状ないし半液状のゴムがポリ
イソブチレンである請求項1に記載のゴム系感圧性接着
剤。
2. The rubber-based pressure-sensitive adhesive according to claim 1, wherein the liquid or semi-liquid rubber of the component b is polyisobutylene.
【請求項3】 基材の両面に請求項1または2に記載の
ゴム系感圧性接着剤の層が設けられてなる接着シ―ト
類。
3. Adhesive sheets having a layer of the rubber-based pressure-sensitive adhesive according to claim 1 or 2 on both sides of a base material.
【請求項4】 基材の一面に請求項1または2に記載の
ゴム系感圧性接着剤の層が設けられ、他面にアクリル系
感圧性接着剤の層が設けられてなる接着シ―ト類。
4. An adhesive sheet in which a layer of the rubber-based pressure-sensitive adhesive according to claim 1 or 2 is provided on one surface of a base material, and an acrylic-based pressure-sensitive adhesive layer is provided on the other surface. Kind.
JP26900791A 1991-09-19 1991-09-19 Rubber-based pressure-sensitive adhesive and its adhesive sheet Expired - Lifetime JP3145742B2 (en)