JPH0330132B2 - - Google Patents

Info

Publication number
JPH0330132B2
JPH0330132B2 JP1814489A JP1814489A JPH0330132B2 JP H0330132 B2 JPH0330132 B2 JP H0330132B2 JP 1814489 A JP1814489 A JP 1814489A JP 1814489 A JP1814489 A JP 1814489A JP H0330132 B2 JPH0330132 B2 JP H0330132B2
Authority
JP
Japan
Prior art keywords
silver
dispersion
silver halide
organic
photosensitive
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired
Application number
JP1814489A
Other languages
Japanese (ja)
Other versions
JPH0243A (en
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed filed Critical
Priority to JP1814489A priority Critical patent/JPH0243A/en
Publication of JPH0243A publication Critical patent/JPH0243A/en
Publication of JPH0330132B2 publication Critical patent/JPH0330132B2/ja
Granted legal-status Critical Current

Description

【発明の詳細な説明】[Detailed description of the invention]

本発明はハロゲン化銀を感光触媒として含有す
る高感度な熱現像性感光材料に関し、特に有機溶
媒中において製造された安定でかつ粒子径の揃つ
た微粒子ハロゲン化銀を含有する熱現像性感光材
料に関するものである。 従来広範囲に使用されているハロゲン化銀写真
法は、ジアゾ写真、電子写真などの所謂非銀塩感
光材料を用いた写真法と比較して、感光性及び階
調性などの写真特性上優れた写真法である。しか
しこの方法に用いられるハロゲン化銀写真材料
は、安定画像を得るために湿式処理工程を必要と
することから時間と手間がかかつたり、化学薬品
を取り扱うため人体に害を及ぼす場合がある等の
問題があつた。従つてハロゲン化銀を用いなが
ら、乾式処理によつて安定画像を得ることができ
る写真法は非常に望まれているもので、これまで
にも多くの研究がなされている。 例えば、特公昭43−4921号公報または同43−
4924号公報などに記載されている被還元性有機銀
塩、還元剤及び該有機銀塩に対し触媒的に接触し
ている感光性ハロゲン化銀の3成分から成る熱現
像性感光材料は最も成功した例である。かかる熱
現像性感光材料は、像露光した後、通常80℃以
上、好ましくは100℃以上の加熱により画像が形
成される。この熱現像性感光材料は、光に対し不
安定な感光性ハロゲン化銀の含有量が少ないため
に、画像形成後特に安定化処理を必要としない。
従つてかかる熱現像性感光材料は、全く湿式工程
を経ずに安定で良質な画像を得ることができる。 かかる熱現像性感光材料において、感光性ハロ
ゲン化銀は熱現像性感光材料の写真特性を決定す
るものとして重要であり、特に微細な粒子状の塩
化銀、臭化銀、塩臭化銀及び沃臭化銀が好ましい
とされている。このハロゲン化銀を調製する方法
は、第1の方法として特公昭43−4924号公報に記
載された被還元性有機銀塩の一部を、例えば臭化
アンモニウムまたは塩化ナトリウムなどによりハ
ロゲン化銀に変換する方法や、特公昭53−40484
号公報に記載されたN−ハロゲノ化合物を加熱分
解させて、被還元性有機銀塩の一部を感光性ハロ
ゲン化銀に変換する方法、所謂現場内ハロゲン化
銀の調製技術を挙げることができる。この第1の
方法においては、被還元性有機銀塩の一部をハロ
ゲン化して感光性ハロゲン化銀に変換するもので
あり、他の大部分の被還元性有機銀塩に不都合な
変化をもたらすことは避けなければならない。こ
の要件を満たした中での感光性ハロゲン化銀の形
成及び増感方法等は、自ずと制限を受けることに
なる。従つて、湿式ハロゲン化銀写真乳剤で用い
られる増感方法、特に化学増感剤を添加して高感
度化を計る方法等を単純に適用することは困難で
ある。 上記の理由から第2の方法、所謂現場外ハロゲ
ン化銀の技術が提唱されている。この現場外ハロ
ゲン化銀を含有する熱現像性感光組成物は、感光
性ハロゲン化銀をあらかじめ被還元性有機銀塩と
は別の場所で形成し、次いで被還元性有機銀塩に
混合して調製される。しかし特公昭43−4921号公
報及び同43−4924号公報で明らかなように、通常
のハロゲン化銀写真乳剤の方法で調製した感光性
ハロゲン化銀は好ましくない。なぜなら保護コロ
イドとしてゼラチンを用いた写真乳剤は、ハロゲ
ン化銀とゼラチンとの吸着が強いために、感光体
であるハロゲン化銀と画像形成成分である被還元
性有機銀塩との十分な接触状態が得られないから
である。また保護コロイド(例えばゼラチン)の
存在しない状態で調製したハロゲン化銀は、ハロ
ゲン化銀粒子間で凝集を生じ熱現像性感光材料の
感光体として不適当である。 このような欠点を補い、被還元性有機銀塩と有
効に接触しうる感光性ハロゲン化銀の製造が数多
く試みられている。例えば、英国特許第1362970
号明細書には、油溶性バインダーを含む有機溶媒
と無機銀化合物の水溶液を超音波分散により乳化
し、この乳化液に有機溶媒中に溶解させた無機ハ
ロゲン化合物を加え、油溶性バインダー中に感光
性ハロゲン化銀を形成する方法が記載されてい
る。しかしこの方法で調製される感光性ハロゲン
化銀は、粒子形及び粒度分布の整つた粒子を製造
できず、また超音波分散や水相を除去するための
デカンテーシヨン等の繁雑な操作を必要とする。
特開昭47−9432号公報及び特公昭52−17415号公
報には、極性有機溶媒(例えばアセトン)可溶性
の無機銀化合物と無機ハロゲン化合物を、油溶性
バインダー中で反応させて感光性ハロゲン化銀を
形成する方法が記載されている。しかしこの方法
によつても粒子形及び粒度分布の揃つたものは得
られず、凝集も生じ易い。特開昭50−32926号公
報及び特開昭54−4117号公報には、水系もしくは
水−有機溶媒の乳化物中で感光性ハロゲン化銀を
形成し、次に被還元性有機銀塩を感光性ハロゲン
化銀と混和して調製する方法が記載されている。
しかしこの方法では、感光性ハロゲン化銀が形成
後、化学的に活性な条件下にさらされたり、高温
の雰囲気下に置かれたりすることから、被還元性
有機銀塩を混和する前に感光性ハロゲン化銀に施
した各種の増感処理の特性を到底維持することは
できない。特開昭47−9171号公報及び特開昭47−
9308号公報には、新アンフイ性コポリマーの存在
下、また特開昭50−32928号公報には界面活性剤
の存在下での感光性ハロゲン化銀の形成について
記載されている。しかしこの方法も操作が困難で
あつたり、粒子の揃つたハロゲン化銀を調製する
ことは困難である。 本発明の目的は、画像濃度が高くかつ硬調な熱
現像性感光材料を提供することにある。 かかる目的を達成するために、本発明者等は
種々の検討を重ねた結果、有機溶媒中に懸濁分散
させた有機脂肪酸銀を所定の温度に保ち、この分
散液に無機、若しくは有機ハロゲン化合物を化学
量論的に加えた場合、ほぼ定量的に感光性ハロゲ
ン化銀が形成されることを見い出した。またこの
様にして形成されたハロゲン化銀粒子は粒度分布
の狭い微粒子であり、かつ長時間の放置によつて
凝集し沈降するようなことはなかつた。またハロ
ゲン化銀形成時保護コロイドとして有機溶媒に可
溶なバインダーを共存させた場合、より好ましい
結果が得られることがわかつた。更にこのように
して形成したハロゲン化銀を感光体として熱現像
性感光材料に使用することにより、感度、画像濃
度及び階調性等の写真特性に優れた、熱現像性感
光材料が得られることがわかつた。 本発明の感光性ハロゲン化銀は、成分(a)の有機
脂肪酸銀を有機溶媒中に懸濁分散させ、この分散
液に成分(b)の無機若しくは有機ハロゲン化合物を
加えることにより形成される。かかる成分(a)の有
機脂肪酸銀は、有機溶媒に難溶若しくは不溶であ
り、好ましくは炭素数5個以上の有機脂肪酸銀で
あり、例えばカプロン酸銀、カプリル酸銀、カプ
リン酸銀、ラウリン酸銀、ミリスチン酸銀、パル
ミチン酸銀、ステアリン酸銀、アラシン酸銀、ベ
ヘン酸銀、リグノセリン酸銀、オレイン酸銀、リ
ノール酸銀、リノレイン酸銀、ヒドロキシステア
リン酸銀、11−ブロモウンデカン酸銀等の置換若
しくは無置換の飽和若しくは不飽和脂肪酸銀を挙
げることができる。有機脂肪酸銀の中で炭素数4
個以下のものは、形状の揃つた粒度分布の狭いハ
ロゲン化銀粒子を製造することが難しいためあま
り好ましくない。かかる有機脂肪酸銀の調製は、
適当な溶媒に溶解させた有機脂肪酸若しくは有機
脂肪酸のアルカリ金属塩等の溶液に硝酸銀、アン
モニア性硝酸銀等の銀塩若しくは銀錯塩等の溶液
を加えて調製する方法が一般的である。 成分(b)の無機若しくは有機ハロゲン化合物は、
成分(a)の有機脂肪酸銀と反応してハロゲン化銀を
形成しうるものである。無機ハロゲン化合物とし
ては、一般式MXnで表わされる化合物を挙げる
ことができる。但し式中Mは、水素原子又は金属
原子(例えば、ストロンチウム、カドミウム、亜
鉛、ナトリウム、バリウム、セシウム、カルシウ
ム、鉄、ニツケル、マグネシウム、カリウム、ア
ルミニウム、アンチモン、金、コバルト、水銀、
鉛、ベリリウム、リチウム、インジウム、イリジ
ウム、ロジウム、パラジウム、白金、ビスマス
等)を表わし、Xは塩素原子、臭素原子及び沃素
原子を、nは各陽イオンの原子価を示す。無機ハ
ロゲン化合物としては、更に含ハロゲン金属錯
体、例えばK2PtCl6,K2PtBr6,HAuCl4
(HN42IrCl6,(HN43IrCl6,(HN43RuCl6
K3RhCl6などを挙げることができる。有機ハロゲ
ン化合物もハロゲン化剤として有効であり、特に
有機ハロゲン化合物を用いた場合には、粒子径及
び形状の整つた感光性ハロゲン化銀を調整でき
る。好ましい有機ハロゲン化合物として、次の一
般式(1)若しくは(2)で表わされる化合物を挙げるこ
とができる。 式中Xは、塩素原子、臭素原子及び沃素原子を
表わし、Zは4〜8員環を形成するに必要な非金
属原子群を表わし、この4〜8員環は他の環と縮
合してもよい。Zは好ましくは5員環あるいは6
員環であり、具体例としてはピロール環、ピロリ
ン環、ピロリジン環、イミダゾリン環、イミダゾ
リジン環、ピラゾリン環、オキサゾリジン環、ピ
ペリジン環、オキサジン環、ピペラジン環、イン
ドリン環等を挙げることができる。さらにZは4
〜8員環のラクタム環、ヒダントイン環、シアヌ
ル環、ヘキサヒドロトリアジン環、インドリン環
などを形成してもよい。さらにこの環には、無置
換若しくは置換アルキル基、無置換若しくは置換
アリール基、アルコキシ基、ハロゲン原子、オキ
ソ基等の置換基を有していてもよい。Aはカルボ
ニル基、またはスルホニル基を表わし、R1およ
びR2は水素原子、無置換若しくは置換アルキル
基、無置換若しくは置換アリール基、アルコキシ
基を表わす。 上記一般式(1)で示される代表的な化合物例とし
て、N−ブロムサクシンイミド、N−ブロムテト
ラフルオロサクシンイミド、N−ブロムフタルイ
ミド、N−ブロムグルタールイミド、1,3−ジ
ブロム−5,5−ジメチル−2,4−イミダゾリ
ジンジオン、N,N′−ジブロム−5,5−ジエ
チルバルビツール酸、N−ブロムイソシアヌル
酸、N,N′−ジブロムイソシアヌル酸、N−ブ
ロムオキサゾリノン、N−ブロムフタラジノン、
N−クロルサクシンイミド、N−ヨードサクシン
イミド、N−クロルフタルイミド、N−ブロムサ
ツカリン、N−ブロムカプロラクタム、N−ブロ
ムブチロラクタム、N,N′−ジブロムチオヒダ
ントイン等を挙げることができる。 上記一般式(2)で示される代表的な化合物例とし
て、N−ブロムアセトアミド、N−ブロムアセト
アニリド、N−ブロムベンゼンスルホニルアニリ
ド、N−ブロムベンズアミド、N−クロルアセト
アミド、N−ブロムナフトアミド、N−ブロム−
P−ヒドロキシベンズアミド等を挙げることがで
きる。 また有機ハロゲン化合物としてハロゲン化メラ
ミンも使用することができ、具体例としてはトリ
ブロムメラミン、トリクロルメラミン等を挙げる
ことができる。 更に有機ハロゲン化合物として下記一般式(3)で
表わされるC−ハロゲン化合物も有効である。 式中、Xは塩素原子、臭素原子及び沃素原子を
表わし、R3,R4,R5は互いに同一でも異なつて
いてもよく、水素原子、無置換若しくは置換のア
ルキル基、無置換若しくは置換アリール基、ニト
ロ基、アシル基、無置換若しくは置換アミド基、
無置換若しくは置換アリール基またはアルキル基
に結合したスルホニル基、又はハロゲン原子を表
わす。但しR3,R4,R5の少なくとも一つはハロ
ゲン原子の放出を助けるものであり、例えばニト
ロ基、無置換若しくは置換のアリール基、アルケ
ニル基、アシル基、アミド基、スルホニル基等を
表わす。 上記一般式(3)で表わされる化合物としては、α
−ハロケトン化合物、α−ハロアミド化合物、ハ
ロスルホニル化合物、ハロニトロ低級アルカン化
合物、ハロゲン原子に対しβ位炭素が不飽和結合
を持つ化合物等を挙げることができる。 一般式(3)で表わされる化合物の具体例として
は、α−ブロムアセトフエノン、α−クロルアセ
トフエノン、α−ブロモ−α−フエニルアセトフ
エノン、α−ブロモ−1,3−ジフエニル−1,
3−プロパンジオン、α−ブロモ−2,5−ジメ
トキシアセトフエノン、α−ブロムメチルスルホ
ニルベンゼン、α−ブロモ−α−ベンゼンスルホ
ニルアセトアミド、α−クロル−α−(P−トリ
ルスルフオニル)アセトアミド、α−ブロモ−γ
−ニトロ−β−フエニルブチロフエノン、α−ヨ
ード−γ−ニトロ−β−フエニルブチロフエノ
ン、2−ブロモ−2−ニトロ−1,3−プロパン
ジオール、2−ブロモ−2−ニトロトリメチレン
−1,3−ビス(フエニルカーボネ−ト)、α−
ブロムトルエン、α,P−ジブロムトルエン、
α,α′−ジブロム−m−キシレン、α,α,α′,
α′−テトラブロム−P−キシレン、3−ブロムプ
ロペン等を挙げることができる。上記の化合物例
の中でも、α−ブロムトルエン、3−ブロムプロ
ペン等のハロゲン原子のβ位の炭素が不飽和結合
を有している化合物は特に有用である。 本発明においてオニウムハライド化合物もハロ
ゲン化剤として有用であり、具体例として、アン
モニウムブロマイド、トリメチルフエニルアンモ
ニウムクロライド、セチルエチルジメチルアンモ
ニウムブロマイド、トリメチルベンジルアンモニ
ウムブロマイド、テトラエチルフオスフオニウム
ブロマイド、トリメチルスルフオニウムクロライ
ド等を挙げることができる。本発明は、前記成分
(a)の有機脂肪酸銀と成分(b)の無機若しくは有機ハ
ロゲン化合物を混合し、成分(a)の有機脂肪酸銀の
全部、若しくはそのほとんどを感光性ハロゲン化
銀に変換する反応を有機溶媒下で行うものである
ので、成分(b)のハロゲン化合物の使用量は成分(a)
の有機脂肪酸銀に対して化学量論的な量でよい。
しかし好ましくは過剰量、すなわち成分(a)の有機
脂肪酸銀1モルに対し、成分(b)のハロゲン化合物
を約1.0モルから約3.0モルの範囲で使用すること
が好ましい。 本発明において、成分(a)の有機脂肪酸銀と成分
(b)のハロゲン化合物の反応に用いられる有機溶媒
は、反応温度で液状であり成分(a)の有機脂肪酸銀
を均一に分散し、かつ成分(b)のハロゲン化合物を
一定量溶解することができれば特に限定されな
い。具体的には、アルコール類、ケトン類、脂肪
族炭化水素類、芳香族炭化水素類、アルコール
類、エーテル類、酸アミド等を単独若しくは混合
物として使用することができる。 アルコール類の具体例としては、メチルアルコ
ール、エチルアルコール、n−プロピルアルコー
ル、イソプロピルアルコール、n−ブチルアルコ
ール、イソブチルアルコール、sec−ブチルアル
コール、n−アミルアルコール、イソアミルアル
コール、n−ヘキシルアルコール等の脂肪族飽和
アルコール、アリルアルコール、プロパルギルア
ルコール等の脂肪族不飽和アルコール、シクロペ
ンタノール、シクロヘキサノール等の脂環式アル
コール、ベンジルアルコール、シンナミルアルコ
ール等のアラルキルアルコール、エチレングリコ
ール、グリセリン等の多価アルコール等を挙げる
ことができる。 ケトン類の具体例としては、アセトン、メチル
エチルケトン、メチルプロピルケトン、イソプロ
ピルメチルケトン、ブチルメチルケトン、イソブ
チルメチルケトン等の脂肪族飽和ケトン、メチル
ビニルケトン、メチルヘプテンケトン等の不飽和
脂肪族ケトン、シクロブタノン、シクロヘキサノ
ン等の脂環式ケトン、アセトフエノン、プロピオ
フエノン、ブチルフエノン等の芳香族ケトンを挙
げることができる。 エステル類の具体例としては、ギ酸メチル、ギ
酸プロピル、ギ酸アミル、酢酸エチル、酢酸メチ
ル、酢酸ブチル、酢酸イソブチル、プロピオン酸
メチル、プロピオン酸エチル、プロピオン酸イソ
プロピル、酪酸メチル、酪酸エチル、イソ酪酸エ
チル、イソ吉草酸メチル、イソ吉草酸イソプロピ
ル、安息香酸メチル、フタル酸エチル等を挙げる
ことができる。 エーテル類の具体例としては、ジメチルエーテ
ル、ジプロピルエーテル、ジイソプロピルエーテ
ル、ジブチルエーテル、メチルブチルエーテル、
エチルプロピルエーテル、エチルイソアミルエー
テル等の飽和脂肪族エーテル、ジアリルエーテ
ル、エチルアリルエーテル等の不飽和脂肪族エー
テル、アニソール、フエニルエーテルのごとき芳
香族エーテル、テトラハイドロフラン、ジオキサ
ン等の環式エーテルを挙げることができる。 脂肪族炭化水素の具体例としては、n−ヘプタ
ン、n−ヘキサン、3−メチルペンタン、2,3
−ジメチルブタン、シクロヘキサン、シクロヘプ
タン等の飽和脂肪族炭化水素、シクロヘキセン、
シクロペンタジエン、シクロペンテン等の不飽和
脂肪族炭化水素を挙げることができる。 芳香族炭化水素類の具体例としては、ベンゼ
ン、トルエン、キシレン、クロルベンゼン、イン
デン、テトラリン等を挙げることができる。この
他に、ジメチルアセトアミド、ジメチルホルムア
ミド、ジメチルスルホキサイド等の窒素原子や硫
黄原子を含む溶媒も使用することができる。 上記の有機溶媒のうち特に好ましいものは、ア
ルコール類若しくはケトン類の単独若しくは上記
の他の溶媒との混合物である。また水−アルコー
ル類、水−ケトン類の混合系も使用できる。 本発明の感光性ハロゲン化銀の調製の際、成分
(a)の有機脂肪酸銀は上記の有機溶媒中に周知の分
散技術、例えばホモミキサー、ボールミル、サン
ドミル、超音波分散機等により懸濁分散される。
この懸濁液を液(A)とし、成分(b)の無機若しくは有
機ハロゲン化合物を上記の有機溶媒に分散、好ま
しくは溶解させた液を液(B)とする。液(A)及び液(B)
の濃度は任意に設定しうるが、好ましくは0.5重
量%から50重量%の範囲である。液(A)と液(B)の混
合方法は、写真技術の分野において公知な技術、
例えば正流法、逆流法、同時混合法等を用いるこ
とができる。しかし簡便で好ましい方法は、撹拌
されている液(A)へ液(B)を添加する方法である。液
(B)の添加方法は、一気に添加する方法、間歇に添
加する方法、及び連続して徐々に添加する方法の
いずれによつても感光性ハロゲン化銀が形成され
る。しかし、ハロゲン化銀粒子の粒子径及び形状
を揃え、粒子を成長させる為には、間歇若しくは
徐々に連続して添加する方法が好ましい。又上記
添加方法に、特公昭54−24012号公報に記載の酸
化還元電位の制御下で添加を行う方法も応用でき
る。液(B)の添加に要する時間は、反応条件、例え
ば撹拌スピード、反応温度により変化することか
ら一義的に設定することはできない。しかし操作
上30分から5時間に設定するのが好ましい。反応
開始から反応終了までの反応時間は、液(B)の添加
終了時までとすることもできるが、一般的には液
(B)の添加終了後さらに30分から24時間の間の反応
を続けるのが好ましい。 本発明の感光性ハロゲン化銀の形成法におい
て、成分(a)の有機脂肪酸銀の銀イオンの解離と、
成分(b)のハロゲン化合物のハロゲンイオンの発生
を助ける為に、反応温度は0℃以上、特に約20℃
以上100℃以下の温度に設定することが好ましい。
かかる反応温度は、用いられる成分(a)の有機脂肪
酸銀、成分(b)のハロゲン化合物及び反応溶媒によ
り定まる。一般的には成分(a)の有機脂肪酸銀のア
ルキル鎖が長い程、高温に設定することが好まし
い。又成分(b)として無機ハロゲン化合物を用いる
場合には、有機ハロゲン化合物を使用する場合に
比べ、やや低めの反応温度に設定できる。更に又
反応溶媒としてアルコール類を主体として用いた
場合には、他の溶媒よりも低い温度に設定でき
る。 本発明の感光性ハロゲン化銀の形成に際し、反
応を促進するために、加熱する他に反応促進剤、
例えばトリフルオロ酢酸のごとき酸性物質あるい
はピリジンのごとき塩基性物質を添加して、有機
溶媒中安定で粗大なハロゲン化銀粒子を形成する
こともできる。 本発明において、反応溶媒中好ましくは液(A)の
分散溶媒中に、この溶媒に可溶なポリマーを添加
しておくことができる。有機溶媒に可溶なポリマ
ーの添加は、成分(a)の有機脂肪酸銀の分散性を良
くし、成分(a)の有機脂肪酸銀と成分(b)のハロゲン
化合物の均一な反応を行わせ、又形成された感光
性ハロゲン化銀の不規則な成長と凝集を防ぐこと
もできる。この目的のために使用できるポリマー
は、例えばポリビニルアセテート、ポリビニルプ
ロピオネート、ポリメチルメタアクリレート、エ
チルセルロース、セルロースアセテート、ニトロ
セルロース、ポリエチレン、エチレン−酢酸ビニ
ル共重合体、塩素化ポリエチレン、ポリ塩化ビニ
ル、塩化ビニル−酢酸ビニル共重合体、塩素化ポ
リプロピレン、ポリビニルアセタール、アクリル
樹脂、ポリスチレン、エポキシ樹脂、変性メラミ
ン樹脂、アルキド樹脂、ポリアミド、塩化ゴム、
アクリロニトリル−ブタジエン−スチレン三元共
重合体、シリコンブロツクコポリマー、ポリビニ
ルピロリドン、ポリエチレンオキサイド、高分子
量パラフイン及び特開昭47−9432号公報に記載さ
れるビニルコポリマー等を挙げることができる。
上記ポリマーの中で好ましいものは、アルコール
類若しくはケトン類の単独若しくは他の有機溶媒
との混合溶媒に溶解しうるもので、特に好ましい
ポリマーはポリビニルアセタール類であ。この有
機溶媒に可溶なポリマーの使用量は、成分(a)の有
機脂肪酸の銀塩1gに対し約0.05gから約20g、
好ましくは約0.1gから約10gの範囲である。 次に本発明の感光性ハロゲン化銀を調製する手
順について、その好ましい態様を記載する。 有機脂肪酸銀を有機溶媒(例えばn−ブタノー
ル)中に均一に分散し、有機溶媒に可溶なポリマ
ー(例えばポリビニルブチラール)を添加して撹
拌し溶解させ、ポリマーを含む有機脂肪酸銀の懸
濁分散液を調製する。この分散液を安全光下で撹
拌しつつ一定の温度に保ち、これに適当な有機溶
媒(例えばアセトン)に溶解させた無機若しくは
有機ハロゲン化合物を約30分から約5時間、好ま
しくは約30分から約3時間で間歇又は徐々に連続
して添加する。添加終了後反応温度を保ち約30分
から約24時間、好ましくは約30分から8時間反応
を続ける(反応の終了時は経験的に定められる
が、特開昭54−24012号公報に記載されている酸
化還元電位を測定することにより判断できる。又
ハロゲン化合物としてN−ハロゲノ化合物を用い
た場合は、特公昭53−40484号公報に記載されて
いるメロシアニン染料の脱色によつても判断でき
る。)。反応終了後反応液を室温にもどし、感光性
ハロゲン化銀と副生成物の有機脂肪酸、若しくは
銀を陽イオンとしない有機脂肪酸との混合分散液
を得る。 本発明により調製される感光性ハロゲン化銀
は、塩化銀、沃化銀、臭化銀、塩臭化銀、沃臭化
銀、沃塩化銀及び塩沃臭化銀である。 本発明により調製された感光性ハロゲン化銀
は、通常の湿式ハロゲン化銀乳剤で用いられる公
知の化学増感方法、例えば硫黄増感、金増感、還
元増感等を施して固有感度を高めることができ
る。 更に本発明により調製された感光性ハロゲン化
銀は、公知の分光増感方法、例えばシアニン色
素、スチリル色素、ヘミシアニン色素、トリフエ
ニルメタン色素、キサンテン色素、オキソノール
色素、メロシアニン色素、特に「ブロダクトライ
センシングインデツクス」92巻、第107〜110頁
(1971年12月発行)、あるいはベルギー特許第
772371号明細書に記載されたものにより分光増感
することができる。 本発明により調製された感光性ハロゲン化銀
は、被還元性有機銀塩及び還元剤からなる酸化−
還元画像形成成分のための感光性成分として極め
て好都合な特性を有するものであり、従つて本発
明により調製された感光性ハロゲン化銀を用いる
ことにより写真特性の優れた熱現像性感光材料を
提供することができる。 即ち支持体上に少なくとも(c)被還元性有機銀塩
及び還元剤からなる酸化−還元画像形成成分、(d)
感光性ハロゲン化銀及び(e)バインダーからなる感
光性組成物の少なくとも一つの層を有する熱現像
性感光材料において、(d)感光性ハロゲン化銀とし
て、本発明に従つて調製された感光性ハロゲン化
銀を好適に用いることができる。 本発明者等は、かかる感光性ハロゲン化銀に関
して長年研究した結果、ハロゲン化銀が0.1μ前後
の微細な粒子である場合に有効であり、特に
〔1.0.0〕の正常晶であるハロゲン化銀粒子が有効
であることを見い出し、更に本発明者等は前述の
有機溶媒中に懸濁分散させた有機脂肪酸銀と無機
若しくは有機ハロゲン化合物との反応によつて形
成される感光性ハロゲン化銀が、上記の条件を満
足しかつ熱現像性感光材料の製造上好ましいこと
を見出した。 これ等の条件を満たす理由としては、 本発明によつて調製される感光性ハロゲン化
銀は、粒度分布が狭くかつ微細であり、高い画
像濃度及び硬調の熱現像性感光材料を提供する
ことができる。 本発明によつて調製される感光性ハロゲン化
銀は、有機溶媒中に容易にまた安定に分散する
ため、熱現像性感光材料の製造上有利である。 本発明によつて調製される感光性ハロゲン化
銀の分散物は再沈、デカンテイシヨン、遠心分
離等の洗浄操作を省いて熱現像性感光材料を製
造しても、熱現像時のカブリの原因とならな
い。 等の事項を挙げることができる。 本発明の熱現像性感光材料は上述したように、
支持体上に設けられた少なくとも1つの層中に上
記(c),(d),(e)の3成分が必須成分として存在す
る。 成分(c)の被還元性有機銀塩および還元剤から成
る酸化−還元画像形成成分において、被還元性有
機銀塩とは、光に対して比較的安定な無色、白
色、若しくは淡色の銀塩であり、共存するハロゲ
ン化銀が感光し生じる金属銀を核として、温度80
℃以上好ましくは100℃以上の温度で加熱された
場合、還元剤と反応して銀画像を形成するもので
ある。具体的には特公昭43−4924号および特開昭
46−6074号公報に記載の有機酸の銀塩、或いはイ
ミノ基又はメルカプト基を有する有機化合物の銀
塩であり、特に炭素数12〜24個の長鎖脂肪酸の銀
塩は、室内光下で暗着色化等の不都合な変化を受
け難いため好ましいものである。具体的には、ベ
ヘン酸銀、ステアリン酸銀、パルミチン酸銀、ミ
リスチン酸銀、ラウリン酸銀、オレイン酸銀又は
ヒドロキシステアリン酸銀を挙げることができ、
そのうち特にベヘン酸銀が最も有効である。又上
記の被還元性有機銀塩は、特公昭43−4924号公
報、同53−40484号公報等に記載される方法によ
つて、その銀塩の一部がハロゲン化銀に変換され
ているものも使用できる。 前述の酸化−還元画像形成成分に用いる還元剤
は種々のものを挙げることができる。一般的に
は、通常のハロゲン化銀感光材料に用いられる現
像薬、具体的にはハイドロキノン、メチルハイド
ロキノン、クロロハイドロキノン、メチルヒドロ
キシナフタレン、N,N′−ジエチル−P−フエ
ニレンジアミン、アミノフエノール、アスコルビ
ン酸、1−フエニル−3−ピラゾリドンなどを挙
げることができ、又これらの他に2,2′−メチレ
ンビス(6−t−ブチル−4−メチルフエノー
ル)、4,4′−ブチリデンビス(6−t−ブチル
−3−メチルフエノール)、4,4′−チオビス
(6−t−ブチル−3−メチルフエノール)など、
更には特開昭46−6074号公報に記載のビスナフト
ール系還元性化合物、或いはベルギー特許第
802519号明細書に記載の4−ベンゼンスルホンア
ミドフエノールなどのスルホンアミドフエノール
系化合物を挙げることができる。更に上記の還元
剤は2種以上を併用してもよい。かかる還元剤の
量は、被還元性有機銀塩1モル当たり約0.05モル
〜約5モル、好ましくは約0.2モル〜約3モルの
範囲である。 本発明における前記成分(d)の感光性ハロゲン化
銀は、前記方法によつて調製されるもので、塩化
銀、臭化銀、沃化銀、塩臭化銀、沃塩化銀、沃臭
化銀、塩沃臭化銀から選ばれる一種若しくは二種
以上の混合物であつて、好ましくは炭素数16個以
上の有機脂肪酸銀より調製され、臭化銀として30
モル%以上を含むものである。 この成分(d)の感光性ハロゲン化銀は、生成され
た後副生成物を含んだまま、若しくは再沈、デカ
ンテイシヨン、遠心分離等の洗浄操作をした後、
再分散して、被還元性有機銀塩を含む分散物と混
合される。成分(d)の感光性ハロゲン化銀の添加時
期は、被還元性有機銀塩と接触可能な同一層に含
有されれば熱現像性感光材料の製造工程中の何れ
の時期であつてもよく、又感光性ハロゲン化銀と
被還元性有機銀塩の均一分散物の調製は、通常の
撹拌機、ボールミル分散、超音波分散等によつて
容易に達成することができる。成分(d)の感光性ハ
ロゲン化銀の添加量は、被還元性有機銀塩1モル
当たり約0.01モルから約0.5モルの範囲であり、
好ましくは約0.05モルから約0.3モルの範囲であ
る。この範囲外の使用量、すなわち0.01モル以下
では実用的な写真特性を得ることができず、また
0.5モル以上では画像形成後の地色変化が著しい。 本発明の成分(e)のバインダーは、単独若しくは
2種以上を組合せて使用できる。バインダーの適
当な材料は疎水性あるいは親水性であることがで
き、又透明若しくは半透明であることができる。
具体的には、ポリビニルブチラール、セルロース
アセテートブチレート、ポリメチルメタアクリレ
ート、ポリビニルピロリドン、エチルセルロー
ズ、酢酸セルローズ、ポリ酢酸ビニル、ポリビニ
ルアルコール、ゼラチン、カナダ特許第774054号
明細書に記載のスルホベタイン繰り返し単位を有
するもの等を挙げることができるが、特にポリビ
ニルブチラールは好ましい。バインダーの使用量
は、被還元性有機銀塩に対して、重量比で約10対
1〜1対10が好ましく、さらに好ましくは約4対
1〜1対2の範囲である。 本発明の熱現像性感光材料は、黒色画像を得る
ために色調剤の1種以上を添加することが好まし
い。例えば米国特許第3080254号明細書に記載の
フタラジノンとその誘導体、特開昭46−6074号公
報に記載の環式イミド類、特開昭50−32927号公
報に記載のフタラジンジオン化合物などを挙げる
ことができる。 本発明の熱現像性感光材料は、現像時の熱カブ
リを防止する目的で公知のカブリ防止剤を使用で
きる。例えば特公昭47−11113号公報に記載され
る水銀化合物、特開昭49−10724号、特公昭54−
25808号及び同54−23813号各公報に記載されるN
−ハロゲノ化合物、米国特許第3645739号明細書
及び特開昭48−89720号公報に記載されているス
テアリン酸、ベヘン酸などの高級脂肪酸や、サリ
チル酸、テトラブロム安息香酸、フタル酸、トリ
メリツト酸などの酸安定剤等を挙げることができ
る。 本発明の熱現像性感光材料には、適当な分光増
感剤を含有することができる。有用な増感色素
は、シアニン色素、メロシアニン色素、キサンテ
ン色素、特に「プロダクトライセシングインデツ
クス」Vol92、第107〜110頁(1971年12月発行)
あるいはベルギー特許第772371号明細書、特開昭
47−6329号、特開昭50−105127号、特開昭51−
127719号、特開昭52−80829号公報などに記載さ
れたものが有用である。 更に、画像形成後の光変色を防止する化合物を
含有することができる。例えば、米国特許第
3839041号明細書に記載されたアゾールチオエー
テルやブロツクされたアゾールチオン類、米国特
許第3700457号明細書に記載されたテトラゾリル
チオン化合物、米国特許第3707377号明細書に記
載された含ハロゲン有機酸化剤、米国特許第
3893859号明細書に記載された1−カルバモイル
−2−テトラゾリン−5−チオン類等を使用する
ことができる。また、その他の適当な添加剤、例
えば現像促進剤、硬化剤、帯電防止剤(層)、紫
外線吸収剤、蛍光増白剤、フイルター染料(層)
なども用いることができる。 本発明の熱現像性感光材料は、成分(c)被還元性
有機銀塩及び還元剤、成分(d)感光性ハロゲン化銀
及び成分(e)バインダーと、上記の各種添加剤を適
当な溶媒に分散若しくは溶解し支持体上に一層若
しくは多層に塗布することにより得られる。さら
には、これら単層若しくは多層で形成された熱現
像性感光層の上に上塗りポリマー層を設けること
もできる。適当なポリマー層としては、例えば、
ポリビニルブチラール、ポリスチレン、ポリメチ
ルメタアクリレート、ポリウレタンゴム、塩化ゴ
ム、エチルセルロース、セルロースアセテートブ
チレート、酢酸セルロース、ポリ塩化ビニル、ポ
リ塩化ビニリデン、ポリカーボネート、ポリビニ
ルピロリドンなどを挙げることができる。 又、上記ポリマーを支持体上で下塗り層として
設け、その上に本発明の熱現像性感光層を重ねる
こともできる。 本発明で用いる支持体は、広範なものから選択
して使用することができる。代表的な支持体とし
ては、ポリエチレン、ポリプロピレン、ポリエチ
レンテレフタレート、ポリカーボネート、酢酸セ
ルロースなどの合成樹脂フイルム、合成紙、ポリ
エチレンなどの樹脂フイルムで被覆された紙、ア
ート紙などの紙類または写真用バライタ紙、アル
ミニウムなどの金属板(箔)類、通常の方法によ
り金属蒸着膜を有する合成樹脂フイルム、ガラス
板などを挙げることができる。 塗布方法は、ロールコート法、エアナイフ法、
キスコート法、カーテンコート法、バーコート
法、及びホツパーコート法などの公知の方法をと
ることができる。 本発明の熱現像性感光材料は、キセノンラン
プ、水銀灯、タングステンランプ、CRTレーザ
光などの光源で露光され、次いで80℃〜180℃、
好ましくは110℃〜150℃の加熱温度範囲で現像さ
れる。上述の温度範囲外でも加熱時間を延長若し
くは短縮することによつて現像することもできる
が、現像時間は通常約1秒〜60秒の範囲にするの
が好ましい。加熱現像する手段は、加熱プレート
または加熱ドラムとに接触させることが通常の手
段であるが、その他に加熱された雰囲気内に一時
保持する手段を採用してもよく、或いは高周波加
熱や赤外光による加熱の手段を採用することもで
きる。 以下、本発明を実施例に基づいてさらに詳細に
説明する。 製造例 1 ステアリン酸銀3.9gをイソプロピルアルコー
ル100mlに加え、ホモミキサーを用いて分散した。
この分散後にポリビニルブチラール3gを加え、
撹拌溶解して銀塩のポリマー懸濁分散液を作つ
た。この分散液を赤色安全光下で50℃に加熱調温
し、撹拌下アセトン30mlに溶解した臭化リチウム
0.9gを1時間かけて滴下した。滴下後2時間反
応温度を保ち撹拌を続けた後、分散液を室温まで
下げ感光性ハロゲン化銀の分散物(1)を得た。得ら
れた分散物(1)は、長時間放置しても分散物の沈澱
はなかつた。この分散液の一部をキシレン/n−
ブタノール(体積比で50/50)の溶液で約5倍に
希釈し、遠心分離操作(6000RPM)の後ポリビ
ニルブチラールを溶解している上澄み液をデカン
テーシヨンにて除き、残渣をガラス板上で乾燥さ
せ試料(1)とした。この試料(1)をレプリカ法による
電子顕微鏡撮影(1000倍、10000倍及び30000倍)
を行い、ハロゲン化銀粒子の型と粒度分布を観察
した(後述する製造列及び比較製造例においても
同様な操作により測定を行つた。)。表−1に得ら
れた結果を示す。
The present invention relates to a highly sensitive heat-developable photosensitive material containing silver halide as a photocatalyst, and more particularly to a heat-developable photosensitive material containing stable, fine-grained silver halide with uniform particle size produced in an organic solvent. It is related to. Silver halide photography, which has been widely used in the past, has superior photographic properties such as photosensitivity and gradation compared to photography methods using so-called non-silver salt photosensitive materials such as diazo photography and electrophotography. It is a photographic method. However, the silver halide photographic materials used in this method require a wet processing step to obtain stable images, which is time-consuming and labor-intensive, and the handling of chemicals can be harmful to the human body. There was a problem. Therefore, a photographic method capable of obtaining stable images through dry processing while using silver halide is highly desired, and much research has been carried out to date. For example, Japanese Patent Publication No. 43-4921 or No. 43-4921
The most successful heat-developable photosensitive material is the three-component composition of a reducible organic silver salt, a reducing agent, and a photosensitive silver halide in catalytic contact with the organic silver salt, as described in Publication No. 4924. This is an example. After imagewise exposure of such a heat-developable photosensitive material, an image is formed by heating the material to usually 80° C. or higher, preferably 100° C. or higher. Since this heat-developable photosensitive material has a low content of photosensitive silver halide, which is unstable to light, it does not require any particular stabilization treatment after image formation.
Therefore, such heat-developable photosensitive materials can provide stable and high-quality images without any wet process. In such heat-developable photosensitive materials, photosensitive silver halide is important as it determines the photographic properties of the heat-developable photosensitive material, and in particular, it contains fine particles of silver chloride, silver bromide, silver chlorobromide, and silver iodine. Silver bromide is said to be preferred. The first method for preparing silver halide is to convert a part of a reducible organic silver salt into silver halide using ammonium bromide or sodium chloride, which is described in Japanese Patent Publication No. 4924/1983. How to convert and Tokuko Sho 53-40484
A method of thermally decomposing an N-halogeno compound and converting a part of the reducible organic silver salt into photosensitive silver halide, which is a so-called in-situ silver halide preparation technique, described in the above publication can be mentioned. . In this first method, a part of the reducible organic silver salt is halogenated to convert it into photosensitive silver halide, which brings about an unfavorable change in most other reducible organic silver salts. This must be avoided. The formation and sensitization methods of photosensitive silver halide that meet these requirements are naturally subject to limitations. Therefore, it is difficult to simply apply the sensitization methods used in wet silver halide photographic emulsions, especially the methods of increasing sensitivity by adding chemical sensitizers. For the above reasons, a second method, the so-called ex-situ silver halide technique, has been proposed. This heat-developable photosensitive composition containing an ex-situ silver halide is produced by forming the photosensitive silver halide in advance at a location separate from the reducible organic silver salt and then mixing it with the reducible organic silver salt. prepared. However, as is clear from Japanese Patent Publications No. 43-4921 and No. 43-4924, photosensitive silver halide prepared by a conventional silver halide photographic emulsion method is not preferred. This is because photographic emulsions using gelatin as a protective colloid have strong adsorption between silver halide and gelatin. This is because it cannot be obtained. Furthermore, silver halide prepared in the absence of a protective colloid (eg, gelatin) causes aggregation between silver halide particles, making it unsuitable for use as a photoreceptor for heat-developable photosensitive materials. Many attempts have been made to compensate for these drawbacks and to produce photosensitive silver halides that can effectively come into contact with reducible organic silver salts. For example, UK Patent No. 1362970
In the specification, an organic solvent containing an oil-soluble binder and an aqueous solution of an inorganic silver compound are emulsified by ultrasonic dispersion, an inorganic halogen compound dissolved in the organic solvent is added to this emulsion, and a photosensitive material is added to the oil-soluble binder. A method of forming a synthetic silver halide is described. However, the photosensitive silver halide prepared by this method cannot produce particles with a uniform shape and size distribution, and requires complicated operations such as ultrasonic dispersion and decantation to remove the aqueous phase. shall be.
JP-A-47-9432 and JP-B-Sho 52-17415 disclose photosensitive silver halide by reacting an inorganic silver compound soluble in a polar organic solvent (for example, acetone) with an inorganic halogen compound in an oil-soluble binder. A method for forming the is described. However, even with this method, particles with uniform particle shape and particle size distribution cannot be obtained, and agglomeration is likely to occur. JP-A-50-32926 and JP-A-54-4117 disclose that photosensitive silver halide is formed in an aqueous or water-organic solvent emulsion, and then a reducible organic silver salt is photosensitive. A method for preparing the compound by mixing it with a silver halide is described.
However, in this method, after the photosensitive silver halide is formed, it is exposed to chemically active conditions or placed in a high temperature atmosphere. It is impossible to maintain the characteristics of the various sensitization treatments applied to sexual silver halide. JP-A-47-9171 and JP-A-47-
No. 9308 describes the formation of photosensitive silver halides in the presence of new amphiphilic copolymers, and JP-A-50-32928 describes the formation of photosensitive silver halides in the presence of surfactants. However, this method is also difficult to operate, and it is difficult to prepare silver halide with uniform grains. An object of the present invention is to provide a heat-developable photosensitive material with high image density and high contrast. In order to achieve such an objective, the present inventors have conducted various studies and found that organic fatty acid silver suspended and dispersed in an organic solvent is maintained at a predetermined temperature, and an inorganic or organic halogen compound is added to this dispersion. It has been found that when stoichiometrically added photosensitive silver halide is almost quantitatively formed. Further, the silver halide grains thus formed were fine grains with a narrow particle size distribution, and did not aggregate or settle when left for a long time. It has also been found that more favorable results can be obtained when a binder soluble in an organic solvent is co-present as a protective colloid during silver halide formation. Furthermore, by using the silver halide thus formed as a photoreceptor in a heat-developable photosensitive material, a heat-developable photosensitive material having excellent photographic properties such as sensitivity, image density, and gradation can be obtained. I understood. The photosensitive silver halide of the present invention is formed by suspending and dispersing component (a), organic fatty acid silver, in an organic solvent, and adding component (b), an inorganic or organic halogen compound, to this dispersion. The organic fatty acid silver of component (a) is poorly soluble or insoluble in organic solvents, and is preferably an organic fatty acid silver having 5 or more carbon atoms, such as silver caproate, silver caprylate, silver caprate, silver lauric acid. Silver, silver myristate, silver palmitate, silver stearate, silver alainate, silver behenate, silver lignocerate, silver oleate, silver linoleate, silver linoleate, silver hydroxystearate, silver 11-bromoundecanoate, etc. Examples include substituted or unsubstituted saturated or unsaturated fatty acid silver. Number of carbons in organic fatty acid silver is 4
If the particle diameter is less than 1, it is difficult to produce silver halide grains with a uniform shape and a narrow particle size distribution, so it is not very preferable. The preparation of such organic fatty acid silver is
A common method is to add a solution of a silver salt such as silver nitrate, ammoniacal silver nitrate, or a silver complex salt to a solution of an organic fatty acid or an alkali metal salt of an organic fatty acid dissolved in an appropriate solvent. The inorganic or organic halogen compound of component (b) is
It is capable of reacting with the organic fatty acid silver of component (a) to form silver halide. Examples of the inorganic halogen compound include compounds represented by the general formula MXn. However, in the formula, M is a hydrogen atom or a metal atom (for example, strontium, cadmium, zinc, sodium, barium, cesium, calcium, iron, nickel, magnesium, potassium, aluminum, antimony, gold, cobalt, mercury,
(lead, beryllium, lithium, indium, iridium, rhodium, palladium, platinum, bismuth, etc.), X represents a chlorine atom, a bromine atom, or an iodine atom, and n represents the valence of each cation. Examples of inorganic halogen compounds include halogen-containing metal complexes such as K 2 PtCl 6 , K 2 PtBr 6 , HAuCl 4 ,
(HN 4 ) 2 IrCl 6 , (HN 4 ) 3 IrCl 6 , (HN 4 ) 3 RuCl 6 ,
Examples include K 3 RhCl 6 . Organic halogen compounds are also effective as halogenating agents, and in particular when organic halogen compounds are used, photosensitive silver halide with uniform grain size and shape can be prepared. Preferred organic halogen compounds include compounds represented by the following general formula (1) or (2). In the formula, X represents a chlorine atom, a bromine atom, or an iodine atom, and Z represents a group of nonmetallic atoms necessary to form a 4- to 8-membered ring, and this 4- to 8-membered ring is fused with another ring. Good too. Z is preferably a 5-membered ring or a 6-membered ring
It is a membered ring, and specific examples include a pyrrole ring, a pyrroline ring, a pyrrolidine ring, an imidazoline ring, an imidazolidine ring, a pyrazoline ring, an oxazolidine ring, a piperidine ring, an oxazine ring, a piperazine ring, and an indoline ring. Furthermore, Z is 4
~8-membered lactam ring, hydantoin ring, cyanuric ring, hexahydrotriazine ring, indoline ring, etc. may be formed. Furthermore, this ring may have a substituent such as an unsubstituted or substituted alkyl group, an unsubstituted or substituted aryl group, an alkoxy group, a halogen atom, or an oxo group. A represents a carbonyl group or a sulfonyl group, and R 1 and R 2 represent a hydrogen atom, an unsubstituted or substituted alkyl group, an unsubstituted or substituted aryl group, or an alkoxy group. Representative examples of compounds represented by the above general formula (1) include N-bromsuccinimide, N-bromotetrafluorosuccinimide, N-bromophthalimide, N-bromglutarimide, 1,3-dibrom-5, 5-dimethyl-2,4-imidazolidinedione, N,N'-dibromo-5,5-diethylbarbituric acid, N-bromoisocyanuric acid, N,N'-dibromoisocyanuric acid, N-bromooxazolinone , N-bromphthalazinone,
Examples include N-chlorsuccinimide, N-iodosuccinimide, N-chlorphthalimide, N-bromusactucalin, N-bromocaprolactam, N-bromobutyrolactam, N,N'-dibromothiohydantoin, and the like. . Representative examples of compounds represented by the above general formula (2) include N-bromoacetamide, N-bromoacetanilide, N-bromobenzenesulfonylanilide, N-bromobenzamide, N-chloroacetamide, N-bromonaphthamide, -Brom-
P-hydroxybenzamide and the like can be mentioned. Further, halogenated melamine can also be used as the organic halogen compound, and specific examples include tribromemelamine, trichloromelamine, and the like. Furthermore, as an organic halogen compound, a C-halogen compound represented by the following general formula (3) is also effective. In the formula, X represents a chlorine atom, a bromine atom, or an iodine atom, and R 3 , R 4 , and R 5 may be the same or different from each other, and represent a hydrogen atom, an unsubstituted or substituted alkyl group, an unsubstituted or substituted alkyl group, Aryl group, nitro group, acyl group, unsubstituted or substituted amide group,
It represents a sulfonyl group bonded to an unsubstituted or substituted aryl group or alkyl group, or a halogen atom. However, at least one of R 3 , R 4 , and R 5 helps release a halogen atom, and represents, for example, a nitro group, an unsubstituted or substituted aryl group, an alkenyl group, an acyl group, an amide group, a sulfonyl group, etc. . As the compound represented by the above general formula (3), α
Examples include -haloketone compounds, α-haloamide compounds, halosulfonyl compounds, halonitro lower alkane compounds, and compounds having an unsaturated bond at the carbon β position relative to the halogen atom. Specific examples of the compound represented by general formula (3) include α-bromoacetophenone, α-chloroacetophenone, α-bromo-α-phenylacetophenone, α-bromo-1,3-diphenyl -1,
3-propanedione, α-bromo-2,5-dimethoxyacetophenone, α-bromomethylsulfonylbenzene, α-bromo-α-benzenesulfonylacetamide, α-chloro-α-(P-tolylsulfonyl)acetamide , α-bromo-γ
-Nitro-β-phenylbutyrophenone, α-iodo-γ-nitro-β-phenylbutyrophenone, 2-bromo-2-nitro-1,3-propanediol, 2-bromo-2-nitrotri Methylene-1,3-bis(phenyl carbonate), α-
Bromotoluene, α,P-dibromotoluene,
α, α′-dibromo-m-xylene, α, α, α′,
Examples include α'-tetrabromo-P-xylene and 3-bromopropene. Among the above-mentioned compound examples, compounds in which the carbon at the β-position of the halogen atom has an unsaturated bond, such as α-bromotoluene and 3-bromopropene, are particularly useful. Onium halide compounds are also useful as halogenating agents in the present invention; specific examples include ammonium bromide, trimethylphenylammonium chloride, cetylethyldimethylammonium bromide, trimethylbenzylammonium bromide, tetraethylphosphonium bromide, and trimethylsulfonium chloride. etc. can be mentioned. The present invention provides the above-mentioned components.
The organic fatty acid silver of (a) and the inorganic or organic halogen compound of component (b) are mixed, and a reaction for converting all or most of the organic fatty acid silver of component (a) into photosensitive silver halide is carried out in an organic solvent. Therefore, the amount of halogen compound used in component (b) is the same as that in component (a).
The amount may be stoichiometric with respect to the organic fatty acid silver.
However, it is preferable to use the halogen compound of component (b) in an excess amount, that is, in the range of about 1.0 mol to about 3.0 mol per 1 mol of organic fatty acid silver of component (a). In the present invention, component (a) organic fatty acid silver and component
The organic solvent used in the reaction of the halogen compound (b) is liquid at the reaction temperature and is capable of uniformly dispersing the organic fatty acid silver of component (a) and dissolving a certain amount of the halogen compound of component (b). If possible, there are no particular limitations. Specifically, alcohols, ketones, aliphatic hydrocarbons, aromatic hydrocarbons, alcohols, ethers, acid amides, and the like can be used alone or as a mixture. Specific examples of alcohols include fatty alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, sec-butyl alcohol, n-amyl alcohol, isoamyl alcohol, and n-hexyl alcohol. Aliphatic unsaturated alcohols such as group saturated alcohols, allyl alcohol and propargyl alcohol, alicyclic alcohols such as cyclopentanol and cyclohexanol, aralkyl alcohols such as benzyl alcohol and cinnamyl alcohol, polyhydric alcohols such as ethylene glycol and glycerin. etc. can be mentioned. Specific examples of ketones include aliphatic saturated ketones such as acetone, methyl ethyl ketone, methyl propyl ketone, isopropyl methyl ketone, butyl methyl ketone, and isobutyl methyl ketone; unsaturated aliphatic ketones such as methyl vinyl ketone and methyl heptene ketone; Examples include alicyclic ketones such as cyclobutanone and cyclohexanone, and aromatic ketones such as acetophenone, propiophenone and butylphenone. Specific examples of esters include methyl formate, propyl formate, amyl formate, ethyl acetate, methyl acetate, butyl acetate, isobutyl acetate, methyl propionate, ethyl propionate, isopropyl propionate, methyl butyrate, ethyl butyrate, and ethyl isobutyrate. , methyl isovalerate, isopropyl isovalerate, methyl benzoate, ethyl phthalate, and the like. Specific examples of ethers include dimethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, methyl butyl ether,
Saturated aliphatic ethers such as ethyl propyl ether and ethyl isoamyl ether, unsaturated aliphatic ethers such as diallyl ether and ethyl allyl ether, aromatic ethers such as anisole and phenyl ether, and cyclic ethers such as tetrahydrofuran and dioxane. can be mentioned. Specific examples of aliphatic hydrocarbons include n-heptane, n-hexane, 3-methylpentane, 2,3
- Saturated aliphatic hydrocarbons such as dimethylbutane, cyclohexane, cycloheptane, cyclohexene,
Unsaturated aliphatic hydrocarbons such as cyclopentadiene and cyclopentene can be mentioned. Specific examples of aromatic hydrocarbons include benzene, toluene, xylene, chlorobenzene, indene, and tetralin. In addition, solvents containing nitrogen atoms or sulfur atoms, such as dimethylacetamide, dimethylformamide, and dimethyl sulfoxide, can also be used. Particularly preferred among the above organic solvents are alcohols or ketones alone or in mixtures with the other solvents mentioned above. Mixed systems of water-alcohols and water-ketones can also be used. In preparing the photosensitive silver halide of the present invention, the ingredients
The organic fatty acid silver (a) is suspended and dispersed in the above-mentioned organic solvent using a well-known dispersion technique such as a homomixer, ball mill, sand mill, ultrasonic disperser, etc.
This suspension is referred to as a liquid (A), and a liquid in which an inorganic or organic halogen compound as a component (b) is dispersed, preferably dissolved, in the above-mentioned organic solvent is referred to as a liquid (B). Liquid (A) and liquid (B)
Although the concentration can be set arbitrarily, it is preferably in the range of 0.5% by weight to 50% by weight. The method of mixing liquid (A) and liquid (B) is a technique known in the field of photographic technology.
For example, a forward flow method, a reverse flow method, a simultaneous mixing method, etc. can be used. However, a simple and preferred method is to add liquid (B) to liquid (A) which is being stirred. liquid
Regarding the addition method of (B), photosensitive silver halide can be formed by any of the methods of adding at once, adding intermittently, and adding gradually continuously. However, in order to make the grain size and shape of the silver halide grains uniform and to grow the grains, a method of adding intermittently or gradually and continuously is preferred. Furthermore, the method of addition under control of the oxidation-reduction potential described in Japanese Patent Publication No. 54-24012 can also be applied to the above-mentioned addition method. The time required for addition of liquid (B) cannot be set uniquely because it changes depending on reaction conditions, such as stirring speed and reaction temperature. However, for operational reasons, it is preferable to set the time to 30 minutes to 5 hours. The reaction time from the start of the reaction to the end of the reaction can be set to the end of addition of liquid (B), but generally speaking
It is preferable to continue the reaction for an additional 30 minutes to 24 hours after the addition of (B) is complete. In the method for forming photosensitive silver halide of the present invention, dissociation of silver ions of organic fatty acid silver as component (a),
In order to help generate halogen ions from the halogen compound of component (b), the reaction temperature is 0°C or higher, especially about 20°C.
It is preferable to set the temperature above 100°C.
The reaction temperature is determined by the organic fatty acid silver used as component (a), the halogen compound used as component (b), and the reaction solvent used. Generally, the longer the alkyl chain of the silver organic fatty acid of component (a), the more preferably the temperature is set. Furthermore, when an inorganic halogen compound is used as component (b), the reaction temperature can be set to a slightly lower temperature than when an organic halogen compound is used. Furthermore, when alcohols are mainly used as the reaction solvent, the temperature can be set lower than that of other solvents. When forming the photosensitive silver halide of the present invention, in addition to heating, a reaction accelerator,
For example, an acidic substance such as trifluoroacetic acid or a basic substance such as pyridine may be added to form coarse silver halide grains that are stable in an organic solvent. In the present invention, a polymer soluble in the reaction solvent, preferably in the dispersion solvent of liquid (A), can be added thereto. The addition of a polymer soluble in an organic solvent improves the dispersibility of the organic fatty acid silver of component (a), allows uniform reaction of the organic fatty acid silver of component (a) and the halogen compound of component (b), It is also possible to prevent irregular growth and aggregation of the photosensitive silver halide formed. Polymers that can be used for this purpose are, for example, polyvinyl acetate, polyvinyl propionate, polymethyl methacrylate, ethyl cellulose, cellulose acetate, nitrocellulose, polyethylene, ethylene-vinyl acetate copolymers, chlorinated polyethylene, polyvinyl chloride, Vinyl chloride-vinyl acetate copolymer, chlorinated polypropylene, polyvinyl acetal, acrylic resin, polystyrene, epoxy resin, modified melamine resin, alkyd resin, polyamide, chlorinated rubber,
Examples include acrylonitrile-butadiene-styrene terpolymer, silicone block copolymer, polyvinylpyrrolidone, polyethylene oxide, high molecular weight paraffin, and the vinyl copolymer described in JP-A-47-9432.
Among the above polymers, preferred are those that can be dissolved in alcohols or ketones alone or in a mixed solvent with other organic solvents, and particularly preferred polymers are polyvinyl acetals. The amount of the polymer soluble in the organic solvent used is about 0.05 g to about 20 g per 1 g of the organic fatty acid silver salt of component (a).
Preferably it ranges from about 0.1 g to about 10 g. Next, preferred embodiments of the procedure for preparing the photosensitive silver halide of the present invention will be described. Organic fatty acid silver is uniformly dispersed in an organic solvent (e.g. n-butanol), a polymer soluble in the organic solvent (e.g. polyvinyl butyral) is added and stirred to dissolve it, and the organic fatty acid silver containing the polymer is suspended and dispersed. Prepare the liquid. This dispersion is maintained at a constant temperature while stirring under a safe light, and an inorganic or organic halogen compound dissolved in a suitable organic solvent (for example, acetone) is added thereto for about 30 minutes to about 5 hours, preferably about 30 minutes to about 5 hours. Add intermittently or gradually continuously over 3 hours. After the addition is completed, the reaction temperature is maintained and the reaction is continued for about 30 minutes to about 24 hours, preferably about 30 minutes to 8 hours. This can be determined by measuring the redox potential. When an N-halogeno compound is used as the halogen compound, it can also be determined by decolorizing a merocyanine dye as described in Japanese Patent Publication No. 40484/1984). After the reaction is completed, the reaction solution is returned to room temperature to obtain a mixed dispersion of photosensitive silver halide and a by-product organic fatty acid or an organic fatty acid that does not use silver as a cation. The photosensitive silver halides prepared according to the invention are silver chloride, silver iodide, silver bromide, silver chlorobromide, silver iodobromide, silver iodochloride and silver chloroiodobromide. The photosensitive silver halide prepared according to the present invention can be subjected to known chemical sensitization methods used in conventional wet silver halide emulsions, such as sulfur sensitization, gold sensitization, reduction sensitization, etc., to increase the inherent sensitivity. be able to. Furthermore, the photosensitive silver halide prepared according to the present invention can be processed by known spectral sensitization methods, such as cyanine dyes, styryl dyes, hemicyanine dyes, triphenylmethane dyes, xanthene dyes, oxonol dyes, merocyanine dyes, especially "product licensing". Index, Volume 92, Pages 107-110 (published December 1971), or Belgian Patent No.
Spectral sensitization can be performed as described in No. 772371. The photosensitive silver halide prepared according to the present invention is an oxidized silver halide comprising a reducible organic silver salt and a reducing agent.
It has extremely favorable properties as a photosensitive component for a reduced image forming component, and therefore, by using the photosensitive silver halide prepared according to the present invention, a heat-developable photosensitive material with excellent photographic properties can be provided. can do. That is, at least (c) an oxidation-reduction image forming component comprising a reducible organic silver salt and a reducing agent, (d)
In a heat-developable photosensitive material having at least one layer of a photosensitive composition consisting of a photosensitive silver halide and (e) a binder, as (d) a photosensitive silver halide, a photosensitive composition prepared according to the present invention; Silver halide can be suitably used. As a result of many years of research on such photosensitive silver halide, the present inventors found that it is effective when the silver halide has fine grains of around 0.1μ, and in particular, when the silver halide is a normal crystal of [1.0.0], The present inventors have discovered that silver particles are effective, and furthermore, the present inventors have discovered that photosensitive silver halide particles formed by the reaction of organic fatty acid silver suspended and dispersed in the above-mentioned organic solvent and an inorganic or organic halide compound. However, it has been found that the above-mentioned conditions are satisfied and it is preferable for the production of heat-developable photosensitive materials. The reason why these conditions are satisfied is that the photosensitive silver halide prepared by the present invention has a narrow and fine particle size distribution, and can provide a heat-developable photosensitive material with high image density and high contrast. can. The photosensitive silver halide prepared according to the present invention is easily and stably dispersed in an organic solvent, and is therefore advantageous in the production of heat-developable photosensitive materials. The photosensitive silver halide dispersion prepared according to the present invention can be used to produce a heat-developable photosensitive material without washing operations such as reprecipitation, decantation, and centrifugation, without causing fogging during heat development. Not a cause. The following points can be mentioned. As mentioned above, the heat-developable photosensitive material of the present invention has the following features:
The above three components (c), (d), and (e) are present as essential components in at least one layer provided on the support. In the oxidation-reduction image forming component consisting of a reducible organic silver salt and a reducing agent as component (c), the reducible organic silver salt is a colorless, white, or light-colored silver salt that is relatively stable to light. The coexisting silver halide is exposed to light, and the metallic silver produced as a core is heated at a temperature of 80°C.
When heated at a temperature of 100° C. or higher, preferably 100° C. or higher, it reacts with a reducing agent to form a silver image. Specifically, Japanese Patent Publication No. 43-4924 and Japanese Patent Publication No.
46-6074, or a silver salt of an organic compound having an imino group or a mercapto group. In particular, a silver salt of a long chain fatty acid having 12 to 24 carbon atoms is This is preferable because it is less susceptible to undesirable changes such as darkening. Specifically, silver behenate, silver stearate, silver palmitate, silver myristate, silver laurate, silver oleate or silver hydroxystearate can be mentioned,
Among them, silver behenate is particularly effective. In addition, a part of the above-mentioned reducible organic silver salt has been converted to silver halide by the method described in Japanese Patent Publication No. 43-4924, Japanese Patent Publication No. 53-40484, etc. You can also use things. Various reducing agents can be used in the above-mentioned oxidation-reduction image forming component. In general, developers used in conventional silver halide photosensitive materials, specifically hydroquinone, methylhydroquinone, chlorohydroquinone, methylhydroxynaphthalene, N,N'-diethyl-P-phenylenediamine, aminophenol, Examples include ascorbic acid, 1-phenyl-3-pyrazolidone, etc. In addition to these, 2,2'-methylenebis(6-t-butyl-4-methylphenol), 4,4'-butylidenebis(6- t-butyl-3-methylphenol), 4,4'-thiobis(6-t-butyl-3-methylphenol), etc.
Furthermore, bisnaphthol-based reducing compounds described in JP-A No. 46-6074 or Belgian Patent No.
Examples include sulfonamidophenol compounds such as 4-benzenesulfonamidophenol described in No. 802519. Furthermore, two or more of the above reducing agents may be used in combination. The amount of such reducing agent ranges from about 0.05 mole to about 5 mole, preferably from about 0.2 mole to about 3 mole per mole of reducible organic silver salt. The photosensitive silver halide of component (d) in the present invention is prepared by the method described above, and includes silver chloride, silver bromide, silver iodide, silver chlorobromide, silver iodochloride, silver iodobromide. It is one or a mixture of two or more selected from silver and silver chloroiodobromide, preferably prepared from organic fatty acid silver having 16 or more carbon atoms, and containing 30% silver bromide.
It contains mol% or more. The photosensitive silver halide of component (d) is produced either while containing by-products or after being subjected to washing operations such as reprecipitation, decantation, and centrifugation.
It is redispersed and mixed with a dispersion containing a reducible organic silver salt. Component (d), the photosensitive silver halide, may be added at any time during the manufacturing process of the heat-developable photosensitive material as long as it is contained in the same layer where it can come into contact with the reducible organic silver salt. Further, the preparation of a uniform dispersion of photosensitive silver halide and reducible organic silver salt can be easily achieved using a conventional stirrer, ball mill dispersion, ultrasonic dispersion, or the like. The amount of photosensitive silver halide added as component (d) is in the range of about 0.01 mol to about 0.5 mol per mol of reducible organic silver salt,
Preferably it ranges from about 0.05 mole to about 0.3 mole. If the amount used is outside this range, i.e. 0.01 mol or less, practical photographic properties cannot be obtained, and
If the amount is 0.5 mol or more, the background color changes significantly after image formation. The binder component (e) of the present invention can be used alone or in combination of two or more. Suitable materials for the binder can be hydrophobic or hydrophilic, and transparent or translucent.
Specifically, polyvinyl butyral, cellulose acetate butyrate, polymethyl methacrylate, polyvinylpyrrolidone, ethyl cellulose, cellulose acetate, polyvinyl acetate, polyvinyl alcohol, gelatin, and the sulfobetaine repeating unit described in Canadian Patent No. 774054. Among them, polyvinyl butyral is particularly preferred. The amount of the binder to be used is preferably about 10:1 to 1:10, more preferably about 4:1 to 1:2, based on the weight ratio of the reducible organic silver salt. The heat-developable photosensitive material of the present invention preferably contains one or more toning agents in order to obtain a black image. Examples include phthalazinone and its derivatives as described in US Pat. No. 3,080,254, cyclic imides as described in JP-A No. 46-6074, and phthalazinedione compounds as described in JP-A-50-32927. be able to. In the heat-developable photosensitive material of the present invention, a known antifoggant can be used for the purpose of preventing thermal fog during development. For example, mercury compounds described in Japanese Patent Publication No. 47-11113, Japanese Patent Publication No. 49-10724, Japanese Patent Publication No. 1977-10724,
N described in each publication No. 25808 and No. 54-23813
- Halogeno compounds, higher fatty acids such as stearic acid and behenic acid described in U.S. Patent No. 3,645,739 and JP-A-48-89720, and acids such as salicylic acid, tetrabromobenzoic acid, phthalic acid, trimellitic acid, etc. Stabilizers and the like can be mentioned. The heat-developable photosensitive material of the present invention may contain a suitable spectral sensitizer. Useful sensitizing dyes include cyanine dyes, merocyanine dyes, and xanthene dyes, especially "Product Licensing Index" Vol. 92, pp. 107-110 (published December 1971)
Or Belgian Patent No. 772371, JP-A-Sho
No. 47-6329, JP-A No. 105127-1987, JP-A-51-
127719, JP-A-52-80829, etc. are useful. Furthermore, it may contain a compound that prevents photodiscoloration after image formation. For example, U.S. Pat.
Azole thioethers and blocked azolethiones described in US Patent No. 3839041, tetrazolylthione compounds described in US Patent No. 3700457, and halogen-containing organic oxidations described in US Patent No. 3707377. Agent, U.S. Patent No.
1-carbamoyl-2-tetrazoline-5-thiones described in No. 3893859 can be used. Other suitable additives, such as development accelerators, curing agents, antistatic agents (layers), ultraviolet absorbers, optical brighteners, filter dyes (layers), may also be added.
etc. can also be used. The heat-developable photosensitive material of the present invention comprises component (c) a reducible organic silver salt and a reducing agent, component (d) a photosensitive silver halide, component (e) a binder, and the various additives mentioned above in a suitable solvent. It can be obtained by dispersing or dissolving the solution in water and coating it on a support in a single layer or in multiple layers. Furthermore, an overcoat polymer layer can be provided on the heat-developable photosensitive layer formed of a single layer or multiple layers. Suitable polymer layers include, for example:
Examples include polyvinyl butyral, polystyrene, polymethyl methacrylate, polyurethane rubber, chlorinated rubber, ethyl cellulose, cellulose acetate butyrate, cellulose acetate, polyvinyl chloride, polyvinylidene chloride, polycarbonate, and polyvinylpyrrolidone. Alternatively, the above polymer may be provided as an undercoat layer on a support, and the heat-developable photosensitive layer of the present invention may be laminated thereon. The support used in the present invention can be selected from a wide variety of supports. Typical supports include synthetic resin films such as polyethylene, polypropylene, polyethylene terephthalate, polycarbonate, and cellulose acetate, synthetic papers, papers coated with resin films such as polyethylene, papers such as art paper, and photographic baryta paper. , metal plates (foils) such as aluminum, synthetic resin films having metal vapor-deposited films by ordinary methods, glass plates, and the like. Application methods include roll coating method, air knife method,
Known methods such as a kiss coating method, a curtain coating method, a bar coating method, and a hopper coating method can be used. The heat-developable photosensitive material of the present invention is exposed to light from a light source such as a xenon lamp, a mercury lamp, a tungsten lamp, or a CRT laser beam, and then heated at 80°C to 180°C.
It is preferably developed at a heating temperature range of 110°C to 150°C. Although development can be carried out outside the above-mentioned temperature range by extending or shortening the heating time, it is preferable that the developing time is usually in the range of about 1 second to 60 seconds. The usual method for heat development is to bring the material into contact with a heating plate or heating drum, but other means for temporarily holding the material in a heated atmosphere may also be used, or high frequency heating or infrared light may be used. It is also possible to employ heating means such as Hereinafter, the present invention will be explained in more detail based on examples. Production Example 1 3.9 g of silver stearate was added to 100 ml of isopropyl alcohol and dispersed using a homomixer.
After this dispersion, add 3g of polyvinyl butyral,
A polymer suspension dispersion of silver salt was prepared by stirring and dissolving. This dispersion was heated to 50℃ under a red safety light, and lithium bromide was dissolved in 30ml of acetone while stirring.
0.9 g was added dropwise over 1 hour. After the dropwise addition, the reaction temperature was maintained for 2 hours and stirring was continued, and then the dispersion was cooled to room temperature to obtain a photosensitive silver halide dispersion (1). The obtained dispersion (1) did not precipitate even after being left for a long time. A part of this dispersion was added to xylene/n-
Diluted approximately 5 times with a solution of butanol (50/50 by volume), centrifuged (6000 RPM), removed the supernatant in which polyvinyl butyral was dissolved by decantation, and placed the residue on a glass plate. It was dried and used as sample (1). Electron microscopy of this sample (1) using the replica method (1000x, 10000x, and 30000x)
The type and particle size distribution of the silver halide grains were observed (measurements were also carried out in the same manner in the production series and comparative production examples described later). Table 1 shows the results obtained.

【表】 表−1の結果より、この方法により調製される
ハロゲン化銀は、結晶型の整つた粒度分布の狭
い、更に極めて微細なハロゲン化銀粒子であるこ
とがわかる。 比較製造例 1 英国特許第1362970号明細書に基づきハロゲン
化銀を調製した。2.35モル濃度の硝酸銀水溶液5
mlと、ポリビニルブチラール7.5gを溶解させた
アセトン/トルエン(体積比で50/100)の溶液
150mlを混合し、超音波分散で乳化させた。この
乳化物を液温25℃に保ち超音波分散を続けなが
ら、これに0.23モル濃度の臭化リチウムのアセト
ン溶液50mlを2分間で、滴下して臭化銀の分散物
(イ)を調製した。この分散物(イ)の一部をエタノール
で希釈し、遠心分離操作によりポリビニルブチラ
ールを除去して試料(イ)を作成した。表−2に得ら
れた結果を示す。
[Table] From the results in Table 1, it can be seen that the silver halide prepared by this method is extremely fine silver halide grains with a well-organized crystal type and narrow particle size distribution. Comparative Production Example 1 Silver halide was prepared according to British Patent No. 1362970. 2.35 molar silver nitrate aqueous solution 5
ml and a solution of acetone/toluene (50/100 by volume) in which 7.5 g of polyvinyl butyral is dissolved.
150ml was mixed and emulsified by ultrasonic dispersion. While maintaining the liquid temperature of this emulsion at 25℃ and continuing ultrasonic dispersion, 50 ml of an acetone solution of 0.23 molar lithium bromide was added dropwise over 2 minutes to form a dispersion of silver bromide.
(a) was prepared. A portion of this dispersion (A) was diluted with ethanol, and polyvinyl butyral was removed by centrifugation to prepare a sample (A). Table 2 shows the results obtained.

【表】 * 電子顕微鏡測定試料作成時に除去
表−2の結果より、この方法により調製される
感光性ハロゲン化銀は、結晶型が不揃いで粒度分
布の広いものであることがわかる。 比較製造例 2 特公昭52−17415号公報の記載に従いハロゲン
化銀を調製した。臭化リチウム1.2gとポリビニ
ルブチラール2.4gを溶解したアセトン溶液40ml
を30℃に保ち、撹拌下この溶液にトリフルオロ酢
酸と酸化銀から合成したトリフルオロ酢酸銀3.0
gを溶解したアセトン溶液40mlを2分で滴下して
分散物(ロ)を調製した。得られた分散物(ロ)の40mlを
時間を置かずに、撹拌されている水400ml中へ投
じ沈澱物を得た。これを濾別し乾燥後、臭化銀−
ポリビニルブチラール固形物(ロ)′を得た。この固
形物をキシレン/n−ブタノール(体積比で50/
50)100mlに再溶解させ、製造例1と同様の操作
により電子顕微鏡用の試料(ロ)を作成した。別にト
リフルオロ酢酸陰イオンとリチウム陽イオンの共
存する上記ハロゲン化銀分散液を2時間放置し
て、一部沈澱を生じた分散液(ハ)を得た。分散物(ハ)
を製造例1と同様に処理して電子顕微鏡用の試料
(ハ)を作成した。表−3に得られた結果を示す。
[Table] *Removed during preparation of sample for electron microscopy From the results in Table 2, it can be seen that the photosensitive silver halide prepared by this method has an irregular crystal type and a wide particle size distribution. Comparative Production Example 2 Silver halide was prepared according to the description in Japanese Patent Publication No. 52-17415. 40ml of acetone solution containing 1.2g of lithium bromide and 2.4g of polyvinyl butyral
Silver trifluoroacetate 3.0 synthesized from trifluoroacetic acid and silver oxide was added to this solution while stirring at 30°C.
A dispersion (b) was prepared by adding 40 ml of an acetone solution containing g dissolved therein dropwise over 2 minutes. 40 ml of the obtained dispersion (b) was immediately poured into 400 ml of water under stirring to obtain a precipitate. After filtering and drying this, silver bromide-
A polyvinyl butyral solid (b)' was obtained. This solid was mixed with xylene/n-butanol (volume ratio: 50/
50) A sample for electron microscopy (b) was prepared by redissolving in 100 ml and performing the same procedure as in Production Example 1. Separately, the above silver halide dispersion in which trifluoroacetic acid anions and lithium cations coexisted was allowed to stand for 2 hours to obtain a dispersion (c) in which some precipitation had occurred. Dispersion (c)
was processed in the same manner as in Production Example 1 to prepare a sample for electron microscopy.
(c) was created. Table 3 shows the results obtained.

【表】 表−3の結果より、この方法によつて調製され
る感光性ハロゲン化銀の粒子径は不揃いであり、
また放置による粒子径の増大も生じ易いことがわ
かる。 製造例 2 ベヘン酸銀4.5gをエタノール100mlに入れホモ
ミキサーを用いて分散し、得られた分散液にポリ
ビニルブチラール3gを加え、撹拌溶解して銀塩
のポリマー分散液を作つた。この分散液を赤色安
全光下で45℃に加熱調温し、撹拌下メタノール30
mlに溶解した臭化アンモニウム1.0gを30分で滴
下した。滴下後1時間温度を保ち撹拌を続け、後
に分散液を室温まで下げ分散物(2)を調製した。こ
の分散物(2)は長時間放置してもハロゲン化銀の沈
降は見られなかつた。この分散物(2)から製造例1
と同様に試料(2)を作成した。分散物(2)と反応温度
を60℃にする以外は同様の方法で分散物(3)を作成
し、分散物(3)より試料(3)を作成した。更に臭化ア
ンモニウムの代わりに塩化アンモニウム0.56gを
用いる他は分散物(3)と同様の条件で分散物(4)を調
製し、分散物(4)より試料(4)を作成した。電子顕微
鏡による得られた試料の測定結果を表−4に示
す。
[Table] From the results in Table 3, the grain size of the photosensitive silver halide prepared by this method is irregular;
It can also be seen that the particle size tends to increase due to standing. Production Example 2 4.5 g of silver behenate was placed in 100 ml of ethanol and dispersed using a homomixer, and 3 g of polyvinyl butyral was added to the resulting dispersion and dissolved with stirring to prepare a polymer dispersion of silver salt. This dispersion was heated to 45°C under a red safety light, and stirred with methanol 30°C.
ml of ammonium bromide was added dropwise over 30 minutes. After the dropwise addition, the temperature was maintained for 1 hour and stirring was continued, and then the dispersion was cooled to room temperature to prepare a dispersion (2). This dispersion (2) showed no precipitation of silver halide even after being left for a long time. Production example 1 from this dispersion (2)
Sample (2) was prepared in the same manner as above. Dispersion (3) was prepared in the same manner as dispersion (2) except that the reaction temperature was changed to 60° C., and sample (3) was prepared from dispersion (3). Further, a dispersion (4) was prepared under the same conditions as dispersion (3) except that 0.56 g of ammonium chloride was used instead of ammonium bromide, and a sample (4) was prepared from the dispersion (4). Table 4 shows the measurement results of the obtained sample using an electron microscope.

【表】 表−4の結果より、この方法により微細な粒度
分布の狭いハロゲン化銀粒子が得られることがわ
かる。 製造例 3 製造例2の分散物(2)において、臭化アンモニウ
ム−メタノールに代えて臭化カリウム1.25g−エ
タノール/グリセリン(体積比は50/50)30mlを
用いて製造例2の分散物(2)と同様に分散物(5)を得
た。この分散物(5)は、室温で沈降を生じるが、デ
カンテーシヨンで沈澱物を分取し、ポリビニルブ
チラール3gをキシレン/n−ブタノールの混合
物100mlに溶かし溶液に再分散したところ、良好
な分散物となつた。この分散物より試料(5)を作成
した。又製造例2の分散物(2)の臭化アンモニウム
−メタノールに代えて、臭化第2水銀3.8g−メ
タノール30mlの溶液を用い分散物(2)と同様に分散
物(6)を調製し、分散物(6)より試料(6)を作成した。
電子顕微鏡による得られた試料(5),(6)の測定結果
を表−5に示す。
[Table] From the results in Table 4, it can be seen that fine silver halide grains with a narrow particle size distribution can be obtained by this method. Production Example 3 In the dispersion (2) of Production Example 2, 1.25 g of potassium bromide-30 ml of ethanol/glycerin (volume ratio 50/50) was used instead of ammonium bromide-methanol. A dispersion (5) was obtained in the same manner as in 2). This dispersion (5) causes precipitation at room temperature, but when the precipitate was separated by decantation and 3 g of polyvinyl butyral was dissolved in 100 ml of a xylene/n-butanol mixture and redispersed in the solution, good dispersion was observed. It became a thing. Sample (5) was prepared from this dispersion. In addition, dispersion (6) was prepared in the same manner as dispersion (2) using a solution of 3.8 g of mercuric bromide and 30 ml of methanol instead of ammonium bromide-methanol in dispersion (2) of Production Example 2. Sample (6) was prepared from dispersion (6).
Table 5 shows the measurement results of samples (5) and (6) obtained using an electron microscope.

【表】 表−5の結果から、この方法により得られる感
光性ハロゲン化銀の粒子は、微細であり、かつ粒
度分布も狭いことがわかる。 製造例 4 製造例1と同様な操作で、カプリン酸銀2.5g
とポリビニルブチラール6gを含むキシレン/n
−ブタノール(体積比で50/50)分散液100mlを
調製した。この分散液を2分して赤色安全光下そ
れぞれ20℃及び45℃に保ち、撹拌下アセトン15ml
に溶解したN−ブロムコハク酸イミド0.93gを1
時間かけて滴下した。滴下後さらに20℃で反応し
たものは12時間、45℃で反応したものについては
2時間反応を続け、室温にもどして分散物(7),(8)
を得た。得られた分散物は極めて安定であつた。
この分散物より試料(7),(8)を作成した。同様の操
作で、パルミチン酸銀3.6g、ベヘン酸銀4.5gに
つき反応を行い、試料(9),(10),(11),(12)を作
成した。表−6に反応条件及び電子顕微鏡による
測定結果を示す。
[Table] From the results in Table 5, it can be seen that the photosensitive silver halide grains obtained by this method are fine and have a narrow particle size distribution. Production Example 4 Using the same procedure as Production Example 1, add 2.5 g of silver caprate.
and xylene/n containing 6 g of polyvinyl butyral
- 100 ml of a butanol (50/50 by volume) dispersion was prepared. This dispersion was divided into two parts and kept at 20℃ and 45℃ under red safety light, respectively, and 15ml of acetone was added under stirring.
0.93 g of N-bromosuccinimide dissolved in
It dripped over time. After the dropwise addition, the reaction continued for 12 hours for those reacted at 20°C, and for 2 hours for those reacted at 45°C, and then returned to room temperature to form dispersions (7), (8).
I got it. The resulting dispersion was extremely stable.
Samples (7) and (8) were prepared from this dispersion. In the same manner, 3.6 g of silver palmitate and 4.5 g of silver behenate were reacted to prepare samples (9), (10), (11), and (12). Table 6 shows the reaction conditions and the results of measurement using an electron microscope.

【表】 表−6の結果より、有機ハロゲン化合物として
N−ハロゲノ化合物を用いると、粒子の形状の揃
つた微細で粒度分布の狭いハロゲン化銀が得られ
ることがわかる。 製造例 5 製造例1と同様な操作で、但し有機脂肪酸銀と
してベヘン酸銀4.5g、反応溶媒としてn−ブタ
ノール100mlを用いて、ポリビニルブチラール3
gを含む銀塩のポリマー分散液を60℃に保ち、赤
色安全光下で撹拌下アセトン30mlに溶解したN−
ヨードコハク酸イミドの2.4gを15等分し5分間
隔で滴下した。滴下終了後更に3時間反応を続
け、次いで室温にもどし強い黄着色の分散物
(13)を得た。この分散物(13)より試料(13)
を作成した。電子顕微鏡による測定結果を表−7
に示す。
[Table] From the results in Table 6, it can be seen that when an N-halogen compound is used as the organic halogen compound, a fine silver halide with a uniform grain shape and a narrow particle size distribution can be obtained. Production Example 5 Polyvinyl butyral 3
A polymer dispersion of silver salt containing g was maintained at 60 °C and dissolved in 30 ml of acetone under red safety light with stirring.
2.4 g of iodosuccinimide was divided into 15 equal parts and added dropwise at 5 minute intervals. After the dropwise addition was completed, the reaction was continued for another 3 hours, and then the mixture was allowed to return to room temperature to obtain a strong yellow dispersion (13). Sample (13) from this dispersion (13)
It was created. Table 7 shows the measurement results using an electron microscope.
Shown below.

【表】 表−7の結果より、ハロゲン化銀が沃化銀であ
つても形状の揃つたハロゲン化銀粒子が得られる
ことがわかる。 製造例 6 製造例5と同様の操作で、但しハロゲン化合物
としてN−ブロムコハク酸イミド1.8gとN−ヨ
ードコハク酸イミド0.12gの混合物を用いて、沃
臭化銀分散物(14)を作成し、この分散物(14)
より試料(14)を作成した。電子顕微鏡による測
定結果を表−8に示す。
[Table] From the results in Table 7, it can be seen that even when silver halide is silver iodide, silver halide grains with uniform shapes can be obtained. Production Example 6 A silver iodobromide dispersion (14) was prepared in the same manner as in Production Example 5, except that a mixture of 1.8 g of N-bromosuccinimide and 0.12 g of N-iodosuccinimide was used as the halogen compound. This dispersion (14)
Sample (14) was prepared from Table 8 shows the measurement results using an electron microscope.

【表】 表−8の結果より、ハロゲン化銀が沃臭化銀で
あつてもハロゲン化銀粒子の形状の揃つた微細で
粒度分布の狭いハロゲン化銀が得られることがわ
かる。 製造例 7 製造例5と同様に、ポリマーを含むベヘン酸銀
のポリマー分散液を調製し、この分散液にN−ブ
ロムコハク酸イミド3.6g(ベヘン酸銀に対し2
倍モルを使用)を、反応温度60℃で1時間で添加
し更に2時間反応した。次いで室温にもどし分散
物(15)を得た。この分散物(15)より試料
(15)を作成した。表−9に電子顕微鏡による測
定結果を示す。
[Table] From the results in Table 8, it can be seen that even if the silver halide is silver iodobromide, fine silver halide grains with uniform shapes and a narrow particle size distribution can be obtained. Production Example 7 In the same manner as Production Example 5, a polymer dispersion of silver behenate containing a polymer was prepared, and 3.6 g of N-bromosuccinimide (2.0 g per silver behenate) was added to this dispersion.
(using twice the molar amount) was added over one hour at a reaction temperature of 60°C, and the reaction was continued for an additional 2 hours. The temperature was then returned to room temperature to obtain a dispersion (15). A sample (15) was prepared from this dispersion (15). Table 9 shows the measurement results using an electron microscope.

【表】 表−9の結果より、ハロゲン化合物を過剰に用
いても、生成するハロゲン化銀粒子の結晶型は整
つており、また微細な粒度分布の狭いハロゲン化
銀が得られることがわかる。 製造例 8 ベヘン酸銀4.5gを次の9種の溶媒、エタノー
ル、n−プロパノール、イソプロピルアルコー
ル、n−ブタノール、イソブチルアルコール、
sec−ブタノール、ベンジルアルコール、メチル
エチルケトン及びn−プロパノール/トルエン
(体積比で50/50)100mlに分散し、更にポリビニ
ルブチラール2gを加え撹拌溶解して銀塩のポリ
マー分散液を調製した。このそれぞれの分散液を
60℃に加温し、赤色安全光下でアセトン30mlに溶
解したN−ブロムアセトアミド1.5gを1時間で
添加し、更に2時間反応を行つた。次いで室温に
もどし得られた分散物から試料(16)〜(24)を
作成した。表−10に電子顕微鏡による測定結果を
示す。
[Table] From the results in Table 9, it can be seen that even if an excessive amount of the halogen compound is used, the crystal type of the silver halide grains produced is well-ordered, and silver halide with a fine and narrow particle size distribution can be obtained. Production Example 8 4.5g of silver behenate was mixed with the following nine solvents: ethanol, n-propanol, isopropyl alcohol, n-butanol, isobutyl alcohol,
The mixture was dispersed in 100 ml of sec-butanol, benzyl alcohol, methyl ethyl ketone, and n-propanol/toluene (50/50 by volume), and 2 g of polyvinyl butyral was added and dissolved with stirring to prepare a polymer dispersion of silver salt. Each of these dispersions
The mixture was heated to 60 DEG C., and 1.5 g of N-bromoacetamide dissolved in 30 ml of acetone was added over 1 hour under a red safety light, and the reaction was continued for an additional 2 hours. Samples (16) to (24) were then prepared from the resulting dispersion which was returned to room temperature. Table 10 shows the measurement results using an electron microscope.

【表】 表−10の結果より、反応溶媒としてアルコール
類、ケトン類及びアルコール類と他の有機溶媒の
混合溶媒を用いた場合、ハロゲン化銀粒子の形状
の整つた微細で粒子分布の狭いハロゲン化銀が得
られることがわかる。 製造例 9 ベヘン酸銀2.3gをシクロヘキサノール50mlに
分散し、更にポリビニルブチラール1.5gを加え
撹拌溶解し、銀塩のポリマー分散液を調製した。
この分散液を70℃に加温して、赤色安全光下α−
ブロムトルエン0.9gをアセトンで稀釈して30ml
としたものを2時間で滴下した。更に1時間反応
を続け、次いで室温にもどし分散物(25)を調製
した。この分散物(25)より試料(25)を作成し
た。電子顕微鏡による測定結果を表−11に示す。
[Table] From the results in Table 10, when alcohols, ketones, and mixed solvents of alcohols and other organic solvents are used as the reaction solvent, the silver halide grains are fine and have a narrow particle distribution. It can be seen that silver oxide can be obtained. Production Example 9 2.3 g of silver behenate was dispersed in 50 ml of cyclohexanol, and 1.5 g of polyvinyl butyral was added and dissolved with stirring to prepare a polymer dispersion of silver salt.
This dispersion was heated to 70℃ and α-
Dilute 0.9g of bromotoluene with acetone and make 30ml
The solution was added dropwise over a period of 2 hours. The reaction was continued for an additional hour, and then the temperature was returned to room temperature, and a dispersion (25) was prepared. A sample (25) was prepared from this dispersion (25). Table 11 shows the measurement results using an electron microscope.

【表】 表−11の結果より、有機ハロゲン化合物として
C−ハロゲン化合物を用いても、ハロゲン化銀の
粒子の形状の整つた微粒子のハロゲン化銀が得ら
れことがわかる。 製造例 10 製造例9と同様の操作で、但しα−ブロムトル
エンに代えて3−ブロモプロペン2.4g及び3−
ブロモプロピル2.5gを使用し、反応温度を80℃
とした。尚この場合の反応は、コンデンサーを設
けた反応容器中で行い、分散物(26),(27)を調
製した。この分散物より試料(26),(27)を作成
した。表−12に電子顕微鏡による測定結果を示
す。
[Table] From the results in Table 11, it can be seen that even when a C-halogen compound is used as the organic halogen compound, fine-grained silver halide particles with well-shaped silver halide grains can be obtained. Production Example 10 Same procedure as Production Example 9, except that 2.4 g of 3-bromopropene and 3-bromopropene were used instead of α-bromotoluene.
Using 2.5g of bromopropyl, the reaction temperature was 80℃.
And so. The reaction in this case was carried out in a reaction vessel equipped with a condenser, and dispersions (26) and (27) were prepared. Samples (26) and (27) were prepared from this dispersion. Table 12 shows the measurement results using an electron microscope.

【表】 表−12の結果より、ハロゲンのβ位の炭素に不
飽和結合を持つ化合物は、本発明のハロゲン化剤
として有効であることがわかる。 製造例 11 製造例8の試料(16)を作成したのと同様の条
件で、但し保護コロイドとしてポリビニルブチラ
ールに代えて、ニトロセルロースを同量用いて分
散物(28)を調製した。この分散物より試料
(28)を作成した。表−13に電子顕微鏡による測
定結果を示す。
[Table] From the results in Table 12, it can be seen that compounds having an unsaturated bond at the β-carbon of the halogen are effective as the halogenating agent of the present invention. Production Example 11 A dispersion (28) was prepared under the same conditions as for preparing sample (16) in Production Example 8, except that polyvinyl butyral was replaced with the same amount of nitrocellulose as the protective colloid. A sample (28) was prepared from this dispersion. Table 13 shows the measurement results using an electron microscope.

【表】 表−13の結果より、保護コロイドとしてニトロ
セルロースを用いても粒子の形状の整つた微粒子
のハロゲン化銀が得られることがわかる。 実施例 1 ベヘン酸銀51g、ベヘン酸39gをキシレン440
ml及びn−ブタノール440mlから成る分散溶媒に
入れホモミキサーを用いて分散した。この分散液
にバインダーとしてポリビニルブチラール80gを
加え、撹拌して銀塩のポリマー分散液を調製し
た。この分散液を82gづつ分け取り、それぞれに
下記に示す臭化銀分散物を混合した。 A 製造例1で調製した分散物(1)の10.0g B 比較製造例2で調製した分散物(ロ)の10.0g C 比較製造例2で調製した固形物(ロ)′の0.42g
をキシレン/n−ブタノール(体積比で50/50)
100mlに再溶解したもの 上記3種類の臭化銀を含むベヘン酸銀のポリマ
ー分散液の各々に、次の成分を順次添加して感光
性スラリーを調製した。 2,2′−ビス−(2−ヒドロキシ−3,5−ジ
メチルフエニル)−3,5,5−トリメチルヘキ
サン4gとエタノール10mlからなる溶液 酢酸第2水銀 0.005g 1−カルボキシメチル−5−〔(3−エチルナフ
ト〔1,2−d〕オキサゾリン−2−イリデン)
−エチリデン〕−3−アリル−チオヒダントイン
0.0013g この3種の感光性スラリーを、塩化ビニル−酢
酸ビニル(87.13重量比)を1m2当たり1gの下
塗り層を設けたアート紙上に、1m2当たり銀量で
0.55gとなる様に塗布し乾燥した。更にこの塗布
面上に下記の上塗り組成物を、乾燥時1m2当たり
1.5gになる様に塗布し、画像試験の為の試料(A),
(B),(C)を作成した。尚、下記の操作は全て赤色安
全光下で行つた。 上塗り組成物 セルロースアセテート 15.0g フタラジノン 7.5g アセトン 300ml 上記の試料(A),(B)及び(C)を赤色安全光下で光学
楔(コダツクステツプタブレツトNo.2)を通しタ
ングステン光700ルツクス秒の露光を与えた。次
いで125℃の温度で10秒間加熱現像を施して、各
光量に応じた階段状の画像を得た。得られた画像
の感度(S),階調度()、反射最大濃度
(Dmax)及び熱カブリ濃度(Dmin)を測定した
(後述する実施例においても同様に測定した。)結
果を表−14に示す。尚、表中の感度は熱カブリ+
0.15の濃度を与えるのに必要な露光量の逆数と
し、試料(B)の感度を100とした相対感度で表示し
た(後述する実施例においても同様に表示した)。
[Table] From the results in Table 13, it can be seen that even when nitrocellulose is used as a protective colloid, fine grained silver halide particles with well-shaped grains can be obtained. Example 1 51 g of silver behenate and 39 g of behenic acid were mixed with 440 g of xylene.
ml and n-butanol, and dispersed using a homomixer. 80 g of polyvinyl butyral was added as a binder to this dispersion and stirred to prepare a polymer dispersion of silver salt. This dispersion was divided into 82 g portions, and each portion was mixed with the silver bromide dispersion shown below. A 10.0 g of dispersion (1) prepared in Production Example 1 B 10.0 g of dispersion (B) prepared in Comparative Production Example 2 C 0.42 g of solid material (B)' prepared in Comparative Production Example 2
xylene/n-butanol (50/50 by volume)
Redissolved in 100 ml The following components were sequentially added to each of the above polymer dispersions of silver behenate containing the three types of silver bromide to prepare photosensitive slurries. Solution consisting of 4 g of 2,2'-bis-(2-hydroxy-3,5-dimethylphenyl)-3,5,5-trimethylhexane and 10 ml of ethanol Mercury acetate 0.005 g 1-Carboxymethyl-5-[ (3-ethylnaphtho[1,2-d]oxazolin-2-ylidene)
-ethylidene]-3-allyl-thiohydantoin
0.0013 g of these three types of photosensitive slurries were applied to art paper with an undercoat layer of 1 g of vinyl chloride-vinyl acetate (87.13 weight ratio) per m 2 at the amount of silver per 1 m 2 .
It was applied to a weight of 0.55g and dried. Furthermore, on this coated surface, apply the following topcoat composition per 1 m 2 when dry.
Coat it to a weight of 1.5g and prepare a sample for image testing (A).
(B) and (C) were created. All of the following operations were performed under red safety light. Topcoat composition Cellulose acetate 15.0 g Phthalazinone 7.5 g Acetone 300 ml Samples (A), (B) and (C) above were exposed to 700 lux of tungsten light through an optical wedge (Kodak Step Tablet No. 2) under red safety light. A second exposure was given. Next, heat development was performed at a temperature of 125° C. for 10 seconds to obtain step-like images corresponding to each amount of light. The sensitivity (S), gradation (), maximum reflection density (Dmax), and thermal fog density (Dmin) of the obtained image were measured (measurements were made in the same manner in the examples described later). The results are shown in Table 14. show. In addition, the sensitivity in the table is thermal fog +
It was expressed as the reciprocal of the exposure amount required to give a density of 0.15, and expressed as a relative sensitivity with the sensitivity of sample (B) set as 100 (the same expression was used in Examples described later).

【表】 表−14の結果より、本発明の熱現像性感光材料
である試料(A)は、従来品の試料(B),(C)に比べ硬調
で高濃度であることがわかる。 実施例 2 実施例1と同様に試料(D),(E)を作成し写真特性
を測定した。尚ハロゲン化銀分散物は下に示す臭
化銀分散物を用いた。 D 製造例4で調製した分散物(9)の11.0g E 製造例4で調製した分散物(11)の11.0g 測定結果を表−15に示す。
[Table] From the results in Table 14, it can be seen that sample (A), which is the heat-developable photosensitive material of the present invention, has a higher contrast and higher density than the conventional samples (B) and (C). Example 2 Samples (D) and (E) were prepared in the same manner as in Example 1, and their photographic properties were measured. As the silver halide dispersion, the silver bromide dispersion shown below was used. D 11.0 g of the dispersion (9) prepared in Production Example 4 E 11.0 g of the dispersion (11) prepared in Production Example 4 The measurement results are shown in Table-15.

【表】 表−15の結果より、有機脂肪酸銀とN−ハロゲ
ン化合物より調製されるハロゲン化銀を感光体と
した熱現像性感光材料は高感度であることがわか
る。 実施例 3 実施例2と同様に、但し臭化銀分散物として製
造例9の分散物(25)12.0gを用いて試料(F)を作
成し、下記の表−16に示す測定結果を得た。
[Table] From the results in Table 15, it can be seen that the heat-developable photosensitive material using a silver halide photoreceptor prepared from organic fatty acid silver and an N-halogen compound has high sensitivity. Example 3 Sample (F) was prepared in the same manner as in Example 2, except that 12.0 g of the dispersion (25) of Production Example 9 was used as the silver bromide dispersion, and the measurement results shown in Table 16 below were obtained. Ta.

【表】 表−16の結果より、有機ハロゲン化合物として
C−ハロゲノ化合物を用いて調製される感光性ハ
ロゲン化銀を感光体とした熱現像性感光材料は、
感度、階調度、最大濃度が高くカブリ濃度の低い
優れた熱現像性感光材料であることがわかる。 実施例 4 実施例2と同様に試料(6)を作成した。但しハロ
ゲン化銀分散物は、製造例7の分散物(15)10.5
gを遠心分離機(8000RPM,30分)にかけ上澄
み液を除去し、残留する沈澱物にポリビニルブチ
ラール0.3gを溶解したキシレン/n−ブタノー
ルの溶液を加え、超音波分散したものを用いた。
得られた試料(G)は、感度、階調度、最大濃度が高
く、最低濃度が低い優れた熱現像性感光材料であ
つた。 実施例 5 実施例2と同様に試料(H)を作成した。但しハロ
ゲン化銀分散物として、製造例6の分散物(14)
10.2gを用いた。表−17に測定結果を示す。
[Table] From the results in Table 16, the heat-developable photosensitive material prepared using a C-halogeno compound as an organic halogen compound and using a photosensitive silver halide as a photoreceptor is as follows:
It can be seen that this is an excellent heat-developable photosensitive material with high sensitivity, gradation, and maximum density, and low fog density. Example 4 Sample (6) was prepared in the same manner as in Example 2. However, the silver halide dispersion is the dispersion of Production Example 7 (15) 10.5
g was centrifuged (8000 RPM, 30 minutes) to remove the supernatant liquid, and a xylene/n-butanol solution in which 0.3 g of polyvinyl butyral was dissolved was added to the remaining precipitate, which was then dispersed by ultrasonic waves.
The obtained sample (G) was an excellent heat-developable photosensitive material having high sensitivity, gradation, and maximum density, and low minimum density. Example 5 Sample (H) was prepared in the same manner as in Example 2. However, as the silver halide dispersion, the dispersion of Production Example 6 (14)
10.2g was used. Table 17 shows the measurement results.

【表】 表−17の結果より、本発明の感光性ハロゲン化
銀が沃臭化銀の場合においても、優れた特性を有
する熱現像性感光材料が得られることがわかる。 実施例 6 実施例2と同様の操作で試料()を作成し
た。但しベヘン酸銀に代えてパルチンミ酸銀0.4
gを用い、ハロゲン化銀分散物は製造例8の分散
物(16)10.0gを用いた。表−18に測定結果を示
す。
[Table] The results in Table 17 show that even when the photosensitive silver halide of the present invention is silver iodobromide, a heat-developable photosensitive material having excellent properties can be obtained. Example 6 A sample () was prepared in the same manner as in Example 2. However, silver partinmate 0.4 is used instead of silver behenate.
g, and 10.0 g of the dispersion (16) of Production Example 8 was used as the silver halide dispersion. Table 18 shows the measurement results.

【表】 表−18の結果より、本発明の試料()は、感
度、階調度及び最大濃度が高いことがわかる。
[Table] From the results in Table 18, it can be seen that the sample () of the present invention has high sensitivity, gradation, and maximum density.

Claims (1)

【特許請求の範囲】 1 支持体上に少なくとも(c)被還元性有機銀塩及
び還元剤から成る酸化−還元画像形成成分、(d)感
光性ハロゲン化銀及び(e)バインダーから成る感光
組成物の少なくとも1つの層を有する熱現像性感
光材料において、(d)感光性ハロゲン化銀があらか
じめ、有機溶媒中で、(a)有機脂肪酸銀を有機溶媒
中に懸濁分散させた状態で、(b)無機若しくは有機
ハロゲン化合物と化学量論的に反応させることに
より形成されたものであることを特徴とする熱現
像性感光材料。 2 (a)有機脂肪酸銀が炭素数5個以上の有機脂肪
酸銀であることを特徴とする特許請求の範囲第1
項記載の熱現像性感光材料。
[Scope of Claims] 1. A photosensitive composition comprising at least (c) an oxidation-reduction image forming component comprising a reducible organic silver salt and a reducing agent, (d) a photosensitive silver halide, and (e) a binder on a support. (d) photosensitive silver halide in an organic solvent, (a) organic fatty acid silver suspended and dispersed in the organic solvent; (b) A heat-developable photosensitive material characterized in that it is formed by a stoichiometric reaction with an inorganic or organic halogen compound. 2 (a) Claim 1 characterized in that the organic fatty acid silver is an organic fatty acid silver having 5 or more carbon atoms.
The heat-developable photosensitive material described in .
JP1814489A 1989-01-27 1989-01-27 Thermodevelopable photosensitive material Granted JPH0243A (en)