JP7906552B2 - Resin compositions, molded articles, laminates, pipes, hot water circulation pipes, insulated multilayer pipes, and fuel pipes - Google Patents

Resin compositions, molded articles, laminates, pipes, hot water circulation pipes, insulated multilayer pipes, and fuel pipes

Info

Publication number
JP7906552B2
JP7906552B2 JP2022164090A JP2022164090A JP7906552B2 JP 7906552 B2 JP7906552 B2 JP 7906552B2 JP 2022164090 A JP2022164090 A JP 2022164090A JP 2022164090 A JP2022164090 A JP 2022164090A JP 7906552 B2 JP7906552 B2 JP 7906552B2
Authority
JP
Japan
Prior art keywords
resin composition
ppm
evoh
content
pipes
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2022164090A
Other languages
Japanese (ja)
Other versions
JP2023104870A (en
Inventor
瑞子 尾下
達也 長谷川
健太郎 吉田
稔 岡本
公男 岡田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kuraray Co Ltd
Original Assignee
Kuraray Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kuraray Co Ltd filed Critical Kuraray Co Ltd
Publication of JP2023104870A publication Critical patent/JP2023104870A/en
Application granted granted Critical
Publication of JP7906552B2 publication Critical patent/JP7906552B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は樹脂組成物、成形体、積層体、パイプ、温水循環用パイプ、断熱多層パイプ、及び燃料用パイプに関する。 This invention relates to resin compositions, molded articles, laminates, pipes, hot water circulation pipes, insulated multilayer pipes, and fuel pipes.

エチレン-ビニルアルコール共重合体(以下「EVOH」と略記する場合がある。)は酸素等のガス遮断性、耐油性、非帯電性、機械強度、溶融成形性等に優れた高分子材料である。このため、EVOH樹脂組成物は容器、シート、フィルム等の成形材料として広く用いられる。また、酸化防止剤を含有するEVOH樹脂組成物は、フロアヒーティング用、地域熱供給用等の温水循環用パイプ、燃料用パイプ等に成形されて利用されている。容器、パイプ等の成形には、一般に溶融成形が多く用いられる。従って、溶融成形に供される樹脂組成物には、長時間の溶融成形を行ってもフィッシュアイ、ストリーク等の欠陥が発生しないといった、ロングラン性に優れる性能が必要とされる。 Ethylene-vinyl alcohol copolymer (hereinafter sometimes abbreviated as "EVOH") is a polymer material with excellent gas barrier properties (such as oxygen), oil resistance, antistatic properties, mechanical strength, and melt-molding properties. Therefore, EVOH resin compositions are widely used as molding materials for containers, sheets, films, etc. Furthermore, EVOH resin compositions containing antioxidants are molded and used for hot water circulation pipes for floor heating and district heating systems, fuel pipes, etc. Melt molding is generally the most common method for molding containers, pipes, etc. Therefore, resin compositions used in melt molding require excellent long-run performance, such as the absence of defects like fisheyes and streaks even after prolonged melt molding.

しかし、EVOHは分子内に比較的活性な水酸基を有するため、酸素がほとんどない状態の押出成形機内部でも、高温溶融状態で酸化・架橋反応が進行し、熱劣化物が生じる場合がある。特に、長期連続運転を行うと上記熱劣化物が成形機内部に堆積し、フィッシュアイの原因となるゲル・ブツを発生させるため、EVOH樹脂組成物はロングラン性が不十分となる場合がある。 However, because EVOH contains relatively active hydroxyl groups within its molecule, oxidation and crosslinking reactions can proceed even inside an extrusion molding machine where oxygen is almost nonexistent, resulting in the formation of thermally degraded products. In particular, prolonged continuous operation can cause these thermally degraded products to accumulate inside the molding machine, generating gel-like particles that cause fisheyes. Therefore, EVOH resin compositions may have insufficient long-run performance.

これに対し、特許文献1には、EVOH及び0.01~100ppmの不飽和アルデヒドを含む樹脂組成物が、フィッシュアイ、ゲル、ストリーク等の欠陥の発生を抑制し、かつ、ロングラン性に優れることが記載されている。 In contrast, Patent Document 1 describes a resin composition containing EVOH and 0.01 to 100 ppm of unsaturated aldehydes that suppresses the occurrence of defects such as fish eyes, gels, and streaks, and exhibits excellent long-run performance.

また、最近の省資源及び省エネルギーの流れの中で、地域熱供給(地域冷暖房)システムが多く導入されるようになっている。地域熱供給システムは、敷設されたパイプラインにより、複数の建物に対して1か所にまとめた冷暖房・給湯設備から、温水・冷水等を供給するものである。ガスや液体を運ぶ内管、この内管を覆う断熱発泡体層、及びこの断熱発泡体層を覆う外管からなる断熱多層パイプが地域熱供給システムのパイプとして用いられており、断熱発泡体層には、断熱発泡剤として二酸化炭素、ペンタン、シクロペンタン等が使用されている。パイプラインに酸素バリア性を有さないパイプを使用すると、パイプを透過して酸素が循環水中に溶け込んでくるため、システム配管内の金属部分の腐食が進行するおそれがある。そこで長期間システムを維持するため、EVOH層を有した多層パイプが多用されている。しかし、長期使用時における空気中の酸素によるEVOHの酸化劣化の進行が問題となっている。この酸化劣化により力学的強度が低下し、EVOH層の長さ方向に平行なクラックが生成すると、パイプから発泡ガスが拡散し、断熱性能が低下するばかりでなく、システムの金属部分の腐食も進行する。このような問題を解決するため、EVOH層のより一層の長寿命化が求められている。 Furthermore, in the recent trend towards resource and energy conservation, district heating and cooling systems (district heating and cooling) are being widely introduced. District heating and cooling systems supply hot water, chilled water, etc., to multiple buildings from a centralized heating, cooling, and hot water supply facility via laid pipelines. Insulated multi-layer pipes, consisting of an inner pipe for transporting gas or liquid, an insulating foam layer covering the inner pipe, and an outer pipe covering the insulating foam layer, are used as pipes in district heating and cooling systems. Insulating foam layers use insulating foam agents such as carbon dioxide, pentane, and cyclopentane. If pipes without oxygen barrier properties are used in the pipeline, oxygen can permeate the pipes and dissolve into the circulating water, potentially leading to corrosion of metal parts within the system piping. Therefore, to maintain the system over the long term, multi-layer pipes with an EVOH layer are widely used. However, the oxidative degradation of EVOH due to oxygen in the air during long-term use remains a problem. This oxidative degradation reduces mechanical strength, and when cracks parallel to the length of the EVOH layer form, foaming gas diffuses from the pipe, not only reducing thermal insulation performance but also accelerating corrosion of the metal parts of the system. To solve these problems, further extending the lifespan of the EVOH layer is required.

国際公開第2013/146961号International Publication No. 2013/146961

上記特許文献1のEVOH樹脂組成物を用いた場合、Tダイによるフィルム成形において、ダイの有効幅より押出されたフィルムの幅の方が小さくなるネックインが問題となる場合があることが分かった。本発明者らが鋭意検討した結果、驚くべきことに、特定の複数種類の不飽和アルデヒドを特定の比率で含むEVOH樹脂組成物が、かかるネックインを抑制できることを見出した。しかしながら、ネックイン抑制を試み複数種類の不飽和アルデヒドの含有量を調整した際に、上記複数種類の不飽和アルデヒドの比率によっては、溶融樹脂組成物の吐出口(ダイリップ)の外面にダイビルドアップ(目ヤニ:ダイリップ外面の堆積物を意味する)が付着しやすくなるという問題が新たに生じることが分かった。 When using the EVOH resin composition described in Patent Document 1, it was found that neck-in, where the width of the extruded film is smaller than the effective width of the die, can occur during film molding using a T-die. After diligent research by the inventors, surprisingly, it was discovered that an EVOH resin composition containing specific types of unsaturated aldehydes in specific ratios can suppress such neck-in. However, when attempting to suppress neck-in by adjusting the content of the multiple types of unsaturated aldehydes, a new problem arose: depending on the ratio of the multiple types of unsaturated aldehydes, die buildup (deposits on the die lip) tends to adhere to the outer surface of the die lip of the molten resin composition.

一方、EVOH層を最外層として共押出することにより積層体のパイプ等を製造するケースがある。上記のダイビルドアップの発生は、EVOHがダイリップに接する範囲が大きい、EVOH層が積層体の最外層として共押出される場合に欠点を生じ、長期間高温で使用した場合、著しく問題となることがある。 On the other hand, there are cases where laminated pipes and other components are manufactured by co-extruding the EVOH layer as the outermost layer. The die build-up described above occurs when the EVOH layer has a large contact area with the die lip, or when the EVOH layer is co-extruded as the outermost layer of the laminate. This defect can become a significant problem when used at high temperatures for extended periods.

本発明は、このような事情に基づいてなされたものであり、その目的は、EVOHを含む樹脂組成物であって、溶融成形の際のネックイン及びダイビルドアップが抑制されており、長期間高温で使用可能な成形体等を得ることができる樹脂組成物、並びにそれを用いた成形体、積層体、パイプ、温水循環用パイプ、断熱多層パイプ及び燃料用パイプを提供するものである。 This invention was made based on the above circumstances, and its objective is to provide a resin composition containing EVOH that suppresses neck-in and die build-up during melt molding, and that can produce molded articles and the like that can be used at high temperatures for extended periods. Furthermore, it provides molded articles, laminates, pipes, hot water circulation pipes, insulated multilayer pipes, and fuel pipes using the same.

上記の目的は、
[1]エチレン単位含有量が20モル%以上60モル%以下であるエチレン-ビニルアルコール共重合体(A)(以下「EVOH(A)」と略記する場合がある)、クロトンアルデヒド(B1)及び酸化防止剤(G)を含み、2,4-ヘキサジエナール(B2)及び2,4,6-オクタトリエナール(B3)からなる群より選ばれる少なくとも1種をさらに含み、下記式(1)及び(2)を満たし、酸化防止剤(G)の含有量gが0.01質量%以上5質量%以下である、樹脂組成物;
2.0≦b1/(b2+b3)<150.0 ・・・(1)
b2+2b3≦0.65 ・・・(2)
上記式(1)及び(2)中、b1は、EVOH(A)に対するクロトンアルデヒド(B1)の含有量(ppm)であり、b2は、EVOH(A)に対する2,4-ヘキサジエナール(B2)の含有量(ppm)であり、b3は、EVOH(A)に対する2,4,6-オクタトリエナール(B3)の含有量(ppm)である。
[2]EVOH(A)に対するクロトンアルデヒド(B1)、2,4-ヘキサジエナール(B2)及び2,4,6-オクタトリエナール(B3)の含有量の合計(b1+b2+b3)が0.01ppm以上7.0ppm以下である、[1]の樹脂組成物;
[3]クロトンアルデヒド(B1)の含有量b1が0.01ppm以上4.0ppm以下である、[1]又は[2]の樹脂組成物;
[4]2,4-ヘキサジエナール(B2)の含有量b2が0.005ppm以上0.65ppm以下である、[1]~[3]のいずれかの樹脂組成物;
[5]2,4,6-オクタトリエナール(B3)の含有量b3が0.325ppm以下である、[1]~[4]のいずれかの樹脂組成物;
[6]共役ポリエン化合物(C)をさらに含み、EVOH(A)に対する共役ポリエン化合物(C)の含有量cが1ppm以上300ppm未満である、[1]~[5]のいずれかの樹脂組成物;
[7]共役ポリエン化合物(C)がソルビン酸である、[6]の樹脂組成物;
[8]熱可塑性エラストマー(F)をさらに含有し、熱可塑性エラストマー(F)のEVOH(A)に対する質量比(F/A)が5/95以上35/65以下である、[1]~[7]のいずれかの樹脂組成物;
[9]熱可塑性エラストマー(F)が、ポリエステル系熱可塑性エラストマー、ポリスチレン系熱可塑性エラストマー及びポリオレフィン系熱可塑性エラストマーからなる群より選ばれる少なくとも1種である、[8]の樹脂組成物;
[10][1]~[9]のいずれかの樹脂組成物からなる部分を有する成形体;
[11][1]~[9]のいずれかの樹脂組成物からなる層を少なくとも1層有する積層体;
[12][1]~[9]のいずれかの樹脂組成物からなる層を有するパイプ;
[13][12]のパイプからなる温水循環用パイプ;
[14]断熱発泡体層をさらに有する[12]のパイプからなる断熱多層パイプ;
[15][12]のパイプからなる燃料用パイプ;
を提供することで達成される。
The purpose of the above is,
[1] A resin composition comprising an ethylene-vinyl alcohol copolymer (A) (which may be abbreviated as "EVOH(A)") having an ethylene unit content of 20 mol% or more and 60 mol% or less, crotonaldehyde (B1), and an antioxidant (G), further comprising at least one selected from the group consisting of 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3), satisfying the following formulas (1) and (2), and having an antioxidant (G) content of 0.01% by mass or more and 5% by mass or less;
2.0≦b 1 /(b 2 +b 3 )<150.0 (1)
b2 + 2b3 ≦0.65...(2)
In formulas (1) and (2) above, b1 is the content of crotonaldehyde (B1) relative to EVOH (A) (ppm), b2 is the content of 2,4-hexadienal (B2) relative to EVOH (A) (ppm), and b3 is the content of 2,4,6-octatrienal (B3) relative to EVOH (A) (ppm).
[2] The resin composition of [1], wherein the total content of crotonaldehyde (B1), 2,4-hexadienal (B2), and 2,4,6-octatrienal (B3) relative to EVOH (A) ( b1 + b2 + b3 ) is 0.01 ppm or more and 7.0 ppm or less;
[3] The resin composition of [1] or [2], wherein the content of crotonaldehyde (B1) b1 is 0.01 ppm or more and 4.0 ppm or less;
[4] A resin composition of any of [1] to [3], wherein the content of 2,4-hexadienal (B2) b2 is 0.005 ppm or more and 0.65 ppm or less;
[5] A resin composition of any of [1] to [4], wherein the content of 2,4,6-octatrienal (B3) b3 is 0.325 ppm or less;
[6] A resin composition according to any of [1] to [5], further comprising a conjugated polyene compound (C), wherein the content c of the conjugated polyene compound (C) relative to EVOH (A) is 1 ppm or more and less than 300 ppm;
[7] The resin composition of [6] wherein the conjugated polyene compound (C) is sorbic acid;
[8] A resin composition according to any of [1] to [7], further containing a thermoplastic elastomer (F), wherein the mass ratio of the thermoplastic elastomer (F) to EVOH (A) (F/A) is 5/95 or more and 35/65 or less;
[9] The resin composition of [8] wherein the thermoplastic elastomer (F) is at least one selected from the group consisting of polyester-based thermoplastic elastomers, polystyrene-based thermoplastic elastomers, and polyolefin-based thermoplastic elastomers;
A molded article having a portion made of any of the resin compositions [10] [1] to [9];
A laminate having at least one layer made of any of the resin compositions of [11] [1] to [9];
[12] A pipe having a layer made of any of the resin compositions of [1] to [9];
A hot water circulation pipe consisting of pipes [13] and [12];
[14] Insulated multilayer pipes consisting of the pipe of [12] further having an insulating foam layer;
Fuel pipe consisting of pipes [15] and [12];
This is achieved by providing [the necessary services/services].

本発明によれば、EVOHを含む樹脂組成物であって、溶融成形の際のネックイン及びダイビルドアップが抑制されており、長期間高温で使用可能な成形体等を得ることができる樹脂組成物、並びにそれを用いた成形体、積層体、パイプ、温水循環用パイプ、断熱多層パイプ及び燃料用パイプを提供できる。 According to the present invention, a resin composition containing EVOH is available that suppresses neck-in and die build-up during melt molding, enabling the production of molded articles and the like that can be used at high temperatures for extended periods. Furthermore, molded articles, laminates, pipes, hot water circulation pipes, insulated multilayer pipes, and fuel pipes using the same are also available.

<樹脂組成物>
本発明の樹脂組成物は、EVOH(A)、クロトンアルデヒド(B1)及び酸化防止剤(G)を含み、2,4-ヘキサジエナール(B2)及び2,4,6-オクタトリエナール(B3)からなる群より選ばれる少なくとも1種をさらに含み、下記式(1)及び(2)を満たし、酸化防止剤(G)の含有量gが、0.01質量%以上5質量%以下である。
2.0≦b1/(b2+b3)<150.0 ・・・(1)
b2+2b3≦0.65 ・・・(2)
上記式(1)及び(2)中、b1は、EVOH(A)に対するクロトンアルデヒド(B1)の含有量(ppm)であり、b2は、EVOH(A)に対する2,4-ヘキサジエナール(B2)の含有量(ppm)であり、b3は、EVOH(A)に対する2,4,6-オクタトリエナール(B3)の含有量(ppm)である。なお、本明細書において、ppmで表される含有量は、質量基準の含有量である。
<Resin composition>
The resin composition of the present invention comprises EVOH (A), crotonaldehyde (B1), and an antioxidant (G), further comprising at least one selected from the group consisting of 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3), satisfying the following formulas (1) and (2), and the content of antioxidant (G) in g is 0.01% by mass or more and 5% by mass or less.
2.0≦b 1 /(b 2 +b 3 )<150.0 (1)
b2 + 2b3 ≦0.65...(2)
In formulas (1) and (2) above, b1 is the content of crotonaldehyde (B1) relative to EVOH (A) (ppm), b2 is the content of 2,4-hexadienal (B2) relative to EVOH (A) (ppm), and b3 is the content of 2,4,6-octatrienal (B3) relative to EVOH (A) (ppm). In this specification, the content expressed in ppm is the content on a mass basis.

b1/(b2+b3)の値が2.0以上150.0未満であることでネックイン耐性が良好となる傾向にある。一方、2,4-ヘキサジエナール(B2)及び2,4,6-オクタトリエナール(B3)は、ダイビルドアップへ影響を与え、特に2,4,6-オクタトリエナール(B3)は、ダイビルドアップへ与える影響が大きい。そのため、b2+2b3の値が0.65ppm以下であることでダイビルドアップが抑制される傾向にある。このため、本発明の樹脂組成物は、溶融成形材料として好適に用いることができる。また、当該樹脂組成物は所定量の酸化防止剤(G)を含むため、当該樹脂組成物からは長期間高温で使用可能な成形体等が得られる。なお、本明細書においてクロトンアルデヒド(B1)、2,4-ヘキサジエナール(B2)及び2,4,6-オクタトリエナール(B3)をまとめて不飽和脂肪族アルデヒド(B)と称する場合がある。 A value of b1 /( b2 + b3 ) between 2.0 and less than 150.0 tends to result in good neck-in resistance. On the other hand, 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3) affect die build-up, and 2,4,6-octatrienal (B3) in particular has a significant effect on die build-up. Therefore, a value of b2 + 2b3 of 0.65 ppm or less tends to suppress die build-up. For this reason, the resin composition of the present invention can be suitably used as a melt molding material. Furthermore, since the resin composition contains a predetermined amount of antioxidant (G), molded articles that can be used at high temperatures for a long period of time can be obtained from the resin composition. In this specification, crotonaldehyde (B1), 2,4-hexadienal (B2), and 2,4,6-octatrienal (B3) may be collectively referred to as unsaturated aliphatic aldehyde (B).

(EVOH(A))
EVOH(A)は、エチレン単位とビニルアルコール単位とを有し、エチレン単位含有量が20モル%以上60モル%以下である共重合体である。EVOH(A)は、通常、エチレン-ビニルエステル共重合体のケン化により得られる。エチレン-ビニルエステル共重合体の製造及びケン化は公知の方法により行うことができる。ビニルエステルとしては、酢酸ビニル、ギ酸ビニル、プロピオン酸ビニル、バレリン酸ビニル、カプリン酸ビニル、ラウリン酸ビニル、ステアリン酸ビニル、ピバリン酸ビニル、バーサティック酸ビニル、及びその他の脂肪族カルボン酸ビニルエステル等が挙げられ、酢酸ビニルが好ましい。
(EVOH(A))
EVOH(A) is a copolymer having ethylene units and vinyl alcohol units, with an ethylene unit content of 20 mol% to 60 mol%. EVOH(A) is usually obtained by saponification of an ethylene-vinyl ester copolymer. The production and saponification of ethylene-vinyl ester copolymers can be carried out by known methods. Examples of vinyl esters include vinyl acetate, vinyl formate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl pivalate, vinyl versaticate, and other aliphatic carboxylic acid vinyl esters, with vinyl acetate being preferred.

EVOH(A)のエチレン単位含有量は20モル%以上であり、25モル%以上が好ましく、27モル%以上がより好ましい。EVOH(A)のエチレン単位含有量は60モル%以下であり、55モル%以下が好ましく、50モル%以下がより好ましい。エチレン単位含有量が20モル%未満では、溶融押出時の熱安定性が低下し、ゲル化しやすくなり、ストリーク、フィッシュアイ、ブツ等が発生する傾向にある。なお、ストリーク、フィッシュアイ、ブツ等の発生は、特に一般的な条件よりも高温または高速で長時間運転する際に顕著になる。エチレン単位含有量が60モル%を超えると、ガスバリア性が低下する傾向にある。 The ethylene unit content of EVOH(A) is 20 mol% or more, preferably 25 mol% or more, and more preferably 27 mol% or more. The ethylene unit content of EVOH(A) is 60 mol% or less, preferably 55 mol% or less, and more preferably 50 mol% or less. If the ethylene unit content is less than 20 mol%, the thermal stability during melt extrusion decreases, gelation becomes more likely, and streaks, fisheyes, and other defects tend to occur. The occurrence of streaks, fisheyes, and other defects becomes particularly noticeable when operating at higher temperatures or speeds for longer periods than typical conditions. If the ethylene unit content exceeds 60 mol%, the gas barrier properties tend to decrease.

EVOH(A)のケン化度は90モル%以上が好ましく、95モル%以上がより好ましく、99モル%以上がさらに好ましい。EVOH(A)のケン化度が90モル%以上であると、本発明の樹脂組成物、及び本発明の樹脂組成物から得られる各種成形体等におけるガスバリア性、熱安定性、耐湿性等が良好となる傾向がある。また、ケン化度は100モル%以下であっても、99.97モル%以下であっても、99.94モル%以下であってもよい。 The degree of saponification of EVOH(A) is preferably 90 mol% or higher, more preferably 95 mol% or higher, and even more preferably 99 mol% or higher. When the degree of saponification of EVOH(A) is 90 mol% or higher, the gas barrier properties, thermal stability, moisture resistance, etc., of the resin composition of the present invention and the various molded articles obtained from the resin composition of the present invention tend to be good. Furthermore, the degree of saponification may be 100 mol% or less, 99.97 mol% or less, or 99.94 mol% or less.

また、EVOH(A)は、本発明の目的が阻害されない範囲で、エチレン単位、ビニルアルコール単位及びビニルエステル単位以外の他の構造単位を有していてもよい。EVOH(A)が上記他の構造単位を有する場合、上記他の構造単位のEVOH(A)の全構造単位に対する含有量は30モル%以下が好ましく、20モル%以下がより好ましく、10モル%以下がさらに好ましく、5モル%以下がよりさらに好ましく、1モル%以下が特に好ましいこともある。また、EVOH(A)が上記他の構造単位を有する場合、その含有量は0.05モル%以上であっても、0.10モル%以上であってもよい。上記他の構造単位は、例えば、アクリル酸、メタクリル酸、クロトン酸、イタコン酸等の不飽和カルボン酸またはその無水物、塩、またはモノ若しくはジアルキルエステル等;アクリロニトリル、メタクリロニトリル等のニトリル;アクリルアミド、メタクリルアミド等のアミド;ビニルスルホン酸、アリルスルホン酸、メタアリルスルホン酸等のオレフィンスルホン酸またはその塩;ビニルトリメトキシシラン、ビニルトリエトキシシラン、ビニルトリ(β-メトキシ-エトキシ)シラン、γ-メタクリルオキシプロピルメトキシシラン等のビニルシラン化合物;アルキルビニルエーテル類、ビニルケトン、N-ビニルピロリドン、塩化ビニル、塩化ビニリデン等に由来する構造単位が挙げられる。 Furthermore, EVOH(A) may have other structural units other than ethylene units, vinyl alcohol units, and vinyl ester units, to the extent that the objectives of the present invention are not hindered. When EVOH(A) has the above-mentioned other structural units, the content of the above-mentioned other structural units relative to the total structural units of EVOH(A) is preferably 30 mol% or less, more preferably 20 mol% or less, even more preferably 10 mol% or less, even more preferably 5 mol% or less, and particularly preferably 1 mol% or less. Also, when EVOH(A) has the above-mentioned other structural units, the content thereof may be 0.05 mol% or more, or 0.10 mol% or more. Other structural units mentioned above include, for example, unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, and itaconic acid, or their anhydrides, salts, or mono- or dialkyl esters; nitriles such as acrylonitrile and methacrylonitrile; amides such as acrylamide and methacrylamide; olefin sulfonic acids such as vinylsulfonic acid, allylsulfonic acid, and methallylsulfonic acid, or their salts; vinylsilane compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxyethoxy)silane, and γ-methacryloxypropylmethoxysilane; and structural units derived from alkyl vinyl ethers, vinyl ketones, N-vinylpyrrolidone, vinyl chloride, vinylidene chloride, etc.

上記他の構造単位は、下記式(I)で表される構造単位(I)、下記式(II)で表される構造単位(II)、及び下記式(III)で表される構造単位(III)の少なくともいずれか一種であってもよい。 The above-mentioned other structural units may be at least one of the structural units represented by formula (I) below (I), structural unit (II) below (II), and structural unit (III) below (III).

式(I)、式(II)及び式(III)中、R1、R2、R3、R4、R5、R6、R7、R8、R9、R10及びR11は、それぞれ独立して、水素原子、炭素数1~10の脂肪族炭化水素基、炭素数3~10の脂環式炭化水素基、炭素数6~10の芳香族炭化水素基または水酸基を表す。また、R1、R2及びR3のうちの一対、R4とR5、R6とR7は結合して環構造の一部を形成していてもよい。上記炭素数1~10の脂肪族炭化水素基、炭素数3~10の脂環式炭化水素基及び炭素数6~10の芳香族炭化水素基が有する水素原子の一部または全部は、水酸基、アルコキシ基、カルボキシ基またはハロゲン原子で置換されていてもよい。式(III)中、R12及びR13は、それぞれ独立して、水素原子、ホルミル基または炭素数2~10のアルカノイル基を表す。 In formulas (I), (II), and (III), R1 , R2 , R3 , R4 , R5 , R6 , R7 , R8 , R9 , R10 , and R11 each independently represent a hydrogen atom, an aliphatic hydrocarbon group having 1 to 10 carbon atoms, an alicyclic hydrocarbon group having 3 to 10 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, or a hydroxyl group. In addition, one pair of R1 , R2 , and R3 , R4 and R5 , and R6 and R7 may be bonded together to form part of a ring structure. Some or all of the hydrogen atoms in the aliphatic hydrocarbon group having 1 to 10 carbon atoms, the alicyclic hydrocarbon group having 3 to 10 carbon atoms, and the aromatic hydrocarbon group having 6 to 10 carbon atoms may be substituted with a hydroxyl group, an alkoxy group, a carboxyl group, or a halogen atom. In formula (III), R 12 and R 13 each independently represent a hydrogen atom, a formyl group, or an alkanoyl group having 2 to 10 carbon atoms.

EVOH(A)が上記構造単位(I)、(II)または(III)を有する場合、樹脂組成物の柔軟性及び加工特性が向上し、得られる各種成形体等における延伸性及び熱成形性等が良好になる傾向がある。 When EVOH(A) contains the above structural units (I), (II), or (III), the flexibility and processing properties of the resin composition tend to improve, and the stretchability and thermoformability of the resulting molded articles tend to be better.

上記構造単位(I)、(II)または(III)において、上記炭素数1~10の脂肪族炭化水素基としてはアルキル基、アルケニル基等が挙げられ、炭素数3~10の脂環式炭化水素基としてはシクロアルキル基、シクロアルケニル基等が挙げられ、炭素数6~10の芳香族炭化水素基としてはフェニル基等が挙げられる。 In the above structural units (I), (II), or (III), examples of aliphatic hydrocarbon groups having 1 to 10 carbon atoms include alkyl groups and alkenyl groups; examples of alicyclic hydrocarbon groups having 3 to 10 carbon atoms include cycloalkyl groups and cycloalkenyl groups; and examples of aromatic hydrocarbon groups having 6 to 10 carbon atoms include phenyl groups.

上記構造単位(I)において、上記R1、R2及びR3は、それぞれ独立に水素原子、メチル基、エチル基、水酸基、ヒドロキシメチル基又はヒドロキシエチル基であることが好ましい。これらの中でも、樹脂組成物における成形性や、得られる各種成形体等における延伸性及び熱成形性をさらに向上させることができる観点から、それぞれ独立に水素原子、メチル基、水酸基又はヒドロキシメチル基であることがより好ましい。 In the above structural unit (I), R1 , R2 , and R3 are preferably each independently a hydrogen atom, a methyl group, an ethyl group, a hydroxyl group, a hydroxymethyl group, or a hydroxyethyl group. Among these, it is more preferable that each independently be a hydrogen atom, a methyl group, a hydroxyl group, or a hydroxymethyl group, from the viewpoint of further improving the moldability of the resin composition and the stretchability and thermoformability of the various molded articles obtained.

EVOH(A)中に上記構造単位(I)を含有させる方法は特に限定されず、例えば、上記エチレンとビニルエステルとの重合において、構造単位(I)に誘導される単量体を共重合させる方法等が挙げられる。構造単位(I)に誘導される単量体としては、例えばプロピレン、ブチレン、ペンテン、ヘキセン等のアルケン;3-ヒドロキシ-1-プロペン、3-アシロキシ-1-プロペン、3-アシロキシ-1-ブテン、4-アシロキシ-1-ブテン、3,4-ジアシロキシ-1-ブテン、3-アシロキシ-4-ヒドロキシ-1-ブテン、4-アシロキシ-3-ヒドロキシ-1-ブテン、3-アシロキシ-4-メチル-1-ブテン、4-アシロキシ-2-メチル-1-ブテン、4-アシロキシ-3-メチル-1-ブテン、3,4-ジアシロキシ-2-メチル-1-ブテン、4-ヒドロキシ-1-ペンテン、5-ヒドロキシ-1-ペンテン、4,5-ジヒドロキシ-1-ペンテン、4-アシロキシ-1-ペンテン、5-アシロキシ-1-ペンテン、4,5-ジアシロキシ-1-ペンテン、4-ヒドロキシ-3-メチル-1-ペンテン、5-ヒドロキシ-3-メチル-1-ペンテン、4,5-ジヒドロキシ-3-メチル-1-ペンテン、5,6-ジヒドロキシ-1-ヘキセン、4-ヒドロキシ-1-ヘキセン、5-ヒドロキシ-1-ヘキセン、6-ヒドロキシ-1-ヘキセン、4-アシロキシ-1-ヘキセン、5-アシロキシ-1-ヘキセン、6-アシロキシ-1-ヘキセン、5,6-ジアシロキシ-1-ヘキセン等の水酸基あるいはエステル基を有するアルケンが挙げられる。中でも、共重合反応性、及び得られる各種成形体等の加工性、ガスバリア性の観点からは、プロピレン、3-アシロキシ-1-プロペン、3-アシロキシ-1-ブテン、4-アシロキシ-1-ブテン、3,4-ジアシロキシ-1-ブテンが好ましい。なお、“アシロキシ”はアセトキシであることが好ましく、具体的には3-アセトキシ-1-プロペン、3-アセトキシ-1-ブテン、4-アセトキシ-1-ブテン及び3,4-ジアセトキシ-1-ブテンが好ましい。エステルを有するアルケンの場合は、ケン化反応の際に、上記構造単位(I)に誘導される。 The method for incorporating the above-mentioned structural unit (I) into EVOH(A) is not particularly limited. For example, in the polymerization of ethylene and vinyl ester, a copolymerization of monomers induced to structural unit (I) can be used. Monomers that can be converted to structural unit (I) include alkenes such as propylene, butylene, pentene, and hexene; 3-hydroxy-1-propene, 3-acyloxy-1-propene, 3-acyloxy-1-butene, 4-acyloxy-1-butene, 3,4-diasiloxy-1-butene, 3-acyloxy-4-hydroxy-1-butene, 4-acyloxy-3-hydroxy-1-butene, 3-acyloxy-4-methyl-1-butene, 4-acyloxy-2-methyl-1-butene, 4-acyloxy-3-methyl-1-butene, 3,4-diasiloxy-2-methyl-1-butene, 4-hydroxy-1-pentene, 5-hydroxy-1-pentene, 4 Examples of alkenes having a hydroxyl group or ester group include 5-dihydroxy-1-pentene, 4-acyloxy-1-pentene, 5-acyloxy-1-pentene, 4,5-diasiloxy-1-pentene, 4-hydroxy-3-methyl-1-pentene, 5-hydroxy-3-methyl-1-pentene, 4,5-dihydroxy-3-methyl-1-pentene, 5,6-dihydroxy-1-hexene, 4-hydroxy-1-hexene, 5-hydroxy-1-hexene, 6-hydroxy-1-hexene, 4-acyloxy-1-hexene, 5-acyloxy-1-hexene, 6-acyloxy-1-hexene, and 5,6-diasiloxy-1-hexene. In particular, propylene, 3-acyloxy-1-propene, 3-acyloxy-1-butene, 4-acyloxy-1-butene, and 3,4-diasiloxy-1-butene are preferred from the viewpoint of copolymerization reactivity and the processability and gas barrier properties of the resulting molded articles. "Asiloxy" is preferably acetoxy, specifically 3-acetoxy-1-propene, 3-acetoxy-1-butene, 4-acetoxy-1-butene, and 3,4-diacetoxy-1-butene. In the case of alkenes containing esters, the above structural unit (I) is derived during the saponification reaction.

上記構造単位(II)において、R4及びR5は共に水素原子であることが好ましい。特にR4及びR5が共に水素原子であり、上記R6及びR7のうちの一方が炭素数1~10の脂肪族炭化水素基、他方が水素原子であることがより好ましい。この脂肪族炭化水素基は、アルキル基及びアルケニル基が好ましい。得られる各種成形体等におけるガスバリア性を特に重視する観点からは、R6及びR7のうちの一方がメチル基またはエチル基、他方が水素原子であることがより好ましい。また上記R6及びR7のうちの一方が(CH2)hOHで表される置換基(但し、hは1~8の整数)、他方が水素原子であることがさらに好ましい。(CH2)hOHで表される置換基において、hは1~4の整数であることが好ましく、1または2であることがより好ましく、1であることがさらに好ましい。 In the above structural unit (II), it is preferable that both R4 and R5 are hydrogen atoms. In particular, it is more preferable that both R4 and R5 are hydrogen atoms, and that one of R6 and R7 is an aliphatic hydrocarbon group having 1 to 10 carbon atoms, and the other is a hydrogen atom. The aliphatic hydrocarbon group is preferably an alkyl group and an alkenyl group. From the viewpoint of particularly emphasizing the gas barrier properties of the resulting molded articles, it is more preferable that one of R6 and R7 is a methyl group or an ethyl group, and the other is a hydrogen atom. Furthermore, it is even more preferable that one of R6 and R7 is a substituent represented by ( CH2 ) hOH (where h is an integer from 1 to 8), and the other is a hydrogen atom. In the substituent represented by ( CH2 ) hOH , h is preferably an integer from 1 to 4, more preferably 1 or 2, and even more preferably 1.

EVOH(A)中に上記構造単位(II)を含有させる方法は特に限定されず、例えば、ケン化反応によって得られたEVOH(A)に一価エポキシ化合物を反応させることにより含有させる方法等が用いられる。一価エポキシ化合物としては、下記式(IV)~(X)で示される化合物が好適に用いられる。 The method for incorporating the above structural unit (II) into EVOH(A) is not particularly limited. For example, a method involving reacting EVOH(A) obtained by a saponification reaction with a monovalent epoxy compound can be used. The compounds represented by the following formulas (IV) to (X) are preferably used as the monovalent epoxy compound.

上記式(IV)~(X)中、R14、R15、R16、R17及びR18は、それぞれ独立して、水素原子、炭素数1~10の脂肪族炭化水素基(アルキル基、アルケニル基等)、炭素数3~10の脂環式炭化水素基(シクロアルキル基、シクロアルケニル基等)または炭素数6~10の脂肪族炭化水素基(フェニル基等)を表す。また、i、j、k、p及びqは、それぞれ独立して、1~8の整数を表す。ただし、R17が水素原子である場合、R18は水素原子以外の基である。 In formulas (IV) to (X) above, R14 , R15 , R16 , R17 , and R18 each independently represent a hydrogen atom, an aliphatic hydrocarbon group having 1 to 10 carbon atoms (alkyl group, alkenyl group, etc.), a cycloalkyl group having 3 to 10 carbon atoms (cycloalkyl group, cycloalkenyl group, etc.), or an aliphatic hydrocarbon group having 6 to 10 carbon atoms (phenyl group, etc.). Also, i, j, k, p, and q each independently represent an integer from 1 to 8. However, if R17 is a hydrogen atom, then R18 is a group other than a hydrogen atom.

上記式(IV)で表される一価エポキシ化合物としては、例えばエポキシエタン(エチレンオキサイド)、エポキシプロパン、1,2-エポキシブタン、2,3-エポキシブタン、3-メチル-1,2-エポキシブタン、1,2-エポキシペンタン、3-メチル-1,2-エポキシペンタン、1,2-エポキシヘキサン、2,3-エポキシヘキサン、3,4-エポキシヘキサン、3-メチル-1,2-エポキシヘキサン、3-メチル-1,2-エポキシヘプタン、4-メチル-1,2-エポキシヘプタン、1,2-エポキシオクタン、2,3-エポキシオクタン、1,2-エポキシノナン、2,3-エポキシノナン、1,2-エポキシデカン、1,2-エポキシドデカン、エポキシエチルベンゼン、1-フェニル-1,2-エポキシプロパン、3-フェニル-1,2-エポキシプロパン等が挙げられる。上記式(V)で表される一価エポキシ化合物としては、各種アルキルグリシジルエーテル等が挙げられる。上記式(VI)で表される一価エポキシ化合物としては、各種アルキレングリコールモノグリシジルエーテルが挙げられる。上記式(VII)で表される一価エポキシ化合物としては、各種アルケニルグリシジルエーテルが挙げられる。上記式(VIII)で表される一価エポキシ化合物としては、グリシドール等の各種エポキシアルカノールが挙げられる。上記式(IX)で表される一価エポキシ化合物としては、各種エポキシシクロアルカンが挙げられる。上記式(X)で表される一価エポキシ化合物としては、各種エポキシシクロアルケンが挙げられる。 Examples of monovalent epoxy compounds represented by the above formula (IV) include epoxyethane (ethylene oxide), epoxypropane, 1,2-epoxybutane, 2,3-epoxybutane, 3-methyl-1,2-epoxybutane, 1,2-epoxypentane, 3-methyl-1,2-epoxypentane, 1,2-epoxyhexane, 2,3-epoxyhexane, 3,4-epoxyhexane, 3-methyl-1,2-epoxyhexane, 3-methyl-1,2-epoxyheptane, 4-methyl-1,2-epoxyheptane, 1,2-epoxyoctane, 2,3-epoxyoctane, 1,2-epoxynonane, 2,3-epoxynonane, 1,2-epoxydecane, 1,2-epoxydodecane, epoxyethylbenzene, 1-phenyl-1,2-epoxypropane, and 3-phenyl-1,2-epoxypropane. Examples of monovalent epoxy compounds represented by the above formula (V) include various alkylglycidyl ethers. Examples of monovalent epoxy compounds represented by formula (VI) include various alkylene glycol monoglycidyl ethers. Examples of monovalent epoxy compounds represented by formula (VII) include various alkenyl glycidyl ethers. Examples of monovalent epoxy compounds represented by formula (VIII) include various epoxy alkanols such as glycidol. Examples of monovalent epoxy compounds represented by formula (IX) include various epoxycycloalkanes. Examples of monovalent epoxy compounds represented by formula (X) include various epoxycycloalkenes.

上記一価エポキシ化合物の中では炭素数が2~8のエポキシ化合物が好ましい。特に化合物の取り扱いの容易さ、及び反応性の観点から、一価エポキシ化合物の炭素数は2~6がより好ましく、2~4がさらに好ましい。また、一価エポキシ化合物は上記式(IV)または式(V)で表される化合物であることが特に好ましい。具体的には、EVOH(A)との反応性、樹脂組成物及び得られる各種成形体等の加工性、ガスバリア性等の観点からは、1,2-エポキシブタン、2,3-エポキシブタン、エポキシプロパン、エポキシエタンまたはグリシドールが好ましく、中でもエポキシプロパンまたはグリシドールがより好ましい。 Among the monovalent epoxy compounds mentioned above, epoxy compounds having 2 to 8 carbon atoms are preferred. Particularly from the viewpoint of ease of handling and reactivity, monovalent epoxy compounds with 2 to 6 carbon atoms are more preferred, and 2 to 4 carbon atoms are even more preferred. Furthermore, it is especially preferred that the monovalent epoxy compound is a compound represented by formula (IV) or formula (V). Specifically, from the viewpoint of reactivity with EVOH(A), processability of the resin composition and the resulting molded articles, and gas barrier properties, 1,2-epoxybutane, 2,3-epoxybutane, epoxypropane, epoxyethane, or glycidol are preferred, with epoxypropane or glycidol being more preferred.

上記構造単位(III)において、R8、R9、R10及びR11は水素原子または炭素数1~5の脂肪族炭化水素基であることが好ましく、かかる脂肪族炭化水素基は、メチル基、エチル基、n-プロピル基、イソプロピル基、n-ブチル基、イソブチル基、tert-ブチル基またはn-ペンチル基が好ましい。 In the above structural unit (III), R8 , R9 , R10 , and R11 are preferably hydrogen atoms or aliphatic hydrocarbon groups having 1 to 5 carbon atoms, and such aliphatic hydrocarbon groups are preferably methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, or n-pentyl groups.

EVOH(A)中に上記構造単位(III)を含有させる方法については、特に限定されず、例えば、特開2014-034647号公報に記載の方法が挙げられる。 The method for incorporating the above structural unit (III) into EVOH(A) is not particularly limited, and for example, the method described in Japanese Patent Application Publication No. 2014-034647 can be cited.

EVOH(A)の融点の下限としては、140℃が好ましく、150℃がより好ましく、160℃がさらに好ましい。一方、この融点の上限としては、220℃が好ましく、210℃がより好ましく、200℃がさらに好ましい。EVOH(A)の融点が上記範囲内である場合、溶融成形性が向上し、溶融成形の際のネックイン及びダイビルドアップがより抑制される傾向にある。EVOH(A)の融点は、実施例に記載の方法により測定される値とすることができる。 The lower limit of the melting point of EVOH(A) is preferably 140°C, more preferably 150°C, and even more preferably 160°C. On the other hand, the upper limit of the melting point is preferably 220°C, more preferably 210°C, and even more preferably 200°C. When the melting point of EVOH(A) is within the above range, melt moldability is improved, and neck-in and die build-up during melt molding tend to be further suppressed. The melting point of EVOH(A) can be the value measured by the method described in the examples.

EVOH(A)は、1種を単独で用いてもよく、2種以上を併用してもよい。 EVOH(A) may be used alone or in combination of two or more types.

本発明の樹脂組成物におけるEVOH(A)の含有量の下限は、ガスバリア性等の観点から、50質量%であってよいが、70質量%が好ましく、80質量%がさらに好ましく、90質量%が特に好ましく、95質量%であっても、99質量%であっても、99.9質量%であってもよい。本発明の樹脂組成物を構成する樹脂が実質的にEVOH(A)のみから構成されていてもよい。一方、本発明の樹脂組成物におけるEVOH(A)の含有量の上限は、例えば99.9質量%であってよく、99質量%、95質量%又は90質量%であってもよい。なお、EVOH(A)の含有量とは、乾燥状態の樹脂組成物における含有量(含有割合)をいう。以下、樹脂組成物を基準にした含有量について同様である。 The lower limit of the EVOH(A) content in the resin composition of the present invention may be 50% by mass, but is preferably 70% by mass, more preferably 80% by mass, particularly preferably 90% by mass, and may also be 95% by mass, 99% by mass, or 99.9% by mass, from the viewpoint of gas barrier properties, etc. The resin constituting the resin composition of the present invention may be substantially composed solely of EVOH(A). On the other hand, the upper limit of the EVOH(A) content in the resin composition of the present invention may be, for example, 99.9% by mass, and may also be 99% by mass, 95% by mass, or 90% by mass. Note that the EVOH(A) content refers to the content (percentage) in the resin composition in a dry state. The same applies hereafter to content based on the resin composition.

(不飽和脂肪族アルデヒド(B))
本発明の樹脂組成物はクロトンアルデヒド(B1)を含み、かつ、2,4-ヘキサジエナール(B2)及び2,4,6-オクタトリエナール(B3)からなる群より選ばれる少なくとも1種をさらに含む。
(Unsaturated aliphatic aldehyde (B))
The resin composition of the present invention comprises crotonaldehyde (B1) and further comprises at least one selected from the group consisting of 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3).

本発明の樹脂組成物におけるEVOH(A)に対するクロトンアルデヒド(B1)の含有量b1の下限は、0.01ppmが好ましく、0.20ppmがより好ましく、0.40ppmがさらに好ましく、0.70ppm又は1.20ppmがよりさらに好ましい場合もある。一方、含有量b1の上限は、4.0ppmが好ましく、3.5ppmがより好ましく、2.7ppmがさらに好ましく、2.0ppm又は1.5ppmがよりさらに好ましい場合もある。含有量b1が上記範囲であると、後述するb1/(b2+b3)、b1+b2+b3及びb2+2b3の値を好適な範囲に調整しやすくなる。また、含有量b1が上記範囲であると着色を抑制できる傾向となる。 The lower limit of the content b1 of crotonaldehyde (B1) relative to EVOH (A) in the resin composition of the present invention is preferably 0.01 ppm, more preferably 0.20 ppm, even more preferably 0.40 ppm, and may be even more preferably 0.70 ppm or 1.20 ppm. On the other hand, the upper limit of the content b1 is preferably 4.0 ppm, more preferably 3.5 ppm, even more preferably 2.7 ppm, and may be even more preferably 2.0 ppm or 1.5 ppm. When the content b1 is within the above range, it becomes easier to adjust the values of b1 /( b2 + b3 ), b1 + b2 + b3 and b2 + 2b3 , which will be described later, to a suitable range. In addition, when the content b1 is within the above range, discoloration tends to be suppressed.

本発明の樹脂組成物は、一実施形態として、2,4-ヘキサジエナール(B2)をクロトンアルデヒド(B1)に対して特定比率で含むことで、ダイビルドアップを抑制しつつ、ネックイン耐性に優れる傾向となる。本発明の樹脂組成物におけるEVOH(A)に対する2,4-ヘキサジエナール(B2)の含有量b2の下限は、0.005ppmが好ましく、0.01ppmがより好ましく、0.02ppmがさらに好ましい。一方、含有量b2の上限は、0.65ppmが好ましく、0.20ppmがより好ましく、0.10ppmがさらに好ましく、0.08ppmがよりさらに好ましく、0.06ppmが特に好ましい。含有量b2が上記範囲であると、後述するb1/(b2+b3)、b1+b2+b3及びb2+2b3の値を好適な範囲に調整しやすくなる。また、含有量b2が上記範囲であると着色を抑制できる傾向となる。 In one embodiment, the resin composition of the present invention contains 2,4-hexadienal (B2) in a specific ratio to crotonaldehyde (B1), which tends to suppress die buildup while exhibiting excellent neck-in resistance. The lower limit of the content b2 of 2,4-hexadienal (B2) relative to EVOH (A) in the resin composition of the present invention is preferably 0.005 ppm, more preferably 0.01 ppm, and even more preferably 0.02 ppm. On the other hand, the upper limit of the content b2 is preferably 0.65 ppm, more preferably 0.20 ppm, even more preferably 0.10 ppm, even more preferably 0.08 ppm, and particularly preferably 0.06 ppm. When the content b2 is within the above range, it becomes easier to adjust the values of b1 /( b2 + b3 ), b1 + b2 + b3 , and b2 + 2b3, which will be described later, to a suitable range. Furthermore, when the content of b2 is within the above range, discoloration tends to be suppressed.

本発明の樹脂組成物は、一実施形態として、2,4,6-オクタトリエナール(B3)をクロトンアルデヒド(B1)に対して特定比率で含むことで、ダイビルドアップを抑制しつつ、ネックイン耐性に優れる傾向となる。2,4,6-オクタトリエナール(B3)は、2,4-ヘキサジエナール(B2)と比べ、添加量に対するダイビルドアップへの影響が大きい。このため、ダイビルドアップを抑制しつつ、ネックイン耐性を向上させる視点からは本発明の樹脂組成物は、2,4,6-オクタトリエナール(B3)よりは、2,4-ヘキサジエナール(B2)を含むことが好ましい。本発明の樹脂組成物におけるEVOH(A)に対する2,4,6-オクタトリエナール(B3)の含有量b3の上限は、0.325ppmが好ましく、0.23ppmがより好ましく、0.07ppmがさらに好ましく、0.04ppmが特に好ましい。含有量B3の下限は、0ppmであってもよく、0.005ppmであってもよい。含有量b3が上記範囲であると、後述するb1/(b2+b3)、b1+b2+b3及びb2+2b3の値を好適な範囲に調整しやすくなる。また、含有量b3が上記範囲であると着色を抑制できる傾向となる。 In one embodiment, the resin composition of the present invention tends to have excellent neck-in resistance while suppressing die buildup by containing 2,4,6-octatrienal (B3) in a specific ratio to crotonaldehyde (B1). Compared to 2,4-hexadienal (B2), 2,4-octatrienal (B3) has a greater effect on die buildup with respect to the amount added. Therefore, from the viewpoint of suppressing die buildup and improving neck-in resistance, the resin composition of the present invention preferably contains 2,4-hexadienal (B2) rather than 2,4,6-octatrienal (B3). The upper limit of the content b3 of 2,4,6-octatrienal (B3) relative to EVOH (A) in the resin composition of the present invention is preferably 0.325 ppm, more preferably 0.23 ppm, even more preferably 0.07 ppm, and particularly preferably 0.04 ppm. The lower limit of the content B3 may be 0 ppm or 0.005 ppm. When the content b3 is within the above range, it becomes easier to adjust the values of b1 /( b2 + b3 ), b1 + b2 + b3 , and b2 + 2b3 , which will be described later, to a suitable range. In addition, when the content b3 is within the above range, discoloration tends to be suppressed.

本発明の樹脂組成物においては、クロトンアルデヒド(B1)の含有量b1(ppm)に対する2,4-ヘキサジエナール(B2)の含有量b2(ppm)と2,4,6-オクタトリエナール(B3)の含有量b3(ppm)との合計の比率(b1/(b2+b3))の値が2.0以上150.0未満であることでネックイン耐性に優れる。かかるネックイン耐性は、不飽和脂肪族アルデヒド(B)のいずれかの化合物を単独で用いた場合には見られない効果であり、b1/(b2+b3)が特定範囲となることで初めて奏される効果である。b1/(b2+b3)の下限は、4.0が好ましく、8.0がより好ましい。一方、b1/(b2+b3)の上限は、60.0が好ましく、25.0がより好ましく、13.0がさらに好ましい。b1/(b2+b3)を上記範囲内とすることで、ネックインをより十分に抑制することができる。 In the resin composition of the present invention, the ratio of the total content of 2,4-hexadienal (B2) b2 (ppm) and 2,4,6-octatrienal (B3) b3 (ppm) to the content of crotonaldehyde (B1) b1 (ppm) ( b1 /( b2 + b3 )) is 2.0 or more and less than 150.0, which results in excellent neck-in resistance. This neck-in resistance is an effect not seen when any of the unsaturated aliphatic aldehyde (B) compounds are used alone, and is only achieved when b1 /( b2 + b3 ) falls within a specific range. The lower limit of b1 /( b2 + b3 ) is preferably 4.0, and more preferably 8.0. On the other hand, the upper limit of b1 /( b2 + b3 ) is preferably 60.0, more preferably 25.0, and even more preferably 13.0. By keeping b1 /( b2 + b3 ) within the above range, neck-in can be suppressed more effectively.

本発明の樹脂組成物においては、2,4-ヘキサジエナール(B2)の含有量b2(ppm)と2,4,6-オクタトリエナール(B3)の含有量b3(ppm)の2倍量との合計(b2+2b3)の上限は、0.65ppm以下であり、0.50ppmが好ましく、0.30ppmがより好ましく、0.10ppmがさらに好ましい。b2+2b3が上記上限を超えると、ダイビルドアップの発生を抑制できない。b2+2b3は、0.005ppm以上であってもよく、0.01ppm以上であってもよい。 In the resin composition of the present invention, the upper limit of the sum of the content of 2,4-hexadienal (B2) b2 (ppm) and twice the content of 2,4,6-octatrienal (B3) b3 (ppm) ( b2 + 2b3 ) is 0.65 ppm or less, preferably 0.50 ppm, more preferably 0.30 ppm, and even more preferably 0.10 ppm. If b2 + 2b3 exceeds the above upper limit, the occurrence of die buildup cannot be suppressed. b2 + 2b3 may be 0.005 ppm or more, or 0.01 ppm or more.

本発明の樹脂組成物において、EVOH(A)に対するクロトンアルデヒド(B1)、2,4-ヘキサジエナール(B2)及び2,4,6-オクタトリエナール(B3)の含有量の合計(b1+b2+b3)の上限は、7.0ppmが好ましく、4.0ppmがより好ましく、3.5ppmがさらに好ましく、3.0ppmがよりさらに好ましく、1.5ppmがよりさらに好ましく、1.0ppmが特に好ましい場合もある。b1+b2+b3を上記上限以下とすることで、樹脂組成物の着色を十分に抑えることができる。一方、b1+b2+b3の下限としては、0.01ppmが好ましく、0.10ppmがより好ましく、0.30ppm又は0.50ppmがさらに好ましい場合もある。 In the resin composition of the present invention, the upper limit of the total content of crotonaldehyde (B1), 2,4-hexadienal (B2), and 2,4,6-octatrienal (B3) relative to EVOH (A) ( b1 + b2 + b3 ) is preferably 7.0 ppm, more preferably 4.0 ppm, even more preferably 3.5 ppm, even more preferably 3.0 ppm, even more preferably 1.5 ppm, and in some cases particularly preferably 1.0 ppm. By keeping b1 + b2 + b3 below the above upper limit, the discoloration of the resin composition can be sufficiently suppressed. On the other hand, the lower limit of b1 + b2 + b3 is preferably 0.01 ppm, more preferably 0.10 ppm, and in some cases even more preferably 0.30 ppm or 0.50 ppm.

(酸化防止剤(G))
本発明の樹脂組成物は、得られる成形体等の耐酸化劣化性等を改善するため、さらに酸化防止剤(G)を含有する。当該樹脂組成物が酸化防止剤をさらに含む場合、当該樹脂組成物から形成されるパイプ等の成形体を長期間高温で使用した場合などのクラックの発生を抑制することができる。
(Antioxidant (G))
The resin composition of the present invention further contains an antioxidant (G) to improve the oxidation resistance and degradation properties of the resulting molded articles. When the resin composition further contains an antioxidant, it is possible to suppress the occurrence of cracks when molded articles such as pipes formed from the resin composition are used at high temperatures for a long period of time.

酸化防止剤(G)は、酸化防止能を有する化合物である。酸化防止剤(G)の融点は必ずしも限定されるものではないが、170℃以下であることが好ましい。酸化防止剤(G)の融点が170℃以下である場合、溶融混合により樹脂組成物を製造する際に、押出機内で溶融し易くなる。このため、酸化防止剤(G)が樹脂組成物中に局在化して高濃度部分が着色することを抑制することができる。また、酸化防止剤(G)の融点は、50℃以上が好ましく、100℃以上がより好ましい場合もある。酸化防止剤(G)の融点が50℃以上である場合、得られた成形体(パイプ等)の表面に酸化防止剤がブリードアウトして外観が不良となることを抑制することができる。 The antioxidant (G) is a compound possessing antioxidant properties. While the melting point of the antioxidant (G) is not necessarily limited, it is preferably 170°C or lower. When the melting point of the antioxidant (G) is 170°C or lower, it melts more easily in the extruder during the production of the resin composition by melt mixing. Therefore, it is possible to suppress the localization of the antioxidant (G) in the resin composition and the resulting discoloration of high-concentration areas. Furthermore, the melting point of the antioxidant (G) is preferably 50°C or higher, and more preferably 100°C or higher. When the melting point of the antioxidant (G) is 50°C or higher, it is possible to suppress the bleeding out of the antioxidant onto the surface of the resulting molded article (pipe, etc.), which can result in a poor appearance.

酸化防止剤(G)の分子量は300以上であることが好ましい。酸化防止剤(G)の分子量が300以上である場合、本発明の樹脂組成物から成形体を得た際に、表面に酸化防止剤がブリードアウトして成形体の外観が不良となることを抑制でき、また、樹脂組成物の熱安定性も高まる。上記分子量は400以上がより好ましく、500以上が特に好ましい。一方、酸化防止剤(G)の分子量の上限は特に限定されないが、分散性の観点から、8000以下が好ましく、6000以下がより好ましく、4000以下がさらに好ましく、2000以下が特に好ましい。 The molecular weight of the antioxidant (G) is preferably 300 or higher. When the molecular weight of the antioxidant (G) is 300 or higher, it is possible to suppress the bleeding of the antioxidant out onto the surface of a molded article obtained from the resin composition of the present invention, which can result in a poor appearance of the molded article, and the thermal stability of the resin composition is also improved. A molecular weight of 400 or higher is more preferable, and 500 or higher is particularly preferable. On the other hand, there is no particular upper limit to the molecular weight of the antioxidant (G), but from the viewpoint of dispersibility, 8000 or less is preferable, 6000 or less is more preferable, 4000 or less is even more preferable, and 2000 or less is particularly preferable.

酸化防止剤(G)としては、ヒンダードフェノール基を有する化合物が好適に用いられる。ヒンダードフェノール基を有する化合物は、それ自身が熱安定性に優れる一方で、酸化劣化の原因である酸素ラジカルを捕捉する能力があり、酸化防止剤として樹脂組成物に配合した場合、酸化劣化を防止する効果に優れるものである。 As the antioxidant (G), compounds having a hindered phenol group are preferably used. Compounds having a hindered phenol group possess excellent thermal stability while also having the ability to capture oxygen radicals, which are the cause of oxidative degradation. Therefore, when incorporated into a resin composition as an antioxidant, they exhibit excellent effectiveness in preventing oxidative degradation.

ヒンダードフェノール基を有する化合物としては、通常市販されているものを用いることができ、例えば、以下の製品が挙げられる。
(1)BASF社製「IRGANOX 1010」:融点110-125℃、分子量1178、ペンタエリスリトールテトラキス〔3-(3,5-ジ-tert-ブチル-4-ヒドロキシフェニル)プロピオネート〕
(2)BASF社製「IRGANOX 1076」:融点50-55℃、分子量531、オクタデシル-3-(3,5-ジ-tert-ブチル-4-ヒドロキシフェニル)プロピオネート
(3)BASF社製「IRGANOX 1098」:融点156-161℃、分子量637、N,N’-(ヘキサン-1,6-ジイル)ビス〔3-(3,5-ジ-tert-ブチル-4-ヒドロキシフェニル)プロピオンアミド〕
(4)BASF社製「IRGANOX 245」:融点76-79℃、分子量587、トリエチレングリコール-ビス[3-(3-tert-ブチル-5-メチル-4-ヒドロキシフェニル)プロピオネート]
(5)BASF社製「IRGANOX 259」:融点104-108℃、分子量639、1,6-ヘキサンジオール-ビス[3-(3,5-ジ-tert-ブチル-4-ヒドロキシフェニル)プロピオネート]
(6)住友化学工業株式会社製「Sumilizer MDP-s」:融点約128℃、分子量341、2,2’-メチレン-ビス(4-メチル-6-tert-ブチルフェノール)
(7)住友化学工業株式会社製「Sumilizer GM」:融点約128℃、分子量395、2-tert-ブチル-6-(3-tert-ブチル-2-ヒドロキシ-5-メチルベンジル)-4-メチルフェニルアクリレート
(8)住友化学工業株式会社製「Sumilizer GA-80」:融点約110℃、分子量741、3,9-ビス〔2-{3-(3-tert-ブチル-4-ヒドロキシ-5-メチルフェニル)プロピオニルオキシ}-1,1-ジメチルエチル〕-2,4,8,10-テトラオキサスピロ〔5,5〕ウンデカン
As compounds having a hindered phenol group, commercially available products can be used, for example, the following products.
(1) BASF's "IRGANOX 1010": Melting point 110-125°C, molecular weight 1178, pentaerythritol tetrakis [3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]
(2) BASF "IRGANOX 1076": Melting point 50-55°C, molecular weight 531, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (3) BASF "IRGANOX 1098": Melting point 156-161°C, molecular weight 637, N,N'-(hexane-1,6-diyl)bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide]
(4) BASF's "IRGANOX 245": Melting point 76-79°C, molecular weight 587, triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate]
(5) BASF's "IRGANOX 259": Melting point 104-108°C, molecular weight 639, 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]
(6) Sumitomo Chemical Co., Ltd.'s "Sumilizer MDP-s": Melting point approximately 128°C, molecular weight 341, 2,2'-methylene-bis(4-methyl-6-tert-butylphenol)
(7) Sumitomo Chemical Co., Ltd.'s "Sumilizer GM": Melting point approximately 128°C, molecular weight 395, 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate (8) Sumitomo Chemical Co., Ltd.'s "Sumilizer GA-80": Melting point approximately 110°C, molecular weight 741, 3,9-bis[2-{3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane

酸化防止剤(G)として、ヒンダードアミン基を有する化合物も好適に用いられる。ヒンダードアミン基を有する化合物は、酸化防止剤(G)として樹脂組成物に配合した場合、EVOH(A)の熱劣化を防止するのみにとどまらず、EVOH(A)の熱分解により生成するアルデヒドを捕捉する効果もあり、分解ガスの発生を低減することで成形時のボイドあるいは気泡の発生を抑制することができる。また、アルデヒドを捕捉する事により、本発明の樹脂組成物を食品包装容器として用いた際に、アルデヒドによる臭気が内容物の味覚を損ねる点も改善される。 Compounds having a hindered amine group are also suitably used as antioxidants (G). When compounds having a hindered amine group are incorporated into the resin composition as antioxidants (G), they not only prevent the thermal degradation of EVOH(A), but also have the effect of capturing aldehydes generated by the thermal decomposition of EVOH(A). This reduces the generation of decomposition gases, thereby suppressing the formation of voids or bubbles during molding. Furthermore, by capturing aldehydes, the problem of aldehyde odors impairing the taste of the contents when the resin composition of the present invention is used as a food packaging container is also improved.

ヒンダードアミン基を有する化合物として好ましいものは、ピペリジン誘導体であり、特に4位に置換基を有する2,2,6,6-テトラアルキルピペリジン誘導体が好ましい。その4位の置換基としては、カルボキシル基、アルコキシ基、アルキルアミノ基が挙げられる。 Preferred compounds having a hindered amine group are piperidine derivatives, and particularly preferred are 2,2,6,6-tetraalkylpiperidine derivatives having a substituent at the 4-position. Examples of substituents at the 4-position include carboxyl groups, alkoxy groups, and alkylamino groups.

また、ヒンダードアミン基のN位にはアルキル基が置換していてもよいが、水素原子が結合しているものを用いる方が熱安定効果に優れ好ましい。 Furthermore, while the N-position of the hindered amine group may be substituted with an alkyl group, using one with a hydrogen atom bonded to it is preferable due to its superior thermal stability.

ヒンダードアミン基を有する化合物としては、通常市販されているものを用いることができ、例えば、以下の製品を挙げることができる。
(9)BASF社製「TINUVIN 770」:融点81-85℃、分子量481、ビス(2,2,6,6-テトラメチル-4-ピペリジル)セバケート
(10)BASF社製「TINUVIN 765」:液状化合物、分子量509、ビス(1,2,2,6,6-ペンタメチル-4-ピペリジル)セバケート及び1,2,2,6,6-ペンタメチル-4-ピペリジルセバケート(混合物)
(11)BASF社製「TINUVIN 622LD」:融点55-70℃、分子量3100-4000、コハク酸ジメチル・1-(2-ヒドロキシエチル)-4-ヒドロキシ-2,2,6,6-テトラメチルピペリジン重縮合物
(12)BASF社製「CHIMASSORB 119FL」:融点130-140℃、分子量2000以上、N,N’-ビス(3-アミノプロピル)エチレンジアミン・2,4-ビス〔N-ブチル-N-(1,2,2,6,6-ペンタメチル-4-ピペリジル)アミノ〕-6-クロロ-1,3,5-トリアジン縮合物
(13)BASF社製「CHIMASSORB 944LD」:融点100-135℃、分子量2000-3100、ポリ〔〔6-(1,1,3,3-テトラメチルブチル)アミノ-1,3,5-トリアジン-2,4-ジイル〕(2,2,6,6-テトラメチル-4-ピペリジル)イミノ〕ヘキサメチレン(2,2,6,6-テトラメチル-4-ピペジリル)イミノ〕〕
(14)BASF社製「TINUVIN 144」:融点146-150℃、分子量685、ビス(1,2,2,6,6-ペンタメチル-4-ピペリジル)〔〔3,5-ビス(1,1-ジメチルエチル)-4-ヒドリキシフェニル〕メチル〕ブチルマロネート
(15)BASF社製「UVINUL 4050H」:融点157℃、分子量450、N,N’-1,6-ヘキサンジイルビス{N-(2,2,6,6-テトラメチル-4-ピペリジニル)-ホルムアミド}
(16)BASF社製「UVINUL 5050H」:融点104-112℃、分子量約3500、下記構造式を有する化合物
As compounds having a hindered amine group, commercially available products can be used, and examples include the following products.
(9) BASF "TINUVIN 770": Melting point 81-85°C, molecular weight 481, bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate (10) BASF "TINUVIN 765": Liquid compound, molecular weight 509, bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate and 1,2,2,6,6-pentamethyl-4-piperidyl sebacate (mixture)
(11) BASF's "TINUVIN 622LD": Melting point 55-70°C, molecular weight 3100-4000, dimethyl succinate/1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine polycondensate (12) BASF's "CHIMASSORB 119FL": Melting point 130-140°C, molecular weight 2000 or more, N,N'-bis(3-aminopropyl)ethylenediamine/2,4-bis[N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino]-6-chloro-1,3,5-triazine condensate (13) BASF's "CHIMASSORB 944LD: Melting point 100-135°C, molecular weight 2000-3100, poly[[6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl](2,2,6,6-tetramethyl-4-piperidyl)imino]hexamethylene(2,2,6,6-tetramethyl-4-pipezyl)imino]]
(14) BASF "TINUVIN 144": Melting point 146-150°C, molecular weight 685, bis(1,2,2,6,6-pentamethyl-4-piperidyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butylmalonate (15) BASF "UVINUL 4050H": Melting point 157°C, molecular weight 450, N,N'-1,6-hexanediylbis{N-(2,2,6,6-tetramethyl-4-piperidinyl)-formamide}
(16) BASF's "UVINUL 5050H": Melting point 104-112°C, molecular weight approximately 3500, compound having the following structural formula

これらのヒンダードフェノール基又はヒンダードアミン基を有する化合物は単独で使用しても、また、2種以上を併用してもよい。 These compounds having hindered phenol or hindered amine groups may be used individually or in combination of two or more.

本発明の樹脂組成物における酸化防止剤(G)の含有量gの下限は、0.01質量%であり、0.1質量%が好ましく、0.3質量%がより好ましい。酸化防止剤(G)の含有量gの上限は、5質量%であり、3質量%が好ましく、1質量%がより好ましい。酸化防止剤(G)の含有量gが上記範囲であると、酸化防止剤(G)が良好に分散し、本発明の樹脂組成物から成形体等を得た場合に外観に優れ、かつ良好な耐酸化劣化性、耐熱性等を発揮できる傾向にある。 The lower limit of the antioxidant (G) content in the resin composition of the present invention is 0.01% by mass, preferably 0.1% by mass, and more preferably 0.3% by mass. The upper limit of the antioxidant (G) content in g is 5% by mass, preferably 3% by mass, and more preferably 1% by mass. When the antioxidant (G) content in g is within the above range, the antioxidant (G) is well dispersed, and when a molded article or the like is obtained from the resin composition of the present invention, it tends to exhibit excellent appearance and good resistance to oxidation degradation, heat resistance, etc.

(共役ポリエン化合物(C))
本発明の樹脂組成物は、共役ポリエン化合物(C)をさらに含むことが好ましい。共役ポリエン化合物(C)は、溶融成形時のEVOH(A)の酸化劣化による色調悪化を抑制することができる。ここで、共役ポリエン化合物(C)とは、炭素-炭素二重結合と炭素-炭素単結合とが交互に繋がってなる構造を有し炭素-炭素二重結合の数が2個以上である、いわゆる共役二重結合を有する化合物である。但し、2,4-ヘキサジエナール(B2)及び2,4,6-オクタトリエナール(B3)は、共役ポリエン化合物(C)には該当しないものとする。共役ポリエン化合物(C)は、共役二重結合を2個有する共役ジエン、3個有する共役トリエン、又はそれ以上の数を有する共役ポリエンであってもよい。また、共役二重結合の構造が1分子中に複数組あってもよい。例えば、桐油のように共役トリエン構造が同一分子内に3個ある化合物も共役ポリエン化合物(C)に含まれる。共役ポリエン化合物(C)の共役二重結合の数の上限としては、7個が好ましい。当該樹脂組成物は、共役二重結合を8個以上有する共役ポリエン化合物(C)を含有すると、ペレットひいては成形体の着色が起こる可能性が高くなる。
(Conjugated polyene compound (C))
The resin composition of the present invention preferably further contains a conjugated polyene compound (C). The conjugated polyene compound (C) can suppress the deterioration of color tone due to oxidative degradation of EVOH (A) during melt molding. Here, the conjugated polyene compound (C) is a compound having a structure in which carbon-carbon double bonds and carbon-carbon single bonds are alternately linked, and the number of carbon-carbon double bonds is two or more, in other words, a compound having a conjugated double bond. However, 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3) are not considered to be conjugated polyene compounds (C). The conjugated polyene compound (C) may be a conjugated diene having two conjugated double bonds, a conjugated triene having three conjugated double bonds, or a conjugated polyene having more than that number. Furthermore, there may be multiple sets of conjugated double bond structures in one molecule. For example, compounds that have three conjugated triene structures in the same molecule, such as tung oil, are also included in the conjugated polyene compound (C). A preferred upper limit for the number of conjugated double bonds in the conjugated polyene compound (C) is seven. If the resin composition contains a conjugated polyene compound (C) having eight or more conjugated double bonds, the likelihood of discoloration of the pellets and, consequently, the molded article increases.

共役ポリエン化合物(C)は、共役二重結合に加えて、カルボキシ基及びその塩、水酸基、エステル基、エーテル基、アミノ基、イミノ基、アミド基、シアノ基、ジアゾ基、ニトロ基、スルホン基及びその塩、スルホニル基、スルホキシド基、スルフィド基、チオール基、リン酸基及びその塩、フェニル基、ハロゲン原子、二重結合、三重結合等のその他の官能基を有していてもよい。 The conjugated polyene compound (C) may have other functional groups in addition to the conjugated double bond, such as carboxyl groups and their salts, hydroxyl groups, ester groups, ether groups, amino groups, imino groups, amide groups, cyano groups, diazo groups, nitro groups, sulfone groups and their salts, sulfonyl groups, sulfoxide groups, sulfide groups, thiol groups, phosphate groups and their salts, phenyl groups, halogen atoms, double bonds, triple bonds, etc.

共役ポリエン化合物(C)の炭素数の下限としては、4が好ましい。また、共役ポリエン化合物(C)の炭素数の上限としては、30が好ましく、10がより好ましい。 The lower limit of the number of carbon atoms in the conjugated polyene compound (C) is preferably 4. Furthermore, the upper limit of the number of carbon atoms in the conjugated polyene compound (C) is preferably 30, and more preferably 10.

共役ポリエン化合物(C)としては、例えばイソプレン、2,3-ジメチル-1,3-ブタジエン、2,3-ジエチル-1,3-ブタジエン、2-t-ブチル-1,3-ブタジエン、1,3-ペンタジエン、2,3-ジメチル-1,3-ペンタジエン、2,4-ジメチル-1,3-ペンタジエン、3,4-ジメチル-1,3-ペンタジエン、3-エチル-1,3-ペンタジエン、2-メチル-1,3-ペンタジエン、3-メチル-1,3-ペンタジエン、4-メチル-1,3-ペンタジエン、1,3-ヘキサジエン、2,4-ヘキサジエン、2,5-ジメチル-2,4-ヘキサジエン、1,3-オクタジエン、1,3-シクロペンタジエン、1,3-シクロヘキサジエン、1-フェニル-1,3-ブタジエン、1,4-ジフェニル-1,3-ブタジエン、1-メトキシ-1,3-ブタジエン、2-メトキシ-1,3-ブタジエン、1-エトキシ-1,3-ブタジエン、2-エトキシ-1,3-ブタジエン、2-ニトロ-1,3-ブタジエン、クロロプレン、1-クロロ-1,3-ブタジエン、1-ブロモ-1,3-ブタジエン、2-ブロモ-1,3-ブタジエン、オシメン、フェランドレン、ミルセン、ファルネセン、ソルビン酸、ソルビン酸エステル、ソルビン酸塩等の共役ジエン化合物;1,3,5-ヘキサトリエン、2,4,6-オクタトリエン-1-カルボン酸、エレオステアリン酸、桐油、コレカルシフェロール、フルベン、トロポン等の共役トリエン化合物;シクロオクタテトラエン、2,4,6,8-デカテトラエン-1-カルボン酸、レチノール、レチノイン酸等が挙げられる。 Examples of conjugated polyene compounds (C) include isoprene, 2,3-dimethyl-1,3-butadiene, 2,3-diethyl-1,3-butadiene, 2-t-butyl-1,3-butadiene, 1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 2,4-dimethyl-1,3-pentadiene, 3,4-dimethyl-1,3-pentadiene, and 3-ethyl-1,3-pentadie. 2-methyl-1,3-pentadiene, 3-methyl-1,3-pentadiene, 4-methyl-1,3-pentadiene, 1,3-hexadiene, 2,4-hexadiene, 2,5-dimethyl-2,4-hexadiene, 1,3-octadiene, 1,3-cyclopentadiene, 1,3-cyclohexadiene, 1-phenyl-1,3-butadiene, 1,4-diphenyl-1,3-butadiene Examples include conjugated diene compounds such as ene, 1-methoxy-1,3-butadiene, 2-methoxy-1,3-butadiene, 1-ethoxy-1,3-butadiene, 2-ethoxy-1,3-butadiene, 2-nitro-1,3-butadiene, chloroprene, 1-chloro-1,3-butadiene, 1-bromo-1,3-butadiene, 2-bromo-1,3-butadiene, ocimene, phellandrene, myrcene, farnesene, sorbic acid, sorbate esters, and sorbates; conjugated triene compounds such as 1,3,5-hexatriene, 2,4,6-octatriene-1-carboxylic acid, eleostearic acid, tung oil, cholecalciferol, flubene, and tropone; and cyclooctatetraene, 2,4,6,8-decatetraene-1-carboxylic acid, retinol, and retinoic acid.

共役ポリエン化合物(C)としては、ソルビン酸、ソルビン酸エステル、ソルビン酸塩、ミルセンまたはこれらのうちの2以上の混合物が好ましく、ソルビン酸、ソルビン酸塩(ソルビン酸ナトリウム、ソルビン酸カリウム等)またはこれらの混合物がより好ましい。ソルビン酸、ソルビン酸塩またはこれらの混合物は、高温での酸化劣化の抑制効果が高く、また食品添加剤としても広く工業的に使用されているため衛生性や入手性の観点からも好ましい。 The conjugated polyene compound (C) is preferably sorbic acid, sorbate ester, sorbate salt, myrcene, or a mixture of two or more of these, and more preferably sorbic acid, sorbate salts (sodium sorbate, potassium sorbate, etc.), or a mixture thereof. Sorbic acid, sorbate salts, or mixtures thereof are preferred from the viewpoint of hygiene and availability because they have a high inhibitory effect on oxidative degradation at high temperatures and are widely used industrially as food additives.

共役ポリエン化合物(C)の分子量としては、通常1,000以下であり、500以下が好ましく、300以下がより好ましい。共役ポリエン化合物(C)の分子量が上記上限以下である場合、樹脂組成物中への共役ポリエン化合物(C)の分散状態が良好になり、溶融成形後の外観が高まる傾向にある。共役ポリエン化合物(C)の分子量の下限は例えば54であり、60であってもよく、80であってもよい。 The molecular weight of the conjugated polyene compound (C) is usually 1,000 or less, preferably 500 or less, and more preferably 300 or less. When the molecular weight of the conjugated polyene compound (C) is below the above upper limit, the dispersion state of the conjugated polyene compound (C) in the resin composition becomes good, and the appearance after melt molding tends to improve. The lower limit of the molecular weight of the conjugated polyene compound (C) is, for example, 54, but it may also be 60 or 80.

本発明の樹脂組成物におけるEVOH(A)に対する共役ポリエン化合物(C)の含有量cの下限は、1ppmが好ましく、3ppmがより好ましい。また、本発明の樹脂組成物におけるEVOH(A)に対する共役ポリエン化合物(C)の含有量cは300ppm未満が好ましく、100ppm以下がより好ましく、70ppm以下がさらに好ましく、30ppm以下がよりさらに好ましく、20ppm以下、10ppm以下が特に好ましい場合もある。共役ポリエン化合物(C)の含有量cが上記範囲であると溶融成形時の色相の悪化をより抑制できる傾向となる。 The lower limit of the content c of the conjugated polyene compound (C) relative to EVOH (A) in the resin composition of the present invention is preferably 1 ppm, more preferably 3 ppm. Furthermore, the content c of the conjugated polyene compound (C) relative to EVOH (A) in the resin composition of the present invention is preferably less than 300 ppm, more preferably 100 ppm or less, even more preferably 70 ppm or less, even more preferably 30 ppm or less, and particularly preferably 20 ppm or less, or 10 ppm or less. When the content c of the conjugated polyene compound (C) is within the above range, the deterioration of hue during melt molding tends to be more suppressed.

(熱可塑性エラストマー(F))
本発明の樹脂組成物は、該樹脂組成物から得られる成形体等の耐屈曲性等を改善するため、さらに熱可塑性エラストマー(F)を含有しても良い。
(Thermoplastic elastomer (F))
The resin composition of the present invention may further contain a thermoplastic elastomer (F) in order to improve the flexibility and other properties of molded articles and the like obtained from the resin composition.

熱可塑性エラストマー(F)としては特に限定されず、ポリエステル系熱可塑性エラストマー、ポリスチレン系熱可塑性エラストマー、ポリオレフィン系熱可塑性エラストマー等を用いることができる。これらは、一種又は二種以上を組み合わせても良い。中でも、耐屈曲性を向上させる観点から、熱可塑性エラストマー(F)は、ポリスチレン系熱可塑性エラストマー及びポリオレフィン系熱可塑性エラストマーからなる群から選択される少なくとも1種であることが好ましい。 The thermoplastic elastomer (F) is not particularly limited, and polyester-based thermoplastic elastomers, polystyrene-based thermoplastic elastomers, polyolefin-based thermoplastic elastomers, etc., can be used. These may be used individually or in combination of two or more. In particular, from the viewpoint of improving flexibility, it is preferable that the thermoplastic elastomer (F) is at least one selected from the group consisting of polystyrene-based thermoplastic elastomers and polyolefin-based thermoplastic elastomers.

熱可塑性エラストマー(F)は、変性熱可塑性エラストマーであることが好ましい。変性熱可塑性エラストマーとしては、不飽和カルボン酸又はその誘導体で変性されていることが好ましく、不飽和カルボン酸又はその誘導体としては、マレイン酸、フマル酸、イタコン酸、無水マレイン酸、無水イタコン酸、マレイン酸モノメチルエステル、マレイン酸モノエチルエステル、マレイン酸ジエチルエステル、フマル酸モノメチルエステル等が挙げられる。中でも無水マレイン酸変性熱可塑性エラストマーであることがより好ましい。熱可塑性エラストマー(F)が変性熱可塑性エラストマーであると、EVOH(A)との相溶性が高まり、ガスバリア性、透明性、柔軟性及び剥離性がより向上するため好ましい。 The thermoplastic elastomer (F) is preferably a modified thermoplastic elastomer. The modified thermoplastic elastomer is preferably modified with an unsaturated carboxylic acid or its derivative. Examples of unsaturated carboxylic acids or their derivatives include maleic acid, fumaric acid, itaconic acid, maleic anhydride, itaconic anhydride, monomethyl maleic acid, monoethyl maleic acid, diethyl maleic acid, and monomethyl fumaric acid. Among these, a maleic anhydride-modified thermoplastic elastomer is more preferable. A modified thermoplastic elastomer (F) is preferable because it improves compatibility with EVOH (A), resulting in enhanced gas barrier properties, transparency, flexibility, and release properties.

上記ポリエステル系熱可塑性エラストマー(以下、TPEEと称することがある)としては、分子中のハードセグメントとしてポリエステルを、ソフトセグメントとしてガラス転移温度(Tg)の低いポリエーテル又はポリエステルを備えるマルチブロックコポリマーが挙げられる。TPEEは、分子構造の違いによって以下のタイプに分けることができ、中でもポリエステル・ポリエーテル型TPEEとポリエステル・ポリエステル型TPEEが好ましい。
(1)ポリエステル・ポリエーテル型TPEE
一般には、ハードセグメントとして芳香族系結晶性ポリエステルを、ソフトセグメントとしてポリエーテルを用いた熱可塑性エラストマーである。
(2)ポリエステル・ポリエステル型TPEE
ハードセグメントとして芳香族系結晶性ポリエステルを、ソフトセグメントとして脂肪族系ポリエステルを用いた熱可塑性エラストマーである。
(3)液晶性TPEE
ハードセグメントとして剛直な液晶分子を、ソフトセグメントとして脂肪族系ポリエステルを用いた熱可塑性エラストマーである。
Examples of the above-mentioned polyester-based thermoplastic elastomers (hereinafter sometimes referred to as TPEE) include multiblock copolymers having polyester as the hard segment in the molecule and a polyether or polyester with a low glass transition temperature (Tg) as the soft segment. TPEEs can be classified into the following types based on differences in molecular structure, with polyester-polyether type TPEEs and polyester-polyester type TPEEs being preferred.
(1) Polyester/Polyether type TPEE
Generally, it is a thermoplastic elastomer using aromatic crystalline polyester as the hard segment and polyether as the soft segment.
(2) Polyester/Polyester-type TPEE
This thermoplastic elastomer uses aromatic crystalline polyester as the hard segment and aliphatic polyester as the soft segment.
(3) Liquid crystalline TPEE
This thermoplastic elastomer uses rigid liquid crystal molecules as the hard segment and aliphatic polyester as the soft segment.

上記ポリエステルセグメントとしては、テレフタル酸、イソフタル酸、ナフタレンジカルボン酸等の芳香族ジカルボン酸;1,4-シクロヘキサンジカルボン酸等の脂環式ジカルボン酸;コハク酸、アジピン酸等の脂肪族ジカルボン酸等のジカルボン酸成分と、エチレングリコール、1,2-プロピレングリコール、1,4-ブタンジオール等の脂肪族ジオール;シクロヘキサン-1,4-ジメタノール等の脂環式ジオール等のジオール成分とからなるポリエステルセグメントが挙げられる。上記ポリエーテルセグメントとしては、ポリエチレングリコール、ポリプロピレングリコール、ポリブチレングリコール等の脂肪族ポリエーテルセグメントが挙げられる。上記ポリエステル系熱可塑性エラストマーは変性ポリエステル系熱可塑性エラストマーであることが好ましく、無水マレイン酸変性ポリエステル系熱可塑性エラストマーであることがより好ましい。 Examples of the above-mentioned polyester segments include those comprising dicarboxylic acid components such as aromatic dicarboxylic acids (terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, etc.), alicyclic dicarboxylic acids (1,4-cyclohexanedicarboxylic acid, etc.), and aliphatic dicarboxylic acids (succinic acid, adipic acid, etc.), and diol components such as aliphatic diols (ethylene glycol, 1,2-propylene glycol, 1,4-butanediol, etc.) and alicyclic diols (cyclohexane-1,4-dimethanol, etc.). Examples of the above-mentioned polyether segments include aliphatic polyether segments such as polyethylene glycol, polypropylene glycol, and polybutylene glycol. The above-mentioned polyester-based thermoplastic elastomer is preferably a modified polyester-based thermoplastic elastomer, and more preferably a maleic anhydride-modified polyester-based thermoplastic elastomer.

上記ポリスチレン系熱可塑性エラストマーとしては、特に限定されないが、通常、ハードセグメントとしてスチレンモノマー重合体ブロック(Hb)を、ソフトセグメントとして共役ジエン化合物重合体ブロック又はその水添ブロック(Sb)を備える。このスチレン系熱可塑性エラストマーの構造としては、Hb-Sbで表されるジブロック構造、Hb-Sb-Hb若しくはSb-Hb-Sbで表されるトリブロック構造、Hb-Sb-Hb-Sbで表されるテトラブロック構造、又はHbとSbとが計5個以上直鎖状に結合しているポリブロック構造であってもよい。 The polystyrene-based thermoplastic elastomer described above is not particularly limited, but typically comprises a styrene monomer polymer block (Hb) as a hard segment and a conjugated diene compound polymer block or its hydrogenated block (Sb) as a soft segment. The structure of this styrene-based thermoplastic elastomer may be a diblock structure represented by Hb-Sb, a triblock structure represented by Hb-Sb-Hb or Sb-Hb-Sb, a tetrablock structure represented by Hb-Sb-Hb-Sb, or a polyblock structure in which five or more Hb and Sb molecules are linked in a linear chain.

上記スチレンモノマー重合体ブロック(Hb)に使用されるスチレン系モノマーとしては、特に限定されず、スチレン及びその誘導体等を挙げることができる。具体的には、スチレン、α―メチルスチレン、2-メチルスチレン、4-メチルスチレン、4-プロピルスチレン、4-t-ブチルスチレン、4-シクロヘキシルスチレン、4-ドデシルスチレン、2-エチル-4-ベンジルスチレン、4-(フェニルブチル)スチレン、2,4,6-トリメチルスチレン、モノフルオロスチレン、ジフルオロスチレン、モノクロロスチレン、ジクロロスチレン、メトキシスチレン、t-ブトキシスチレン等のスチレン類;1-ビニルナフタレン、2-ビニルナフタレン等のビニルナフタレン類等のビニル基含有芳香族化合物;インデン、アセナフチレン等のビニレン基含有芳香族化合物等が挙げられる。中でもスチレンが好ましい。スチレン系モノマーは1種のみでも良く、2種以上であっても良い。 The styrene monomer used in the above-mentioned styrene monomer polymer block (Hb) is not particularly limited, and examples include styrene and its derivatives. Specifically, examples include styrenes such as styrene, α-methylstyrene, 2-methylstyrene, 4-methylstyrene, 4-propylstyrene, 4-t-butylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, 2,4,6-trimethylstyrene, monofluorostyrene, difluorostyrene, monochlorostyrene, dichlorostyrene, methoxystyrene, and t-butoxystyrene; vinyl group-containing aromatic compounds such as vinylnaphthalenes such as 1-vinylnaphthalene and 2-vinylnaphthalene; and vinylene group-containing aromatic compounds such as indene and acenaphthylene. Among these, styrene is preferred. The styrene monomer may be used alone or in combination of two or more types.

上記共役ジエン化合物重合体ブロック又はその水添ブロック(Sb)に使用される共役ジエン化合物も、特に限定されず、例えば、ブタジエン、イソプレン、2,3-ジメチルブタジエン、ペンタジエン、ヘキサジエン等を挙げることができる。中でも、ブタジエンが好ましい。共役ジエン化合物は1種のみでも良く、2種以上であっても良い。さらに、他の共単量体、例えば、エチレン、プロピレン、ブチレン、スチレンを共重合することもできる。また、共役ジエン化合物重合体ブロックは、部分的又は完全に水素添加されている水素添加体であっても良い。 The conjugated diene compound used in the above-mentioned conjugated diene compound polymer block or its hydrogenated block (Sb) is not particularly limited, and examples include butadiene, isoprene, 2,3-dimethylbutadiene, pentadiene, hexadiene, etc. Among these, butadiene is preferred. The conjugated diene compound may be used alone or in combination of two or more. Furthermore, other comonomers, such as ethylene, propylene, butylene, and styrene, can also be copolymerized. The conjugated diene compound polymer block may also be a hydrogenated product, partially or completely hydrogenated.

ポリスチレン系熱可塑性エラストマーの具体例としては、スチレン-イソプレンジブロック共重合体(SI)、スチレン-ブタジエンジブロック共重合体(SB)、スチレン-イソプレン-スチレントリブロック共重合体(SIS)、スチレン-ブタジエン/イソプレン-スチレントリブロック共重合体(SB/IS)、及びスチレン-ブタジエン-スチレントリブロック共重合体(SBS)並びにその水素添加体が挙げられる。中でも、スチレン-イソプレンジブロック共重合体の水素添加体(SEP)、スチレン-ブタジエンジブロック共重合体の水素添加体(SEB)、スチレン-イソプレン-スチレントリブロック共重合体の水素添加体(SEPS)、スチレン-ブタジエン/イソプレン-スチレントリブロック共重合体の水素添加体(SEEPS)、及びスチレン-ブタジエン-スチレントリブロック共重合体の水素添加体(SEBS)からなる群から選択される少なくとも1種が好ましい。上記ポリスチレン系熱可塑性エラストマーは変性ポリスチレン系熱可塑性エラストマーであることが好ましく、無水マレイン酸変性ポリスチレン系熱可塑性エラストマーであることがより好ましい。 Specific examples of polystyrene-based thermoplastic elastomers include styrene-isoprene diblock copolymer (SI), styrene-butadiene diblock copolymer (SB), styrene-isoprene-styrene triblock copolymer (SIS), styrene-butadiene/isoprene-styrene triblock copolymer (SB/IS), and styrene-butadiene-styrene triblock copolymer (SBS), as well as their hydrogenated derivatives. Among these, at least one selected from the group consisting of hydrogenated styrene-isoprene diblock copolymer (SEP), hydrogenated styrene-butadiene diblock copolymer (SEB), hydrogenated styrene-isoprene-styrene triblock copolymer (SEPS), hydrogenated styrene-butadiene/isoprene-styrene triblock copolymer (SEEPS), and hydrogenated styrene-butadiene-styrene triblock copolymer (SEBS) is preferred. The above polystyrene-based thermoplastic elastomer is preferably a modified polystyrene-based thermoplastic elastomer, and more preferably a maleic anhydride-modified polystyrene-based thermoplastic elastomer.

上記ポリオレフィン系熱可塑性エラストマーには、ハードセグメントとしてポリプロピレンやポリエチレン等のポリオレフィンブロックを、ソフトセグメントとしてエチレン-プロピレン-ジエン共重合体等のゴムブロックを備える熱可塑性エラストマー等が含まれる。なお、かかる熱可塑性エラストマーには、ブレンド型とインプラント化型がある。また、変性ポリオレフィン系熱可塑性エラストマーとしては、無水マレイン酸変性エチレン-ブテン-1共重合体、無水マレイン酸変性エチレン-プロピレン共重合体、ハロゲン化ブチル系ゴム、変性ポリプロピレン、変性ポリエチレン等を挙げることもできる。上記ポリオレフィン系熱可塑性エラストマーは変性ポリオレフィン系熱可塑性エラストマーであることが好ましく、無水マレイン酸変性ポリオレフィン系熱可塑性エラストマーであることがより好ましい。 The above-mentioned polyolefin-based thermoplastic elastomers include thermoplastic elastomers comprising polyolefin blocks such as polypropylene and polyethylene as hard segments and rubber blocks such as ethylene-propylene-diene copolymers as soft segments. Such thermoplastic elastomers are available in blended and implantable types. Furthermore, modified polyolefin-based thermoplastic elastomers can also be described as maleic anhydride-modified ethylene-butene-1 copolymer, maleic anhydride-modified ethylene-propylene copolymer, halogenated butyl rubber, modified polypropylene, modified polyethylene, etc. The above-mentioned polyolefin-based thermoplastic elastomer is preferably a modified polyolefin-based thermoplastic elastomer, and more preferably a maleic anhydride-modified polyolefin-based thermoplastic elastomer.

本発明の樹脂組成物における熱可塑性エラストマー(F)のEVOH(A)に対する質量比(F/A)の下限は、5/95が好ましく、8/92がより好ましく、12/88がさらに好ましく、15/85又は25/75がさらに好ましい場合もある。質量比(F/A)を上記下限以上とすることで、得られる成形体等の耐屈曲性等を高めることができる。一方、この質量比(F/A)の上限としては、35/65が好ましく、30/70がより好ましく、25/75がさらに好ましい場合もある。質量比(F/A)を上記上限以下とすることで、ガスバリア性等をより高めることができる。 In the resin composition of the present invention, the lower limit of the mass ratio (F/A) of thermoplastic elastomer (F) to EVOH (A) is preferably 5/95, more preferably 8/92, even more preferably 12/88, and in some cases even more preferably 15/85 or 25/75. By setting the mass ratio (F/A) to be above the above lower limit, the bending resistance and other properties of the resulting molded article can be improved. On the other hand, the upper limit of this mass ratio (F/A) is preferably 35/65, more preferably 30/70, and in some cases even more preferably 25/75. By setting the mass ratio (F/A) to be below the above upper limit, gas barrier properties and other properties can be further improved.

(相分離構造)
本発明の樹脂組成物において、EVOH(A)のマトリックス中に熱可塑性エラストマー(F)の粒子が分散していることが好ましい。すなわち、本発明の樹脂組成物は、海島構造を有し、海相が主にEVOH(A)からなり、島相が主に熱可塑性エラストマー(F)からなる海島構造であることが好ましい。このように、海相が主にEVOH(A)からなることで、ガスバリア性を保ちつつ、柔軟性が向上する。
(phase separation structure)
In the resin composition of the present invention, it is preferable that particles of thermoplastic elastomer (F) are dispersed in a matrix of EVOH (A). That is, it is preferable that the resin composition of the present invention has a sea-island structure in which the sea phase mainly consists of EVOH (A) and the island phase mainly consists of thermoplastic elastomer (F). In this way, by having the sea phase mainly consist of EVOH (A), flexibility is improved while maintaining gas barrier properties.

本発明の樹脂組成物が海島構造を有し、海相が主にEVOH(A)からなり、島相が主に熱可塑性エラストマー(F)からなる場合、透明性を向上させる観点から、熱可塑性エラストマー(F)からなる島相の平均粒子径は4.5μm以下が好ましく、3.5μm以下がより好ましく、3.0μm以下がさらに好ましく、2.5μm以下が特に好ましく、2.0μm以下が最も好ましい。熱可塑性エラストマー(F)の平均粒子径は0.1μm以上であってもよい。熱可塑性エラストマー(F)からなる島相の平均粒子径が上記範囲であると、ガスバリア性及び透明性を保ちつつ、柔軟性が向上し、さらに剥離性が向上するため好ましい。熱可塑性エラストマー(F)の平均粒子径は、混錬強度の調整、及びEVOH(A)と熱可塑性エラストマー(F)との組成比により調整できる。 When the resin composition of the present invention has a sea-island structure, with the sea phase mainly consisting of EVOH(A) and the island phase mainly consisting of thermoplastic elastomer(F), from the viewpoint of improving transparency, the average particle size of the island phase consisting of thermoplastic elastomer(F) is preferably 4.5 μm or less, more preferably 3.5 μm or less, even more preferably 3.0 μm or less, particularly preferably 2.5 μm or less, and most preferably 2.0 μm or less. The average particle size of the thermoplastic elastomer(F) may be 0.1 μm or more. When the average particle size of the island phase consisting of thermoplastic elastomer(F) is within the above range, it is preferable because flexibility is improved while maintaining gas barrier properties and transparency, and furthermore, release properties are improved. The average particle size of the thermoplastic elastomer(F) can be adjusted by adjusting the kneading strength and the composition ratio of EVOH(A) and thermoplastic elastomer(F).

本発明の樹脂組成物において、EVOH(A)と熱可塑性エラストマー(F)との屈折率差は0.05以下が好ましく、0.04以下がより好ましく、0.03以下がさらに好ましい。該屈折率差は、0.005以上であってもよい。該屈折率差が上記範囲であると、本発明の樹脂組成物の透明性がより良好になるため好ましい。 In the resin composition of the present invention, the refractive index difference between EVOH (A) and thermoplastic elastomer (F) is preferably 0.05 or less, more preferably 0.04 or less, and even more preferably 0.03 or less. The refractive index difference may also be 0.005 or more. A refractive index difference within the above range is preferable because it results in better transparency of the resin composition of the present invention.

(その他の任意成分)
本発明の樹脂組成物は、EVOH(A)、不飽和脂肪族アルデヒド(B)、酸化防止剤(G)、共役ポリエン化合物(C)及び熱可塑性エラストマー(F)以外のその他の任意成分として、ホウ素化合物、カルボン酸類、リン化合物、金属イオン、紫外線吸収剤、可塑剤、帯電防止剤、滑剤、着色剤、充填剤、熱安定剤、EVOH(A)及び熱可塑性エラストマー(F)以外の他の樹脂、高級脂肪族カルボン酸の金属塩等を含んでいてもよい。本発明の樹脂組成物は、これらの成分を2種以上含有してもよい。本発明の樹脂組成物が、その他の任意成分を含む場合、その合計含有量の上限は1質量%が好ましく、0.5質量%が好ましい場合もある。
(Other optional components)
The resin composition of the present invention may contain, as other optional components besides EVOH (A), unsaturated aliphatic aldehyde (B), antioxidant (G), conjugated polyene compound (C), and thermoplastic elastomer (F), boron compounds, carboxylic acids, phosphorus compounds, metal ions, ultraviolet absorbers, plasticizers, antistatic agents, lubricants, colorants, fillers, heat stabilizers, other resins other than EVOH (A) and thermoplastic elastomer (F), metal salts of higher aliphatic carboxylic acids, etc. The resin composition of the present invention may contain two or more of these components. If the resin composition of the present invention contains other optional components, the upper limit of their total content is preferably 1% by mass, and may also be preferably 0.5% by mass.

ホウ素化合物は、溶融成形時のゲル化を抑制すると共に押出成形機等のトルク変動(加熱時の粘度変化)を抑制するものである。上記ホウ素化合物としては、例えばオルトホウ酸、メタホウ酸、四ホウ酸等のホウ酸類;ホウ酸トリエチル、ホウ酸トリメチル等のホウ酸エステル;上記ホウ酸類のアルカリ金属塩又はアルカリ土類金属塩、ホウ砂等のホウ酸塩;水素化ホウ素類などが挙げられる。これらの中でも、ホウ酸類が好ましく、オルトホウ酸(以下、「ホウ酸」ともいう)がより好ましい。EVOH(A)に対するホウ素化合物の含有量の下限としては、100ppmが好ましく、500ppmがより好ましい。また、EVOH(A)に対するホウ素化合物の含有量の上限としては、5,000ppmが好ましく、3,000ppmがより好ましく、1,000ppmがさらに好ましい。ホウ素化合物の含有量を上記下限以上とすることで、押出成形機等のトルク変動を十分に抑制することができる。一方、ホウ素化合物の含有量を上記上限以下とすることで、溶融成形時にゲル化が起こりにくくなり樹脂組成物ひいては成形体の外観が向上する。なお、ホウ素化合物の含有量は、ホウ素化合物のオルトホウ酸換算含有量である。 Boron compounds suppress gelation during melt molding and also suppress torque fluctuations (viscosity changes during heating) in extrusion molding machines, etc. Examples of the above boron compounds include boric acids such as orthoboric acid, metaboric acid, and tetraboric acid; boric acid esters such as triethyl borate and trimethyl borate; alkali metal salts or alkaline earth metal salts of the above boric acids, borates such as borax; and boron hydrides. Among these, boric acids are preferred, and orthoboric acid (hereinafter also referred to as "boric acid") is more preferred. The lower limit of the content of the boron compound relative to EVOH(A) is preferably 100 ppm, and more preferably 500 ppm. The upper limit of the content of the boron compound relative to EVOH(A) is preferably 5,000 ppm, more preferably 3,000 ppm, and even more preferably 1,000 ppm. By keeping the boron compound content above the lower limit mentioned above, torque fluctuations in extrusion molding machines and other equipment can be sufficiently suppressed. On the other hand, by keeping the boron compound content below the upper limit mentioned above, gelation during melt molding becomes less likely, improving the appearance of the resin composition and, consequently, the molded product. Note that the boron compound content is expressed as the orthoboric acid equivalent of the boron compound.

カルボン酸類は、樹脂組成物ひいては成形体の着色を防止すると共に溶融成形時のゲル化を抑制するものである。カルボン酸類としては、ギ酸、酢酸、プロピオン酸、酪酸、乳酸、これらの塩等が挙げられる。カルボン酸類としては、炭素数4以下のカルボン酸類又は飽和カルボン酸類が好ましく、酢酸類がより好ましい。この酢酸類は、酢酸及び酢酸塩を含む。酢酸類としては、酢酸及び酢酸塩を併用することが好ましく、酢酸及び酢酸ナトリウムを併用することがより好ましい。EVOH(A)に対するカルボン酸類の含有量の下限としては、50ppmが好ましく、100ppmがより好ましく、150ppmがさらに好ましい。また、EVOH(A)に対するカルボン酸類の含有量の上限としては、1,000ppmが好ましく、500ppmがより好ましく、400ppmがさらに好ましい。カルボン酸類の含有量を上記下限以上とすることで、十分な着色抑制効果が得られ、黄変の発生を十分に抑制することができる。一方、カルボン酸類の含有量を上記上限以下とすることで、溶融成形時、特に長時間に及ぶ溶融成形時にゲル化が生じにくくなり、成形体等の外観が良好になる。 Carboxylic acids prevent discoloration of the resin composition and, consequently, the molded article, and also suppress gelation during melt molding. Examples of carboxylic acids include formic acid, acetic acid, propionic acid, butyric acid, lactic acid, and their salts. Preferred carboxylic acids are those with four or fewer carbon atoms or saturated carboxylic acids, with acetic acid being more preferred. Acetic acids include acetic acid and acetate salts. It is preferable to use acetic acid and acetate salts in combination, and more preferable to use acetic acid and sodium acetate in combination. The lower limit of the carboxylic acid content relative to EVOH(A) is preferably 50 ppm, more preferably 100 ppm, and even more preferably 150 ppm. The upper limit of the carboxylic acid content relative to EVOH(A) is preferably 1,000 ppm, more preferably 500 ppm, and even more preferably 400 ppm. By setting the carboxylic acid content above the above lower limit, a sufficient discoloration suppression effect can be obtained, and the occurrence of yellowing can be sufficiently suppressed. On the other hand, by keeping the carboxylic acid content below the above upper limit, gelation is less likely to occur during melt molding, especially during long melt molding periods, resulting in a better appearance for molded products.

リン化合物は、ストリーク、フィッシュアイ等の欠陥の発生及び着色を抑制すると共に、ロングラン性を向上させるものである。このリン化合物としては、例えばリン酸、亜リン酸等のリン酸塩等が挙げられる。上記リン酸塩としては、第一リン酸塩、第二リン酸塩及び第三リン酸塩のいずれの形でもよい。また、リン酸塩のカチオン種についても特に限定されるものではないが、アルカリ金属塩及びアルカリ土類金属塩が好ましく、これらのうちリン酸二水素ナトリウム、リン酸二水素カリウム、リン酸水素二ナトリウム及びリン酸水素二カリウムがより好ましく、リン酸二水素ナトリウム及びリン酸水素二カリウムがさらに好ましい。EVOH(A)に対するリン化合物の含有量の下限としては、1ppmが好ましく、10ppmがより好ましく、20ppmがさらに好ましく、30ppmが特に好ましい。EVOH(A)に対するリン化合物の含有量の上限としては、200ppmが好ましく、150ppmがより好ましく、100ppmがさらに好ましい。リン化合物の含有量を上記下限以上とすること、又は上記上限以下とすることで、熱安定性が向上し、長時間にわたる溶融成形を行なう際のゲル状ブツの発生、着色等が生じにくくなる。 Phosphorus compounds suppress the occurrence of defects such as streaks and fish eyes, as well as discoloration, and improve long-run performance. Examples of phosphorus compounds include phosphates such as phosphoric acid and phosphorous acid. The above phosphates may be in the form of monophosphates, diphosphates, or tertiary phosphates. The cation species of the phosphate is not particularly limited, but alkali metal salts and alkaline earth metal salts are preferred, of which sodium dihydrogen phosphate, potassium dihydrogen phosphate, disodium hydrogen phosphate, and dipotassium hydrogen phosphate are more preferred, and sodium dihydrogen phosphate and dipotassium hydrogen phosphate are even more preferred. The lower limit of the phosphorus compound content relative to EVOH(A) is preferably 1 ppm, more preferably 10 ppm, even more preferably 20 ppm, and particularly preferably 30 ppm. The upper limit of the phosphorus compound content relative to EVOH(A) is preferably 200 ppm, more preferably 150 ppm, and even more preferably 100 ppm. By setting the phosphorus compound content above the lower limit or below the upper limit, thermal stability is improved, reducing the likelihood of gel-like formation and discoloration during prolonged melt molding.

金属イオンとしては、一価金属イオン、二価金属イオン、その他遷移金属イオンが挙げられ、これらは1種又は複数種からなっていてもよい。中でも一価金属イオン及び二価金属イオンが好ましい。一価金属イオンとしては、アルカリ金属イオンが好ましく、例えばリチウム、ナトリウム、カリウム、ルビジウム及びセシウムのイオンが挙げられ、工業的な入手容易性の点からはナトリウム又はカリウムのイオンが好ましい。また、アルカリ金属イオンを与えるアルカリ金属塩としては、例えば脂肪族カルボン酸塩、芳香族カルボン酸塩、炭酸塩、塩酸塩、硝酸塩、硫酸塩、リン酸塩及び金属錯体が挙げられる。中でも、脂肪族カルボン酸塩及びリン酸塩が入手容易である点から好ましく、具体的には、酢酸ナトリウム、酢酸カリウム、リン酸ナトリウム及びリン酸カリウムが好ましい。金属イオンとして二価金属イオンを含むことが好ましい場合もある。金属イオンが二価金属イオンを含むと、例えばトリムを回収して再利用した際のEVOHの熱劣化が抑制され、得られる成形体のゲル及びブツの発生が抑制される場合がある。二価金属イオンとしては、例えばベリリウム、マグネシウム、カルシウム、ストロンチウム、バリウム及び亜鉛のイオンが挙げられるが、工業的な入手容易性の点からはマグネシウム、カルシウム又は亜鉛のイオンが好ましい。また、二価金属イオンを与える二価金属塩としては、例えばカルボン酸塩、炭酸塩、塩酸塩、硝酸塩、硫酸塩、リン酸塩及び金属錯体が挙げられカルボン酸塩が好ましい。カルボン酸塩を構成するカルボン酸としては、炭素数1~30のカルボン酸が好ましく、具体的には、酢酸、プロピオン酸、酪酸、ステアリン酸、ラウリン酸、モンタン酸、ベヘン酸、オクチル酸、セバシン酸、リシノール酸、ミリスチン酸、パルミチン酸等が挙げられ、中でも、酢酸及びステアリン酸が好ましい。EVOH(A)に対する金属イオンの含有量の下限は1ppmが好ましく、100ppmがより好ましく、150ppmがさらに好ましい。一方、金属イオンの含有量の上限は1,000ppmが好ましく、400ppmがより好ましく、350ppmがさらに好ましい。EVOH(A)に対する金属イオンの含有量が1ppm以上であると、得られる積層体の層間接着性が良好となる傾向となる。一方、金属イオンの含有量が1,000ppm以下であると、着色耐性が良好となる傾向となる。 Examples of metal ions include monovalent metal ions, divalent metal ions, and other transition metal ions, which may consist of one or more types. Among these, monovalent metal ions and divalent metal ions are preferred. Among monovalent metal ions, alkali metal ions are preferred, such as lithium, sodium, potassium, rubidium, and cesium ions, with sodium or potassium ions being preferred from the viewpoint of industrial availability. Examples of alkali metal salts that provide alkali metal ions include aliphatic carboxylates, aromatic carboxylates, carbonates, hydrochlorides, nitrates, sulfates, phosphates, and metal complexes. Among these, aliphatic carboxylates and phosphates are preferred from the viewpoint of availability, and specifically, sodium acetate, potassium acetate, sodium phosphate, and potassium phosphate are preferred. It is also preferable to include divalent metal ions as metal ions. When the metal ions include divalent metal ions, for example, the thermal degradation of EVOH when trim is recovered and reused may be suppressed, and the generation of gel and blemishes in the resulting molded article may be suppressed. Examples of divalent metal ions include beryllium, magnesium, calcium, strontium, barium, and zinc ions, but magnesium, calcium, or zinc ions are preferred from the viewpoint of industrial availability. Examples of divalent metal salts that provide divalent metal ions include carboxylates, carbonates, hydrochlorides, nitrates, sulfates, phosphates, and metal complexes, with carboxylates being preferred. Preferred carboxylic acids constituting the carboxylates are carboxylic acids having 1 to 30 carbon atoms, specifically including acetic acid, propionic acid, butyric acid, stearic acid, lauric acid, montanic acid, behenic acid, octic acid, sebacic acid, ricinoleic acid, myristic acid, palmitic acid, etc., with acetic acid and stearic acid being preferred among them. The lower limit of the metal ion content relative to EVOH(A) is preferably 1 ppm, more preferably 100 ppm, and even more preferably 150 ppm. On the other hand, the upper limit of the metal ion content is preferably 1,000 ppm, more preferably 400 ppm, and even more preferably 350 ppm. When the metal ion content relative to EVOH(A) is 1 ppm or more, the resulting laminate tends to have good interlayer adhesion. Conversely, when the metal ion content is 1,000 ppm or less, the color resistance tends to be good.

可塑剤としては、例えばフタル酸ジメチル、フタル酸ジエチル、フタル酸ジオクチル、ワックス、流動パラフィン、リン酸エステル等が挙げられる。帯電防止剤としては、例えばペンタエリスリットモノステアレート、ソルビタンモノパルミテート、硫酸化ポリオレフィン類、ポリエチレンオキシド、ポリエチレングリコール(商品名:カーボワックス)等が挙げられる。 Examples of plasticizers include dimethyl phthalate, diethyl phthalate, dioctyl phthalate, waxes, liquid paraffin, and phosphate esters. Examples of antistatic agents include pentaerythritol monostearate, sorbitan monopalmitate, sulfated polyolefins, polyethylene oxide, and polyethylene glycol (trade name: Carbowax).

滑剤としては、例えばエチレンビスステアロアミド、ブチルステアレート等が挙げられる。着色剤としては、例えばカーボンブラック、フタロシアニン、キナクリドン、インドリン、アゾ系顔料、ベンガラ等が挙げられる。充填剤としては、例えばグラスファイバー、ウォラストナイト、ケイ酸カルシウム、タルク、モンモリロナイト等が挙げられる。熱安定剤としては、例えばヒンダードフェノール系化合物、ヒンダードアミン系化合物等が挙げられる。 Examples of lubricants include ethylene bisstearamide and butyl stearate. Examples of colorants include carbon black, phthalocyanine, quinacridone, indoline, azo pigments, and red iron oxide. Examples of fillers include glass fiber, wollastonite, calcium silicate, talc, and montmorillonite. Examples of heat stabilizers include hindered phenol compounds and hindered amine compounds.

EVOH(A)及び熱可塑性エラストマー(F)以外の他の樹脂としては、例えばポリアミド、ポリオレフィン等が挙げられる。高級脂肪族カルボン酸の金属塩としては、例えばステアリン酸ナトリウム、ステアリン酸カリウム、ステアリン酸カルシウム、ステアリン酸マグネシウム等が挙げられる。 Other resins besides EVOH (A) and thermoplastic elastomer (F) include, for example, polyamides and polyolefins. Examples of metal salts of higher aliphatic carboxylic acids include, for example, sodium stearate, potassium stearate, calcium stearate, and magnesium stearate.

本発明の樹脂組成物において、EVOH(A)、不飽和脂肪族アルデヒド(B)(クロトンアルデヒド(B1)、2,4-ヘキサジエナール(B2)及び2,4,6-オクタトリエナール(B3))及び酸化防止剤(G)の合計含有量は、90質量%以上が好ましく、95質量%以上がより好ましく、98質量%以上がさらに好ましく、99質量%以上が特に好ましい。本発明の樹脂組成物は実質的にEVOH(A)、不飽和脂肪族アルデヒド(B)及び酸化防止剤(G)のみから構成されていてもよく、本発明の樹脂組成物はEVOH(A)、不飽和脂肪族アルデヒド(B)及び酸化防止剤(G)のみから構成されていてもよい。なお、本明細書において「実質的に~のみからなる」とは、本発明の効果に影響を与えない範囲で任意成分の含有を許容するものであり、本明細書において「のみからなる」とは、不可避的に含まれてしまう不純物以外の任意成分を除外するものである。 In the resin composition of the present invention, the total content of EVOH (A), unsaturated aliphatic aldehyde (B) (crotonaldehyde (B1), 2,4-hexadienal (B2), and 2,4,6-octatrienal (B3)), and antioxidant (G) is preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 98% by mass or more, and particularly preferably 99% by mass or more. The resin composition of the present invention may consist substantially only of EVOH (A), unsaturated aliphatic aldehyde (B), and antioxidant (G), or it may consist only of EVOH (A), unsaturated aliphatic aldehyde (B), and antioxidant (G). In this specification, "substantially consisting only of" means that the inclusion of optional components is permitted within a range that does not affect the effects of the present invention, and "consisting only of" means that optional components other than impurities that are inevitably included are excluded.

本発明の樹脂組成物の210℃、2,160g荷重下でのメルトフローレート(MFR)の下限としては、0.5g/10分が好ましく、1g/10分がより好ましい。一方、このMFRの上限としては、30g/10分が好ましく、20g/10分がより好ましい。本発明の樹脂組成物のMFRが上記範囲であることで、溶融成形性等を高めることができる。また、本発明の樹脂組成物のMFRが上記範囲であると、ネックイン耐性がより良好となる傾向となる。 The lower limit of the melt flow rate (MFR) of the resin composition of the present invention at 210°C and a load of 2,160 g is preferably 0.5 g/10 min, and more preferably 1 g/10 min. On the other hand, the upper limit of the MFR is preferably 30 g/10 min, and more preferably 20 g/10 min. Having the MFR of the resin composition of the present invention within the above range improves melt moldability and other properties. Furthermore, having the MFR of the resin composition of the present invention within the above range tends to result in better neck-in resistance.

<樹脂組成物の調製方法>
本発明の樹脂組成物の製造方法は、EVOH(A)と不飽和脂肪族アルデヒド(B)とを含む樹脂組成物を製造した後、この樹脂組成物と酸化防止剤(G)とを混合する方法、EVOH(A)、不飽和脂肪族アルデヒド(B)及び酸化防止剤(G)を一括して混合する方法などが挙げられる。当該製造方法は、例えば、
(1)エチレンとビニルエステルとを共重合させる工程、及び
(2)工程(1)により得られた共重合体をケン化する工程
を備える樹脂組成物の製造方法であって、上記樹脂組成物中に所定量及び所定比率の不飽和脂肪族アルデヒド(B)及び酸化防止剤(G)を含有させることを特徴とする製造方法等が挙げられる。
<Method for preparing resin composition>
Methods for producing the resin composition of the present invention include a method of producing a resin composition containing EVOH (A) and an unsaturated aliphatic aldehyde (B), and then mixing this resin composition with an antioxidant (G), or a method of mixing EVOH (A), an unsaturated aliphatic aldehyde (B), and an antioxidant (G) all at once. For example, the production method is as follows:
Examples of methods for producing a resin composition include (1) a step of copolymerizing ethylene and a vinyl ester, and (2) a step of saponifying the copolymer obtained in step (1), characterized in that the resin composition contains a predetermined amount and a predetermined ratio of an unsaturated aliphatic aldehyde (B) and an antioxidant (G).

樹脂組成物中に不飽和脂肪族アルデヒド(B)を含有させる方法としては、特に限定されないが、例えば、上記工程(1)において不飽和脂肪族アルデヒド(B)を添加する方法、上記工程(2)において不飽和脂肪族アルデヒド(B)を添加する方法、上記工程(2)により得られたEVOH(A)に、不飽和脂肪族アルデヒド(B)を添加する方法等が挙げられる。なお、上記工程(1)において不飽和脂肪族アルデヒド(B)を添加する方法、又は上記工程(2)において不飽和脂肪族アルデヒド(B)を添加する方法を採用する場合には、得られる樹脂組成物中に所望量の不飽和脂肪族アルデヒド(B)を含有させるために、上記工程(1)における重合反応、上記工程(2)におけるケン化反応で消費される量を考慮して添加量を多くする必要がある。したがって、重合反応やケン化反応工程で不飽和脂肪族アルデヒド(B)を添加する場合は消費される不飽和脂肪族アルデヒド(B)の量を加算して添加することが好ましい。一方、上記工程(2)より得られたEVOH(A)に不飽和脂肪族アルデヒド(B)を添加する方法は工程内での消費を考慮せずに添加できるため、操作性に優れている。 There are no particular limitations on the method for incorporating unsaturated aliphatic aldehyde (B) into the resin composition. Examples include adding unsaturated aliphatic aldehyde (B) in step (1), adding unsaturated aliphatic aldehyde (B) in step (2), or adding unsaturated aliphatic aldehyde (B) to EVOH (A) obtained in step (2). When adopting the method of adding unsaturated aliphatic aldehyde (B) in step (1) or step (2), it is necessary to increase the amount added, taking into account the amount consumed in the polymerization reaction in step (1) and the saponification reaction in step (2), in order to contain the desired amount of unsaturated aliphatic aldehyde (B) in the resulting resin composition. Therefore, when adding unsaturated aliphatic aldehyde (B) in the polymerization or saponification reaction steps, it is preferable to add the amount of unsaturated aliphatic aldehyde (B) that will be consumed. On the other hand, the method of adding unsaturated aliphatic aldehyde (B) to EVOH (A) obtained from step (2) above offers superior operability because the addition can be done without considering consumption within the process.

EVOH(A)に不飽和脂肪族アルデヒド(B)を添加する方法としては、例えば1)不飽和脂肪族アルデヒド(B)を予めEVOH(A)に配合してペレットを造粒する方法、2)エチレン-ビニルエステル共重合体のケン化後にペーストを析出させる工程で析出させたストランドに不飽和脂肪族アルデヒド(B)を含浸させる方法、3)析出させたストランドをカットした後に不飽和脂肪族アルデヒド(B)を含浸させる方法、4)乾燥樹脂組成物のチップを再溶解したものに不飽和脂肪族アルデヒド(B)を添加する方法、5)EVOH(A)及び不飽和脂肪族アルデヒド(B)の各成分をブレンドしたものを溶融混練する方法、6)押出機の途中からEVOH(A)溶融物に不飽和脂肪族アルデヒド(B)をフィードし含有させる方法、7)不飽和脂肪族アルデヒド(B)をEVOH(A)の一部に高濃度で配合して造粒したマスターバッチを作成しEVOH(A)とドライブレンドして溶融混練する方法等が挙げられる。 Methods for adding an unsaturated aliphatic aldehyde (B) to EVOH (A) include, for example, 1) a method of granulating pellets by pre-mixing the unsaturated aliphatic aldehyde (B) with EVOH (A), 2) a method of impregnating strands precipitated in a process of precipitating a paste after saponification of ethylene-vinyl ester copolymer with the unsaturated aliphatic aldehyde (B), 3) a method of impregnating the precipitated strands with the unsaturated aliphatic aldehyde (B) after cutting them, and 4) a method of re-processing chips of a dried resin composition. Methods include: 5) adding unsaturated aliphatic aldehyde (B) to a dissolved substance; 6) melt-kneading a blend of EVOH (A) and unsaturated aliphatic aldehyde (B); 7) feeding unsaturated aliphatic aldehyde (B) into the EVOH (A) molten material from the middle of an extruder; and 8) creating a masterbatch by granulating a high-concentration blend of unsaturated aliphatic aldehyde (B) with a portion of EVOH (A), dry-blending it with EVOH (A), and then melt-kneading it.

これらのうち、EVOH(A)中に微量の不飽和脂肪族アルデヒド(B)を均一性高く分散することができる観点から、1)の不飽和脂肪族アルデヒド(B)を予めEVOH(A)に配合してペレットを造粒する方法が好ましい。具体的には、EVOH(A)を水/メタノール混合溶媒等の良溶媒に溶解させた溶液に、不飽和脂肪族アルデヒド(B)を添加し、その混合溶液をノズル等から貧溶媒中に押出して析出及び/又は凝固させ、それを洗浄及び/又は乾燥することにより、EVOH(A)に不飽和脂肪族アルデヒド(B)が均一性高く混合された樹脂組成物ペレットを得ることができる。 Of these methods, from the viewpoint of uniformly dispersing a trace amount of unsaturated aliphatic aldehyde (B) in EVOH (A), the method of granulating pellets by pre-mixing the unsaturated aliphatic aldehyde (B) with EVOH (A) (as in method 1) is preferred. Specifically, by dissolving EVOH (A) in a good solvent such as a water/methanol mixed solvent, adding the unsaturated aliphatic aldehyde (B) to the solution, extruding the mixed solution into a poor solvent through a nozzle or the like to precipitate and/or solidify it, and then washing and/or drying it, a resin composition pellet in which the unsaturated aliphatic aldehyde (B) is uniformly mixed with EVOH (A) can be obtained.

EVOH(A)及び不飽和脂肪族アルデヒド(B)を含む樹脂組成物と、酸化防止剤(G)とを混合する方法としては、溶融混練等の公知の方法によって行うことができる。この際、さらに他の成分を加えて溶融混練等してもよい。EVOH(A)、不飽和脂肪族アルデヒド(B)及び酸化防止剤(G)を一括して混合する方法としては、上記混合物を製造する4)、5)、6)又は7)の方法において、不飽和脂肪族アルデヒド(B)と共に、酸化防止剤(G)をドライブレンド又は添加する方法が挙げられる。この際、同様に、さらに他の成分をドライブレンド又は添加してもよい。なお、その他成分の混合には、リボンブレンダー、高速ミキサーコニーダー、ミキシングロール、押出機、インテンシブミキサー等を用いることができる。 A resin composition containing EVOH (A) and an unsaturated aliphatic aldehyde (B) can be mixed with an antioxidant (G) by known methods such as melt kneading. In this case, other components may be added and then melt kneaded. A method for mixing EVOH (A), an unsaturated aliphatic aldehyde (B), and an antioxidant (G) together is to dry blend or add the antioxidant (G) together with the unsaturated aliphatic aldehyde (B) in the methods 4), 5), 6), or 7) for producing the above mixture. In this case, other components may also be dry blended or added. For mixing other components, a ribbon blender, a high-speed mixer/kneader, a mixing roll, an extruder, an intensive mixer, etc., can be used.

本発明の樹脂組成物は、ペレット形状であることが、取扱性が容易である点から好ましい。本発明の樹脂組成物のペレットの形状は特に限定されるものではないが、円柱状、角柱状、球状、略球状(lenticular)などが挙げられ、中でも、ペレットの搬送安定性、取扱性、生産性等の観点から、円柱状、球状または略球状(lenticular)が好ましい。円柱状の場合、直径は1mm以上10mm以下が好ましく、2mm以上8mm以下がより好ましく、高さは1mm以上10mm以下が好ましく、2mm以上8mm以下がより好ましく、3mm以上5mm以下がさらに好ましい。球状または略球状(lenticular)である場合、短手方向の長さは1mm以上10mm以下が好ましく、2mm以上8mm以下がより好ましく、長手方向の長さは1mm以上10mm以下が好ましく、2mm以上8mm以下がより好ましい。 The resin composition of the present invention is preferably in pellet form for ease of handling. While the shape of the pellets of the resin composition of the present invention is not particularly limited, examples include cylindrical, prismatic, spherical, and lenticular shapes. Among these, cylindrical, spherical, or lenticular shapes are preferred from the viewpoint of pellet transport stability, handling, and productivity. For cylindrical pellets, the diameter is preferably 1 mm to 10 mm, more preferably 2 mm to 8 mm; the height is preferably 1 mm to 10 mm, more preferably 2 mm to 8 mm, and even more preferably 3 mm to 5 mm. For spherical or lenticular pellets, the length in the short direction is preferably 1 mm to 10 mm, more preferably 2 mm to 8 mm; and the length in the long direction is preferably 1 mm to 10 mm, more preferably 2 mm to 8 mm.

<成形体>
本発明の樹脂組成物は、溶融成形等により、フィルム、シート、チューブ、袋、ボトル等の成形体に形成できる。本発明の樹脂組成物からなる部分を有する成形体は、ネックイン及びダイビルドアップを抑制できるため、本発明の成形体は、生産性が高い。なお、本発明の成形体は、本発明の樹脂組成物から形成された部分を有すればよい。すなわち、本発明の成形体は、本発明の樹脂組成物のみからなる成形体であってもよいし、本発明の樹脂組成物のみからなる部分と、他の部分とから構成される成形体であってもよい。本明細書においてフィルムとは通常300μm未満の厚みを有するものをいい、シートとは通常300μm以上の厚みを有するものをいう。溶融成形の方法としては、例えば、押出成形、キャスト成形、インフレーション押出成形、ブロー成形、溶融紡糸、射出成形、射出ブロー成形、共押出ブロー成形等が挙げられる。溶融成形温度はEVOH(A)の融点等により異なるが、150~270℃程度が好ましい。これらの成形体は再使用の目的で粉砕し再度成形することも可能である。また、フィルム、シート等を一軸または二軸延伸することも可能である。
<Molded product>
The resin composition of the present invention can be formed into molded articles such as films, sheets, tubes, bags, and bottles by melt molding or the like. Molded articles having a portion made of the resin composition of the present invention can suppress neck-in and die build-up, thus the molded articles of the present invention have high productivity. The molded articles of the present invention only need to have a portion formed from the resin composition of the present invention. That is, the molded articles of the present invention may be made only of the resin composition of the present invention, or they may be made of a portion made only of the resin composition of the present invention and other portions. In this specification, a film usually refers to one with a thickness of less than 300 μm, and a sheet usually refers to one with a thickness of 300 μm or more. Examples of melt molding methods include extrusion molding, cast molding, inflation extrusion molding, blow molding, melt spinning, injection molding, injection blow molding, and co-extrusion blow molding. The melt molding temperature varies depending on the melting point of EVOH(A), but is preferably around 150 to 270°C. These molded articles can also be crushed and remolded for reuse. Furthermore, films, sheets, etc. can be uniaxially or biaxially stretched.

(フィルム及びシート)
本発明の樹脂組成物から形成されるフィルム及びシート(以下、「フィルム等」と略記する場合がある。)は、ネックイン及びダイビルドアップの発生が抑制されているため、生産性が高い。かかるフィルム等としては、単層のフィルム等及び多層のフィルム等が含まれる。当該フィルム等は、各種包装材料等として用いることができる。
(Films and sheets)
Films and sheets formed from the resin composition of the present invention (hereinafter sometimes abbreviated as "films, etc.") have high productivity because the occurrence of neck-in and die build-up is suppressed. Such films, etc. include single-layer films, etc. and multi-layer films, etc. Such films, etc. can be used as various packaging materials, etc.

フィルム等は、上述の成形体を製造する方法として示したものと同様の方法で製造できる。中でも、本発明の樹脂組成物をキャスティングロール上に溶融押出するキャスト成形工程、本発明の樹脂組成物から得られる無延伸フィルムを延伸する工程(一軸延伸工程、逐次二軸工程、同時二軸延伸工程、インフレーション成形工程等)を備える方法が好ましい。かかるフィルム等の製造方法によれば、これらの工程を備えることで、耐破断性を向上できる。 The film and the like can be manufactured by the same method as described above for manufacturing the molded article. Among these, a method comprising a cast molding step in which the resin composition of the present invention is melt-extruded onto a casting roll, and a stretching step (uniaxial stretching step, sequential biaxial stretching step, simultaneous biaxial stretching step, inflation molding step, etc.) of the unstretched film obtained from the resin composition of the present invention is preferred. By incorporating these steps, the break resistance can be improved in such a film manufacturing method.

<積層体>
本発明の積層体は、本発明の樹脂組成物からなる層(以下、「バリア層」又は「EVOH層」ともいう)を少なくとも1層有し、他の成分からなる層をさらに有する。積層体は、単層構造の成形体に比べて、機能向上などの利点がある。また、本発明の積層体は、ネックイン及びダイビルドアップが抑制された樹脂組成物を用いて製造されているため、連続生産性が高い。積層体の層数の下限は、2層であってもよく、3層であってもよい。積層体の層数の上限としては、1000層であってもよく、100層であってもよく、10層であってもよい。また、本発明の積層体は、樹脂以外の成分から形成される層、例えば紙から形成される層、金属層等をさらに有していてもよい。
<Laminated structure>
The laminate of the present invention has at least one layer made of the resin composition of the present invention (hereinafter also referred to as the "barrier layer" or "EVOH layer"), and further has layers made of other components. The laminate has advantages such as improved functionality compared to a single-layer molded article. Furthermore, since the laminate of the present invention is manufactured using a resin composition that suppresses neck-in and die build-up, it has high continuous productivity. The lower limit of the number of layers in the laminate may be two or three. The upper limit of the number of layers in the laminate may be 1000, 100, or 10. Furthermore, the laminate of the present invention may further have layers formed from components other than resin, such as layers formed from paper, metal layers, etc.

他の成分からなる層としては、熱可塑性樹脂から形成される熱可塑性樹脂層が好ましい。本発明の積層体の層構造は特に限定されず、バリア層をE、接着性樹脂から得られる層をAd、熱可塑性樹脂から得られる層をT、直接積層されていることを「/」で表わす場合、例えばT/E/T、E/Ad/T、T/Ad/E/Ad/T、E/Ad/T/Ad/E、E/Ad/T/Ad/E/Ad/T/Ad/E等の構造が挙げられる。これらの各層は単層であっても多層であってもよい。なお、接着性樹脂から得られる層Adは、熱可塑性樹脂から形成される熱可塑性樹脂層に含まれる場合もある。 As for the layers composed of other components, a thermoplastic resin layer formed from a thermoplastic resin is preferred. The layer structure of the laminate of the present invention is not particularly limited. When the barrier layer is represented by E, the layer obtained from the adhesive resin by Ad, the layer obtained from the thermoplastic resin by T, and direct lamination is represented by "/", examples of structures include T/E/T, E/Ad/T, T/Ad/E/Ad/T, E/Ad/T/Ad/E, E/Ad/T/Ad/E/Ad/T/Ad/E, etc. Each of these layers may be a single layer or a multilayer. Note that the layer Ad obtained from the adhesive resin may also be included in the thermoplastic resin layer formed from the thermoplastic resin.

熱可塑性樹脂としては、例えば直鎖状低密度ポリエチレン、低密度ポリエチレン、中密度ポリエチレン、高密度ポリエチレン、エチレン-酢酸ビニル共重合体、エチレン-プロピレン共重合体、ポリプロピレン、プロピレン-α-オレフィン(炭素数4~20のα-オレフィン)共重合体、ポリブテン、ポリペンテン等のオレフィンの単独またはその共重合体;ポリエチレンテレフタレート等のポリエステル;ポリエステルエラストマー;ナイロン-6、ナイロン-66等のポリアミド;ポリスチレン;ポリ塩化ビニル、ポリ塩化ビニリデン、アクリル系樹脂、ビニルエステル系樹脂、ポリウレタンエラストマー、ポリカーボネート、塩素化ポリエチレン、塩素化ポリプロピレン等が挙げられる。中でも、ポリプロピレン、ポリエチレン、エチレン-プロピレン共重合体、エチレン-酢酸ビニル共重合体、ポリアミド、ポリスチレン及びポリエステルが好ましく用いられる。 Examples of thermoplastic resins include linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, polypropylene, propylene-α-olefin (α-olefin with 4 to 20 carbon atoms) copolymer, polybutene, polypentene, and other olefins alone or copolymers thereof; polyesters such as polyethylene terephthalate; polyester elastomers; polyamides such as nylon-6 and nylon-66; polystyrene; polyvinyl chloride, polyvinylidene chloride, acrylic resins, vinyl ester resins, polyurethane elastomers, polycarbonate, chlorinated polyethylene, and chlorinated polypropylene. Among these, polypropylene, polyethylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, polyamide, polystyrene, and polyester are preferred.

接着性樹脂としては、ガスバリア層及び他の成分からなる層との接着性を有していれば特に限定されないが、カルボン酸変性ポリオレフィンを含有する接着性樹脂が好ましい。カルボン酸変性ポリオレフィンとしては、オレフィン系重合体にエチレン性不飽和カルボン酸、そのエステルまたはその無水物を化学的に結合させたカルボキシル基を含有する変性オレフィン系重合体が好ましい。ここでオレフィン系重合体とは、ポリエチレン、直鎖状低密度ポリエチレン、ポリプロピレン、ポリブテン等のポリオレフィン、及びオレフィンと他のモノマーとの共重合体を意味する。中でも、直鎖状低密度ポリエチレン、エチレン-酢酸ビニル共重合体及びエチレン-アクリル酸エチル共重合体が好ましく、直鎖状低密度ポリエチレン及びエチレン-酢酸ビニル共重合体が特に好ましい。 The adhesive resin is not particularly limited as long as it has adhesion to the gas barrier layer and the layers made of other components, but an adhesive resin containing a carboxylic acid-modified polyolefin is preferred. As the carboxylic acid-modified polyolefin, a modified olefin polymer containing a carboxyl group obtained by chemically bonding an ethylenically unsaturated carboxylic acid, its ester, or its anhydride to an olefin polymer is preferred. Here, olefin polymer refers to polyolefins such as polyethylene, linear low-density polyethylene, polypropylene, and polybutene, and copolymers of olefins and other monomers. Among these, linear low-density polyethylene, ethylene-vinyl acetate copolymer, and ethylene-ethyl acrylate copolymer are preferred, and linear low-density polyethylene and ethylene-vinyl acetate copolymer are particularly preferred.

本発明の積層体はダイビルドアップが抑制される観点から、最外層にバリア層を備える態様も好適に用いられる。最外層にバリア層を備える場合、本発明の積層体は共押出成形にて作製されることが好ましく、その後、かかる積層体のバリア層上に無機蒸着層を形成してもよいし、他の成分からなる層をラミネートしてもよい。EVOHは無機蒸着層、特にアルミニウムまたは酸化アルミニウムの蒸着層との親和性が高いため、バリア層と無機蒸着層との層間接着性が良好となる傾向となる。最外層にバリア層を備える層構成としては、バリア層をE、接着性樹脂から得られる層をAd、熱可塑性樹脂から得られる層をT、直接積層されていることを「/」で表わす場合、E/Ad/T、E/Ad/T/Ad/E、E/Ad/T/Ad/E/Ad/T/Ad/E等が挙げられる。なお、最外層にバリア層を備える積層体である場合、リサイクル性を良好にする観点からTはポリオレフィンであることが好ましい。 From the viewpoint of suppressing die build-up, the laminate of the present invention is also preferably used in a form in which a barrier layer is provided as the outermost layer. When a barrier layer is provided as the outermost layer, the laminate of the present invention is preferably manufactured by co-extrusion molding. Afterward, an inorganic vapor-deposited layer may be formed on the barrier layer of such laminate, or a layer made of other components may be laminated. Since EVOH has high affinity for inorganic vapor-deposited layers, particularly aluminum or aluminum oxide vapor-deposited layers, the interlayer adhesion between the barrier layer and the inorganic vapor-deposited layer tends to be good. Examples of layer configurations with a barrier layer as the outermost layer include E/Ad/T, E/Ad/T/Ad/E, E/Ad/T/Ad/E/Ad/T/Ad/E, etc., where E represents the barrier layer, Ad represents the layer obtained from the adhesive resin, T represents the layer obtained from the thermoplastic resin, and "/" indicates direct lamination. Furthermore, when the laminate has a barrier layer as the outermost layer, T is preferably a polyolefin from the viewpoint of improving recyclability.

本発明の積層体を製造する方法は特に限定されず、例えば本発明の樹脂組成物からなる成形体(フィルム、シート等)に他の成分を溶融押出する方法、本発明の樹脂組成物と他の成分を共押出する方法、本発明の樹脂組成物と他の成分を共射出成形する方法、本発明の樹脂組成物からなるバリア層と他の成分からなる層とを有機チタン化合物、イソシアネート化合物、ポリエステル系化合物等の公知の接着剤を用いてラミネートする方法等が挙げられる。 The method for manufacturing the laminate of the present invention is not particularly limited. Examples include melt-extrusion of other components into a molded article (film, sheet, etc.) made of the resin composition of the present invention; co-extrusion of the resin composition of the present invention and other components; co-injection molding of the resin composition of the present invention and other components; and lamination of a barrier layer made of the resin composition of the present invention and a layer made of other components using known adhesives such as organic titanium compounds, isocyanate compounds, and polyester compounds.

本発明の樹脂組成物と他の成分の共押出の方法は特に限定されず、マルチマニホールド合流方式Tダイ法、フィードブロック合流方式Tダイ法、インフレーション法等を挙げることができる。 The method for co-extruding the resin composition of the present invention with other components is not particularly limited and can include the multi-manifold confluence T-die method, the feedblock confluence T-die method, the inflation method, and the like.

本発明の積層体が、多層のフィルム又はシートである場合、平均厚さは特に限定されず、下限は例えば1μm、5μm又は10μmであってよい。一方、平均厚さの上限は例えば3mm、1mm、300μm又は100μmであってもよい。当該積層体の形状は積層構造を有するものであれば特に限定されるものではない。多層の熱成形容器、多層のブロー成形容器、多層のパイプ、蒸着フィルム等も当該積層体の形態に含まれる。 When the laminate of the present invention is a multilayer film or sheet, the average thickness is not particularly limited, and the lower limit may be, for example, 1 μm, 5 μm, or 10 μm. On the other hand, the upper limit of the average thickness may be, for example, 3 mm, 1 mm, 300 μm, or 100 μm. The shape of the laminate is not particularly limited as long as it has a multilayer structure. Multilayer thermoformed containers, multilayer blow-molded containers, multilayer pipes, vapor-deposited films, etc., are also included in the form of the laminate.

本発明の成形体、積層体等は、フィルム状又はシート状であってよく、様々な形状に成形されてもよい。本発明の成形体、積層体等は、包装材料、容器、チューブ等に用いることができ、また、熱成形容器等の熱成形用の材料としても好適に用いることができる。本発明の積層体から得られる熱成形体は、スジ等の欠陥が少なく、外観性に優れる。かかる熱成形体も本発明の成形体、積層体等の一実施形態である。さらに、本発明の成形体、積層体等においては、バリア層(EVOH層)に酸化防止剤が含有されていることにより、長期間高温で使用した場合であっても、バリア層(EVOH層)に酸化劣化によるクラックが発生しにくい。このため、屋外で使用される日用品、包装材、機械部品等に好適である。上記成形体、積層体等の特徴が特に効果的に発揮される用途の例としては、飲食品用包装材、容器用パッキング材、フィルム、農業用フィルム、ジオメンブレン、医療用輸液バッグ材、高圧タンク材、ガソリンタンク材、燃料容器、タイヤ用チューブ材、靴用クッション材、バッグインボックス用内袋材、有機液体貯蔵用タンク材、パイプ(有機液体輸送用パイプ材、暖房用温水パイプ材(床暖房用温水パイプ材等)等)、樹脂製壁紙、植物培地等が挙げられる。特に、屋外で使用され、熱や光による劣化が生じ易く、EVOH層が積層体の最外層として共押出されたフィルム、パイプ、農業用フィルム、植物培地及びジオメンブレンとして、本発明の成形体及び積層体等が好適に用いられる。 The molded articles, laminates, etc. of the present invention may be in the form of films or sheets, and may be molded into various shapes. The molded articles, laminates, etc. of the present invention can be used as packaging materials, containers, tubes, etc., and can also be suitably used as materials for thermoforming, such as thermoformed containers. Thermoformed articles obtained from the laminates of the present invention have few defects such as streaks and have excellent appearance. Such thermoformed articles are also one embodiment of the molded articles, laminates, etc. of the present invention. Furthermore, in the molded articles, laminates, etc. of the present invention, because an antioxidant is contained in the barrier layer (EVOH layer), cracks due to oxidative degradation are less likely to occur in the barrier layer (EVOH layer) even when used at high temperatures for a long period of time. For this reason, they are suitable for daily necessities, packaging materials, machine parts, etc. used outdoors. Examples of applications where the above-described features of the molded articles, laminates, etc., are particularly effective include packaging materials for food and beverages, packing materials for containers, films, agricultural films, geomembranes, medical infusion bag materials, high-pressure tank materials, gasoline tank materials, fuel containers, tire tube materials, shoe cushioning materials, inner bag materials for bag-in-box systems, tank materials for organic liquid storage, pipes (pipe materials for organic liquid transport, hot water pipe materials for heating (hot water pipe materials for underfloor heating, etc.)), resin wallpaper, plant growing media, etc. In particular, the molded articles and laminates of the present invention are preferably used as films, pipes, agricultural films, plant growing media, and geomembranes that are used outdoors and are prone to degradation due to heat and light, and in which the EVOH layer is co-extruded as the outermost layer of the laminate.

<パイプ>
本発明のパイプは、本発明の樹脂組成物からなる層を有する。当該パイプは、溶融成形時のスジ等の欠陥が少なく、外観性に優れ、同じEVOHを用いたものと比較して長期間高温で使用した場合の安定性が改善されている。
<Pipe>
The pipe of the present invention has a layer made of the resin composition of the present invention. This pipe has fewer defects such as streaks during melt molding, has excellent appearance, and shows improved stability when used at high temperatures for extended periods compared to pipes using the same EVOH.

また、当該パイプが有する、本発明の樹脂組成物からなる層においては、この樹脂組成物が所定量の不飽和脂肪族アルデヒド(B)及び酸化防止剤(G)を含有している。これにより、欠点が少ない成形体となることによって、クラックの発生等が抑制され、長期間使用することなどが可能となる。 Furthermore, the layer of the pipe made of the resin composition of the present invention contains a predetermined amount of unsaturated aliphatic aldehyde (B) and antioxidant (G). This results in a molded article with fewer defects, suppressing crack formation and enabling long-term use.

当該パイプは、単層パイプであってもよく、多層パイプであってもよい。当該パイプが多層パイプである場合、この層構造は、上述した本発明の積層体と同様の層構造の例を挙げることができる。例えば、当該多層パイプの層構造は、本発明の樹脂組成物からなる層をE、接着層をAd、他の熱可塑性樹脂から得られる層をTで表わす場合、T/E/T、E/Ad/T、T/Ad/E/Ad/T等の構造が挙げられる。これらの各層は単層であっても多層であってもよい。接着層及び他の熱可塑性樹脂から得られる層に用いられる樹脂の具体例としては、本発明の積層体におけるこれらの層に用いられる樹脂と同様のものが挙げられる。また、当該パイプの製造方法も特に限定されず、本発明の樹脂組成物を溶融成形する方法として例示した各種成形方法を採用することができる。 The pipe may be a single-layer pipe or a multi-layer pipe. If the pipe is a multi-layer pipe, the layer structure can be similar to that of the laminate of the present invention described above. For example, if the layers of the multi-layer pipe are represented by E (the resin composition of the present invention), Ad (the adhesive layer), and T (the layer obtained from another thermoplastic resin), then structures such as T/E/T, E/Ad/T, and T/Ad/E/Ad/T are possible. Each of these layers may be single-layer or multi-layer. Specific examples of resins used in the adhesive layer and the layer obtained from another thermoplastic resin include those similar to those used in these layers in the laminate of the present invention. Furthermore, the method of manufacturing the pipe is not particularly limited, and various molding methods exemplified as methods for melt-molding the resin composition of the present invention can be employed.

当該パイプの用途は特に限定されず、例えば温水循環用パイプ、断熱多層パイプ、燃料用パイプ、ガス用パイプ等として使用することができる。 The use of this pipe is not particularly limited; for example, it can be used as a hot water circulation pipe, a multi-layered insulated pipe, a fuel pipe, a gas pipe, etc.

本発明のパイプが多層パイプであり、この多層パイプが温水循環用パイプとして用いられる場合には、上記樹脂組成物からなる層を最外層とするT/Ad/Eの3層構成が一般的に採用される。これは、既存の架橋ポリオレフィンなど単層パイプの製造ラインに、本発明の樹脂組成物と接着性樹脂の共押出コーティング設備を付加する事により、容易に多層パイプの製造ラインに転用でき、実際に多くのパイプメーカーがこの構成を採用しているためである。 When the pipe of the present invention is a multilayer pipe and is used as a hot water circulation pipe, a three-layer configuration of T/Ad/E, with the layer made of the above-mentioned resin composition as the outermost layer, is generally adopted. This is because existing single-layer pipe manufacturing lines, such as those for cross-linked polyolefins, can be easily converted into multilayer pipe manufacturing lines by adding co-extrusion coating equipment for the resin composition of the present invention and an adhesive resin. In fact, many pipe manufacturers have adopted this configuration.

本発明の樹脂組成物からなる層の両側にポリオレフィン層などを設けて、該樹脂組成物層を中間層として使用することは、該樹脂組成物層の傷付き防止などに有効である。しかしながら、多層パイプを床暖房パイプなどの温水循環用パイプとして用いる場合には、通常床下に埋設されるため、物理的な衝撃による本発明の樹脂組成物からなる層の傷付きなどのリスクは比較的小さい。従って、むしろガスバリア性の観点から、該樹脂組成物層を最外層に配することが望ましい。一般的にEVOH(A)のガスバリア性は大きな湿度依存性を示し、高湿度条件下ではバリア性が低下する。そこで、本発明の樹脂組成物からなる層を最外層に配することにより、主としてEVOH(A)から構成される本発明の樹脂組成物からなる層が水と接触するパイプ内表面より最も遠い場所に位置することとなり、多層パイプのバリア性能面からは最も有利な層構成となる。一方で、一般的にEVOH層を最外層に配する場合、空気と直接接触するため、酸化劣化の影響を受けやすい。このような環境下において、高温下でも酸化劣化しにくい本発明の樹脂組成物からなる層を最外層に配することにより、良好なバリア性を有しつつ酸化劣化によるクラックの発生を低減した多層パイプを提供するという効果がより有効に発揮される。 Providing polyolefin layers or the like on both sides of a layer made of the resin composition of the present invention, and using the resin composition layer as an intermediate layer, is effective in preventing damage to the resin composition layer. However, when multilayer pipes are used as hot water circulation pipes such as floor heating pipes, they are usually buried under the floor, so the risk of damage to the resin composition layer due to physical impact is relatively small. Therefore, from the viewpoint of gas barrier properties, it is preferable to place the resin composition layer as the outermost layer. Generally, the gas barrier properties of EVOH(A) show a large humidity dependence, and the barrier properties decrease under high humidity conditions. Therefore, by placing the layer made of the resin composition of the present invention as the outermost layer, the layer made of the resin composition of the present invention, which is mainly composed of EVOH(A), is located at the furthest point from the inner surface of the pipe that comes into contact with water, resulting in the most advantageous layer configuration in terms of the barrier performance of the multilayer pipe. On the other hand, when the EVOH layer is generally placed as the outermost layer, it comes into direct contact with air and is therefore susceptible to oxidative degradation. In such environments, by placing a layer made of the resin composition of the present invention, which is resistant to oxidative degradation even at high temperatures, as the outermost layer, the effect of providing a multilayer pipe with good barrier properties while reducing the occurrence of cracks due to oxidative degradation is more effectively demonstrated.

また、本発明のパイプが地域冷暖房などの断熱多層パイプに用いられる場合には、本発明の樹脂組成物からなる層を熱可塑性樹脂層より内側に配するT/Ad/Eの3層構成(以下、積層体1と略称することがある)、もしくは該樹脂組成物層の傷付き防止の観点からT/Ad/E/Ad/Tの5層構成(以下、積層体2と略称することがある)を有することが好ましい。 Furthermore, when the pipe of the present invention is used in a multi-layer insulated pipe for district heating and cooling, it is preferable to have a three-layer configuration of T/Ad/E (hereinafter sometimes abbreviated as laminate 1) in which the layer made of the resin composition of the present invention is arranged inside the thermoplastic resin layer, or a five-layer configuration of T/Ad/E/Ad/T (hereinafter sometimes abbreviated as laminate 2) from the viewpoint of preventing damage to the resin composition layer.

地域冷暖房などの断熱多層パイプの構成は特に限定されないが、例えば、内側から、内管、内管の周りを覆う断熱発泡体層、そして外層として本発明の樹脂組成物からなる層を有する上記積層体1又は2の順で配置されることが好ましい。 The configuration of the insulated multilayer pipes for district heating and cooling is not particularly limited, but it is preferable that, for example, the laminates 1 or 2 described above are arranged in the following order from the inside out: an inner pipe, an insulating foam layer surrounding the inner pipe, and an outer layer made of the resin composition of the present invention.

内管に使われるパイプの種類(素材)、形状及び大きさは、ガスや液体などの熱媒体を輸送できるものであれば特に限定はなく、熱媒体の種類や、配管材の用途及び使用形態等に応じて適宜選択することができる。具体的には、鋼、ステンレス、アルミニウム等の金属、ポリオレフィン(ポリエチレン、架橋ポリエチレン(PEX)、ポリプロピレン、ポリ1-ブテン、ポリ4-メチル-1-ペンテンなど)、及び本発明の樹脂組成物からなる層を有する上記積層体1又は2などが挙げられ、これらの中でも架橋ポリエチレン(PEX)が好適に用いられる。 The type (material), shape, and size of the pipe used for the inner tube are not particularly limited as long as they can transport a heat transfer medium such as gas or liquid, and can be appropriately selected according to the type of heat transfer medium, the application and usage of the piping material, etc. Specifically, examples include the laminate 1 or 2 having layers made of metals such as steel, stainless steel, and aluminum, polyolefins (polyethylene, cross-linked polyethylene (PEX), polypropylene, poly-1-butene, poly-4-methyl-1-pentene, etc.), and the resin composition of the present invention. Among these, cross-linked polyethylene (PEX) is preferably used.

断熱発泡体層を構成する断熱発泡体には、ポリウレタンフォーム、ポリエチレンフォーム、ポリスチレンフォーム、フェノールフォーム、ポリイソシアヌレートフォームを用いることができ、断熱性能向上の観点から、ポリウレタンフォームが好適に用いられる。 The insulating foam that makes up the insulating foam layer can be polyurethane foam, polyethylene foam, polystyrene foam, phenolic foam, or polyisocyanurate foam. From the viewpoint of improving insulating performance, polyurethane foam is preferably used.

断熱発泡体の発泡剤としてはフロンガス、各種代替フロン、水、塩化炭化水素、炭化水素、二酸化炭素等が用いられるが、発泡効果、環境への影響の観点から炭化水素、具体的にはn-ペンタン又はシクロペンタンが好適に用いられる。 As blowing agents for insulating foams, fluorocarbons, various alternative fluorocarbons, water, chlorinated hydrocarbons, hydrocarbons, carbon dioxide, etc., are used. However, from the viewpoint of blowing effect and environmental impact, hydrocarbons, specifically n-pentane or cyclopentane, are preferably used.

断熱多層パイプの製造方法としては、例えば、熱媒体を輸送する内管を、パイプ状の外層の中に入れて内管をスペーサーで固定し二重管とした後、内管と外層の間隙部に各種発泡体原液を注入し、発泡及び固化させる方法が挙げられる。上記スペーサーの素材は特に限定されないが、スペーサーによる内管及び外層への傷を減らすため、ポリエチレン又はポリウレタンであることが好ましい。 One method for manufacturing a multi-layered insulated pipe is to place an inner tube for transporting a heat transfer medium inside a pipe-shaped outer layer, fix the inner tube with a spacer to form a double-walled pipe, and then inject various foam concentrates into the gap between the inner tube and the outer layer, allowing them to foam and solidify. While the material of the spacer is not particularly limited, polyethylene or polyurethane is preferred to reduce damage to the inner tube and outer layer caused by the spacer.

本発明のパイプが燃料用パイプに用いられる場合には、本発明の樹脂組成物からなる層は、熱可塑性エラストマー(F)をさらに含有することがより好ましい。熱可塑性エラストマー(F)を含有することにより、パイプの耐クラック性等がより高まる。 When the pipe of the present invention is used as a fuel pipe, it is more preferable that the layer made of the resin composition of the present invention further contains a thermoplastic elastomer (F). The inclusion of the thermoplastic elastomer (F) further enhances the crack resistance and other properties of the pipe.

燃料用パイプに用いられる場合には、最内側層は導電性であるように形成される。そのために、最内側層の熱可塑性樹脂に、それ自体は知られている導電性添加物、例えば、カーボンブラック、グラファイト繊維等が混合される。 When used in fuel pipes, the innermost layer is formed to be conductive. To achieve this, the thermoplastic resin of the innermost layer is mixed with conductive additives that are known to be conductive, such as carbon black or graphite fibers.

<パイプ等の製造方法>
以下、パイプの一例として多層パイプの製造方法について説明するが、この製造方法の一部又は全部は他の成形体(フィルム、シート等)の製造方法にも適用することができる。多層パイプは、上述のように架橋ポリオレフィンなどの単層パイプの上に本発明の樹脂組成物と接着性樹脂を共押出コーティングすることにより製造することができる。単層パイプ上に本発明の樹脂組成物と接着性樹脂の共押出コーティングを実施する際は、単純に単層パイプ上に本発明の樹脂組成物と接着性樹脂の溶融したフィルムをコートしても良いが、単層パイプとコート層の間の接着力が不十分な場合があり、長期間の使用中にコート層が剥離してガスバリア性を失う可能性がある。その対策としては、コート前にコートするパイプの表面をフレーム処理及び/又はコロナ放電処理することが有効である。
<Methods for manufacturing pipes, etc.>
The following describes a method for manufacturing a multilayer pipe as an example of a pipe, but some or all of this manufacturing method can also be applied to the manufacturing of other molded articles (films, sheets, etc.). As described above, a multilayer pipe can be manufactured by co-extruding a resin composition of the present invention and an adhesive resin onto a single-layer pipe such as a cross-linked polyolefin. When co-extruding a resin composition of the present invention and an adhesive resin onto a single-layer pipe, it is possible to simply coat the single-layer pipe with a molten film of the resin composition of the present invention and an adhesive resin. However, the adhesive strength between the single-layer pipe and the coating layer may be insufficient, and the coating layer may peel off during long-term use, resulting in a loss of gas barrier properties. As a countermeasure, it is effective to flame-treat and/or corona-discharge treat the surface of the pipe to be coated before coating.

多層パイプを製造するためのその他の多層成形方法としては、樹脂層の種類に対応する数の押出機を使用し、この押出機内で溶融された樹脂の流れを重ねあわせた層状態で同時押出成形する、いわゆる共押出成形により実施する方法が挙げられる。また、ドライラミネーションなどの多層成形方法も採用され得る。 Other multilayer molding methods for manufacturing multilayer pipes include co-extrusion, which involves using a number of extruders corresponding to the types of resin layers and simultaneously extruding the molten resin flows within these extruders in overlapping layers. Other multilayer molding methods, such as dry lamination, may also be employed.

多層パイプの製造方法は、成形直後に10~70℃の水で冷却を行う工程を含むとよい。すなわち、溶融成形後、本発明の樹脂組成物からなる層が固化する前に10~70℃の水で冷却することにより、該樹脂組成物層を固化させることが望ましい。冷却水の温度が低すぎると、続く二次加工工程において多層パイプを屈曲させる場合に、屈曲部の本発明の樹脂組成物からなる層に歪みによるクラックが生じやすい。歪みによるクラックが生じやすくなる原因の詳細は明らかでないが、成形物中の残留応力が影響しているものと推測される。この観点から、冷却水の温度は15℃以上がより好ましく、20℃以上がさらに好ましい。一方、冷却水の温度が高すぎても、二次加工の際に屈曲部の本発明の樹脂組成物からなる層に歪みによるクラックを生じやすい。この原因の詳細も十分に解明されていないが、本発明の樹脂組成物からなる層の結晶化度が大きくなりすぎるためと推定される。この観点より冷却水の温度は60℃以下がより好ましく、50℃以下がさらに好ましい。 The manufacturing method for multilayer pipes preferably includes a step of cooling with water at 10 to 70°C immediately after molding. That is, it is desirable to solidify the resin composition layer by cooling it with water at 10 to 70°C after melt molding, before the layer made of the resin composition of the present invention solidifies. If the cooling water temperature is too low, cracks due to strain are likely to occur in the layer made of the resin composition of the present invention at the bent portion when the multilayer pipe is bent in the subsequent secondary processing step. The detailed cause of this increased likelihood of cracking due to strain is not clear, but it is presumed that residual stress in the molded product plays a role. From this viewpoint, a cooling water temperature of 15°C or higher is more preferable, and 20°C or higher is even more preferable. On the other hand, if the cooling water temperature is too high, cracks due to strain are likely to occur in the layer made of the resin composition of the present invention at the bent portion during secondary processing. The detailed cause of this is also not fully understood, but it is presumed that the degree of crystallinity of the layer made of the resin composition of the present invention becomes too high. From this viewpoint, a cooling water temperature of 60°C or lower is more preferable, and 50°C or lower is even more preferable.

上記の方法で得られた多層パイプを二次加工することにより、各種成形体を得ることができる。二次加工法としては、特に限定されず、公知の二次加工法を適宜用いることができるが、例えば、多層パイプを80~160℃に加熱した後所望の形に変形させた状態で、1分~2時間固定することにより加工する方法が挙げられる。 Various molded products can be obtained by secondary processing of the multilayer pipes obtained by the above method. The secondary processing method is not particularly limited, and known secondary processing methods can be used as appropriate. For example, one method involves heating the multilayer pipe to 80-160°C, deforming it into the desired shape, and then fixing it for 1 minute to 2 hours.

また、本発明のパイプが単層パイプである場合も、本発明の樹脂組成物を溶融成形する方法として上述した公知の成形方法により製造することができる。 Furthermore, even when the pipe of the present invention is a single-layer pipe, it can be manufactured by the known molding method described above as a method for melt-molding the resin composition of the present invention.

以下、実施例を挙げて本発明を詳細に説明するが、本発明はこれらの実施例に限定されるものではない。 The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[評価方法]
(1)エチレン単位含有量及びケン化度の測定
合成例で得られたEVOHの粗乾燥物について、真空乾燥機にて120℃で12時間乾燥した。真空乾燥したEVOHを、内部標準物質としてテトラメチルシラン(TMS)、添加剤としてトリフルオロ酢酸(TFA)を含む重ジメチルスルホキシド(DMSO-d6)に溶解し、500MHzの1H-NMR(日本電子株式会社製「GX-500」)を用いて80℃で測定し、エチレン単位、ビニルアルコール単位、ビニルエステル単位のピーク強度比よりエチレン単位含有量及びケン化度を求めた。
[Evaluation Method]
(1) Measurement of ethylene unit content and degree of saponification The crude dried EVOH obtained in the synthesis example was dried in a vacuum dryer at 120°C for 12 hours. The vacuum-dried EVOH was dissolved in deuterated dimethyl sulfoxide (DMSO-d6) containing tetramethylsilane (TMS) as an internal standard and trifluoroacetic acid (TFA) as an additive, and measured at 80°C using a 500 MHz 1H -NMR (GX-500, manufactured by JEOL Ltd.). The ethylene unit content and degree of saponification were determined from the peak intensity ratios of ethylene units, vinyl alcohol units, and vinyl ester units.

(2)ナトリウムイオン含有量、リン酸含有量及びホウ酸含有量
参考例及び参考比較例で得られた乾燥樹脂組成物ペレット0.5gをテフロン(登録商標)製圧力容器に入れ、ここに濃硝酸5mLを加えて室温で30分間分解させた。30分後に蓋をし、湿式分解装置(株式会社アクタック製「MWS-2」)を用いて150℃で10分間、次いで180℃で5分間加熱することで分解させ、その後室温まで冷却した。この処理液を50mLのメスフラスコ(TPX(登録商標)製)に移し純水でメスアップした。この溶液について、ICP発光分光分析装置(パーキンエルマー社製「OPTIMA4300DV」)で含有金属の分析を行い、ナトリウムイオン(ナトリウム元素)、リン酸及びホウ酸の含有量を測定した。リン酸の含有量に関してはリン酸根換算値として、ホウ酸の含有量についてはオルトホウ酸換算値として算出した。なお、定量に際しては、それぞれ市販の標準液を使用して作成した検量線を用いた。
(2) Sodium ion content, phosphoric acid content, and boric acid content 0.5 g of the dried resin composition pellets obtained in the reference example and reference comparative example were placed in a Teflon® pressure vessel, and 5 mL of concentrated nitric acid was added and decomposed at room temperature for 30 minutes. After 30 minutes, the lid was closed and the decomposition was carried out by heating at 150°C for 10 minutes, then at 180°C for 5 minutes, using a wet decomposition apparatus (MWS-2, manufactured by Actac Co., Ltd.), and then cooled to room temperature. This processed solution was transferred to a 50 mL volumetric flask (TPX®) and diluted with pure water. The metal content of this solution was analyzed using an ICP emission spectrometer (OPTIMA4300DV, manufactured by PerkinElmer), and the content of sodium ions (element sodium), phosphoric acid, and boric acid was measured. The phosphoric acid content was calculated as a phosphate root equivalent value, and the boric acid content was calculated as an orthoboric acid equivalent value. Calibration curves prepared using commercially available standard solutions were used for quantification.

(3)酢酸含有量
参考例及び参考比較例で得られた乾燥樹脂組成物ペレット20gをイオン交換水100mLに投入し、95℃で6時間加熱抽出した。フェノールフタレインを指示薬として、1/50規定のNaOHで抽出液を中和滴定し、酢酸含有量を定量した。
(3) Acetic acid content 20 g of the dried resin composition pellets obtained in the reference example and reference comparative example were placed in 100 mL of deionized water and heated at 95°C for 6 hours for extraction. The extract was neutralized and titrated with 1/50 N NaOH using phenolphthalein as an indicator to quantify the acetic acid content.

(4)メルトフローレート(MFR)
参考例及び参考比較例で得られた乾燥樹脂組成物ペレットを、メルトインデクサーL244(宝工業株式会社製)の内径9.55mm、長さ162mmのシリンダーに充填し、210℃で溶融した後、溶融した樹脂組成物に対して、質量2,160g、直径9.48mmのプランジャーを使用して均等に荷重をかけた。シリンダーの中央に設けた径2.1mmのオリフィスより単位時間当たりに押出される樹脂組成物量(g/10分)を測定し、これをMFRとした。
(4) Melt flow rate (MFR)
The dried resin composition pellets obtained in the reference example and reference comparative example were filled into a 9.55 mm inner diameter, 162 mm long cylinder of a melt indexer L244 (manufactured by Takara Kogyo Co., Ltd.), melted at 210°C, and then a uniform load was applied to the molten resin composition using a plunger with a mass of 2,160 g and a diameter of 9.48 mm. The amount of resin composition extruded per unit time (g/10 min) from a 2.1 mm diameter orifice located in the center of the cylinder was measured and defined as the MFR.

(5)クロトンアルデヒド、2,4-ヘキサジエナール及び2,4,6-オクタトリエナールの定量
参考例、参考比較例、実施例及び比較例で得られた乾燥樹脂組成物ペレット0.50gを凍結粉砕して得られたサンプルを、加熱脱着ガスクロマトグラフ質量分析装置用ガラスチューブに50.0mg秤量し、サンプルチューブを作成した。下記の加熱脱着ガスクロマトグラフ質量分析装置を用い、下記条件にてサンプルを加熱して揮発性ガスをサンプルから吸着管に一度全量吸着させた後、吸着管から再放出されるガスをカラムで分離し、成分毎のピークを検出した。クロトンアルデヒド、2,4-ヘキサジエナール及び2,4,6-オクタトリエナールの標準サンプルのピーク面積から検量線を作成し、絶対検量線法により、それぞれ定量した。なお、標準サンプルを測定する際は、吸着管(Tenax(登録商標)/Carboxen(登録商標)製)に標準サンプルを染み込ませ、サンプルチューブの代わりに標準サンプルを染み込ませた吸着管を用い、サンプル吸着後の放出時の温度について、サンプルチューブの温度170℃から吸着管の温度260℃に変更した以外は、サンプルチューブの測定の場合と同様の方法で測定した。
(加熱脱着部)
装置:TurboMatrix-ATD (パーキンエルマージャパン社製)
吸着管へサンプルを吸着する時の温度:170℃(サンプルチューブ)、-30℃(吸着管)、250℃(バルブ)、260℃(トランスファーライン)
吸着管への吸着時間:10分
サンプル吸着後の放出時の温度:170℃(サンプルチューブ)、260℃(吸着管)、250℃(バルブ)、260℃(トランスファーライン)
吸着管放出時間:35分
キャリアガス:ヘリウムカラムへのキャリアガスの流速:1.0ml/min
圧力:120kPa
(ガスクロマトグラフ質量分析部)
装置:7890B GC System, 7977B MSD (アジレント・テクノロジー社製)
カラム:DB-WAX UI (長さ:30m、内径:0.25mm、膜厚:0.50μm)
カラムオーブン温度:40℃で5分保持後10℃/minの昇温速度で240℃まで温調後10分保持(合計測定温度35分)
トランスファーライン(接続部)温度:240℃
イオン化条件:EI+
検出イオン質量範囲:m/z=29-600
検出方法:SCAN
(標準サンプル)
クロトンアルデヒド:Aldrich社製
2,4-ヘキサジエナール:Aldrich社製
2,4,6-オクタトリエナール:ナード研究所製
(5) Determination of crotonaldehyde, 2,4-hexadienal and 2,4,6-octatrienal A sample was prepared by freeze-pulverizing 0.50 g of dried resin composition pellets obtained in the Reference Example, Reference Comparative Example, Example, and Comparative Example, and weighing 50.0 mg of the sample into a glass tube for a thermal desorption gas chromatograph mass spectrometer. Using the thermal desorption gas chromatograph mass spectrometer described below, the sample was heated under the conditions described below to adsorb the volatile gas from the sample into an adsorption tube, and then the gas re-released from the adsorption tube was separated by a column to detect the peaks for each component. Calibration curves were created from the peak areas of standard samples of crotonaldehyde, 2,4-hexadienal and 2,4,6-octatrienal, and each was quantified using the absolute calibration curve method. When measuring the standard sample, the standard sample was impregnated into an adsorption tube (manufactured by Tenax®/Carboxen®), and the adsorption tube impregnated with the standard sample was used instead of the sample tube. The temperature at which the sample was released after adsorption was changed from the sample tube temperature of 170°C to the adsorption tube temperature of 260°C, but the measurement was performed in the same manner as when measuring the sample tube.
(Heat desorption section)
Equipment: TurboMatrix-ATD (manufactured by PerkinElmer Japan)
Temperature when adsorbing the sample onto the adsorption tube: 170°C (sample tube), -30°C (adsorption tube), 250°C (valve), 260°C (transfer line)
Adsorption time to the adsorption tube: 10 minutes. Temperature upon release after sample adsorption: 170°C (sample tube), 260°C (adsorption tube), 250°C (valve), 260°C (transfer line).
Adsorption tube release time: 35 minutes; Carrier gas: Helium; Flow rate of carrier gas into column: 1.0 ml/min
Pressure: 120 kPa
(Gas Chromatography Mass Spectrometry Department)
Equipment: 7890B GC System, 7977B MSD (manufactured by Agilent Technologies)
Column: DB-WAX UI (Length: 30m, Inner diameter: 0.25mm, Film thickness: 0.50μm)
Column oven temperature: Hold at 40°C for 5 minutes, then raise to 240°C at a heating rate of 10°C/min, and hold for 10 minutes (total measurement time: 35 minutes).
Transfer line (connection point) temperature: 240°C
Ionization conditions: EI+
Detected ion mass range: m/z = 29–600
Detection method: SCAN
(Standard sample)
Crotonaldehyde: Manufactured by Aldrich 2,4-Hexadienal: Manufactured by Aldrich 2,4,6-Octatrienal: Manufactured by NARD Institute

(6)ソルビン酸及びミルセンの定量
参考例、参考比較例、実施例及び比較例で得られた乾燥樹脂組成物ペレットを凍結粉砕し、粉砕物22gをソックスレー抽出器に充填し、クロロホルム100mLを用いて16時間抽出処理した。得られたクロロホルム抽出液中のソルビン酸及びミルセンの量を高速液体クロマトグラフィーにて定量分析して、樹脂組成物中のソルビン酸及びミルセンの含有量を定量した。なお、定量に際しては、ソルビン酸及びミルセンの標品を用いて作成した検量線を使用した。
(6) Determination of sorbic acid and myrcene The dried resin composition pellets obtained in the Reference Example, Reference Comparative Example, Example, and Comparative Example were freeze-dried and pulverized. 22 g of the pulverized material was loaded into a Soxhlet extractor and extracted with 100 mL of chloroform for 16 hours. The amounts of sorbic acid and myrcene in the obtained chloroform extract were quantitatively analyzed by high-performance liquid chromatography to determine the content of sorbic acid and myrcene in the resin composition. Calibration curves prepared using sorbic acid and myrcene standards were used for the quantification.

(7)ダイビルドアップ評価
参考例、参考比較例、実施例及び比較例で得られた乾燥樹脂組成物ペレットを下記条件で、押出機から吐出させ、60分後のダイス周辺(ダイリップ)のダイビルドアップ(目ヤニ)を目視で確認し、以下の基準で評価した。A~Dの場合、ダイビルドアップが抑制できていると判断した。
(押出機条件)
・装置:20mmφ単軸押出機(D2020、東洋精機製作所社製)
・L/D:20
・スクリュー:フルフライト
・スクリーンメッシュ:50メッシュ/100メッシュ/50メッシュ
・ダイス:φ1mm、1穴
・設定温度:C1/C2/C3/D=180℃/220℃/220℃/220℃
・吐出量:1.44kg/h
・回転数:100rpm
(評価:判断基準)
A(良好):目ヤニは付着していない。
B(やや良好):目ヤニがごくわずかに付着している。
C(可):少量の目ヤニが付着している。
D(やや不良):明確な目ヤニが付着している。
E(不良):大粒の目ヤニがダイホール全周にわたって付着している。
(7) Die build-up evaluation The dried resin composition pellets obtained in the reference example, reference comparative example, example, and comparative example were extruded from an extruder under the following conditions, and the die build-up (die lip) around the die was visually checked after 60 minutes and evaluated according to the following criteria. If the result was A to D, it was determined that the die build-up was suppressed.
(Extruder conditions)
• Equipment: 20mmφ single-screw extruder (D2020, manufactured by Toyo Seiki Seisakusho Co., Ltd.)
L/D: 20
• Screw: Full flight • Screen mesh: 50 mesh/100 mesh/50 mesh • Die: φ1 mm, 1 hole • Set temperature: C1/C2/C3/D = 180℃/220℃/220℃/220℃
・Discharge amount: 1.44kg/h
• Rotational speed: 100 rpm
(Evaluation: Judgment Criteria)
A (Good): No eye discharge is present.
B (Fairly good): There is a very small amount of eye discharge.
C (Acceptable): A small amount of eye discharge is present.
D (Slightly Poor): Clear eye discharge is present.
E (Defective): Large particles of eye discharge are attached all around the die hole.

(8)色相評価
参考例、参考比較例、実施例及び比較例で得られた乾燥樹脂組成物ペレットのイエローインデックス(YI)値をHunter社製LAB Scan XEを用いて、JIS K7373:2006に従って測定、算出した。数値が小さいほど黄変が抑制されており、色相に優れていると判断した。
(8) Hue Evaluation The yellow index (YI) values of the dried resin composition pellets obtained in the Reference Example, Reference Comparative Example, Example, and Comparative Example were measured and calculated using a Hunter LAB Scan XE in accordance with JIS K7373:2006. A smaller value indicates that yellowing is suppressed and the hue is considered to be superior.

(9)製膜時のネックイン耐性評価
参考例、参考比較例、実施例及び比較例で得られた乾燥樹脂組成物ペレットを用いて、下記の条件にて一軸押出機より樹脂組成物を押出し、乾燥樹脂組成物ペレットを投入して10分後のTダイから吐き出される溶融樹脂(メルトカーテン)の、リップ(Tダイの吐出口)から100mmの位置での幅を測定した。溶融樹脂の幅を、下記基準で評価した。A~Cの場合、ネックインを抑制できていると判断した。
(押出機条件)
・押出機:L/D=26、40mmφの一軸押出機
・スクリュー:フルフライト
・スクリュー回転数:50rpm
・スクリーンメッシュ:50メッシュ/100メッシュ/50メッシュ
・ダイス形状:T型、リップ幅550mm、リップ間隔0.7mm
・設定温度:C1/C2/C3/D=170℃/240℃/260℃/260℃
(評価:判断基準)
A(良好):リップ幅の85%以上
B(やや良好):リップ幅の82.5%以上85%未満
C(やや不良):リップ幅の80%以上82.5%未満
D(不良):リップ幅の80%未満
(9) Evaluation of neck-in resistance during film formation Using the dry resin composition pellets obtained in the Reference Example, Reference Comparative Example, Example, and Comparative Example, the resin composition was extruded from a single-screw extruder under the following conditions, and the width of the molten resin (melt curtain) discharged from the T-die 10 minutes after feeding the dry resin composition pellets was measured at a position 100 mm from the lip (discharge port of the T-die). The width of the molten resin was evaluated according to the following criteria. In cases A to C, it was determined that neck-in was suppressed.
(Extruder conditions)
• Extruder: L/D = 26, 40 mmφ single-screw extruder • Screw: Full flight • Screw rotation speed: 50 rpm
• Screen mesh: 50 mesh / 100 mesh / 50 mesh • Die shape: T-shaped, lip width 550 mm, lip spacing 0.7 mm
・Set temperature: C1/C2/C3/D=170℃/240℃/260℃/260℃
(Evaluation: Judgment Criteria)
A (Good): More than 85% of the lip width
B (Fairly Good): 82.5% to less than 85% of lip width
C (Slightly Poor): 80% to less than 82.5% of lip width D (Poor): Less than 80% of lip width

(10)融点測定
合成例で得られたEVOHの粗乾燥物について、真空乾燥機にて120℃で12時間乾燥した。真空乾燥したEVOHについてTA Instruments製の示差走査型熱量計「Q2000」を用い、30℃から250℃までを10℃/分の速度で昇温し、50℃/分で冷却したのち、二次昇温で測定されるピーク温度より融点を求めた。
(10) Melting point measurement The crudely dried EVOH obtained in the synthesis example was dried in a vacuum dryer at 120°C for 12 hours. The vacuum-dried EVOH was heated from 30°C to 250°C at a rate of 10°C/min using a differential scanning calorimeter "Q2000" manufactured by TA Instruments, and after cooling at 50°C/min, the melting point was determined from the peak temperature measured by secondary heating.

(11)耐酸化劣化性
[単層フィルムの作製]
実施例及び比較例で得られた各樹脂組成物ペレットを下記条件で製膜し、厚さ20μmの単層フィルムを得た。
・装置:20mmφ単軸押出機(D2020、東洋精機製作所社製)
・L/D:20
・スクリュー:フルフライト
・ダイス幅:30cm
・引取りロール温度:80℃
・スクリュー回転数:40rpm
・引取りロール速度:3.0~3.5m/分
・設定温度:C1/C2/C3/D=180℃/210℃/210℃/210℃
(11) Oxidation degradation resistance [Preparation of single-layer film]
Each resin composition pellet obtained in the examples and comparative examples was fabricated under the following conditions to obtain a single-layer film with a thickness of 20 μm.
• Equipment: 20mmφ single-screw extruder (D2020, manufactured by Toyo Seiki Seisakusho Co., Ltd.)
L/D: 20
• Screw: Full flight • Die width: 30 cm
• Take-up roll temperature: 80°C
Screw rotation speed: 40 rpm
• Take-up roll speed: 3.0-3.5 m/min • Set temperature: C1/C2/C3/D = 180°C/210°C/210°C/210°C

上記で得られた各単層フィルムについて、以下の評価条件にて加熱処理時間を変えた複数のサンプルを測定することで、引張強伸度の経時変化を評価した。破断伸度が加熱処理を行っていないサンプルの1/4になる時間を求め、耐酸化劣化性の指標とした。
(評価条件)
所定の時間、140℃に設定した熱風乾燥機内で処理した後、取り出した。その後、20℃の水中に5日間浸漬し、表面水を拭き取って、20℃-65%RHの室内に2週間静置してから、以下の条件で引張強伸度測定を行った。
(測定条件)
サンプル幅15mm
チャック間隔30mm
引張スピード50mm/分
測定雰囲気20℃-65%RH
For each single-layer film obtained above, the change in tensile strength over time was evaluated by measuring multiple samples with varying heat treatment times under the following evaluation conditions. The time at which the elongation at break became 1/4 of that of the untreated sample was determined and used as an indicator of oxidation degradation resistance.
(Evaluation criteria)
After being treated in a hot air dryer set to 140°C for a specified time, the samples were removed. Subsequently, they were immersed in 20°C water for 5 days, the surface water was wiped off, and they were left to stand in a room at 20°C and 65% RH for 2 weeks before tensile strength and elongation measurements were performed under the following conditions.
(Measurement conditions)
Sample width: 15 mm
Chuck spacing: 30 mm
Tensile speed 50 mm/min, measurement atmosphere 20°C - 65% RH

上記評価において、破断伸度が1/4以下になると酸化劣化によるクラックの発生に起因するEVOH層のガスバリア性の悪化が顕著になることから、破断伸度が1/4になる時間を、EVOHの高温での酸化劣化による寿命の指標の一つとして考えることができる。破断伸度が1/4になる時間はアレニウス型の温度依存性を示し、80℃において破断伸度が1/4になる時間(寿命)を100年以上にしようとすると、140℃において破断伸度が1/4になる時間を210時間以上にする必要がある。 In the above evaluation, when the elongation at break falls below 1/4, the deterioration of the gas barrier properties of the EVOH layer due to crack formation caused by oxidative degradation becomes significant. Therefore, the time it takes for the elongation at break to fall to 1/4 can be considered one of the indicators of the lifespan of EVOH due to oxidative degradation at high temperatures. The time it takes for the elongation at break to fall to 1/4 shows an Arrhenius-type temperature dependence. To achieve a lifespan of 100 years or more at 80°C, the time it takes for the elongation at break to fall to 1/4 at 140°C must be 210 hours or more.

(12)パイプのガスバリア性評価
(多層パイプの作製)
高密度ポリエチレン(三菱油化株式会社製「ユカロンハードBX-50」、密度0.952g/cc、MFR0.5g/10分)100質量部、アセトンに溶解したビニルトリメトキシシラン2質量部及びジクミルパーオキサイド0.2質量部を混合した。その混合物を、一軸スクリューを用いて230℃でストランド状に押し出し、ビニルシランが1.5質量%付加された変性ポリエチレンのペレットを得た。次に、このペレット100質量部に対して、ジブチルスズラウレートを2質量%の割合で配合した上記高密度ポリエチレン5質量部を配合したものを1台目の押出機に、実施例又は比較例で得られた各樹脂組成物ペレットを2台目の押出機に、更に接着性樹脂として三井化学株式会社製「アドマーNF408E」を3台目の押出機に入れ、3種3層の円形ダイを用いて、外径20mmの多層パイプを押出成形し、直後に40℃に調整した冷却水槽を通して冷却して固化させた。多層パイプの層構成は樹脂組成物層が最外層であり、樹脂組成物層/接着性樹脂層/高密度ポリエチレン層=100μm/100μm/2000μmであった。得られた多層パイプを1mに切断し、140℃の熱風乾燥機に10分間入れて加熱した後、中央付近を外径150mmのステンレスパイプに沿わせて90°折り曲げて5分間固定して折り曲げ加工を行った。
(12) Evaluation of the gas barrier properties of pipes (fabrication of multilayer pipes)
100 parts by mass of high-density polyethylene (Yukalon Hard BX-50, manufactured by Mitsubishi Petrochemical Co., Ltd., density 0.952 g/cc, MFR 0.5 g/10 min), 2 parts by mass of vinyltrimethoxysilane dissolved in acetone, and 0.2 parts by mass of dicumyl peroxide were mixed. The mixture was extruded into strands at 230°C using a single-screw extruder to obtain modified polyethylene pellets with 1.5% by mass of vinylsilane added. Next, 5 parts by mass of the high-density polyethylene, which was compounded with 2% by mass of dibutylsulcanized laurate, was placed in the first extruder, the resin composition pellets obtained in the examples or comparative examples were placed in the second extruder, and Mitsui Chemicals, Inc.'s Admer NF408E was placed in the third extruder as an adhesive resin. Using three types of three-layer circular dies, a multi-layer pipe with an outer diameter of 20 mm was extruded and immediately cooled and solidified by passing it through a cooling water bath adjusted to 40°C. The layer structure of the multilayer pipe consisted of a resin composition layer as the outermost layer, with a density of 100 μm/100 μm/2000 μm for the resin composition layer/adhesive resin layer/high-density polyethylene layer. The obtained multilayer pipe was cut to 1 m length, heated in a 140°C hot air dryer for 10 minutes, then bent at a 90° angle near the center along a 150 mm outer diameter stainless steel pipe and held in place for 5 minutes to complete the bending process.

(OTR(酸素透過度)測定)
作製した多層パイプの一端をシリコンゴム栓および接着剤を用いて密閉し、もう一端を酸素透過量測定装置(モダンコントロール社製OX-TRAN-10/50A)に接続することにより、20℃/65%RHの条件下で加熱処理前の酸素透過度を測定した。
(OTR (Oxygen Transmissibility) Measurement)
One end of the fabricated multilayer pipe was sealed using a silicone rubber stopper and adhesive, and the other end was connected to an oxygen permeability measuring device (OX-TRAN-10/50A, manufactured by Modern Control Co., Ltd.). The oxygen permeability before heat treatment was measured under conditions of 20°C/65% RH.

次いで、多層パイプを100℃の熱風乾燥機に入れ、216時間加熱処理を行った。加熱処理後の多層パイプを用いて上記方法で加熱処理後の酸素透過度を測定した。 Next, the multilayer pipes were placed in a 100°C hot air dryer and heat-treated for 216 hours. The oxygen permeability after heat treatment was measured using the multilayer pipes following the heat treatment using the method described above.

(13)パイプダイビルドアップ評価
上記(12)パイプのガスバリア性評価における多層パイプ作製時の60分後のダイス周辺(ダイリップ)のダイビルドアップ(目ヤニ)を目視で確認し、以下の基準で評価した。A~Dの場合、ダイビルドアップが抑制できていると判断した。
(評価:判断基準)
A(良好):目ヤニは付着していない。
B(やや良好):目ヤニがごくわずかに付着している。
C(可):少量の目ヤニが付着している。
D(やや不良):明確な目ヤニが付着している。
E(不良):大粒の目ヤニがダイホール全周にわたって付着している。
(13) Evaluation of pipe die buildup The die buildup (die residue) around the die (die lip) after 60 minutes of manufacturing the multilayer pipe as described in (12) above for evaluation of the gas barrier properties of the pipe was visually checked and evaluated according to the following criteria. If the result was A to D, it was determined that the die buildup was suppressed.
(Evaluation: Judgment Criteria)
A (Good): No eye discharge is present.
B (Fairly good): There is a very small amount of eye discharge.
C (Acceptable): A small amount of eye discharge is present.
D (Slightly Poor): Clear eye discharge is present.
E (Defective): Large particles of eye discharge are attached all around the die hole.

<合成例1>
ジャケット、撹拌機、窒素導入口、エチレン導入口及び開始剤添加口を備えた200L加圧反応槽に、酢酸ビニル(以下、VAcと称することがある)を75.0kg、メタノール(以下、MeOHと称することがある。)を7.2kg仕込み、30分間窒素バブリングして反応槽内を窒素置換した。次いで、反応槽内の温度を65℃に調整した後、反応槽圧力(エチレン圧力)が4.13MPaとなるようにエチレンを導入し、重合開始剤として9.4gの2,2’-アゾビス(2,4-ジメチルバレロニトリル)(富士フィルム和光純薬工業株式会社製「V-65」)を添加し、重合を開始した。重合中はエチレン圧力を4.13MPaに、重合温度を65℃に維持した。4時間後にVAcの転化率(VAc基準の重合率)が49.7%となったところで冷却するとともに、酢酸銅0.2gを20kgのメタノールに溶解させた溶液を容器内に投入して重合を停止した。反応槽を開放して脱エチレンした後、窒素ガスをバブリングして脱エチレンを完全に行った。次いで重合液を容器から抜き取り、20LのMeOHで希釈した。この液を塔型容器の塔頂よりフィードし、塔底よりMeOHの蒸気をフィードして、重合液内に残る未反応モノマーをMeOH蒸気と共に除去して、エチレン-酢酸ビニル共重合体(以下、EVAcと称することがある。)のMeOH溶液を得た。
<Synthesis Example 1>
In a 200 L pressurized reactor equipped with a jacket, stirrer, nitrogen inlet, ethylene inlet, and initiator addition port, 75.0 kg of vinyl acetate (hereinafter sometimes referred to as VAc) and 7.2 kg of methanol (hereinafter sometimes referred to as MeOH) were charged, and the reactor was purged with nitrogen by bubbling with nitrogen for 30 minutes. Next, after adjusting the temperature inside the reactor to 65°C, ethylene was introduced so that the reactor pressure (ethylene pressure) reached 4.13 MPa, and 9.4 g of 2,2'-azobis (2,4-dimethylvaleronitrile) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., "V-65") was added as a polymerization initiator to start polymerization. During polymerization, the ethylene pressure was maintained at 4.13 MPa and the polymerization temperature at 65°C. After 4 hours, when the conversion rate of VAc (polymerization rate based on VAc) reached 49.7%, the mixture was cooled, and a solution of 0.2 g of copper acetate dissolved in 20 kg of methanol was added to the container to stop the polymerization. The reaction vessel was opened to remove ethylene, and then nitrogen gas was bubbled through to completely remove the ethylene. Next, the polymerization solution was withdrawn from the container and diluted with 20 L of MeOH. This solution was fed from the top of a tower-type container, and MeOH vapor was fed from the bottom of the tower to remove any unreacted monomers remaining in the polymerization solution along with the MeOH vapor, thereby obtaining an MeOH solution of ethylene-vinyl acetate copolymer (hereinafter sometimes referred to as EVAc).

次いで、ジャケット、撹拌機、窒素導入口、還流冷却器及び溶液添加口を備えた300L反応槽にEVAcの20質量%MeOH溶液150kgを仕込んだ。この溶液に窒素ガスを吹き込みながら60℃に昇温し、水酸化ナトリウムの濃度が2規定のMeOH溶液を450mL/分の速度で2時間添加した。水酸化ナトリウムMeOH溶液の添加を終えた後、系内の温度を60℃に保ち、反応槽外にMeOH及びケン化反応で生成した酢酸メチルを流出させながら、2時間撹拌してケン化反応を進行させた。その後酢酸を8.7kg添加してケン化反応を停止した。 Next, 150 kg of EVAc's 20% MeOH solution was charged into a 300 L reaction vessel equipped with a jacket, stirrer, nitrogen inlet, reflux condenser, and solution addition port. While blowing nitrogen gas into this solution, the temperature was raised to 60°C, and a 2 N sodium hydroxide MeOH solution was added at a rate of 450 mL/min for 2 hours. After the addition of the sodium hydroxide MeOH solution was complete, the system temperature was maintained at 60°C, and the saponification reaction was allowed to proceed by stirring for 2 hours while allowing the MeOH and methyl acetate produced by the saponification reaction to drain out of the reaction vessel. Then, 8.7 kg of acetic acid was added to stop the saponification reaction.

その後、80℃で加熱攪拌しながら、イオン交換水120Lを添加し、反応槽外にMeOHを流出させ、EVOHを析出させた。デカンテーションで析出したEVOHを収集し、粉砕機で粉砕した。得られたEVOH粉末を1g/Lの酢酸水溶液(浴比20:粉末1kgに対して水溶液20Lの割合)に投入して2時間攪拌洗浄した。これを脱液し、さらに1g/Lの酢酸水溶液(浴比20)に投入して2時間攪拌洗浄した。これを脱液したものを、イオン交換水(浴比20)に投入して攪拌洗浄を2時間行い脱液する操作を3回繰り返して精製を行った。洗浄液の電気伝導度は、3μS/cm(東亜電波工業株式会社の「CM-30ET」で測定)であった。次いで、得られた精製物を酢酸0.5g/L及び酢酸ナトリウム0.1g/Lを含有する水溶液250Lに4時間攪拌浸漬してから脱液し、これを60℃で16時間乾燥させることでEVOHの粗乾燥物を16.1kg得た。 Subsequently, while heating and stirring at 80°C, 120 L of deionized water was added to drain MeOH from the reaction vessel and precipitate EVOH. The EVOH precipitated by decantation was collected and pulverized using a pulverizer. The obtained EVOH powder was placed in a 1 g/L aqueous acetic acid solution (bath ratio 20: 20 L of aqueous solution per 1 kg of powder) and stirred and washed for 2 hours. This was then dehydrated and placed in another 1 g/L aqueous acetic acid solution (bath ratio 20) and stirred and washed for 2 hours. The dehydrated mixture was then placed in deionized water (bath ratio 20), stirred and washed for 2 hours, and dehydrated. This process was repeated three times to purify the EVOH. The electrical conductivity of the washing solution was 3 μS/cm (measured with a "CM-30ET" from Toa Denpa Kogyo Co., Ltd.). Next, the purified product was immersed in 250 L of an aqueous solution containing 0.5 g/L of acetic acid and 0.1 g/L of sodium acetate for 4 hours with stirring, then drained, and dried at 60°C for 16 hours to obtain 16.1 kg of crude dried EVOH.

上記のEVOHの合成に係る操作を再度行い、EVOHの粗乾燥物を15.9kg得ることで、合計32.0kgのEVOH(A1)の粗乾燥物を得た。EVOH(A1)の粗乾燥物について、上記評価方法(1)及び(10)に記載の方法にしたがって、エチレン単位含有量、ケン化度及び融点を測定した。結果を表2に示す。 The above procedure for synthesizing EVOH was repeated, yielding 15.9 kg of crude dried EVOH, for a total of 32.0 kg of crude dried EVOH(A1). The ethylene unit content, degree of saponification, and melting point of the crude dried EVOH(A1) were measured according to the methods described in evaluation methods (1) and (10) above. The results are shown in Table 2.

<合成例2~8>
加圧反応槽のサイズ、VAc及びMeOHの仕込量、エチレン圧力、重合開始剤の添加量、反応槽内温度(重合時の温度)、反応時間、VAcの転化率、ケン化工程におけるEVAcのMeOH溶液の仕込量、並びに水酸化ナトリウムMeOH溶液の添加速度を表1に示す通りとし、合成を1回のみとした以外は合成例1と同様にして各EVOH(A2)~EVOH(A8)の粗乾燥物を得た。EVOH(A2)~EVOH(A8)の粗乾燥物について、上記評価方法(1)及び(10)に記載の方法にしたがって、エチレン単位含有量、ケン化度及び融点を測定した。結果を表2に示す。
<Synthesis Examples 2-8>
The size of the pressurized reaction vessel, the amounts of VAc and MeOH charged, the ethylene pressure, the amount of polymerization initiator added, the temperature inside the reaction vessel (temperature during polymerization), the reaction time, the conversion rate of VAc, the amount of EVAc MeOH solution charged in the saponification step, and the rate of addition of sodium hydroxide MeOH solution are as shown in Table 1. The crude dried products of each EVOH(A2) to EVOH(A8) were obtained in the same manner as in Synthesis Example 1, except that the synthesis was performed only once. The ethylene unit content, degree of saponification, and melting point of the crude dried products of EVOH(A2) to EVOH(A8) were measured according to the methods described in Evaluation Methods (1) and (10) above. The results are shown in Table 2.

<参考例1>
ジャケット、撹拌機及び還流冷却器を備えた60L撹拌槽に、合成例1で得たEVOH(A1)の粗乾燥物2kg、水0.8kg及びMeOH2.2kgを仕込み、60℃で5時間攪拌し完全に溶解させた。得られた溶液に、ソルビン酸、クロトンアルデヒド、2,4-ヘキサジエナール及び2,4,6-オクタトリエナールを添加した。この溶液を径4mmの金板を通して-5℃に冷却した水/MeOH=90/10の混合液中に押し出してストランド状に析出させ、このストランドをストランドカッターでペレット状にカットすることでEVOHの含水ペレットを得た。得られたEVOHの含水ペレットの含水率をメトラー社製ハロゲン水分計「HR73」で測定したところ、52質量%であった。
<Reference example 1>
In a 60 L stirring tank equipped with a jacket, stirrer, and reflux condenser, 2 kg of the crudely dried EVOH (A1) obtained in Synthesis Example 1, 0.8 kg of water, and 2.2 kg of MeOH were charged and stirred at 60°C for 5 hours until completely dissolved. Sorbic acid, crotonaldehyde, 2,4-hexadienal, and 2,4,6-octatrienal were added to the resulting solution. This solution was extruded through a 4 mm diameter gold plate into a water/MeOH = 90/10 mixture cooled to -5°C to precipitate in strand form, and these strands were cut into pellets with a strand cutter to obtain hydrated EVOH pellets. The moisture content of the obtained hydrated EVOH pellets was measured using a Mettler halogen moisture meter "HR73" and was found to be 52% by mass.

得られたEVOHの含水ペレットを1g/Lの酢酸水溶液(浴比20)に投入して2時間撹拌洗浄した。これを脱液し、さらに1g/Lの酢酸水溶液(浴比20)に投入して2時間撹拌洗浄した。脱液後、酢酸水溶液を更新し同様の操作を行った。酢酸水溶液で洗浄してから脱液したものを、イオン交換水(浴比20)に投入して撹拌洗浄を2時間行い脱液する操作を3回繰り返して、洗浄液の電気伝導度が、3μS/cm以下(東亜電波工業株式会社の「CM-30ET」で測定)となるまで精製を行い、ケン化反応時の触媒残渣が除去されたEVOHの含水ペレットを得た。 The obtained EVOH-containing pellets were placed in a 1 g/L acetic acid aqueous solution (bath ratio 20) and stirred and washed for 2 hours. This was then dehydrated and placed again in a 1 g/L acetic acid aqueous solution (bath ratio 20) and stirred and washed for another 2 hours. After dehydration, the acetic acid aqueous solution was refreshed and the same procedure was repeated. The pellets washed in acetic acid aqueous solution and then dehydrated were placed in ion-exchanged water (bath ratio 20) and stirred and washed for 2 hours, followed by dehydration. This process was repeated three times until the electrical conductivity of the washing solution was 3 μS/cm or less (measured using Toa Denpa Kogyo Co., Ltd.'s "CM-30ET"), thereby obtaining EVOH-containing pellets from which the catalyst residue from the saponification reaction had been removed.

得られた含水ペレットを酢酸ナトリウム濃度0.510g/L、酢酸濃度0.8g/L、及びリン酸濃度0.04g/Lである水溶液(浴比20)に投入し、定期的に撹拌しながら4時間浸漬させ化学処理を行った。このペレットを脱液し、酸素濃度1体積%以下の窒素気流下80℃で3時間、及び105℃で16時間乾燥させることで、EVOH(A1)、酢酸、リン酸、ナトリウムイオン(ナトリウム塩)、クロトンアルデヒド、2,4-ヘキサジエナール、2,4,6-オクタトリエナール及びソルビン酸を含有した、円柱状(平均直径2.8mm、平均高さ3.2mm)の乾燥樹脂組成物ペレットを得た。得られた乾燥樹脂組成物ペレットについて、上記評価方法(2)~(9)に記載の方法に従って評価した。乾燥樹脂組成物ペレット中のナトリウムイオン含有量は100ppm、リン酸含有量はリン酸根換算値で40ppm、酢酸含有量は200ppmであった。EVOH以外の各成分の含有量は、いずれもEVOHの含有量を基準とした量である。その他の評価結果は表3に示す。なお、クロトンアルデヒド、2,4-ヘキサジエナール、2,4,6-オクタトリエナール及びソルビン酸の各成分の含有量が表3に記載の通りとなるように、各成分の添加量を調整した。 The obtained water-containing pellets were placed in an aqueous solution (bath ratio 20) with a sodium acetate concentration of 0.510 g/L, an acetic acid concentration of 0.8 g/L, and a phosphoric acid concentration of 0.04 g/L, and immersed for 4 hours with periodic stirring to perform chemical treatment. These pellets were dehydrated and dried at 80°C for 3 hours and at 105°C for 16 hours under a nitrogen stream with an oxygen concentration of 1 vol% or less to obtain cylindrical (average diameter 2.8 mm, average height 3.2 mm) dried resin composition pellets containing EVOH (A1), acetic acid, phosphoric acid, sodium ions (sodium salt), crotonaldehyde, 2,4-hexadienal, 2,4,6-octatrienal, and sorbic acid. The obtained dried resin composition pellets were evaluated according to the methods described in evaluation methods (2) to (9) above. The sodium ion content in the dried resin composition pellets was 100 ppm, the phosphoric acid content was 40 ppm (calculated as phosphate root), and the acetic acid content was 200 ppm. The content of each component other than EVOH is based on the EVOH content. Other evaluation results are shown in Table 3. The amounts of each component added were adjusted so that the content of crotonaldehyde, 2,4-hexadienal, 2,4,6-octatrienal, and sorbic acid were as shown in Table 3.

[参考例2~61、参考比較例1~4、6~24]
EVOH(A)の種類、不飽和脂肪族アルデヒド(B)の種類及び含有量、共役ポリエン化合物(C)の種類及び含有量、並びにホウ酸の含有量を表3~表10に示した通りとなるように調整した以外は、参考例1と同様にして乾燥樹脂組成物ペレットを作製し、評価した。なお、ホウ酸を800ppm含む場合は、酢酸ナトリウム等を含む水溶液(浴比20)をホウ酸濃度0.25g/Lとなるように調整した水溶液を用い、ホウ酸を1800ppm含む場合は、酢酸ナトリウム等を含む水溶液(浴比20)をホウ酸濃度0.57g/Lとなるように調整した水溶液を用いた。それぞれの乾燥樹脂組成物ペレット中のEVOHのナトリウムイオン含有量は100ppm、リン酸含有量はリン酸根換算値で40ppm、酢酸含有量は200ppmであった。その他の評価結果は表3~表10に示す。EVOH以外の各成分の含有量は、いずれもEVOHの含有量を基準とした量である。
[Reference Examples 2 to 61, Reference Comparative Examples 1 to 4, 6 to 24]
Dry resin composition pellets were prepared and evaluated in the same manner as in Reference Example 1, except that the type of EVOH (A), the type and content of unsaturated aliphatic aldehyde (B), the type and content of conjugated polyene compound (C), and the content of boric acid were adjusted to match those shown in Tables 3 to 10. For the 800 ppm boric acid content, an aqueous solution containing sodium acetate, etc. (bath ratio 20) was used, adjusted to a boric acid concentration of 0.25 g/L. For the 1800 ppm boric acid content, an aqueous solution containing sodium acetate, etc. (bath ratio 20) was used, adjusted to a boric acid concentration of 0.57 g/L. The sodium ion content of EVOH in each dry resin composition pellet was 100 ppm, the phosphoric acid content was 40 ppm (based on phosphate root), and the acetic acid content was 200 ppm. Other evaluation results are shown in Tables 3 to 10. The content of each component other than EVOH is based on the EVOH content.

<参考比較例5>
クロトンアルデヒド、2,4-ヘキサジエナール及び2,4,6-オクタトリエナールを添加せず、ケン化反応時の触媒残渣が除去されたEVOHの含水ペレットをメタノール中(浴比10)に投入して撹拌洗浄を2時間行い脱液する操作を2回繰り返し、得られたペレットをイオン交換水(浴比20)に投入して撹拌洗浄を2時間行い脱液する操作を3回繰り返す操作を追加で行った以外は、参考例1と同様にして乾燥樹脂組成物ペレットを作製し、評価した。乾燥樹脂組成物ペレット中のナトリウムイオン含有量は100ppm、リン酸含有量はリン酸根換算値で40ppm、酢酸含有量は200ppmであった。EVOH以外の各成分の含有量は、いずれもEVOHの含有量を基準とした量である。その他の評価結果は表3に示す。なお、クロトンアルデヒド、2,4-ヘキサジエナール、2,4,6-オクタトリエナール及びソルビン酸の各成分の含有量は検出限界以下であった。
<Reference Comparison Example 5>
Dry resin composition pellets were prepared and evaluated in the same manner as in Reference Example 1, except that crotonaldehyde, 2,4-hexadienal, and 2,4,6-octatrienal were not added, and the hydrated EVOH pellets, from which the catalyst residue from the saponification reaction had been removed, were placed in methanol (bath ratio 10), stirred and washed for 2 hours, and dehydrated. This process was repeated twice, and the resulting pellets were placed in ion-exchanged water (bath ratio 20), stirred and washed for 2 hours, and dehydrated. This process was repeated three times. The sodium ion content in the dry resin composition pellets was 100 ppm, the phosphoric acid content was 40 ppm (based on phosphate root), and the acetic acid content was 200 ppm. The content of each component other than EVOH is based on the EVOH content. Other evaluation results are shown in Table 3. Furthermore, the levels of crotonaldehyde, 2,4-hexadienal, 2,4,6-octatrienal, and sorbic acid were below the detection limit.

参考例及び参考比較例から、b1/(b2+b3)が2.0以上150.0未満であるとネックイン耐性が良好であり、b1+b2+b3が小さいほどYIが低く、共役ポリエン化合物(C)の含有量cが少量であるとYIが低く、b2+2b3が0.65ppm以下であるとダイビルドアップが抑制されていることがわかる。 From the reference examples and reference comparative examples, it can be seen that when b1 /( b2 + b3 ) is 2.0 or more and less than 150.0, neck-in resistance is good, the smaller b1 + b2 + b3 is, the lower the YI, the lower the content of the conjugated polyene compound (C) c, and when b2 + 2b3 is 0.65 ppm or less, die build-up is suppressed.

表3に基づいてより詳細に考察すれば、以下の通りである。不飽和脂肪族アルデヒド(B)が含有されない参考比較例5及び不飽和脂肪族アルデヒド(B)の各種を単独で含有している参考比較例1~3、6~9は、ネックインが抑制されていない。また、b1/(b2+b3)の値が2.0未満である参考比較例10でもネックインが抑制されていない。一方で参考例からわかるようにb1/(b2+b3)の値が2.0以上150.0未満の範囲にあるとネックインが抑制され、特に参考例4、5、13、14、21及び24のようにb1/(b2+b3)の値が10付近(例えば、8.0以上13.0以下)であると最もネックインが抑制される。また、b2+2b3が0.65ppmを超える参考比較例4はダイビルドアップが抑制されないのに対し、参考例からわかるようにb2+2b3が0.65ppm以下である場合はダイビルドアップが抑制され、特にb2+2b3が0.10ppm以下である場合に、よりダイビルドアップが抑制されている。また、クロトンアルデヒド(B1)、2,4-ヘキサジエナール(B2)及び2,4,6-オクタトリエナール(B3)の合計含有量b1+b2+b3については、参考比較例4、参考例1~7、12~26等から読み取れるように、合計含有量が低いほど色相に優れることが分かる。さらに、参考例6、9~11より共役ポリエン化合物の含有量が少量である方が色相に優れることがわかる。 A more detailed examination based on Table 3 reveals the following: Reference Comparative Example 5, which does not contain unsaturated aliphatic aldehyde (B), and Reference Comparative Examples 1-3, 6-9, which contain various unsaturated aliphatic aldehydes (B) individually, do not suppress neck-in. Similarly, Reference Comparative Example 10, where the value of b1 /( b2 + b3 ) is less than 2.0, also does not suppress neck-in. On the other hand, as can be seen from the reference examples, neck-in is suppressed when the value of b1 /( b2 + b3 ) is in the range of 2.0 or more and less than 150.0, and in particular, neck-in is most suppressed when the value of b1 /( b2 + b3 ) is around 10 (for example, 8.0 or more and 13.0 or less), as in Reference Examples 4, 5, 13, 14, 21, and 24. Furthermore, in Comparative Example 4, where b² + 2b³ exceeds 0.65 ppm, dye buildup is not suppressed, whereas, as can be seen from the reference examples, when b² + 2b³ is 0.65 ppm or less, dye buildup is suppressed, and in particular, when b² + 2b³ is 0.10 ppm or less, dye buildup is suppressed even more. In addition, regarding the total content of crotonaldehyde (B1), 2,4-hexadienal (B2), and 2,4,6-octatrienal (B3), b² + b³ , as can be seen from Comparative Example 4, Reference Examples 1-7, 12-26, etc., it can be seen that the lower the total content, the better the hue. Furthermore, from Reference Examples 6, 9-11 , it can be seen that a smaller content of conjugated polyene compounds results in better hue.

<酸化防止剤(G)を含む樹脂組成物の調製>
[実施例1]
参考例5で得られた乾燥樹脂組成物ペレット100質量部及び酸化防止剤としてN,N’-(ヘキサン-1,6-ジイル)ビス[3-(3,5-ジ-tert-ブチル-4-ヒドロキシフェニル)プロピオンアミド](BASFジャパン社製「Irganox1098」、分子量:637)0.5質量部をドライブレンドし、30mmφの同方向二軸押出機(株式会社日本製鋼所製「TEX-30N」)を用いて220℃の押出温度、窒素雰囲気下で押出すことで樹脂組成物ペレットを得た。
<Preparation of resin composition containing antioxidant (G)>
[Example 1]
100 parts by mass of the dry resin composition pellets obtained in Reference Example 5 and 0.5 parts by mass of N,N'-(hexane-1,6-diyl)bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide] (BASF Japan's "Irganox 1098", molecular weight: 637) as an antioxidant were dry blended and extruded at an extrusion temperature of 220°C under a nitrogen atmosphere using a 30 mmφ co-screw extruder (Japan Steel Works Ltd. "TEX-30N") to obtain resin composition pellets.

[実施例2、4~7、比較例1~3]
用いた乾燥樹脂組成物ペレット及び酸化防止剤の配合量を表11に示す通りとした以外は実施例1と同様にして、実施例2、4~7及び比較例1~3の各樹脂組成物ペレットを得た。
[Examples 2, 4-7, Comparative Examples 1-3]
Resin composition pellets for Examples 2, 4-7, and Comparative Examples 1-3 were obtained in the same manner as in Example 1, except that the amounts of dried resin composition pellets and antioxidants used were as shown in Table 11.

[実施例3]
参考例48で得られた乾燥樹脂組成物ペレット90質量部、熱可塑性エラストマー(F-1)として「タフマー(登録商標)MH7020」(三井化学株式会社製、無水マレイン酸変性エチレン-ブテン共重合体)10質量部、及び上記酸化防止剤(Irganox1098)0.5質量部をドライブレンドした後、以下の条件で押出すことで樹脂組成物ペレットを得た。
(押出機条件)
・装置:30mmφ二軸押出機
・L/D:45.5
・スクリュー:同方向完全噛合型
・押出し温度(℃):220℃
・回転数:200rpm
・吐出量:20kg/hr
[Example 3]
The resin composition pellets were obtained by dry blending 90 parts by mass of the dried resin composition pellets obtained in Reference Example 48, 10 parts by mass of "Tafmer® MH7020" (manufactured by Mitsui Chemicals, Inc., maleic anhydride-modified ethylene-butene copolymer) as a thermoplastic elastomer (F-1), and 0.5 parts by mass of the above antioxidant (Irganox 1098), and then extruding under the following conditions.
(Extruder conditions)
• Equipment: 30mmφ twin-screw extruder • L/D ratio: 45.5
• Screw: Fully meshing in the same direction • Extrusion temperature (°C): 220°C
• Rotational speed: 200 rpm
・Discharge amount: 20kg/hr

得られた実施例及び比較例の各乾燥樹脂組成物ペレットを用いて上記評価方法(5)~(9)、(11)~(13)に記載の方法に従って評価した。評価結果を表11、12に示す。 The dried resin composition pellets obtained from the examples and comparative examples were evaluated according to the evaluation methods described in (5) to (9) and (11) to (13) above. The evaluation results are shown in Tables 11 and 12.

表11、12に示されるように、実施例1~7の各樹脂組成物は、ネックイン及びダイビルドアップが抑制されており、得られる成形体の耐酸化劣化性等も優れたものであった。実施例の各樹脂組成物からは、長期間高温で使用可能な成形体等が得られることが確認できた。b2+2b3が0.65ppm以下ではない比較例1の樹脂組成物は、ダイビルドアップが抑制できず、b1/(b2+b3)が2.0以上150.0未満ではない比較例2の樹脂組成物は、ネックイン耐性が悪かった。所定量の酸化防止剤を含有しない比較例3の樹脂組成物は、得られる成形体(単層フィルム又はパイプ)における耐酸化劣化性及び加熱処理後のガスバリア性が低かった。
なお、各参考例の結果から、b1/(b2+b3)が2.0以上150.0未満であるとネックイン耐性が良好であり、b2+2b3が0.65ppm以下であるとダイビルドアップが抑制されることがわかる。従って、各参考例の樹脂組成物に対して所定量の酸化防止剤を含有して得られるいずれの樹脂組成物においても、実施例1~7の各樹脂組成物と同様の効果が奏されると推測できる。
As shown in Tables 11 and 12, each resin composition in Examples 1 to 7 suppressed neck-in and die build-up, and the resulting molded articles exhibited excellent resistance to oxidation degradation. It was confirmed that molded articles usable at high temperatures for extended periods could be obtained from each resin composition in the Examples. The resin composition of Comparative Example 1, in which b² + 2b³ was not 0.65 ppm or less, failed to suppress die build-up, and the resin composition of Comparative Example 2, in which b¹ /( b² + b³ ) was not 2.0 or more and less than 150.0, exhibited poor resistance to neck-in. The resin composition of Comparative Example 3, which did not contain a predetermined amount of antioxidant, showed low resistance to oxidation degradation and poor gas barrier properties after heat treatment in the resulting molded articles (single-layer films or pipes).
Furthermore, the results from each reference example show that when b1 /( b2 + b3 ) is 2.0 or more and less than 150.0, neck-in resistance is good, and when b2 + 2b3 is 0.65 ppm or less, die build-up is suppressed. Therefore, it can be inferred that any resin composition obtained by adding a predetermined amount of antioxidant to the resin composition of each reference example will exhibit the same effects as the resin compositions of Examples 1 to 7.

Claims (15)

エチレン単位含有量が20モル%以上60モル%以下であるエチレン-ビニルアルコール共重合体(A)、クロトンアルデヒド(B1)及び酸化防止剤(G)を含み、
2,4-ヘキサジエナール(B2)及び2,4,6-オクタトリエナール(B3)からなる群より選ばれる少なくとも1種をさらに含み、
下記式(1)及び(2)を満たし、
酸化防止剤(G)の含有量gが、0.01質量%以上5質量%以下である、樹脂組成物。
2.0≦b1/(b2+b3)<150.0 ・・・(1)
b2+2b3≦0.65 ・・・(2)
上記式(1)及び(2)中、b1は、エチレン-ビニルアルコール共重合体(A)に対するクロトンアルデヒド(B1)の含有量(ppm)であり、b2は、エチレン-ビニルアルコール共重合体(A)に対する2,4-ヘキサジエナール(B2)の含有量(ppm)であり、b3は、エチレン-ビニルアルコール共重合体(A)に対する2,4,6-オクタトリエナール(B3)の含有量(ppm)である。
It contains an ethylene-vinyl alcohol copolymer (A) having an ethylene unit content of 20 mol% or more and 60 mol% or less, crotonaldehyde (B1), and an antioxidant (G),
It further comprises at least one selected from the group consisting of 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3),
The following equations (1) and (2) are satisfied,
A resin composition having an antioxidant (G) content of 0.01% by mass or more and 5% by mass or less.
2.0≦b 1 /(b 2 +b 3 )<150.0 (1)
b2 + 2b3 ≦0.65...(2)
In formulas (1) and (2) above, b1 is the content (ppm) of crotonaldehyde (B1) in the ethylene-vinyl alcohol copolymer (A), b2 is the content (ppm) of 2,4-hexadienal (B2) in the ethylene-vinyl alcohol copolymer (A), and b3 is the content (ppm) of 2,4,6-octatrienal (B3) in the ethylene-vinyl alcohol copolymer (A).
エチレン-ビニルアルコール共重合体(A)に対するクロトンアルデヒド(B1)、2,4-ヘキサジエナール(B2)及び2,4,6-オクタトリエナール(B3)の含有量の合計(b1+b2+b3)が0.01ppm以上7.0ppm以下である、請求項1に記載の樹脂組成物。 The resin composition according to claim 1, wherein the total content of crotonaldehyde (B1), 2,4-hexadienal (B2), and 2,4,6-octatrienal (B3) relative to the ethylene-vinyl alcohol copolymer (A) ( b1 + b2 + b3 ) is 0.01 ppm or more and 7.0 ppm or less. クロトンアルデヒド(B1)の含有量b1が0.01ppm以上4.0ppm以下である、請求項1又は2に記載の樹脂組成物。 The resin composition according to claim 1 or 2, wherein the content of crotonaldehyde (B1) b1 is 0.01 ppm or more and 4.0 ppm or less. 2,4-ヘキサジエナール(B2)の含有量b2が0.005ppm以上0.65ppm以下である、請求項1又は2に記載の樹脂組成物。 The resin composition according to claim 1 or 2, wherein the content of 2,4-hexadienal (B2) b2 is 0.005 ppm or more and 0.65 ppm or less. 2,4,6-オクタトリエナール(B3)の含有量b3が0.325ppm以下である、請求項1又は2に記載の樹脂組成物。 The resin composition according to claim 1 or 2, wherein the content of 2,4,6-octatrienal (B3) is 0.325 ppm or less. 共役ポリエン化合物(C)をさらに含み、エチレン-ビニルアルコール共重合体(A)に対する共役ポリエン化合物(C)の含有量cが1ppm以上300ppm未満である、請求項1又は2に記載の樹脂組成物。 The resin composition according to claim 1 or 2, further comprising a conjugated polyene compound (C), wherein the content c of the conjugated polyene compound (C) relative to the ethylene-vinyl alcohol copolymer (A) is 1 ppm or more and less than 300 ppm. 共役ポリエン化合物(C)がソルビン酸である、請求項6に記載の樹脂組成物。 The resin composition according to claim 6, wherein the conjugated polyene compound (C) is sorbic acid. 熱可塑性エラストマー(F)をさらに含有し、
熱可塑性エラストマー(F)のエチレン-ビニルアルコール共重合体(A)に対する質量比(F/A)が5/95以上35/65以下である、請求項1又は2に記載の樹脂組成物。
It further contains a thermoplastic elastomer (F),
The resin composition according to claim 1 or 2, wherein the mass ratio (F/A) of the thermoplastic elastomer (F) to the ethylene-vinyl alcohol copolymer (A) is 5/95 or more and 35/65 or less.
熱可塑性エラストマー(F)が、ポリエステル系熱可塑性エラストマー、ポリスチレン系熱可塑性エラストマー及びポリオレフィン系熱可塑性エラストマーからなる群より選ばれる少なくとも1種である、請求項8に記載の樹脂組成物。 The resin composition according to claim 8, wherein the thermoplastic elastomer (F) is at least one selected from the group consisting of polyester-based thermoplastic elastomers, polystyrene-based thermoplastic elastomers, and polyolefin-based thermoplastic elastomers. 請求項1又は2に記載の樹脂組成物からなる部分を有する成形体。 A molded article having a portion made of the resin composition described in claim 1 or 2. 請求項1又は2に記載の樹脂組成物からなる層を少なくとも1層有する積層体。 A laminate having at least one layer made of the resin composition described in claim 1 or 2. 請求項1又は2に記載の樹脂組成物からなる層を有するパイプ。 A pipe having a layer made of the resin composition described in claim 1 or 2. 請求項12に記載のパイプからなる温水循環用パイプ。 A hot water circulation pipe comprising the pipe described in claim 12. 断熱発泡体層をさらに有する請求項12に記載のパイプからなる断熱多層パイプ。 A multilayer insulated pipe comprising the pipe according to claim 12, further comprising an insulating foam layer. 請求項12に記載のパイプからなる燃料用パイプ。 A fuel pipe comprising the pipe described in claim 12.
JP2022164090A 2022-01-17 2022-10-12 Resin compositions, molded articles, laminates, pipes, hot water circulation pipes, insulated multilayer pipes, and fuel pipes Active JP7906552B2 (en)