JP6589009B2 - Transfer material, recorded matter, and method for producing recorded matter - Google Patents

Transfer material, recorded matter, and method for producing recorded matter Download PDF

Info

Publication number
JP6589009B2
JP6589009B2 JP2018088285A JP2018088285A JP6589009B2 JP 6589009 B2 JP6589009 B2 JP 6589009B2 JP 2018088285 A JP2018088285 A JP 2018088285A JP 2018088285 A JP2018088285 A JP 2018088285A JP 6589009 B2 JP6589009 B2 JP 6589009B2
Authority
JP
Japan
Prior art keywords
transparent sheet
receiving layer
sheet
transfer material
image
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2018088285A
Other languages
Japanese (ja)
Other versions
JP2018149814A (en
Inventor
裕輔 澄川
裕輔 澄川
喬紘 筒井
喬紘 筒井
平林 弘光
弘光 平林
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Canon Finetech Nisca Inc
Original Assignee
Canon Finetech Nisca Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Canon Finetech Nisca Inc filed Critical Canon Finetech Nisca Inc
Priority to JP2018088285A priority Critical patent/JP6589009B2/en
Publication of JP2018149814A publication Critical patent/JP2018149814A/en
Application granted granted Critical
Publication of JP6589009B2 publication Critical patent/JP6589009B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は、画像が記録される転写材、転写材に記録された画像が転写される記録物、および記録物の製造方法に関するものである。 The present invention relates to a transfer material on which an image is recorded, a recorded material on which an image recorded on the transfer material is transferred, and a method for manufacturing the recorded material .

特許文献1,2には、インクジェット方式によって記録した画像を記録物(被転写材)に転写する技術が提案されている。例えば、転写材の色材受容層にインクジェット方式によって画像を記録し、この転写材と記録物とを重ね合わせて加熱することにより、画像が記録された色材受容層を記録物に転写する。また、本発明者らも、インクジェット方式によって画像が形成される転写材の色材受容層に対して、その色材受容層の無機微粒子および水溶性樹脂の分子量を制御する技術を提案している(特許文献3)。   Patent Documents 1 and 2 propose a technique for transferring an image recorded by an ink jet method to a recorded material (a material to be transferred). For example, an image is recorded on the color material receiving layer of the transfer material by an inkjet method, and the transfer material and the recorded material are superposed and heated, whereby the color material receiving layer on which the image is recorded is transferred to the recorded material. The present inventors have also proposed a technique for controlling the molecular weight of the inorganic fine particles and the water-soluble resin in the color material receiving layer of the transfer material on which an image is formed by the inkjet method. (Patent Document 3).

特表2006−517871号公報JP 2006-517871 A 特開平8−207450号公報JP-A-8-207450 特開2015−110321号公報JP2015-110321A

インクジェット方式においては、十分な画像濃度を実現するために、多量のインクを転写材の色材受容層に吸収させる必要があり、そのため色材受容層および転写材自体が厚くなる。一方、クレジットカード等の記録物においては強固な耐久性が要求され、例えば、長時間の水による浸積試験によっても変化しない耐久性が求められる。しかしながら、表面が透明シート(保護シート)によって覆われる色材受容層が転写された記録物を長時間水に漬けた場合には、色材受容層の端部が表面に露出しているため、色材受容層は、その端部から水分を大量に吸収する。そのため、その後の乾燥の過程において、透明シートの表面全体にひび割れやクラックが発生するおそれがある。このような現象は、色材受容層にインクを付与して画像を記録するインクジェット方式等において特有のものであり、水を吸収する色材受容層を必要としない熱転写方式においては発生しない。すなわち、熱転写方式においては、サーマルヘッドなどによって転写層を加熱して画像を形成してから、その転写層を被転写材に転写するため、水を吸収する色材受容層を必要としない。   In the ink jet system, in order to realize a sufficient image density, it is necessary to absorb a large amount of ink in the color material receiving layer of the transfer material, so that the color material receiving layer and the transfer material itself become thick. On the other hand, a recorded material such as a credit card is required to have a strong durability, for example, a durability that does not change even by a long-time immersion test with water. However, when the recorded material on which the color material receiving layer whose surface is covered with a transparent sheet (protective sheet) is transferred is immersed in water for a long time, the end of the color material receiving layer is exposed on the surface. The colorant receiving layer absorbs a large amount of moisture from its end. Therefore, in the subsequent drying process, there is a possibility that cracks and cracks may occur on the entire surface of the transparent sheet. Such a phenomenon is peculiar in an ink jet system that records an image by applying ink to the color material receiving layer, and does not occur in a thermal transfer system that does not require a color material receiving layer that absorbs water. That is, in the thermal transfer system, since the transfer layer is heated by a thermal head or the like to form an image, and then the transfer layer is transferred to the transfer material, a color material receiving layer that absorbs water is not required.

特許文献1,2,3には、このような水を吸収する色材受容層の耐水性に関しての記載がない。特許文献3においては、透明シート(保護シート)に耐候性を持たせるために、それを厚くして強度を高めている。そのため、色材受容層の耐水性に影響するひび割れやクラックの発生を抑える効果はあるものの、クレジットカード等の記録物において要求される高い耐水性を実現することは難しい。   Patent Documents 1, 2, and 3 do not describe the water resistance of the colorant receiving layer that absorbs such water. In patent document 3, in order to give a weather resistance to a transparent sheet (protective sheet), it is thickened to increase the strength. Therefore, although there is an effect of suppressing the occurrence of cracks and cracks that affect the water resistance of the colorant-receiving layer, it is difficult to achieve the high water resistance required for recorded matter such as credit cards.

本発明の目的は、記録物の耐水性の向上を達成することが可能な転写材、記録物、および記録物の製造方法を提供することにある。 An object of the present invention is to provide a transfer material, a recorded matter, and a method for producing the recorded matter that can achieve improvement in water resistance of the recorded matter .

本発明の転写材は、基材シート、保護シート、および色材受容層が、この順に積層された転写材であって、前記保護シートは、平均重合度が1,500以上5,000以下のポリビニルアルコールを含有することを特徴とする転写材。 The transfer material of the present invention is a transfer material in which a base sheet, a protective sheet, and a colorant receiving layer are laminated in this order, and the protective sheet has an average polymerization degree of 1,500 to 5,000. A transfer material comprising polyvinyl alcohol .

本発明によれば、保護シートを通して色材受容層内の水分を外部に放出することにより、耐水性の優れた記録物を提供することができる。   According to the present invention, a recorded matter with excellent water resistance can be provided by releasing moisture in the colorant receiving layer to the outside through the protective sheet.

転写材の断面図である。It is sectional drawing of a transfer material. 転写材に記録される画像の説明図である。It is explanatory drawing of the image recorded on a transfer material. 膨潤吸収型の色材受容層とインクとの関係の説明図である。It is explanatory drawing of the relationship between a swelling absorption type color material receiving layer and ink. 転写工程における位置合わせの説明図である。It is explanatory drawing of the position alignment in a transcription | transfer process. 転写材の他の例を説明するための断面図である。It is sectional drawing for demonstrating the other example of a transfer material. 記録物の製造段階の説明図である。It is explanatory drawing of the manufacturing stage of a recorded matter. 基材シートの剥離工程を説明するための断面図である。It is sectional drawing for demonstrating the peeling process of a base material sheet. 両面に転写体が貼付された画像支持体の説明図である。It is explanatory drawing of the image support body by which the transfer body was affixed on both surfaces. 記録物の第1の製造装置の説明図である。It is explanatory drawing of the 1st manufacturing apparatus of recorded matter. 記録物の製造装置における制御系の構成を説明するためのブロック図である。It is a block diagram for demonstrating the structure of the control system in the manufacturing apparatus of recorded matter. 図10における記録部の制御系の構成を説明するためのブロック図である。It is a block diagram for demonstrating the structure of the control system of the recording part in FIG. 製造装置の動作を説明するためのフローチャートである。It is a flowchart for demonstrating operation | movement of a manufacturing apparatus. 記録物の第2の製造装置の説明図である。It is explanatory drawing of the 2nd manufacturing apparatus of recorded matter. 転写材に画像を記録するプリンタの説明図である。It is explanatory drawing of the printer which records an image on a transfer material. 図16のプリンタと転写材との関係の説明図である。It is explanatory drawing of the relationship between the printer of FIG. 16, and a transfer material. 転写材を画像支持体に加熱圧着する転写部の説明図である。It is explanatory drawing of the transfer part which heat-presses a transfer material to an image support body. 記録物の第6の製造装置におけるプリンタ部と、転写材と、関係の説明図である。It is explanatory drawing of the relationship between the printer part in the 6th manufacturing apparatus of recorded matter, and a transfer material. 記録物の第7の製造装置におけるプリンタ部の説明図である。It is explanatory drawing of the printer part in the 7th manufacturing apparatus of recorded matter. 記録物の第7の製造装置における転写部の説明図である。It is explanatory drawing of the transfer part in the 7th manufacturing apparatus of recorded matter. 記録物の第8の製造装置の説明図である。It is explanatory drawing of the 8th manufacturing apparatus of recorded matter. 記録物の第9の製造装置におけるプリンタ部の説明図である。It is explanatory drawing of the printer part in the 9th manufacturing apparatus of recorded matter. 異なる構成例の転写材の断面図である。It is sectional drawing of the transfer material of a different structural example. 記録物の製造方法の説明図である。It is explanatory drawing of the manufacturing method of recorded matter. 記録物の製造方法の他の例の説明図である。It is explanatory drawing of the other example of the manufacturing method of recorded matter. 記録物の製造方法のさらに他の例の説明図である。It is explanatory drawing of the further another example of the manufacturing method of recorded matter. 記録物の製造方法のさらに他の例の説明図である。It is explanatory drawing of the further another example of the manufacturing method of recorded matter. 穿孔加工部を含む記録装置の説明図である。It is explanatory drawing of the recording device containing a punching process part. 記録物の第2の製造装置の説明図である。It is explanatory drawing of the 2nd manufacturing apparatus of recorded matter. 記録物の第3の製造装置の説明図である。It is explanatory drawing of the 3rd manufacturing apparatus of recorded matter. 記録物の第4の製造装置の説明図である。It is explanatory drawing of the 4th manufacturing apparatus of recorded matter. 記録物の第5の製造装置の説明図である。It is explanatory drawing of the 5th manufacturing apparatus of recorded matter. 透明シートの浸漬耐水試験におけるひび割れの発生メカニズムの説明図である。It is explanatory drawing of the generation | occurrence | production mechanism of the crack in the immersion water resistance test of a transparent sheet. 異なる構成例の記録物の断面図である。It is sectional drawing of the recorded matter of a different structural example. 浸漬耐水試験後における記録物の断面図である。It is sectional drawing of the recorded matter after an immersion water resistance test. 透明シートの表面に汚染水が付着した状態を説明するための断面図である。It is sectional drawing for demonstrating the state which contaminated water adhered to the surface of the transparent sheet. 発泡による細孔の形成方法の異なる例の説明図である。It is explanatory drawing of the example from which the formation method of the pore by foaming differs. 多孔質粒子による細孔の形成方法の異なる例の説明図である。It is explanatory drawing of the example from which the formation method of the pore by a porous particle differs. 中空粒子による細孔の形成方法の異なる例の説明図である。It is explanatory drawing of the example from which the formation method of the pore by a hollow particle differs. 透明シートに対する穿孔加工の異なる例の説明図である。It is explanatory drawing of the example from which the punching process with respect to a transparent sheet differs. 透明シートに対する穿孔加工の他の異なる例の説明図である。It is explanatory drawing of the other different example of the punching process with respect to a transparent sheet. 透明シートに対する穿孔加工のさらに他の異なる例の説明図である。It is explanatory drawing of the further another example of the punching process with respect to a transparent sheet. 透明シートに対する穿孔加工のさらに他の異なる例の説明図である。It is explanatory drawing of the further another example of the punching process with respect to a transparent sheet. 延伸加工装置の説明図である。It is explanatory drawing of an extending | stretching processing apparatus. クレイズ加工装置の説明図である。It is explanatory drawing of a craze processing apparatus. クレイズ加工による細孔の形成方法の異なる例の説明図である。It is explanatory drawing of the example from which the formation method of the pore by a crazing process differs. 穿孔処理方法の異なる例の説明図である。It is explanatory drawing of the example from which a punching processing method differs. 記録物の製造方法のさらに他の例の説明図である。It is explanatory drawing of the further another example of the manufacturing method of recorded matter. 記録物の製造方法のさらに他の例の説明図である。It is explanatory drawing of the further another example of the manufacturing method of recorded matter. 記録物の製造方法のさらに他の例の説明図である。It is explanatory drawing of the further another example of the manufacturing method of recorded matter. 記録物の第6の製造装置における細孔の形成方法の異なる例の説明図である。It is explanatory drawing of the example from which the formation method of the pore in the 6th manufacturing apparatus of recorded matter differs. 記録物の第6の製造装置における転写部の異なる例の説明図である。It is explanatory drawing of the example from which the transcription | transfer part differs in the 6th manufacturing apparatus of recorded matter. 記録物の第7の製造装置における細孔の形成方法の異なる例の説明図である。It is explanatory drawing of the example from which the formation method of the pore in the 7th manufacturing apparatus of recorded matter differs. 記録物の第7の製造装置における転写部の異なる例の説明図である。It is explanatory drawing of the example from which the transcription | transfer part differs in the 7th manufacturing apparatus of recorded matter. 記録物の第8の製造装置における細孔の形成方法の異なる例の説明図である。It is explanatory drawing of the example from which the formation method of the pore in the 8th manufacturing apparatus of recorded matter differs. 記録物の第9の製造装置における細孔の形成方法の異なる例の説明図である。It is explanatory drawing of the example from which the formation method of the pore in the 9th manufacturing apparatus of recorded matter differs. 記録物の第6の製造装置における細孔の形成方法の異なる例の説明図である。It is explanatory drawing of the example from which the formation method of the pore in the 6th manufacturing apparatus of recorded matter differs. 独立した穿孔加工部の構成例の説明図である。It is explanatory drawing of the structural example of the independent punching part. 独立した穿孔加工部の他の構成例の説明図である。It is explanatory drawing of the other structural example of the independent punching process part. 第2の発明における記録物を長時間水に浸漬させた後の断面図である。It is sectional drawing after the recorded material in 2nd invention was immersed in water for a long time. 第2の発明における記録物の断面である。It is a cross section of the recorded matter in 2nd invention. 複数層の透明シートを含む記録物の異なる例の説明図である。It is explanatory drawing of the example from which the recorded matter containing a multi-layered transparent sheet differs. 複数層の透明シートを含む転写材の異なる例の説明図である。It is explanatory drawing of the example from which the transfer material containing a multilayered transparent sheet differs. 記録物に汚染水が付着した状態の説明図である。It is explanatory drawing of the state which contaminated water adhered to the recorded matter. 記録物に汚染水が付着した状態の他の例の説明図である。It is explanatory drawing of the other example of the state which contaminated water adhered to the recorded matter. 記録装置の構成例の説明図である。It is explanatory drawing of the structural example of a recording device. プライマー層を備えた転写材の異なる例を説明するための断面図である。It is sectional drawing for demonstrating the example from which the transfer material provided with the primer layer differs. 基材シートを剥離する工程を説明するための斜視図である。It is a perspective view for demonstrating the process of peeling a base material sheet. 第2の発明における転写材の断面図である。It is sectional drawing of the transfer material in 2nd invention. 第2の発明における記録物の断面図である。It is sectional drawing of the recorded matter in 2nd invention. 第2の発明における記録物の製造方法の異なる例の説明図である。It is explanatory drawing of the example from which the manufacturing method of the recorded matter in 2nd invention differs. 本発明の転写材を画像支持体に加熱圧着した状態を示す説明図である。It is explanatory drawing which shows the state which heat-pressed the transfer material of this invention to the image support body.

以下、本発明について図面を参照しながら詳細に説明する。ただし、本発明は下記の実施形態に限定されず、その発明特定事項を有する全ての対象を含むものである。なお、同一構造の部材については図面において同一の符号を付し、その説明を省略する場合がある。   Hereinafter, the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the following embodiments, and includes all objects having the invention-specific matters. In addition, about the member of the same structure, the same code | symbol is attached | subjected in drawing, The description may be abbreviate | omitted.

本発明者等は、上述の課題について鋭意検討を行った結果、インクジェット記録物を水に長時間浸漬したときに発生する透明シート(保護シート)のひび割れを防ぐことが可能なインクジェット記録物等を実現することができた。まず始めに、従来のインクジェット記録物において、浸漬耐水後に透明シートのひび割れが発生するメカニズムについて図を用いて説明する。   As a result of intensive studies on the above-described problems, the present inventors have found an inkjet recorded product that can prevent cracking of a transparent sheet (protective sheet) that occurs when the inkjet recorded product is immersed in water for a long time. Could be realized. First, the mechanism of cracking of a transparent sheet after immersion water resistance in a conventional inkjet recording material will be described with reference to the drawings.

図32は、浸漬耐水試験前の従来の一般的なインクジェット記録物を示す断面図である。このインクジェット記録物は、透明シート52、色材受容層53、および画像支持体55が順次積層された構造である。色材受容層53の表面は、水不溶性樹脂からなる透明シート52によって覆われているため水分を吸収できない。しかし、色材受容層53の端部517は外部に露出しているため、インクジェット記録物を水に浸漬したときに、その端部517から水分を大量に吸収してしまう。   FIG. 32 is a cross-sectional view showing a conventional general inkjet recorded matter before the immersion water resistance test. This ink jet recording has a structure in which a transparent sheet 52, a color material receiving layer 53, and an image support 55 are sequentially laminated. Since the surface of the color material receiving layer 53 is covered with the transparent sheet 52 made of a water-insoluble resin, it cannot absorb moisture. However, since the end portion 517 of the color material receiving layer 53 is exposed to the outside, a large amount of moisture is absorbed from the end portion 517 when the ink-jet recorded material is immersed in water.

図32は、インクジェット記録物を長時間水に浸漬させた後、水から取り出したときの変化を示す。色材受容層53は、その端部517から水を大量に吸収すると大きく膨張する。部分519は、膨張した部分である。なお、色材受容層53単独では、48時間の浸漬により約1.5倍程度膨張する場合がある。次に、インクジェット記録物を水から出すと色材受容層53中の水分の蒸発が始まる。このとき、色材受容層53の表面は透明シート52で覆われているため、その表面からは水分が蒸発せず、外部に露出している端部517からのみ水分が蒸発する。そのため、水分が蒸発した色材受容層53は、吸水時に膨張した部分519が部分520のように収縮する。色材受容層53は、その端部517から収縮が始まるため、図中の矢印Eのように、収縮時の応力が透明シート52の中央部518に集中する。そのため、透明シート52の部分518にひび割れが生じ、場合によっては、その部分518の一部が破断して、その表面にクラックが発生するおそれもある。   FIG. 32 shows a change when the ink jet recorded material is immersed in water for a long time and then taken out from water. The colorant receiving layer 53 expands greatly when absorbing a large amount of water from its end 517. Portion 519 is an expanded portion. Note that the color material receiving layer 53 alone may expand about 1.5 times when immersed for 48 hours. Next, when the ink-jet recorded matter is taken out of water, evaporation of moisture in the color material receiving layer 53 starts. At this time, since the surface of the colorant receiving layer 53 is covered with the transparent sheet 52, the water does not evaporate from the surface, but the water evaporates only from the end portion 517 exposed to the outside. Therefore, in the color material receiving layer 53 in which the water has evaporated, the portion 519 that has expanded during water absorption contracts like the portion 520. Since the color material receiving layer 53 starts to contract from the end portion 517 thereof, stress at the time of contraction is concentrated on the central portion 518 of the transparent sheet 52 as indicated by an arrow E in the drawing. Therefore, a crack is generated in the portion 518 of the transparent sheet 52, and in some cases, a portion of the portion 518 may be broken and a crack may be generated on the surface.

すなわち、一旦全面に亘って吸水膨張した色材受容層は、その端部から順次乾燥収縮して柔軟性を失い、画像支持体に固定されてゆく。これにより、未だ吸水膨潤している色材受容層の中心側に歪みが徐々に蓄積されつつ、乾燥収縮が徐々に色材受容層の中心部へ進行する。このように、遅れて乾燥収縮する色材受容層と透明シートの部分に、順次蓄積されてきた歪みが集中して、収縮時の応力に耐え切れなくなった透明シートの部分に、ひび割れやクラックが生ずるものと考えられる。   In other words, the colorant receiving layer that has once absorbed and expanded over the entire surface is dried and shrunk sequentially from its end portion, loses its flexibility, and is fixed to the image support. As a result, while the strain gradually accumulates on the center side of the color material receiving layer that is still swollen with water, the drying shrinkage gradually proceeds to the center of the color material receiving layer. In this way, the accumulated strain concentrates on the colorant receiving layer and the transparent sheet portion that dry and shrinks with delay, and cracks and cracks occur on the transparent sheet portion that cannot withstand the stress during shrinkage. It is thought to occur.

上述のように、透明シートのひび割れの原因は、色材受容層からの水分蒸発が端部からのみしか行われず、その収縮の応力が透明シートの特定の1箇所または特定の複数箇所に集中にことにある。本発明は、このような点に着目し、色材受容層への水分の吸収および蒸発に伴って生じる透明シートの応力を分散する構成を確立した。すなわち本発明では、記録物(被転写材)の表面となる透明シートに、その表面を通して水分を排出する通路を設けることにより、色材受容層が吸収した不要な水分を透明シートの表層面全体から暫時蒸発可能とする。このようにして、吸水伸張した色材受容層が暫時乾燥する過程において、透明シートへの応力集中を分散させることにより、浸漬耐水試験における透明シートのひび割れを解消させることができた。   As described above, the cause of cracks in the transparent sheet is that the evaporation of moisture from the colorant receiving layer is performed only from the end, and the stress of the contraction is concentrated in one specific place or a plurality of specific places on the transparent sheet. There is. The present invention pays attention to such points, and has established a configuration that disperses the stress of the transparent sheet caused by the absorption and evaporation of moisture into the colorant receiving layer. In other words, in the present invention, the transparent sheet serving as the surface of the recorded material (transfer material) is provided with a passage through which moisture is discharged, thereby removing unnecessary moisture absorbed by the color material receiving layer over the entire surface of the transparent sheet. Evaporate for a while. In this way, cracks in the transparent sheet in the immersion water resistance test could be eliminated by dispersing the stress concentration on the transparent sheet in the course of drying of the colorant receiving layer that has absorbed water for a while.

(第1の発明)
以下、第1の発明について説明する。
(First invention)
The first invention will be described below.

透明シートは、記録物の表面を保護する保護シートとしての機能するものであり、第1の発明においては、記録物の表面となる透明シートに、色材受容層にまで貫通する細孔を設けている。図33(a)から(f)は、記録物の支持体55に、本発明の転写材の色材受容層53と透明シート52を転写して作成した記録物を示す。色材受容層53には、後述するように反転画像72が記録されている。本発明における透明シート52は細孔52Aを有するため、色材受容層53に吸収された水分が透明シート52の細孔52Aを通して、透明シート52の表面521,553,554,555から蒸発させることができる。記録物は、図33(a)のように少なくとも透明シート52に細孔52Aが形成されていればよく、図33(b),(c)のように色材受容層53にも細孔53Aを形成されてもよい。また図33(d)から(f)のように、透明シート52に多数の空隙を形成して、それらが透明シート52を貫通する細孔52Aを形成するように連なる連泡構造553,554,555としてもよい。これらの細孔について後述する。透明シート52の細孔52Aは、透明シート52が水分透過性もしくは透湿性を発現できるように構成されている。すなわち、その細孔52Aは、透明シート52に接触した水が液体の状態もしくは気体の状態で透明シート52を通過させる性質を持つ。   The transparent sheet functions as a protective sheet that protects the surface of the recorded matter. In the first invention, the transparent sheet that is the surface of the recorded matter is provided with pores that penetrate to the colorant receiving layer. ing. 33 (a) to 33 (f) show a recorded material created by transferring the color material receiving layer 53 and the transparent sheet 52 of the transfer material of the present invention to a support 55 of the recorded material. A reverse image 72 is recorded on the color material receiving layer 53 as described later. Since the transparent sheet 52 in the present invention has the pores 52A, the water absorbed in the colorant receiving layer 53 is evaporated from the surfaces 521, 553, 554, and 555 of the transparent sheet 52 through the pores 52A of the transparent sheet 52. Can do. The recorded material only needs to have pores 52A formed at least in the transparent sheet 52 as shown in FIG. 33 (a), and the pores 53A also exist in the colorant receiving layer 53 as shown in FIGS. 33 (b) and 33 (c). May be formed. Also, as shown in FIGS. 33 (d) to (f), a large number of voids are formed in the transparent sheet 52, and the open cell structures 553, 554 are continuous so as to form pores 52A penetrating the transparent sheet 52. It may be 555. These pores will be described later. The pores 52A of the transparent sheet 52 are configured such that the transparent sheet 52 can exhibit moisture permeability or moisture permeability. That is, the pores 52A have the property that the water in contact with the transparent sheet 52 passes through the transparent sheet 52 in a liquid state or a gas state.

図34(a)は、図33の記録物を長時間水に浸漬させた後、水から取り出した状態を示す。本発明の記録物73は水から取り出すと、色材受容層53に吸収された水分は、色材受容層53の端部517からだけでなく、透明シート52の表面521からも蒸発する。このように、透明シートの表面からも色材受容層の水分を蒸発させることにより、色材受容層の収縮時の応力は、矢印Cのように透明シートの表面全体に広く分散され、この結果、透明シートのひび割れを防ぐことができる。   FIG. 34A shows a state in which the recorded matter of FIG. 33 is immersed in water for a long time and then taken out from water. When the recorded matter 73 of the present invention is taken out of water, the moisture absorbed in the color material receiving layer 53 evaporates not only from the end portion 517 of the color material receiving layer 53 but also from the surface 521 of the transparent sheet 52. In this way, by evaporating the moisture of the color material receiving layer from the surface of the transparent sheet, the stress at the time of contraction of the color material receiving layer is widely dispersed over the entire surface of the transparent sheet as indicated by arrow C. As a result, Can prevent cracking of transparent sheet.

本実施形態における記録物は、図23から図26および図47,図48,図49に示すように、まず、転写材の色材受容層53に、インクジェット方式の記録ヘッド607によって反転画像72を記録する(工程1)。次に、ヒートローラ21を用いて、転写材と画像支持体55とを加熱圧着して、画像支持体55に転写材を転写させる(工程2)。最後に、剥離ロール88を用いて転写材の基材シート50を剥離することにより(工程3)、画像が記録された色材受容層、および保護シートが積層された記録物を得る。記録物の表面となる透明シート52は、細孔52Aを有する。   As shown in FIGS. 23 to 26 and FIGS. 47, 48, and 49, the recorded material in the present embodiment first has a reverse image 72 formed on a color material receiving layer 53 of a transfer material by an ink jet recording head 607. Record (step 1). Next, the transfer material and the image support 55 are heat-pressed using the heat roller 21 to transfer the transfer material to the image support 55 (step 2). Finally, the base material sheet 50 of the transfer material is peeled using the peeling roll 88 (Step 3) to obtain a recorded matter in which the color material receiving layer on which the image is recorded and the protective sheet are laminated. The transparent sheet 52 serving as the surface of the recorded material has pores 52A.

[1]転写材
本実施形態の転写材は、上述のように、基材シート、透明シート、および色材受容層がこの順で積層された積層構造を有するインクジェット記録用の転写材であって、透明シートが水分を系外に放出可能である。より好ましくは、転写材は、その色材受容層が少なくとも水溶性樹脂を含有し、その透明シートは、その細孔構造により少なくとも水分透過性または透湿性を有することを特徴とする。さらに好ましくは、透明シートは透湿性かつ水分透過性であることを特徴とする。図22(a)から(h)は、転写材の異なる構成例の断面図である。転写材1は、基材シート50、透明シート52、および色材受容層53がこの順で積層された積層構造を有する。図22(a)から(e)の色材受容層53は少なくとも水分を吸収できる水溶性樹脂を含有し、少なくとも透明シート52には細孔52Aが形成されており、その細孔52Aは、基材シート50と色材受容層53との間を連通する。
[1] Transfer Material The transfer material of the present embodiment is a transfer material for ink jet recording having a laminated structure in which a base sheet, a transparent sheet, and a color material receiving layer are laminated in this order as described above. The transparent sheet can release moisture out of the system. More preferably, the transfer material is characterized in that the color material receiving layer contains at least a water-soluble resin, and the transparent sheet has at least moisture permeability or moisture permeability due to its pore structure. More preferably, the transparent sheet is characterized by being moisture permeable and moisture permeable. 22A to 22H are cross-sectional views of different configuration examples of the transfer material. The transfer material 1 has a laminated structure in which a base sheet 50, a transparent sheet 52, and a color material receiving layer 53 are laminated in this order. The colorant receiving layer 53 in FIGS. 22A to 22E contains at least a water-soluble resin capable of absorbing moisture, and at least the transparent sheet 52 has pores 52A formed therein. The material sheet 50 and the color material receiving layer 53 are communicated with each other.

図22(a)の転写材1は、透明シート52のみに細孔52Aが形成され、図22(b)の転写材1は、透明シート52に細孔52Aが形成され、かつ色材受容層53にも細孔53Aが形成されている。図22(c)の転写材1は、透明シート52に細孔52Aが形成され、かつ基材シート50にも細孔50Aが形成されている。図22(d),(e)の転写材1は、透明シート52,色材受容層53,基材シート50のそれぞれに細孔52A,53A,50Aが形成されている。また、図22(f)から(h)の透明シート52は、透明シート52内に、その両面の間を貫通するように連なる多数の空隙が形成されている。これらの空隙は、透明シート52を貫通する細孔52Aを形成するように連なる連泡構造553,554,555を成す。   The transfer material 1 in FIG. 22A has pores 52A formed only in the transparent sheet 52, and the transfer material 1 in FIG. 22B has pores 52A formed in the transparent sheet 52 and a color material receiving layer. 53 also has pores 53A. In the transfer material 1 in FIG. 22C, pores 52 </ b> A are formed in the transparent sheet 52, and pores 50 </ b> A are also formed in the base material sheet 50. In the transfer material 1 of FIGS. 22D and 22E, pores 52A, 53A, and 50A are formed in the transparent sheet 52, the color material receiving layer 53, and the base material sheet 50, respectively. Further, in the transparent sheet 52 of FIGS. 22 (f) to 22 (h), a large number of voids are formed in the transparent sheet 52 so as to penetrate between both surfaces. These voids form continuous bubble structures 553, 554, and 555 that are continuous so as to form pores 52A that penetrate the transparent sheet 52.

このような転写材1は、色材受容層53に画像が記録された後、図33のように記録物の画像支持体55に、色材受容層53が透明シート52と共に転写される。したがって転写材1は、記録物に転写される色材受容層53と透明シート52とを含む中間シートとして機能する。図33(a)は、図22(c)の転写材1を用いて作成されて記録物、図33(b)は、図22(c)または(d)の転写材1を用いて作成されて記録物の断面図である。図33(c)は、図22(b)または(e)の転写材1を用いて作成されて記録物の断面図である。図図33(d),(e),(f)は、それぞれ図22(f),(g),(h)の転写材1を用いて作成されて記録物の断面図である。転写材1は、図1(b)のように、その透明シート52に予め細孔52Aが形成されていないものを用いることもできる。この場合には、工程1〜3のいずれかの工程の前後に、透明シート52に細孔52Aを形成すればよい。   In such a transfer material 1, after an image is recorded on the color material receiving layer 53, the color material receiving layer 53 is transferred together with the transparent sheet 52 to the image support 55 of the recorded material as shown in FIG. Therefore, the transfer material 1 functions as an intermediate sheet including the color material receiving layer 53 and the transparent sheet 52 transferred to the recorded matter. FIG. 33 (a) is a recorded material created using the transfer material 1 of FIG. 22 (c), and FIG. 33 (b) is created using the transfer material 1 of FIG. 22 (c) or (d). FIG. FIG. 33 (c) is a cross-sectional view of a recorded matter created using the transfer material 1 of FIG. 22 (b) or (e). FIGS. 33D, 33E, and 33F are cross-sectional views of recorded matter created using the transfer material 1 shown in FIGS. 22F, 22G, and 22H, respectively. As the transfer material 1, as shown in FIG. 1B, the transparent sheet 52 in which the pores 52A are not formed in advance can be used. In this case, the pores 52 </ b> A may be formed in the transparent sheet 52 before and after any of the steps 1 to 3.

[1−1]色材受容層
色材受容層は、インクジェット記録方式によるインクを受容する層であり、少なくとも水溶性樹脂を含有する。色材受容層としては、水溶性樹脂を主体として、水溶性高分子の網目構造中にインクを受容する膨潤吸収型と、水溶性樹脂と少なくとも無機微粒子とを含有して、微細な空隙構造にインクを受容する空隙吸収型と、の色材受容層のどちらも使用できる。
[1-1] Color Material Receiving Layer The color material receiving layer is a layer that receives ink by an ink jet recording method and contains at least a water-soluble resin. The colorant receiving layer is mainly composed of a water-soluble resin, contains a swelling absorption type that accepts ink in a network structure of a water-soluble polymer, contains a water-soluble resin and at least inorganic fine particles, and has a fine void structure. Either a void absorbing type for receiving ink or a colorant receiving layer can be used.

色材受容層53を、水溶性樹脂を主体とした膨潤吸収型の色材受容層とした場合には、水の吸収速度が遅いため、記録物を水に浸漬させた場合でも、短期間であれば透明シート(52)のひび割れは生じにくい。このような色材受容層53が転写された記録物は、耐水性の観点ではやや有利であるものの、色材受容層53におけるインクの吸収速度も遅くなる。そのため、膨潤吸収型の色材受容層は、制限された条件下では十分に機能するものの、画像の記録速度が制限されて高速記録には適さない場合もある。また、膨潤吸収型の色材受容層の場合は、インク中の水分により色材受容層が膨潤して、色材受容層の表面に凹凸が発生するため、画像支持体に対する色材受容層の接着性を低下させるおそれがある。   When the color material receiving layer 53 is a swelling absorption type color material receiving layer mainly composed of a water-soluble resin, the absorption speed of water is slow, so even when the recorded matter is immersed in water, the color material receiving layer 53 can be obtained in a short period of time. If it exists, the crack of a transparent sheet (52) does not arise easily. Although the recorded matter to which the color material receiving layer 53 is transferred is somewhat advantageous from the viewpoint of water resistance, the ink absorption speed in the color material receiving layer 53 is also slow. Therefore, although the swelling absorption type colorant receiving layer functions sufficiently under the limited conditions, the recording speed of the image is limited and may not be suitable for high-speed recording. In the case of a swelling absorption type color material receiving layer, the color material receiving layer swells due to moisture in the ink, and irregularities are generated on the surface of the color material receiving layer. There is a risk of reducing the adhesion.

一方、空隙型の色材受容層は、水溶性樹脂と、少なくとも無機微粒子と、を含有する組成物から構成されている。色材受容層53を空隙吸収型にした場合には、記録物を水に浸漬させると、上述したように記録物の端部の色材受容層から水がより浸入しやすくなり、耐水性に問題が生じて透明シートのひび割れやクラックが発生しやすくなる。しかし、本発明においては、透明シートに細孔を設けることにより、色材転写層が万一多量の水分を吸収した場合でも、応力集中による透明シートのひび割れやクラックは発生しにくい構成としている。また、空隙吸収型の色材受容層は、無機微粒子によって形成される空隙がインクを速やかに吸収することができるため、高速のインクジェット記録が可能となる。また、空隙吸収型の色材受容層は、膨潤型の色材受容層とは異なり、色材受容層が膨潤することなく平滑に保たれる。特に顔料インクを用いた場合は、顔料インク中の顔料成分は色材受容層の表面で定着し、一方、インク中の水分及び溶媒成分は、色材受容層の内部まで浸透して、顔料成分と分離(固液分離)する。そのため、転写時には色材受容層の表面が乾燥した状態になる。無機微粒子により形成される空隙によって、色材受容層の表面が乾燥した状態になるため、転写材を記録物の画像支持体に加熱圧着させる際に、インク中の水分または溶媒が急激に突沸することが抑制される。この結果、転写材と記録物の支持体とが十分に密着しない密着性不良、および転写材と記録物の画像支持体との間に気泡が残る気泡残りの発生を抑制することができる。   On the other hand, the void-type color material receiving layer is composed of a composition containing a water-soluble resin and at least inorganic fine particles. In the case where the color material receiving layer 53 is of the gap absorption type, when the recorded material is immersed in water, as described above, water can more easily enter from the color material receiving layer at the end of the recorded material, thereby improving water resistance. Problems arise and cracks and cracks of the transparent sheet are likely to occur. However, in the present invention, by providing pores in the transparent sheet, even if the color material transfer layer absorbs a large amount of moisture, the transparent sheet is not easily cracked or cracked due to stress concentration. . Further, since the void formed by the inorganic fine particles can absorb the ink quickly, the gap absorption type color material receiving layer can perform high-speed inkjet recording. Further, unlike the swelling type color material receiving layer, the space absorption type color material receiving layer is kept smooth without swelling. In particular, when a pigment ink is used, the pigment component in the pigment ink is fixed on the surface of the color material receiving layer, while the moisture and solvent components in the ink penetrate into the color material receiving layer and the pigment component. (Solid-liquid separation). Therefore, the surface of the colorant receiving layer is in a dry state at the time of transfer. Since the surface of the colorant receiving layer is in a dry state due to the voids formed by the inorganic fine particles, the moisture or solvent in the ink suddenly boils when the transfer material is heat-pressed to the image support of the recorded material. It is suppressed. As a result, it is possible to suppress the poor adhesion that the transfer material and the support for the recorded material are not sufficiently in contact, and the generation of remaining bubbles that remain between the transfer material and the image support for the recorded material.

また、色材受容層が無機微粒子を含有することにより、転写後に転写材の基材シートを剥離する際に、色材受容層の無機微粒子の隙間にクラックが入りやすくなって、記録物の端部にバリが残らないようにすることができる。そこで、色材受容層53は空隙吸収型の色材受容層とすることが好ましい。すなわち、本発明によれば、耐水性を損なうことなく、空隙吸収型の色材転写層を利用した画像の高速記録が可能となる。   In addition, since the color material receiving layer contains inorganic fine particles, when the transfer material base sheet is peeled off after transfer, cracks are easily formed in the gaps between the inorganic fine particles of the color material receiving layer, and the edges of the recorded material are reduced. It is possible to prevent burrs from remaining in the part. Therefore, the color material receiving layer 53 is preferably a void absorption type color material receiving layer. That is, according to the present invention, high-speed recording of an image using a gap absorption type color material transfer layer is possible without impairing water resistance.

[1−1−1]無機微粒子
無機微粒子は、無機材料からなる微粒子である。無機微粒子は色材受容層に色材を受容する空隙を形成する機能を有する。
[1-1-1] Inorganic fine particles The inorganic fine particles are fine particles made of an inorganic material. The inorganic fine particles have a function of forming voids for receiving the color material in the color material receiving layer.

無機微粒子を構成する無機材料の種類としては特に制限はない。ただし、インク吸収能が高く、発色性に優れ、高品位の画像が形成可能な無機材料であることが好ましい。例えば、炭酸カルシウム、炭酸マグネシウム、カオリン、クレー、タルク、ハイドロタルサイト、珪酸アルミニウム、珪酸カルシウム、珪酸マグネシウム、ケイソウ土、アルミナ、コロイダルアルミナ、水酸化アルミニウム、ベーマイト構造のアルミナ水和物、擬ベーマイト構造のアルミナ水和物、リトポン(硫酸バリウムと硫化亜鉛の混合物)、ゼオライト等を挙げることができる。   There is no restriction | limiting in particular as a kind of inorganic material which comprises an inorganic fine particle. However, it is preferably an inorganic material that has high ink absorbability, excellent color developability, and can form a high-quality image. For example, calcium carbonate, magnesium carbonate, kaolin, clay, talc, hydrotalcite, aluminum silicate, calcium silicate, magnesium silicate, diatomaceous earth, alumina, colloidal alumina, aluminum hydroxide, boehmite structure alumina hydrate, pseudo boehmite structure And alumina hydrate, lithopone (a mixture of barium sulfate and zinc sulfide), zeolite and the like.

これらの無機材料からなる無機微粒子の中でも、アルミナ及びアルミナ水和物からなる群より選択される少なくとも1種の物質からなるアルミナ微粒子が好ましい。アルミナ水和物としては、ベーマイト構造のアルミナ水和物、擬ベーマイト構造のアルミナ水和物等を挙げることができる。アルミナ、ベーマイト構造のアルミナ水和物、擬ベーマイト構造のアルミナ水和物は、色材受容層の透明性及び画像の記録濃度を向上させることができる点において好ましい。   Among the inorganic fine particles made of these inorganic materials, alumina fine particles made of at least one substance selected from the group consisting of alumina and alumina hydrate are preferable. Examples of the alumina hydrate include boehmite-structured alumina hydrate and pseudoboehmite-structured alumina hydrate. Alumina, boehmite-structured alumina hydrate, and pseudoboehmite-structured alumina hydrate are preferred in that the transparency of the colorant-receiving layer and the image recording density can be improved.

ベーマイト構造のアルミナ水和物は、長鎖のアルミニウムアルコキシドに対して酸を添加して加水分解・解膠を行うことによって得ることができる(特開昭56−120508号公報参照)。解膠には有機酸、無機酸のいずれを用いてもよい。ただし、硝酸を用いることが好ましい。硝酸を用いることにより、加水分解の反応効率を向上させることができ、形状が制御されたアルミナ水和物を得ることができ、分散性が良好な分散液を得ることができる。   Boehmite-structured alumina hydrate can be obtained by adding an acid to a long-chain aluminum alkoxide for hydrolysis and peptization (see JP-A-56-120508). Either an organic acid or an inorganic acid may be used for peptization. However, it is preferable to use nitric acid. By using nitric acid, the reaction efficiency of hydrolysis can be improved, an alumina hydrate having a controlled shape can be obtained, and a dispersion having good dispersibility can be obtained.

無機微粒子は、平均粒子径を精密に制御することが好ましく、その平均粒子径が120〜200nmであることが好ましい。平均粒子径を、好ましくは120nm以上、さらに好ましくは140nm以上とすることにより、色材受容層のインク吸収性を向上させて、記録後の画像におけるインクの滲みやビーディングを抑制することができる。一方、平均粒子径を、好ましくは200nm以下、さらに好ましくは170nm以下とすることにより、無機微粒子による光散乱を抑制して、色材受容層の透明性を向上させることができる。また、色材受容層の単位面積当たりの無機微粒子数を増加させることができるため、インク吸収性を向上させることができる。従って、画像の記録濃度を向上させることができ、記録後の画像のくすみを抑制することができる。これにより、色材受容層の透明性(透過性)、および透明シートの側からの画像の視認性を向上させることができる。色材として、色材受容層に浸透しにくい顔料インクを使用した場合においても、インクの付与密度が高まり、多量のインクを受容させるために、色材受容層の厚さを増大させる必要がない。このため、転写材延いては記録物の全体を薄厚化することができる。   The inorganic fine particles preferably have a precisely controlled average particle size, and the average particle size is preferably 120 to 200 nm. By setting the average particle size to preferably 120 nm or more, and more preferably 140 nm or more, it is possible to improve the ink absorbability of the colorant receiving layer and to suppress ink bleeding and beading in the image after recording. . On the other hand, when the average particle diameter is preferably 200 nm or less, more preferably 170 nm or less, light scattering by the inorganic fine particles can be suppressed and the transparency of the colorant receiving layer can be improved. Further, since the number of inorganic fine particles per unit area of the colorant receiving layer can be increased, ink absorbability can be improved. Accordingly, the recording density of the image can be improved, and dullness of the image after recording can be suppressed. Thereby, the transparency (transmittance) of the color material receiving layer and the visibility of the image from the transparent sheet side can be improved. Even when a pigment ink that does not easily penetrate into the color material receiving layer is used as the color material, it is not necessary to increase the thickness of the color material receiving layer in order to increase the ink application density and accept a large amount of ink. . For this reason, it is possible to reduce the thickness of the transfer material and the entire recorded material.

無機微粒子は、公知の無機微粒子をそのまま用いてもよいし、粉砕分散機等を用いて公知の無機微粒子の平均粒子径、多分散指数を調整したものを用いてもよい。粉砕分散機の種類としては特に制限はない。例えば、高圧ホモジナイザー、超音波ホモジナイザー、湿式メディア型粉砕機(サンドミル、ボールミル)、連続式高速撹拌型分散機、超音波分散機等の従来公知の粉砕分散機を用いることができる。   As the inorganic fine particles, known inorganic fine particles may be used as they are, or those obtained by adjusting the average particle diameter and polydispersity index of known inorganic fine particles using a pulverizer / disperser may be used. There are no particular restrictions on the type of pulverizer. For example, a conventionally known pulverizer such as a high-pressure homogenizer, an ultrasonic homogenizer, a wet media type pulverizer (sand mill, ball mill), a continuous high-speed agitation type disperser, or an ultrasonic disperser can be used.

粉砕分散機をより具体的に例示すると、以下全て商品名で、マントンゴーリンホモジナイザー、ソノレータ(以上、同栄商事製);マイクロフルイタイザー(みずほ工業製);ナノマイザー(月島機械製);アルティマイザー(伊藤忠産機製);パールミル、グレンミル、トルネード(以上、浅田鉄鋼製);ビスコミル(アイメックス製);マイティーミル、RSミル、SΓミル(以上、井上製作所製);荏原マイルダー(荏原製作所製);ファインフローミル、キャビトロン(以上、太平洋機工製);等を挙げることができる。   More specific examples of the pulverizing and dispersing machine are as follows: Manton Gorin homogenizer, Sonator (above, manufactured by Doei Sei); Microfluidizer (manufactured by Mizuho Industries); Nanomizer (manufactured by Tsukishima Kikai); Pearl mill, Glen mill, Tornado (above Asada Steel); Visco mill (Imex); Mighty mill, RS mill, SΓ mill (Inoue Seisakusho); Sugawara Milder (Ebara Seisakusho); Fine Flow Mill, Cavitron (made by Taiheiyo Kiko);

また、無機微粒子は、平均粒子径の範囲を満たし、かつ、多分散指数(μ/<Γ>2)が0.01〜0.20であることが好ましく、0.01〜0.18とすることがさらに好ましい。上述の範囲に設定することで粒子の大きさを一定に保つことが可能になるため、色材受容層の光沢性及び透明性を向上させることができる。従って、画像の記録濃度を向上させることができ、記録後の画像のくすみを抑制することができる。 The inorganic fine particles preferably satisfy the range of the average particle diameter and have a polydispersity index (μ / <Γ> 2 ) of 0.01 to 0.20, preferably 0.01 to 0.18. More preferably. By setting the particle size within the above range, the particle size can be kept constant, so that the glossiness and transparency of the colorant-receiving layer can be improved. Accordingly, the recording density of the image can be improved, and dullness of the image after recording can be suppressed.

なお、本明細書にいう平均粒子径及び多分散指数は動的光散乱法によって測定された値を、「高分子の構造(2)散乱実験と形態観察 第1章 光散乱」(共立出版 高分子学会編)、又はJ.Chem.Phys.,70(B),15 Apl.,3965(1979)に記載のキュムラント法によって解析することにより求めることができる。動的光散乱の理論によれば、異なる粒径を持つ微粒子が混在している場合、散乱光からの時間相関関数の減衰に分布を有する。この時間相関関数をキュムラント法により解析することにより、減衰速度の平均(<Γ>)と分散(μ)が求まる。減衰速度(Γ)は粒子の拡散係数と散乱ベクトルの関数で表わされるため、ストークス−アインシュタイン式を用いて、流体力学的平均粒径を求めることができる。従って、減衰速度の分散(μ)を平均の二乗(<Γ>2)で除した多分散指数(μ/<Γ>2)は、粒径の散らばりの度合いを表わしており、値が0に近づく程、粒径の分布は狭くなることを意味する。本実施の形態で定義される平均粒子径及び多分散指数は、例えば、レーザ粒径解析装置PARIII(大塚電子製)等を用いて容易に測定することができる。 The average particle diameter and polydispersity index referred to in this specification are the values measured by the dynamic light scattering method, “polymer structure (2) scattering experiment and morphology observation Chapter 1 light scattering” (Kyoritsu Publishing High Edited by Molecular Society), or J. Org. Chem. Phys. , 70 (B), 15 ApI. 3965 (1979). According to the theory of dynamic light scattering, when fine particles having different particle diameters are mixed, there is a distribution in the decay of the time correlation function from the scattered light. By analyzing this time correlation function by the cumulant method, the average (<Γ>) and dispersion (μ) of the decay rate can be obtained. Since the decay rate (Γ) is expressed as a function of the particle diffusion coefficient and the scattering vector, the hydrodynamic average particle diameter can be obtained using the Stokes-Einstein equation. Therefore, the polydispersity index (μ / <Γ> 2 ) obtained by dividing the dispersion of the decay rate (μ) by the mean square (<Γ> 2 ) represents the degree of dispersion of the particle size, and the value is zero. The closer it is, the narrower the particle size distribution. The average particle size and polydispersity index defined in the present embodiment can be easily measured using, for example, a laser particle size analyzer PARIII (manufactured by Otsuka Electronics).

無機微粒子は1種を単独で、又は2種以上を混合して用いることができる。「2種以上」とは、材質自体が異なるものの他、平均粒子径、多分散指数等の特性が異なるものも含まれる。   An inorganic fine particle can be used individually by 1 type or in mixture of 2 or more types. “Two or more types” includes not only materials different from each other but also materials having different characteristics such as average particle diameter and polydispersity index.

[1−1−2]水溶性樹脂
水溶性樹脂は、25℃において、水と十分に混和するか、水に対する溶解度が1(g/100g)以上の樹脂である。膨潤型色材受容層の場合、水溶性樹脂は、水溶性高分子の網目構造中にインクを受容する層として作用する。また、空隙吸収型の場合、水溶性樹脂は、無機微粒子を結着するバインダーとして機能する。
[1-1-2] Water-soluble resin The water-soluble resin is a resin that is sufficiently mixed with water at 25 ° C. or has a solubility in water of 1 (g / 100 g) or more. In the case of the swelling type colorant receiving layer, the water-soluble resin acts as a layer for receiving ink in the network structure of the water-soluble polymer. In the case of the void absorption type, the water-soluble resin functions as a binder for binding the inorganic fine particles.

水溶性樹脂としては、下式(1)を満たすものであれば、特に制限はない。|ΔSP|が0.6以上になると水溶性樹脂と後述するエマルジョンE1の分子間力が弱くなり、色材受容層と透明シートの密着性が低下して、テープ剥離等の試験において透明シートと色材受容層との間で剥がれが生じるため好ましくない。|ΔSP|を下式(1)の範囲にすることにより、水溶性樹脂とエマルジョンE1の分子間力によって強力に接着して、透明シートと色材受容層の密着性を向上させることができる。
0≦ΔSP≦0.6 (1)
The water-soluble resin is not particularly limited as long as it satisfies the following formula (1). When | ΔSP | is 0.6 or more, the intermolecular force between the water-soluble resin and the emulsion E1 described later is weakened, the adhesion between the colorant-receiving layer and the transparent sheet is lowered, and in the test such as tape peeling, Since peeling occurs between the colorant receiving layer and the colorant receiving layer, it is not preferable. By setting | ΔSP | in the range of the following formula (1), the water-soluble resin and the emulsion E1 can be strongly bonded by the intermolecular force, and the adhesion between the transparent sheet and the colorant receiving layer can be improved.
0 ≦ ΔSP ≦ 0.6 (1)

例えば、澱粉、ゼラチン、カゼイン及びこれらの変性物;
メチルセルロース、カルボキシメチルセルロース、ヒドロキシエチルセルロース等のセルロース誘導体;
ポリビニルアルコール(完全けん化、部分ケン化、低けん化等)又はこれらの変性物(カチオン変性物、アニオン変性物、シラノール変性物等);
尿素系樹脂、メラミン系樹脂、エポキシ系樹脂、エピクロルヒドリン系樹脂、ポリウレタン系樹脂、ポリエチレンイミン系樹脂、ポリアミド系樹脂、ポリビニルピロリドン系樹脂、ポリビニルブチラール系樹脂、ポリ(メタ)アクリル酸又はその共重合体樹脂、アクリルアミド系樹脂、無水マレイン酸系共重合体樹脂、ポリエステル系樹脂等の樹脂;等を挙げることができる。
For example, starch, gelatin, casein and modified products thereof;
Cellulose derivatives such as methylcellulose, carboxymethylcellulose, and hydroxyethylcellulose;
Polyvinyl alcohol (complete saponification, partial saponification, low saponification, etc.) or a modified product thereof (cation modified product, anion modified product, silanol modified product, etc.);
Urea resin, melamine resin, epoxy resin, epichlorohydrin resin, polyurethane resin, polyethyleneimine resin, polyamide resin, polyvinyl pyrrolidone resin, polyvinyl butyral resin, poly (meth) acrylic acid or copolymer thereof And resins such as resins, acrylamide resins, maleic anhydride copolymer resins, and polyester resins.

水溶性樹脂の中でも、ポリビニルアルコール、特にポリ酢酸ビニルを加水分解(けん化)することにより得られる、けん化ポリビニルアルコールが好ましい。ポリビニルアルコールのSP値は後述するPVCやPET−GのSP値と値が近い。したがって、転写時の熱で水溶性樹脂および画像支持体が溶融すると両者の相溶性が高まり、水溶性樹脂は画像支持体に強固に接着される。ポリビニルアルコールは、画像支持体としてPVCやPET−Gを使用した場合に、画像支持体と色材受容層との密着性(転写性能)を向上させることができ、特に好ましく用いられる。   Among water-soluble resins, polyvinyl alcohol, particularly saponified polyvinyl alcohol obtained by hydrolyzing (saponifying) polyvinyl acetate is preferable. The SP value of polyvinyl alcohol is close to the SP value of PVC and PET-G described later. Therefore, when the water-soluble resin and the image support are melted by heat at the time of transfer, the compatibility of both increases, and the water-soluble resin is firmly bonded to the image support. Polyvinyl alcohol can improve the adhesion (transfer performance) between the image support and the colorant receiving layer when PVC or PET-G is used as the image support, and is particularly preferably used.

色材受容層は、けん化度70〜100mol%のポリビニルアルコールを含有する組成物からなることが好ましい。けん化度とは、ポリビニルアルコールの酢酸基と水酸基の合計モル数に対する水酸基のモル数の百分率を意味する。   The colorant receiving layer is preferably made of a composition containing polyvinyl alcohol having a saponification degree of 70 to 100 mol%. The degree of saponification means the percentage of the number of moles of hydroxyl groups relative to the total number of moles of acetate groups and hydroxyl groups of polyvinyl alcohol.

けん化度を、好ましくは70mol%以上、さらに好ましくは86mol%以上とすることにより、色材受容層に適度な硬さを付与することができる。したがって、剥離工程において色材受容層の箔切れ性が向上し、端部のバリの発生を抑制することができる。また、無機微粒子とポリビニルアルコールを含む塗工液の粘度を低下させることができる。従って、透明シートに対して塗工液を塗工し易くなり、転写材の生産性を向上させることができる。一方、けん化度を、好ましくは100mol%以下、さらに好ましくは90mol%以下とすることにより、色材受容層に適度な柔軟性を付与することができる。これにより、透明シートと色材受容層との接着強度を向上させて、接着強度の不足による透明シートからの色材受容層の剥離を抑制することができる。また、色材受容層に適度な親水性を付与することができ、インクの吸収性が良好となる。従って、色材受容層に高品位の画像を記録することが可能となる。   By setting the saponification degree to 70 mol% or more, more preferably 86 mol% or more, an appropriate hardness can be imparted to the colorant receiving layer. Therefore, the foil breakability of the colorant receiving layer is improved in the peeling step, and the occurrence of burrs at the end can be suppressed. Moreover, the viscosity of the coating liquid containing inorganic fine particles and polyvinyl alcohol can be reduced. Therefore, it becomes easy to apply the coating liquid to the transparent sheet, and the productivity of the transfer material can be improved. On the other hand, when the degree of saponification is preferably 100 mol% or less, more preferably 90 mol% or less, moderate flexibility can be imparted to the color material receiving layer. Thereby, the adhesive strength between the transparent sheet and the color material receiving layer can be improved, and the peeling of the color material receiving layer from the transparent sheet due to insufficient adhesive strength can be suppressed. Moreover, moderate hydrophilicity can be imparted to the colorant receiving layer, and the ink absorbability is improved. Therefore, a high-quality image can be recorded on the color material receiving layer.

けん化度の範囲を満たす、けん化ポリビニルアルコールとしては、完全けん化ポリビニルアルコール(けん化度98〜99mol%)、部分けん化ポリビニルアルコール(けん化度87〜89mol%)、低けん化ポリビニルアルコール(けん化度78〜82mol%)等を挙げることができる。中でも、部分けん化ポリビニルアルコールが好ましい。   As saponified polyvinyl alcohol satisfying the range of saponification degree, fully saponified polyvinyl alcohol (saponification degree 98-99 mol%), partially saponified polyvinyl alcohol (saponification degree 87-89 mol%), low saponified polyvinyl alcohol (saponification degree 78-82 mol%). And the like. Among these, partially saponified polyvinyl alcohol is preferable.

色材受容層は、平均重合度が2,000〜5,000のポリビニルアルコールを含有する組成物からなることが好ましい。   The colorant receiving layer is preferably made of a composition containing polyvinyl alcohol having an average degree of polymerization of 2,000 to 5,000.

平均重合度を、好ましくは2,000以上、さらに好ましくは3,000以上とすることにより、に適度な柔軟性を付与することができる。したがって、剥離工程において色材受容層の箔切れ性が向上し、端部のバリの発生を抑制することができる。一方、平均重合度を、好ましくは5,000以下、さらに好ましくは4,500以下とすることにより、色材受容層に適度な硬さを付与することができる。これにより、透明シートと色材受容層との接着強度を向上させて、接着強度の不足による透明シートからの色材受容層の剥離を抑制することができる。また、無機微粒子とポリビニルアルコールを含む塗工液の粘度を低下させることができる。従って、透明シートに対して塗工液を塗工し易くなり、転写材の生産性を向上させることができる。また、色材受容層の細孔が埋まることを防止し、細孔の開口状態を良好に保つことができ、インクの吸収性が良好となる。従って、色材受容層に高品位の画像を記録することが可能となる。   When the average degree of polymerization is preferably 2,000 or more, more preferably 3,000 or more, moderate flexibility can be imparted. Therefore, the foil breakability of the colorant receiving layer is improved in the peeling step, and the occurrence of burrs at the end can be suppressed. On the other hand, when the average degree of polymerization is preferably 5,000 or less, more preferably 4,500 or less, an appropriate hardness can be imparted to the colorant receiving layer. Thereby, the adhesive strength between the transparent sheet and the color material receiving layer can be improved, and the peeling of the color material receiving layer from the transparent sheet due to insufficient adhesive strength can be suppressed. Moreover, the viscosity of the coating liquid containing inorganic fine particles and polyvinyl alcohol can be reduced. Therefore, it becomes easy to apply the coating liquid to the transparent sheet, and the productivity of the transfer material can be improved. In addition, the pores of the colorant receiving layer can be prevented from being filled, the opening state of the pores can be kept good, and the ink absorbability is good. Therefore, a high-quality image can be recorded on the color material receiving layer.

平均重合度の値は、JIS−K−6726に記載の方法に準拠して算出された値である。   The average degree of polymerization is a value calculated according to the method described in JIS-K-6726.

水溶性樹脂は、1種を単独で、又は2種以上を混合して用いることができる。「2種以上」とは、けん化度、平均重合度等の特性が異なるものも含まれる。   A water-soluble resin can be used individually by 1 type or in mixture of 2 or more types. “Two or more” includes those having different characteristics such as saponification degree and average degree of polymerization.

水溶性樹脂の量は、無機微粒子100質量部に対し、3.3〜20質量部とすることが好ましい。水溶性樹脂の量を、好ましくは3.3質量部以上、さらに好ましくは5質量部以上とすることにより、色材受容層のひび割れや粉落ちが発生し難くなる。一方、水溶性樹脂の量を、好ましくは20質量部以下、さらに好ましくは15質量部以下とすることにより、インクの吸収性が良好となる。   The amount of the water-soluble resin is preferably 3.3 to 20 parts by mass with respect to 100 parts by mass of the inorganic fine particles. When the amount of the water-soluble resin is preferably 3.3 parts by mass or more, more preferably 5 parts by mass or more, the colorant receiving layer is less likely to crack or fall off. On the other hand, when the amount of the water-soluble resin is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, the ink absorbability is improved.

[1−1−3]カチオン性樹脂
カチオン性樹脂は、分子中にカチオン性の原子団(例えば、4級アンモニウム等)を有する樹脂である。また、カチオン性樹脂のSP値は、画像支持体を構成する樹脂のSP値と近い値を示すだけでなく、画像支持体に転写材を加熱圧着させる際の熱で容易に溶融し、また、静電気的な結合も促進するため、画像支持体と色材受容層との接着性を更に強固なものとし、画像支持体と色材受容層との密着性(転写性能)を向上させることができる。すなわち、カチオン性樹脂は一般的にマイナスに帯電しているインクと静電気的に結合するため、色材受容層中にインクを定着させることができるが、この機能に加え、カチオン性樹脂は、(1)画像支持体のSP値に近い値となるようなものを選択しているため、画像支持体と親和性が高く、転写時の画像支持体と色材受容層との接着性を向上させることができる。また、カチオン性樹脂は、(2)融点が低く、転写時の熱で容易に溶融するので、画像支持体と色材受容層との接着性をさらに強くする。さらに、本発明で使用するカチオン性樹脂は、(3)分子量が小さいため、色材受容層への添加量が少なくても、色材受容層中に多くの分子を添加できる。よって、一般的にマイナスに帯電している画像支持体と静電気的に結合できるカチオン基を、色材受容層の表面に介在させることができ、結果として、画像支持体と接着性を向上させることができる。さらに(4)後述する樹脂分散顔料との接着性を高めることができる。すなわち、樹脂分散顔料の分散樹脂のSP値は、カチオン性樹脂のSP値と近いため、転写時の熱でカチオン性樹脂および分散樹脂が溶融すると両者の相溶性が高まり、樹脂分散顔料は色材受容層に強固に接着される。これにより、色材受容層の画像支持体への転写性能が向上する。さらに(5)透明シートの主成分として用いられるエマルションはマイナスに帯電しており、カチオン性樹脂と強固に接着し、透明シートと色材受容層との接着性を高めることができる。したがって、本発明で使用するカチオン性樹脂は、上記5つの効果により、色材受容層の画像支持体への転写性能を高める役目を果たしている。
[1-1-3] Cationic resin The cationic resin is a resin having a cationic atomic group (for example, quaternary ammonium or the like) in the molecule. Further, the SP value of the cationic resin not only shows a value close to the SP value of the resin constituting the image support, but is easily melted by heat when the transfer material is thermocompression bonded to the image support. Since electrostatic bonding is also promoted, the adhesion between the image support and the colorant receiving layer can be further strengthened, and the adhesion (transfer performance) between the image support and the colorant receiving layer can be improved. . That is, since the cationic resin generally binds electrostatically with negatively charged ink, the ink can be fixed in the colorant receiving layer. In addition to this function, the cationic resin is ( 1) Since a value close to the SP value of the image support is selected, the affinity to the image support is high, and the adhesion between the image support and the colorant receiving layer during transfer is improved. be able to. In addition, the cationic resin (2) has a low melting point and is easily melted by heat at the time of transfer, thereby further strengthening the adhesion between the image support and the colorant receiving layer. Furthermore, since the cationic resin used in the present invention has a small molecular weight, (3) even if the addition amount to the color material receiving layer is small, many molecules can be added to the color material receiving layer. Therefore, a cationic group that can be electrostatically bonded to a negatively charged image support in general can be interposed on the surface of the colorant receiving layer, and as a result, the adhesion to the image support can be improved. Can do. Furthermore, (4) Adhesiveness with a resin-dispersed pigment described later can be enhanced. That is, since the SP value of the dispersed resin of the resin dispersed pigment is close to the SP value of the cationic resin, when the cationic resin and the dispersed resin are melted by the heat during transfer, the compatibility between the two increases. It is firmly bonded to the receiving layer. Thereby, the transfer performance of the color material receiving layer to the image support is improved. Furthermore, (5) the emulsion used as the main component of the transparent sheet is negatively charged, and can firmly adhere to the cationic resin, thereby enhancing the adhesion between the transparent sheet and the colorant receiving layer. Therefore, the cationic resin used in the present invention plays the role of enhancing the transfer performance of the color material receiving layer to the image support due to the above five effects.

このようなカチオン性樹脂としては、例えばポリアリルアミン(例えば、アリルアミン系重合物、ジアリルアミン系重合物等)及びウレタン系重合物から選択される少なくとも1種の重合物を用いることが好ましい。これらの中でも、特に後述する低分子のポリアリルアミンは、(1)融点が80℃付近と低く、画像支持体に転写材を加熱圧着させる際に容易に溶融すること、(2)分子構造が小さいために、色材受容層表面において単位面積当たりのカチオン基を多く存在させることができ、画像支持体に対する静電気的な結合を促進することができること、等の理由から、特に好ましく用いることができる。   As such a cationic resin, it is preferable to use at least one polymer selected from, for example, polyallylamine (for example, allylamine polymer, diallylamine polymer, etc.) and urethane polymer. Among these, the low-molecular polyallylamine described below particularly has (1) a melting point as low as about 80 ° C., and is easily melted when a transfer material is heat-pressed on an image support, and (2) a molecular structure is small. Therefore, a large amount of cationic groups per unit area can be present on the surface of the colorant receiving layer, and electrostatic bonding to the image support can be promoted.

なお、ポリアリルアミンは、下記一般式(8)で示される少なくとも1種のポリアリルアミンであることが好ましい。   The polyallylamine is preferably at least one polyallylamine represented by the following general formula (8).

(式中、R3、R4、R5は、水素原子、置換基を有してもよいアルキル基、アルケニル基、アルカノール基、アリルアルキル基、アリルアルケニル基を示す。また、R3、R4、R5はそれぞれ同一であっても異なっていてもよい。X-は、無機系、有機系の陰イオンを示す。nは重合度を示す整数である。) (Wherein R 3 , R 4 and R 5 represent a hydrogen atom, an alkyl group which may have a substituent, an alkenyl group, an alkanol group, an allylalkyl group or an allylalkenyl group. Also, R 3 , R 4 and R 5 may be the same or different from each other, X represents an inorganic or organic anion, and n is an integer indicating the degree of polymerization.

カチオン性樹脂の重量平均分子量は、好ましくは1,000〜15,000、さらに好ましくは1,000〜10,000、特に好ましくは1,000〜5,000である。重量平均分子量を範囲内とすることで塗工液の安定性を向上させることができることに加えて、色材受容層の空隙が減少し難く、色材の吸収性を維持することができる。さらに、カチオン性樹脂の分子量5,000以下とすると、画像支持体と接する色材受容層の表面にカチオン基(則ち、静電気的な結合を行う吸着サイト)をより多く分布させて、画像支持体と色材受容層との密着性(転写性能)をさらに向上させることができる。なお、平均分子量が15000より大きくなると画像支持体と接する色材受容層の表面にカチオン基(則ち、静電気的な結合を行う吸着サイト)が少なくなるため、色材受容層との密着性(転写性能)が低下する。一方、重量平均分子量が1000より小さいと、印刷時のインク溶媒とともに色材受容層内部にカチオン性樹脂が移動してしまい色材受容層の表面に分布するカチオン基の量が少なくなるため、好ましくない   The weight average molecular weight of the cationic resin is preferably 1,000 to 15,000, more preferably 1,000 to 10,000, and particularly preferably 1,000 to 5,000. By making the weight average molecular weight within the range, the stability of the coating liquid can be improved, and the voids of the colorant receiving layer are hardly reduced, and the colorant absorbability can be maintained. Further, when the molecular weight of the cationic resin is 5,000 or less, more cationic groups (that is, adsorption sites that perform electrostatic bonding) are more distributed on the surface of the colorant receiving layer in contact with the image support to support the image. The adhesion (transfer performance) between the body and the colorant receiving layer can be further improved. When the average molecular weight is larger than 15000, the surface of the color material receiving layer in contact with the image support has fewer cationic groups (that is, adsorption sites that perform electrostatic bonding), and thus the adhesion to the color material receiving layer ( Transfer performance) decreases. On the other hand, when the weight average molecular weight is less than 1000, the cationic resin moves inside the color material receiving layer together with the ink solvent at the time of printing, and the amount of cationic groups distributed on the surface of the color material receiving layer is reduced. Absent

カチオン性樹脂の使用量は無機微粒子(アルミナ水和物等)に対して0.01〜5質量%とすることが好ましく、0.01〜3質量%とすることがさらに好ましい。カチオン性樹脂の使用量が上述の範囲を超えると、無機微粒子の分散液や分散液にバインダーを添加した塗工液の粘度が高くなり、分散液又は塗工液の保存性や塗工性が低下する場合がある。   The amount of the cationic resin used is preferably 0.01 to 5% by mass and more preferably 0.01 to 3% by mass with respect to the inorganic fine particles (alumina hydrate or the like). When the amount of the cationic resin used exceeds the above range, the dispersion of the inorganic fine particles and the viscosity of the coating liquid obtained by adding a binder to the dispersion liquid become high, and the storage stability and coating property of the dispersion liquid or the coating liquid are increased. May decrease.

カチオン性樹脂の融点は、60〜160℃であることが好ましい。カチオン性樹脂の融点を上述の範囲内とすることにより、画像支持体に対して転写材を加熱圧着させる際にカチオン性樹脂を溶融させることができ、画像支持体と色材受容層との接着性(転写性能)を向上させることができる。   The melting point of the cationic resin is preferably 60 to 160 ° C. By setting the melting point of the cationic resin within the above-mentioned range, the cationic resin can be melted when the transfer material is thermocompression-bonded to the image support, and the adhesion between the image support and the colorant receiving layer can be achieved. (Transfer performance) can be improved.

[1−1−4]厚さ
色材受容層の厚さとしては特に制限はないが、インク吸収性の観点からは厚いほうが良い。一方、本発明の記録物では、インクジェット記録面とは反対側の透明シート側から画像情報を見ることになるので、色材受容層自体の透明性も考慮する必要がある。インクジェット記録の液滴径にも拠るが、インクの吸収性と加熱圧着転写性との兼ね合いと、水分吸収時の膨張収縮性の観点から、色材受容層の厚さは40μm以下であることが好ましい。さらに好ましくは30μ以下とすることにより、色材受容層の透明性を一段と向上させることができるとともに、画像支持体に加熱圧着転写させる際にも熱伝導をより良好にして、画像支持体と色材受容層との密着性(転写性能)をより向上させることができる。さらに、吸水時の色材受容層の膨張収縮による応力も小さくすることが可能となる。
[1-1-4] Thickness The thickness of the colorant receiving layer is not particularly limited, but it is preferably thick from the viewpoint of ink absorbability. On the other hand, in the recorded matter of the present invention, since the image information is viewed from the transparent sheet side opposite to the ink jet recording surface, it is necessary to consider the transparency of the colorant receiving layer itself. Although depending on the droplet diameter of inkjet recording, the thickness of the colorant receiving layer may be 40 μm or less from the viewpoint of the balance between ink absorbability and thermocompression transferability and expansion / contraction properties during moisture absorption. preferable. More preferably, by setting the thickness to 30 μm or less, the transparency of the colorant-receiving layer can be further improved, and the heat conduction is further improved when transferring the image to the image support by thermocompression bonding. The adhesion (transfer performance) with the material receiving layer can be further improved. Furthermore, it is possible to reduce the stress due to expansion and contraction of the colorant receiving layer during water absorption.

一方、インクジェット記録におけるインクの液滴径によっては、色材受容層の厚さが2μm以上であれば良好な画像記録ができる場合がある。さらに好ましくは、色材受容層の厚さを5μm以上とすることでインクの吸収性を安定的に確保することができ、インクの吸収速度及びインクの定着性が良好となる。すなわち、色材受容層の厚さは、5〜30μmであることがより好ましい。本発明では、透明シート及び色材受容層の厚さのバランスに加えて、細孔の構成も用途に応じて適宜選定する必要がある。また、画像支持体としてプラスチックカードを用いた場合、記録物全体の厚さは、JIS6301に記載される総厚さ0.84mm以下に抑制することが必要となる。この場合、色材受容層を良好なインクジェット記録を可能とする最小限の厚みとすることは、実用上のバランス設計の観点から好ましい。   On the other hand, depending on the ink droplet diameter in inkjet recording, good image recording may be possible if the thickness of the colorant receiving layer is 2 μm or more. More preferably, when the thickness of the colorant receiving layer is 5 μm or more, the ink absorbability can be stably secured, and the ink absorption speed and the ink fixability are improved. That is, the thickness of the color material receiving layer is more preferably 5 to 30 μm. In the present invention, in addition to the balance of the thickness of the transparent sheet and the colorant receiving layer, the structure of the pores needs to be appropriately selected according to the application. Further, when a plastic card is used as the image support, it is necessary to suppress the thickness of the entire recorded matter to a total thickness of 0.84 mm or less described in JIS6301. In this case, it is preferable from the viewpoint of practical balance design that the colorant receiving layer has a minimum thickness that enables good ink jet recording.

[1−2]透明シート
転写材1は、図22のように透明シート52を備えており、透明シート52が色材受容層内の水分を外部に放出可能な通路を含むことを特徴としている。具体的には、透明シート52は、前述したように基材シート50と色材受容層53との間を貫通する細孔52Aを有している。また、図1(b)のように透明シート52に予め細孔52Aが形成されていない転写材1を用いる場合には、工程1〜3のいずれかの工程の前後に、転写材1の少なくとも透明シート52に細孔52Aが形成される。
[1-2] Transparent Sheet The transfer material 1 includes a transparent sheet 52 as shown in FIG. 22, and the transparent sheet 52 includes a passage that can release moisture in the color material receiving layer to the outside. . Specifically, the transparent sheet 52 has pores 52 </ b> A penetrating between the base material sheet 50 and the color material receiving layer 53 as described above. Further, when using the transfer material 1 in which the pores 52A are not formed in advance in the transparent sheet 52 as shown in FIG. 1B, at least before the transfer material 1 before and after any of the steps 1 to 3. The pore 52A is formed in the transparent sheet 52.

細孔は、透明シートが水分透過性もしくは透湿性を発現できるように構成される。すなわち透明シートには、それに接触した水を液体の状態もしくは気体の状態で通過させる性質を持たせる。そのため本発明の記録物においては、図34(b)のように、色材受容装置53に多量の水分を吸水させた後に乾燥させた耐水性試験においても、透明シート52の全表面から水分が蒸発放散されて、ひび割れの発生が抑えられる。   The pores are configured so that the transparent sheet can exhibit moisture permeability or moisture permeability. That is, the transparent sheet has a property of allowing water in contact therewith to pass through in a liquid state or a gas state. Therefore, in the recorded matter of the present invention, as shown in FIG. 34 (b), even in a water resistance test in which a large amount of moisture is absorbed by the color material receiving device 53 and dried, moisture is absorbed from the entire surface of the transparent sheet 52. Evaporation is released and cracking is suppressed.

このように透明シートは水分透過性であり、色材受容層の水吸収および蒸発に起因するひび割れの発生を効果的に抑制する。記録物の作成後、色材受容層にまで貫通する細孔を有する水分透過性の透明シートは、図34(b)のように、水蒸気550を通すことができると共に、液体状の水551も通すことができ。したがって、色材受容層が吸水した水分の、透明シートの全表面からの蒸発が促進される。   Thus, the transparent sheet is permeable to moisture, and effectively suppresses the occurrence of cracks due to water absorption and evaporation of the colorant receiving layer. After creation of the recorded material, the moisture-permeable transparent sheet having pores that penetrate to the colorant receiving layer can pass water vapor 550 as shown in FIG. Can pass through. Therefore, the evaporation of the water absorbed by the color material receiving layer from the entire surface of the transparent sheet is promoted.

[1−2−1]細孔の大きさ
記録物を水に浸漬させたときに、透明シートの細孔の内部に存在する空気によって、細孔の入り口に水のメニスカスを形成することにより、透明シートの表面からの水の吸収を抑えることができる。そのためには、細孔の大きさは100μm以下とすることが好ましい。さらに、色材受容層に多量の水分が吸収されている場合には、色材受容層と接する側の細孔の入り口では水のメニスカスが形成されにくい。したがって細孔の径が小さくすることにより、それを毛細管として作用させて、色材受容層中の水分を透明シートの細孔を介して透明シート表層に輸送して、その蒸発が促進することができる。
[1-2-1] Size of pores When a recorded material is immersed in water, air present inside the pores of the transparent sheet forms a meniscus of water at the entrance of the pores. Absorption of water from the surface of the transparent sheet can be suppressed. For this purpose, the pore size is preferably 100 μm or less. Further, when a large amount of water is absorbed in the color material receiving layer, a meniscus of water is hardly formed at the entrance of the pores in contact with the color material receiving layer. Therefore, by reducing the diameter of the pores, it can act as a capillary tube, transporting moisture in the colorant receiving layer to the surface of the transparent sheet through the pores of the transparent sheet, thereby promoting its evaporation. it can.

色材受容層の厚みに対して、透明シートの厚みが十分に大きい場合には、透明シートの細孔の大きさを100〜300μmの範囲に設定することにより、ある程度の水分を透過させることができて、ひび割れの発生が防止できる。すなわち透明シートは、色材受容層の厚みに対して十分に厚ければ十分な強度を持ち、吸水膨張および乾燥収縮の応力を吸収することができるため、透明シートの水透過性および透湿性が低くてもひび割れは起こりにくい。しかしながら、透明シートの厚みが色材受容層の厚みに対して著しく薄くい場合には、透明シートの強度が相対的に低くなり、色材受容層の収縮が相対的に大きくなって、透明シートのひび割れが起こりやすくなる。この場合には、透明シートの水透過性および透湿性を高くしなければならない。例えば、100μm以下の細孔を高密度に配置することにより、単位面積当たりの水透過性および透湿性を高めて、ひび割れを防ぐことができる。一方、細孔の大きさが300μmを超えた場合には、ひび割れの防止効果がさらに大きくなることが期待できるものの、記録物を水に浸漬させた場合に、細孔の入り口において水のメニスカスが形成され難くなる。この場合には、透明シートを介しての、色材転写層の吸水が促進される一方に、液体状の汚れなどが侵入しやすくなる。したがって細孔の大きさは、用途に応じて好ましい範囲に選択する必要がある。   When the thickness of the transparent sheet is sufficiently large relative to the thickness of the colorant receiving layer, a certain amount of moisture can be transmitted by setting the pore size of the transparent sheet in the range of 100 to 300 μm. It can prevent the occurrence of cracks. That is, since the transparent sheet has sufficient strength if it is sufficiently thick relative to the thickness of the colorant receiving layer and can absorb the stress of water absorption expansion and drying shrinkage, the transparent sheet has water permeability and moisture permeability. Even if it is low, cracks are unlikely to occur. However, when the thickness of the transparent sheet is remarkably thin relative to the thickness of the color material receiving layer, the strength of the transparent sheet is relatively low, and the shrinkage of the color material receiving layer is relatively large. Cracks tend to occur. In this case, the water permeability and moisture permeability of the transparent sheet must be increased. For example, by arranging fine pores of 100 μm or less at a high density, water permeability and moisture permeability per unit area can be improved and cracking can be prevented. On the other hand, when the pore size exceeds 300 μm, the effect of preventing cracking can be expected to be further increased. However, when the recorded material is immersed in water, the meniscus of water at the entrance of the pore It becomes difficult to form. In this case, water absorption of the color material transfer layer through the transparent sheet is promoted, but liquid stains and the like easily enter. Therefore, the size of the pores needs to be selected in a preferable range depending on the application.

[1−2−2]厚さ
透明シートの厚さは特に制限されない。透明シートの細孔の効果に加えて、色材受容層の厚みに関連して透明シートの厚みを設定することにより、耐水性をより向上させることができる。すなわち、上述したように透明シートは、その厚みが色材受容層の厚みに対して十分に大きければ十分な強度を持つため、水透過性および透湿性は少なくてもひび割れは起こりにくい。しかしながら、透明シートの厚みが色材受容層の厚みに対して小さい場合には、透明シートの強度が相対的に小さくなってひび割れが起こりやすくなるため、透明シートの透湿性および水透過性を高めなければならない。透明シートの水透過性および透湿性は、上述したように細孔の平均径、および細孔の密度によって制御できる。透明シートの厚み(A)と色材受容層の厚み(B)の比率(A/B)は、下式(1A)の範囲であることが好ましい。
0.07≦A/B≦3.00 (1)
[1-2-2] Thickness The thickness of the transparent sheet is not particularly limited. In addition to the effect of the pores of the transparent sheet, the water resistance can be further improved by setting the thickness of the transparent sheet in relation to the thickness of the colorant receiving layer. That is, as described above, since the transparent sheet has sufficient strength if the thickness thereof is sufficiently larger than the thickness of the colorant receiving layer, even if the water permeability and moisture permeability are small, cracks are unlikely to occur. However, when the thickness of the transparent sheet is smaller than the thickness of the colorant receiving layer, the strength of the transparent sheet becomes relatively small and cracking is likely to occur, so that the moisture permeability and water permeability of the transparent sheet are increased. There must be. As described above, the water permeability and moisture permeability of the transparent sheet can be controlled by the average diameter of the pores and the density of the pores. The ratio (A / B) between the thickness (A) of the transparent sheet and the thickness (B) of the colorant receiving layer is preferably in the range of the following formula (1A).
0.07 ≦ A / B ≦ 3.00 (1)

比率(A/B)が大きければ、透明シートは、十分な強度を持って収縮の応力を吸収することができるため、透明シートの水透過性および透湿性が低くてもひび割れは起こりにくい。記録物の利用目的によっては、画像の長期保存性や耐候性、あるいはセキュリティー性の観点から、保護層である透明シートの厚みを数十μm以上にする必要がある場合も生じる。この場合には、記録物の画像支持体と転写材の色材受容層との間の接着力、および色材受容層と透明シートとの間の接着力を考慮し、水溶性樹脂を含む色材受容層の吸水膨張および乾燥収縮に程度に応じて、透明シートに細孔を設けて応力を緩和する。例えば、透明シートが厚い場合には、細孔の径を小さくしたり、細孔の分布密度を小さくする。一方、比率(A/B)が小さければ、透明シートの厚みが色材受容層の厚みに対して薄くなって透明シートのひび割れは起こりやすくなるため、透明シートの水透過性および透湿性を高める。   If the ratio (A / B) is large, the transparent sheet has sufficient strength and can absorb the stress of shrinkage. Therefore, even if the water permeability and moisture permeability of the transparent sheet are low, cracking hardly occurs. Depending on the purpose of use of the recorded matter, the thickness of the transparent sheet as the protective layer may need to be several tens of μm or more from the viewpoint of long-term storage stability, weather resistance, and security. In this case, in consideration of the adhesive force between the image support of the recorded material and the color material receiving layer of the transfer material and the adhesive force between the color material receiving layer and the transparent sheet, a color containing a water-soluble resin is used. Depending on the degree of water absorption expansion and drying shrinkage of the material receiving layer, pores are provided in the transparent sheet to relieve stress. For example, when the transparent sheet is thick, the pore diameter is reduced or the pore distribution density is reduced. On the other hand, if the ratio (A / B) is small, the thickness of the transparent sheet becomes thinner than the thickness of the colorant receiving layer, and cracking of the transparent sheet is likely to occur, so that the water permeability and moisture permeability of the transparent sheet are increased. .

透明シートの厚さは、実用的には、1〜40μmであることが好ましい。透明シートの厚さを5μm以上とすることにより、透明シートの耐水性や耐擦過性をさらに向上させることができる。一方、透明シートの厚みが厚くなり過ぎると、画像支持体へ透明シートと色材受容層を加熱圧着する際の熱伝達に、大きなエネルギーが必要となる。また、浸漬耐水試験後の乾燥において、透明シートの細孔を介した色材受容層からの水分の蒸発が進み難くなるため、40μm以下の厚さとすることが望ましい。さらに好ましくは、透明シートの厚さを20μ以下とすることにより、透明シートとしての基本機能である透明性および保護機能に加えて、加熱圧着時のエネルギー、および水分透過性などの付随的な機能とのバランスも得られやすくなる。   Practically, the thickness of the transparent sheet is preferably 1 to 40 μm. By setting the thickness of the transparent sheet to 5 μm or more, the water resistance and scratch resistance of the transparent sheet can be further improved. On the other hand, if the thickness of the transparent sheet becomes too thick, a large amount of energy is required for heat transfer when the transparent sheet and the colorant receiving layer are thermocompression bonded to the image support. Further, in the drying after the immersion water resistance test, it is difficult for the water from evaporating from the colorant receiving layer through the pores of the transparent sheet, so that the thickness is preferably 40 μm or less. More preferably, by setting the thickness of the transparent sheet to 20 μm or less, in addition to the transparency and protection functions that are the basic functions of the transparent sheet, additional functions such as energy during thermocompression bonding and moisture permeability are provided. It becomes easy to obtain a balance.

[1−2−3]細孔の分布密度
透明シートの細孔の分布密度については特に制限されないが、1cm2当たり5個〜200万個が好ましい。それを1cm2当たり5個以上とすることにより、透明シートの表面から、応力分散にほぼ必要な量の水を蒸発させることができる。また、それを200万個以下にすることにより、透明シートの強度と透明性を保つことができる。
[1-2-3] Pore Distribution Density The pore distribution density of the transparent sheet is not particularly limited, but is preferably 5 to 2 million per 1 cm 2 . By setting it to 5 or more per 1 cm 2, it is possible to evaporate an amount of water almost necessary for stress dispersion from the surface of the transparent sheet. Moreover, the intensity | strength and transparency of a transparent sheet can be maintained by making it 2 million or less.

透明シートにおける細孔の平均径のみならず、その分布密度によっても透湿の度合いを制御して、ひび割れをより抑制することができる。本発明者の検討によれば、透明シートに細孔構造がなくて、その端部からの吸水成分が蒸発するだけではひび割れが発生した。一方、透明シートの全面に亘って5mm間隔で細孔を設けた場合には、乾燥後の透明シートの表面に筋状の微かなシワ跡が見られる程度であり、ひび割れは発生しなかった。透明シートの全面に亘って2mm間隔で細孔を設けた場合には、乾燥後の透明シートの表面には微かなシワ跡すらも発現せず、記録物の耐水性が確保できた。   The degree of moisture permeation can be controlled not only by the average diameter of the pores in the transparent sheet but also by the distribution density, and cracks can be further suppressed. According to the study of the present inventor, the transparent sheet does not have a pore structure, and cracking occurs only by evaporating the water absorption component from the end portion. On the other hand, when pores were provided at intervals of 5 mm over the entire surface of the transparent sheet, fine streaks of streaks were observed on the surface of the dried transparent sheet, and no cracks were generated. When pores were provided at intervals of 2 mm over the entire surface of the transparent sheet, even fine wrinkle marks did not appear on the surface of the transparent sheet after drying, and the water resistance of the recorded material was ensured.

すなわち、20μm厚程度の空隙吸収型の色材転写層に、保護層としてとして10μm厚程度の透明シートを設けた構成において、4平方mm当たり1つ以上の細孔を設けるように透明シートの細孔の分布密度を設定することにより、ひび割れが防止できた。また、通常の環境下であれば、転写材は、吸水した水分が30分程度で蒸発して乾燥されるため、透明シートの透湿度が5g/m2・h以上であれば、耐水性をより向上させることができる。すなわち、透明シートの透湿度を上記の値以上に設定することにより、吸水後の色材受容層が収縮するときの応力がより広く分散されて、ひび割れをより防止することができる。 That is, in a configuration in which a transparent sheet having a thickness of about 10 μm is provided as a protective layer on a gap absorption type color material transfer layer having a thickness of about 20 μm, the fineness of the transparent sheet is provided so as to provide one or more pores per 4 mm 2. Cracks could be prevented by setting the distribution density of the holes. In addition, under normal circumstances, the transferred material evaporates and dries the absorbed water in about 30 minutes. Therefore, if the water vapor transmission rate of the transparent sheet is 5 g / m 2 · h or more, the transfer material has water resistance. It can be improved further. That is, by setting the water vapor transmission rate of the transparent sheet to the above value or more, the stress when the colorant receiving layer after water absorption contracts is more widely dispersed, and cracking can be further prevented.

[1−2−3−2]細孔の面積
透明シート表面の全細孔面積については、特に制限されない。端部の色材受容層の全面積(D)に対する透明シート表面の全細孔面積(C)の割合(C/D)は、すなわち色材受容層端部からの蒸発と透明シート表面からの蒸発の比率を表すものである。透明シート表面の全細孔面積はC/Dが好ましくは0.02〜50倍、より好ましくは0.1〜10倍、さらにより好ましくは0.2〜5倍であるように制御することが好ましい。C/Dが好ましくは0.02倍以上、より好ましくは0.1倍以上、さらにより好ましくは0.2倍以上とすることで、透明シート表面からの水分蒸発の割合を増やし、端部からの蒸発による応力集中を抑えて、ひび割れを防止することができる。また、C/Dが好ましくは、50倍以下、より好ましくは10倍以下、さらにより好ましくは5倍以下とすることで、透明シートの強度低下を抑えて、耐擦過性を向上することができる。一方、0.02倍以下になると端部からの蒸発の割合が多くなり、応力が十分に分散されず、ひび割れが発生する場合がある。さらに、50倍以上になると透明シートの強度が低下し、耐擦過性が低下する場合がある。
[1-2-3-2] Area of pores The total pore area on the surface of the transparent sheet is not particularly limited. The ratio (C / D) of the total pore area (C) of the transparent sheet surface to the total area (D) of the color material receiving layer at the edge, ie, evaporation from the edge of the color material receiving layer and from the transparent sheet surface It represents the rate of evaporation. The total pore area of the transparent sheet surface may be controlled so that C / D is preferably 0.02 to 50 times, more preferably 0.1 to 10 times, and even more preferably 0.2 to 5 times. preferable. C / D is preferably 0.02 times or more, more preferably 0.1 times or more, and even more preferably 0.2 times or more, thereby increasing the rate of moisture evaporation from the transparent sheet surface, It is possible to prevent cracking by suppressing the stress concentration due to evaporation of the. Further, the C / D is preferably 50 times or less, more preferably 10 times or less, and even more preferably 5 times or less, thereby suppressing a decrease in strength of the transparent sheet and improving scratch resistance. . On the other hand, if it becomes 0.02 times or less, the rate of evaporation from the end portion increases, the stress is not sufficiently dispersed, and cracks may occur. Furthermore, when it becomes 50 times or more, the strength of the transparent sheet is lowered, and the scratch resistance may be lowered.

透明シートの表面に汚染水などの液体状の汚れが付着した場合は、図35(a)のように、透明シート52の細孔52Aを透過して、汚染水552が色材受容層53に接触して吸収されるおそれがある。この場合には、反転画像72によって記録された情報の一部が背景側から汚染水552によって着色されて、その情報の一部が消えてしまうおそれがある。透明シートは、記録物の保護を目的として記録物の表面に構成されており、その保護性能は、下記の(1)から(4)の4つに大きく分けることができる。(1)は、水、薬品、汚染水など液体状の汚れからの保護性能、(2)は、オゾンや汚染ガスなど気体状の汚れからの保護性能、(3)は、紫外光などの光学的劣化に対する保護性能、(4)は、擦れ、引っ掻き、打坤などの機械的な力からの保護性能である。保護性能(2),(3),(4)については、透明シートの細孔によって大きく変化することはない。しかし、透明シートの細孔が水分透過性であった場合には、(1)の液体汚れからの保護性能についてはやや低下するおそれがある。   When liquid dirt such as contaminated water adheres to the surface of the transparent sheet, the contaminated water 552 passes through the pores 52A of the transparent sheet 52 as shown in FIG. May be absorbed by contact. In this case, a part of the information recorded by the reverse image 72 may be colored by the contaminated water 552 from the background side, and a part of the information may disappear. The transparent sheet is formed on the surface of the recorded material for the purpose of protecting the recorded material, and the protection performance can be roughly divided into the following four (1) to (4). (1) Protection performance against liquid dirt such as water, chemicals, and contaminated water, (2) Protection performance against gaseous dirt such as ozone and polluted gas, and (3) Optical such as ultraviolet light (4) is a protection performance against mechanical forces such as rubbing, scratching and hammering. About protection performance (2), (3), (4), it does not change a lot by the pore of a transparent sheet. However, when the pores of the transparent sheet are permeable to moisture, the protection performance from (1) liquid stains may be slightly reduced.

好ましくは、図35(b)のように、透明シート52の細孔52Aに透湿性を持たせ、かつ、水分難透過性を持たせるように構成する。これにより透明シート52は、水蒸気550は通すものの、液体状の水、薬品、液体汚れ(汚染水552)などは通し難くなる。したがって、万一、汚染水552が透明シート52の表面に付着しても、それは色材受容層53までは到達せず、記録情報が液体汚れから保護され、また透明シートの本来の保護機能が損なわれるおそれもない。さらに、透明シート52は細孔52Aの透湿性によって水蒸気を通すため、万一、色材受容層53が多量の水分を吸収した後に乾燥される過程においても、透明シート52の全面に色材受容層53の収縮の応力を分散させて、ひび割れの発生を抑制することができる。このように、透明シートの細孔に水分難透過性を持たせることにより、透明シートの表面からの水、薬品、汚染水などの液体状の汚れの進入を防いで透明シートの本来の保護性能を維持し、かつ細孔に透湿性を持たせることによりひび割れを抑制することができる。   Preferably, as shown in FIG. 35B, the pores 52A of the transparent sheet 52 are configured to have moisture permeability and moisture permeability. Thereby, although the water vapor | steam 550 lets the transparent sheet 52 pass, it becomes difficult to let liquid water, a chemical | medical agent, liquid dirt (contaminated water 552), etc. pass. Therefore, even if the contaminated water 552 adheres to the surface of the transparent sheet 52, it does not reach the color material receiving layer 53, the recorded information is protected from liquid stains, and the original protective function of the transparent sheet is There is no risk of damage. Furthermore, since the transparent sheet 52 allows water vapor to pass therethrough due to the moisture permeability of the pores 52A, even if the color material receiving layer 53 is dried after absorbing a large amount of water, the color material is received on the entire surface of the transparent sheet 52. The stress of the shrinkage of the layer 53 can be dispersed to suppress the occurrence of cracks. In this way, by providing moisture permeability to the pores of the transparent sheet, the original protective performance of the transparent sheet is prevented by preventing the entry of liquid dirt such as water, chemicals, and contaminated water from the surface of the transparent sheet. It is possible to suppress cracking by keeping the pores and providing the pores with moisture permeability.

細孔を持つ透明シートの透湿性および水分透過性は、主として細孔の平均径によって制御される。透明シートの細孔の平均径を0.001〜0.8000μmにすることにより、色材受容層への液体汚れに対する保護性能を損なうことなく、透明シートのひび割れを防止することができる。水滴の大きさは約100μm程度であり、また数10μm径程度の細孔は、通常、その先端において水の表面張力によるメニスカスが形成されるため、水分は透過し難にくくなる。しかし、圧力の作用、細孔の内面の濡れ性、および毛管力などの条件により、1μm径程度の細孔でも水分が透過する場合がある。そのため、細孔の平均径を0.8000μm以下とすることにより、十分な水分難透過性を確保して、ほぼ液体状の水分の透過を抑制することが可能となる。また、温度湿度気圧などの環境条件、および水に含まれる不純物や溶解成分などによる粘度や表面張力に応じて、水分の透過し易さが変化するため、細孔の平均径を0.2000μm以下とすることにより、実用上十分な水分難透過性を得ることができる。一方、水蒸気の水分子の大きさからして、細孔の平均径を0.0004μm以上にすれば水蒸気を透過させることができ、その平均径を0.001μm以上とすることにより十分に実用性のある透湿性を得ることができる。より好ましくは、細孔構造の均一性を考慮して、細孔の平均径を0.002μm以上とすることにより安定的に水蒸気を透過させることができる。   The moisture permeability and moisture permeability of the transparent sheet having pores are mainly controlled by the average diameter of the pores. By setting the average diameter of the pores of the transparent sheet to 0.001 to 0.8000 μm, it is possible to prevent cracking of the transparent sheet without impairing the protection performance against liquid stains on the colorant receiving layer. The size of the water droplet is about 100 μm, and a pore having a diameter of about several tens of μm usually forms a meniscus due to the surface tension of water at the tip, so that it is difficult for moisture to permeate. However, depending on conditions such as the action of pressure, wettability of the inner surface of the pores, and capillary force, moisture may permeate through pores having a diameter of about 1 μm. Therefore, by setting the average diameter of the pores to 0.8000 μm or less, it is possible to ensure sufficient moisture permeability and suppress the transmission of substantially liquid moisture. In addition, since the ease of moisture permeation changes depending on environmental conditions such as temperature, humidity and pressure, and viscosity and surface tension due to impurities and dissolved components contained in water, the average diameter of the pores is 0.2000 μm or less. As a result, practically sufficient moisture permeability can be obtained. On the other hand, considering the water molecule size of the water vapor, if the average diameter of the pores is 0.0004 μm or more, water vapor can be transmitted, and if the average diameter is 0.001 μm or more, it is sufficiently practical. A certain moisture permeability can be obtained. More preferably, in consideration of the uniformity of the pore structure, water vapor can be stably transmitted by setting the average diameter of the pores to 0.002 μm or more.

したがって、透明シートの細孔の平均径を0.002〜0.2000μmとすることにより、透明シートのひび割れを十分に抑制しつつ、水分透過性を十分抑えて、表面汚れの保護性能を実使用上問題ないレベルにまで高めることができる。しかし、液体状の汚れは色材受容層の端部から侵入する可能性がある。しかし、汚染水の成分の各々の転写材中における浸透拡散度合いの違いから、汚れ成分自体が浸透する範囲は端部から数mmにも及ばない。しかも、記録物の搬送精度など機械的な制約の観点から、記録部の端部に対する情報の記録は稀有であるため、実使用上、液体状の汚れによる情報の消失には至らない。   Therefore, by setting the average diameter of the pores of the transparent sheet to 0.002 to 0.2000 μm, the moisture permeability is sufficiently suppressed while the cracks of the transparent sheet are sufficiently suppressed, and the surface dirt protection performance is actually used. It can be raised to a level where there is no problem. However, liquid stains may enter from the end of the colorant receiving layer. However, due to the difference in the degree of permeation and diffusion of the contaminated water component in each transfer material, the range in which the contaminated component permeates does not reach several mm from the end. In addition, from the viewpoint of mechanical restrictions such as the conveyance accuracy of the recorded matter, recording of information on the end portion of the recording unit is rare, and therefore, in actual use, information is not lost due to liquid contamination.

[1−2−4]エマルジョン
本例の透明シート52は、異なるガラス転移温度を有する2種類のエマルジョン(エマルジョンE1、エマルジョンE2)を含有する。以下、エマルジョンE1とE2についてさらに詳細に説明する。
[1-2-4] Emulsion The transparent sheet 52 of this example contains two types of emulsions (emulsion E1 and emulsion E2) having different glass transition temperatures. Hereinafter, the emulsions E1 and E2 will be described in more detail.

[1−2−4−1]エマルジョンの状態
エマルジョンE1が造膜し、少なくともエマルジョンE2が粒子として残存している状態であることが好ましい。エマルジョンの「造膜状態」とは、ガラス転移温度以上の温度で加熱処理されたことを意味する。一方、エマルジョンの「粒子状態」とは、ガラス転移温度以上の加熱処理がされていないことを意味する。エマルジョン塗工後の乾燥温度をエマルジョンE1のガラス転移温度Tg1以上、エマルジョンE2のガラス転移温度Tg2以下とすることで、エマルジョンE1が造膜し、少なくともエマルジョンE2が粒子として残存している透明シートを製造することができる。このような構成により、図71に示すように、加熱圧着時に、画像支持体55と色材受容層が接着している部分963の透明シート部分980と、画像支持体と色材受容層が接着していない部分964の透明シート部分981と、で膜状態が異なるように制御することができる。すなわち、加熱圧着時において、透明シート部分980はヒートロールの熱が伝わりやすいため、エマルジョンE2の一部が膜化して一部粒子が残存した状態(図71)、あるいは透明シートのエマルジョンE2が完全に皮膜化した状態(図71)になる。このとき、一部あるいは完全に膜化したエマルジョンE2は、予め膜化しているエマルジョンE1と結合力が強化されて透明シートの膜強度を強化することができる。一方、透明シート部分981はヒートロールの熱が伝わらないため、エマルジョンE2を粒子状態のままにすることができる。透明シート部分980と透明シート部分981では膜の状態が異なるため、剥離工程では、境界部982を基点としてクラックが入りやすくなる。以上から、2種類のエマルジョンを用いて、エマルジョンE2の膜状態を加熱圧着時の温度を利用して変化させることにより、箔切れが良好することができる。
[1-2-4-1] Emulsion State It is preferable that the emulsion E1 forms a film and at least the emulsion E2 remains as particles. The “film-forming state” of the emulsion means that it has been heat-treated at a temperature equal to or higher than the glass transition temperature. On the other hand, the “particle state” of the emulsion means that the heat treatment at a temperature higher than the glass transition temperature has not been performed. By setting the drying temperature after the emulsion coating to the glass transition temperature Tg1 or higher of the emulsion E1 and the glass transition temperature Tg2 or lower of the emulsion E2, the emulsion E1 forms a film and at least the emulsion E2 remains as particles. Can be manufactured. With this configuration, as shown in FIG. 71, the transparent sheet portion 980 of the portion 963 where the image support 55 and the color material receiving layer are bonded to each other and the image support and the color material receiving layer are bonded to each other at the time of thermocompression bonding. It can be controlled so that the film state is different between the transparent sheet portion 981 of the portion 964 that is not. That is, at the time of thermocompression bonding, since the heat of the heat roll is easily transmitted to the transparent sheet portion 980, a part of the emulsion E2 is formed into a film and some particles remain (FIG. 71), or the emulsion E2 of the transparent sheet is completely In this state, a film is formed (FIG. 71). At this time, the emulsion E2 that is partially or completely formed into a film can strengthen the bonding strength with the emulsion E1 that has been formed into a film in advance, thereby enhancing the film strength of the transparent sheet. On the other hand, since the heat of the heat roll is not transmitted to the transparent sheet portion 981, the emulsion E2 can be left in a particle state. Since the film state is different between the transparent sheet portion 980 and the transparent sheet portion 981, cracks are easily generated in the peeling step with the boundary portion 982 as a base point. As described above, the foil breakage can be improved by using two types of emulsions and changing the film state of the emulsion E2 using the temperature at the time of thermocompression bonding.

[1−2−4−2]エマルジョンのガラス転移温度
ガラス転移温度(Tg)とは、非晶質の固体を加熱した場合に、低温では結晶なみに堅く(剛性率が大きく)流動性がなかった(粘度が測定不可能なほど大きかった)固体が、ある狭い温度範囲で急速に剛性と粘度が低下して流動性が増す温度である。ガラス転移温度Tgは、各モノマーの単独重合体(ホモポリマー)のガラス転移温度(Tg)及び該モノマーの質量分率(質量基準の共重合割合)に基づいて、フォックス(Fox)の式から算出される値である。
[1-2-4-2] Glass Transition Temperature of Emulsion Glass transition temperature (Tg) means that when an amorphous solid is heated, it is hard like a crystal at low temperatures (high rigidity) and has no fluidity. In addition, solids (viscosity was so large that they could not be measured) are temperatures at which rigidity and viscosity rapidly decrease and fluidity increases in a narrow temperature range. The glass transition temperature Tg is calculated from the Fox equation based on the glass transition temperature (Tg) of the homopolymer of each monomer and the mass fraction (copolymerization ratio based on mass) of the monomer. Is the value to be

なお、本例においてガラス転移温度を表す数値の単位は、特に断りのない限り「℃」である。例えば、三種類のモノマーabcからなる共重合体のガラス転移温度は、下式(9)によって求められる。   In this example, the unit of the numerical value representing the glass transition temperature is “° C.” unless otherwise specified. For example, the glass transition temperature of a copolymer composed of three types of monomers abc can be obtained by the following formula (9).

1/Tg=Wa/Tga+Wb/Tgb+Wc/Tgc (9)
Tga,Tgb,Tgc:各abcモノマーのホモポリマーのガラス転移温度
W:各モノマーの重量
Tg:共重合体のガラス転移温度
1 / Tg = Wa / Tga + Wb / Tgb + Wc / Tgc (9)
Tga, Tgb, Tgc: Glass transition temperature of homopolymer of each abc monomer W: Weight of each monomer Tg: Glass transition temperature of copolymer

上記ホモポリマーのTgとしては、公知資料に記載の値を採用するものとする。ここに開示される技術においては、上記ホモポリマーのTgとして、具体的に以下の値を用いるものとする。   As the Tg of the homopolymer, the value described in known materials is adopted. In the technique disclosed here, the following values are specifically used as the Tg of the homopolymer.

2−エチルヘキシルアクリレート −70℃
n−ブチルアクリレート −55℃
エチルアクリレート −22℃
メチルアクリレート 8℃
メチルメタクリレート 105℃
イソボルニルアクリレート 94℃
イソボルニルメタクリレート 180℃
酢酸ビニル 32℃
2−ヒドロキシエチルアクリレート −15℃
スチレン 100℃
アクリル酸 106℃
メタクリル酸 130℃
2-Ethylhexyl acrylate -70 ° C
n-Butyl acrylate -55 ° C
Ethyl acrylate -22 ° C
Methyl acrylate 8 ℃
Methyl methacrylate 105 ° C
Isobornyl acrylate 94 ° C
Isobornyl methacrylate 180 ° C
Vinyl acetate 32 ° C
2-hydroxyethyl acrylate -15 ° C
Styrene 100 ° C
Acrylic acid 106 ℃
Methacrylic acid 130 ° C

上記のように例示した以外のホモポリマーのTgについては、「Polymer Handbook」(第3版、John Wiley & Sons,Inc、1989年)に記載の数値を用いるものとする。「Polymer Handbook」(第3版、John Wiley & Sons,Inc、1989年)にも記載されていない場合には、以下の測定方法により得られる値を用いるものとする(特開2007−51271号公報参照)。   For the Tg of homopolymers other than those exemplified above, the values described in “Polymer Handbook” (3rd edition, John Wiley & Sons, Inc, 1989) are used. When not described in "Polymer Handbook" (3rd edition, John Wiley & Sons, Inc, 1989), values obtained by the following measurement method are used (Japanese Patent Laid-Open No. 2007-51271). reference).

[1−2−4−3]エマルジョンE1
本例において、エマルジョンE1は透明シートの形成時に造膜状態にある。エマルジョンE1を造膜させることにより、色材受容層との接触面積を増大させることができる。この結果、透明シートと色材受容層との接着性が向上し、テープ剥離等の試験において透明シート(保護層)と色材受容層との間で剥がれないように制御することができる。
[1-2-4-3] Emulsion E1
In this example, the emulsion E1 is in a film-forming state when the transparent sheet is formed. By forming the emulsion E1 into a film, the contact area with the colorant receiving layer can be increased. As a result, the adhesiveness between the transparent sheet and the colorant receiving layer is improved, and it can be controlled so that it does not peel off between the transparent sheet (protective layer) and the colorant receiving layer in tests such as tape peeling.

[1−2−4−4]エマルジョンE1のTg
エマルジョンE1のガラス転移温度Tg1は、50℃より大きく90℃未満である。Tg1は、より好ましくは55℃より大きく80℃未満、さらにより好ましくは55℃より大きく70℃未満である。Tg1を50℃より大きく、さらに好ましくは55℃より大きくすることで、エマルジョンE1のガラス転移温度が高くなって、透明シートの膜部分は硬く伸びにくくなる。そのため、端部を切るときに膜が伸びるのを押さえ、端部を綺麗に保つことができて端部の切れ性が向上する。それに加えて、Tg1を上記範囲に制御することで、樹脂が手の油脂や汗になじみにくくなると共に、膜の伸び性が抑えられて、透明シートに手が触れた場合でも、透明シートが手に密着しにくく、透明シートのべたつきを抑える効果もある。さらに、Tg1を高くするとエマルジョン樹脂の分子鎖間に働く力が強くなり、アルコール等の薬品に溶解しにくくなって、記録物の耐薬品性を著しく向上させることができる。一方、好ましくは90℃未満、より好ましくは80℃未満、さらに好ましくは70℃未満とすることで、透明シートを形成時の造膜を容易に行うことができ、透明シートと色材受容層の接着性を向上させることができる。さらには膜の脆さを改善して、耐水試験での透明シートはがれ等を防止することもできる。また、実際の製造工程上、乾燥温度を完全に一定に保つのは難しく、ある程度の幅ができる。乾燥温度に幅がある場合、Tg1とTg2が近い値であると、E1を膜化させようとしたときに過剰な熱が掛り、乾燥温度がTg2を超えて、E2の粒子状態を維持しにくい場合がある。したがって、Tg1とTg2が下記式(13)の関係を満たして、Tg2とTg1に10℃程度の差があることにより、乾燥温度に幅があった場合でも、過剰な熱がかかることなく、E1が膜、E2が粒子の状態を維持しやすくなるため好ましい。Tg1が50℃以下になると、樹脂が手の油脂や汗になじんでしまい、べたつきが発生しやすい。また、ロール形状にした時のブロッキングも発生しやすい。Tg1が90℃以上になると、E1が造膜しにくいため透明シートと色材受容層の接着性が低下して、透明シートの剥がれが発生しやすい。さらには、膜が脆くなり、耐水試験での透明シートはがれが発生しやすくなる。
Tg2−Tg1≧10 (13)
[1-2-4-4] Tg of emulsion E1
The glass transition temperature Tg1 of the emulsion E1 is greater than 50 ° C. and less than 90 ° C. Tg1 is more preferably greater than 55 ° C and less than 80 ° C, and even more preferably greater than 55 ° C and less than 70 ° C. By making Tg1 larger than 50 ° C., more preferably larger than 55 ° C., the glass transition temperature of the emulsion E1 becomes high, and the film portion of the transparent sheet becomes hard and hardly stretched. Therefore, when the end portion is cut, the film is prevented from extending, and the end portion can be kept clean, so that the end portion is cut. In addition, by controlling Tg1 within the above range, the resin is less likely to become familiar with oils and sweat of the hand, and the stretchability of the film is suppressed, so that even if the transparent sheet is touched by the hand, the transparent sheet is There is also an effect of suppressing stickiness of the transparent sheet. Further, when Tg1 is increased, the force acting between the molecular chains of the emulsion resin is increased, and it becomes difficult to dissolve in chemicals such as alcohol, so that the chemical resistance of the recorded matter can be remarkably improved. On the other hand, it is preferably less than 90 ° C., more preferably less than 80 ° C., and even more preferably less than 70 ° C., so that the film formation at the time of forming the transparent sheet can be easily performed. Adhesiveness can be improved. Furthermore, the brittleness of the film can be improved to prevent the transparent sheet from peeling off in the water resistance test. Moreover, it is difficult to keep the drying temperature completely constant in the actual manufacturing process, and a certain range can be achieved. When there is a range of drying temperatures, if Tg1 and Tg2 are close to each other, excessive heat is applied when E1 is formed into a film, the drying temperature exceeds Tg2, and it is difficult to maintain the particle state of E2. There is a case. Therefore, Tg1 and Tg2 satisfy the relationship of the following formula (13), and there is a difference of about 10 ° C. between Tg2 and Tg1, so that even when there is a range in drying temperature, excessive heat is not applied. Is preferable because the film and E2 can easily maintain the particle state. When Tg1 is 50 ° C. or lower, the resin becomes familiar with the oils and sweat of the hands, and stickiness tends to occur. Further, blocking is also likely to occur when the roll is formed. When Tg1 is 90 ° C. or higher, since E1 is difficult to form a film, the adhesiveness between the transparent sheet and the colorant-receiving layer is lowered, and the transparent sheet is easily peeled off. Furthermore, the film becomes brittle, and the transparent sheet peels easily in the water resistance test.
Tg2−Tg1 ≧ 10 (13)

[1−2−4−5]エマルジョンE1のSP値
また、エマルジョンE1のSP値と、色材受容層の水溶性樹脂のSP値と、の差ΔSPが下式(1)の範囲にあることが好ましい。このような範囲に差ΔSPを設定することにより、加熱圧着時において、エマルジョンE1は水溶性樹脂との相溶性が増し、膜化したエマルションE1と色材受容層の水溶性樹脂との分子間距離が短くなる。そのため、それらは水素結合やファンデルワールス力などから構成される分子間力により強力に接着することができ、透明シートと色材受容層との密着性を向上させることができる。差ΔSPが0.6より大きくなると、相溶性が低下して、膜化したエマルションE1と水溶性樹脂との分子間距離が長くなり、分子間力が低下して接着力が低下するため好ましくない。
0≦|ΔSP|≦0.6 (1)
[1-2-4-5] SP Value of Emulsion E1 Also, the difference ΔSP between the SP value of emulsion E1 and the SP value of the water-soluble resin of the colorant receiving layer is in the range of the following formula (1). Is preferred. By setting the difference ΔSP in such a range, the emulsion E1 becomes more compatible with the water-soluble resin during thermocompression bonding, and the intermolecular distance between the film-formed emulsion E1 and the water-soluble resin of the colorant receiving layer. Becomes shorter. Therefore, they can be strongly bonded by intermolecular forces composed of hydrogen bonds, van der Waals forces, etc., and the adhesion between the transparent sheet and the colorant receiving layer can be improved. When the difference ΔSP is larger than 0.6, the compatibility is lowered, the intermolecular distance between the filmed emulsion E1 and the water-soluble resin is increased, the intermolecular force is lowered, and the adhesive force is lowered, which is not preferable. .
0 ≦ | ΔSP | ≦ 0.6 (1)

[1−2−4−6]エマルジョンE1の材質
上述したエマルジョンE1の材質としては、アクリル系樹脂、酢ビ樹脂、塩ビ樹脂、エチレン/酢ビ共重合樹脂、ポリアミド樹脂、ポリエステル樹脂、ポリウレタン樹脂、ポリオレフィン樹脂等の樹脂又はそれらの共重合体樹脂が好ましい。上記の中でもアクリル系樹脂は、比較的低温での造膜が可能で、塗膜の透明性が高くかつ水溶性樹脂として含有されるけん化ポリビニルアルコールへとのSP値が近く密着性を向上させることができるため、特に好ましく使用される。
[1-2-4-6] Material of Emulsion E1 As the material of emulsion E1, the acrylic resin, vinyl acetate resin, vinyl chloride resin, ethylene / vinyl acetate copolymer resin, polyamide resin, polyester resin, polyurethane resin, A resin such as a polyolefin resin or a copolymer resin thereof is preferable. Among these, acrylic resins can be formed at relatively low temperatures, have high transparency of the coating film, and have an SP value close to saponified polyvinyl alcohol contained as a water-soluble resin, improving adhesion. Therefore, it is particularly preferably used.

アクリル系樹脂としては、(メタ)アクリル酸エステル単独又はこれを用いた共重合体を用いることができる。(メタ)アクリル酸エステルの具体例としては、(メタ)アクリル酸メチル、(メタ)アクリル酸エチル、(メタ)アクリル酸イソプロピル、(メタ)アクリル酸−n−ブチル、(メタ)アクリル酸−n−ヘキシル、(メタ)アクリル酸−n−オクチル、(メタ)アクリル酸−2−エチルヘキシル、(メタ)アクリル酸イソノニル、(メタ)アクリル酸ラウリル等を挙げることができる。これらの(メタ)アクリル酸エステルは単独、又は組み合わせて用いることができる。さらに、これらの(メタ)アクリル酸エステルと共重合可能な単量体を追加重合して用いることができ、このような単量体としては、(メタ)アクリル酸、クロトン酸、マレイン酸、フマル酸、イタコン酸等の不飽和カルボン酸;(メタ)アクリル酸ヒドロキシルエチル、(メタ)アクリル酸ヒドロキシルプロピル、(メタ)アクリル酸(4) 特開2002−121515号公報に記載のヒドロキシルブチル等の水酸基を有する単量体;(メタ)アクリル酸メトキシエチル、(メタ)アクリル酸エトキシエチル等のアルコキシ基を有する単量体;(メタ)アクリル酸グリシジル、アリルグリシジルエーテル等のグリシジル基を有する単量体;(メタ)アクリロニトリルニトリル基を有する単量体;スチレン、(メタ)アクリル酸フェニル、(メタ)アクリル酸ベンジル等の芳香環を有する単量体;(メタ)アクリルアミド等のアミド基を有する単量体;N−アルコキシ基を有する単量体やN−メトキシメチル(メタ)アクリルアミド、N−メトキシエチル(メタ)アクリルアミド等のN−アルコキシアルキル基を有する単量体;N−メチロール(メタ)アクリルアミド、N−ブチロール(メタ)アクリルアミド等の、N−アルキロール基を有する単量体;ビニルクロライド、ビニルブロマイド、アリルクロライド、2−クロロエチル(メタ)アクリレート、クロロメチルスチレン、フッ化ビニル等のハロゲン原子が結合した基を有する単量体;エチレン、プロピレン、ブタジエン等のオレフィン系単量体等を挙げることができる。以上示した材料の反応性の基を利用して部分架橋することも可能である。   As the acrylic resin, (meth) acrylic acid ester alone or a copolymer using the same can be used. Specific examples of (meth) acrylic acid ester include methyl (meth) acrylate, ethyl (meth) acrylate, isopropyl (meth) acrylate, (meth) acrylate-n-butyl, (meth) acrylic acid-n. -Hexyl, (meth) acrylic acid-n-octyl, (meth) acrylic acid-2-ethylhexyl, isononyl (meth) acrylate, lauryl (meth) acrylate, and the like. These (meth) acrylic acid esters can be used alone or in combination. Furthermore, these monomers that can be copolymerized with (meth) acrylic acid esters can be used after additional polymerization. Examples of such monomers include (meth) acrylic acid, crotonic acid, maleic acid, fumaric acid. Unsaturated carboxylic acids such as acid and itaconic acid; hydroxylethyl (meth) acrylate, hydroxylpropyl (meth) acrylate, (meth) acrylic acid (4) hydroxyl groups such as hydroxylbutyl described in JP-A-2002-121515 A monomer having an alkoxy group such as methoxyethyl (meth) acrylate and ethoxyethyl (meth) acrylate; a monomer having a glycidyl group such as glycidyl (meth) acrylate and allyl glycidyl ether Monomer having a (meth) acrylonitrile nitrile group; styrene, phenyl (meth) acrylate, Monomers having an aromatic ring such as meth) benzyl acrylate; monomers having an amide group such as (meth) acrylamide; monomers having an N-alkoxy group, N-methoxymethyl (meth) acrylamide, N- Monomers having an N-alkoxyalkyl group such as methoxyethyl (meth) acrylamide; Monomers having an N-alkylol group such as N-methylol (meth) acrylamide and N-butyrol (meth) acrylamide; Vinyl chloride , Monomers having a group to which halogen atoms are bonded, such as vinyl bromide, allyl chloride, 2-chloroethyl (meth) acrylate, chloromethylstyrene, vinyl fluoride; olefin monomers such as ethylene, propylene, butadiene, etc. Can be mentioned. It is also possible to partially crosslink using the reactive group of the material shown above.

本実施形態に用いられるエマルジョンは、一般的によく知られた公知の技術により合成できるものであり、市販の材料を使うことも可能である。エマルジョンに用いられる樹脂のTgは、モノマー成分とその比率をかえることにより調整することができる。エマルジョンE1は1種類のエマルジョンとしてもよいし、複数のエマルジョンをブレンドして用いてもよい。   The emulsion used in this embodiment can be synthesized by a well-known technique that is generally well known, and commercially available materials can also be used. The Tg of the resin used in the emulsion can be adjusted by changing the monomer component and its ratio. The emulsion E1 may be a single type of emulsion, or a plurality of emulsions may be blended.

[1−2−4−7]エマルジョンE2
本実施形態において、エマルジョンE2は、透明シートの形成時に粒子状態にある。エマルジョンE2を粒子状態にすることにより、転写時における端部の切れ性を良好にすることができる。
[1-2-4-7] Emulsion E2
In this embodiment, the emulsion E2 is in a particle state when the transparent sheet is formed. By making the emulsion E2 into a particle state, it is possible to improve the edge cutability during transfer.

[1−2−4−8]エマルジョンE2のTg
エマルジョンE2のガラス転移温度Tg2は、90℃以上120℃以下である。より好ましくは95〜115℃、さらにより好ましくは100〜110℃である。エマルジョンのガラス転移温度Tgを90℃以上、より好ましくは95℃以上、さらにより好ましくは100℃以上である。
[1-2-4-8] Tg of Emulsion E2
The glass transition temperature Tg2 of the emulsion E2 is 90 ° C. or higher and 120 ° C. or lower. More preferably, it is 95-115 degreeC, More preferably, it is 100-110 degreeC. The glass transition temperature Tg of the emulsion is 90 ° C. or higher, more preferably 95 ° C. or higher, and even more preferably 100 ° C. or higher.

この範囲にすることで、図71に示すように加熱圧着時に、画像支持体55と色材受容層が接着している部分963の透明シート部分980と、画像支持体と色材受容層が接着していない部分964の透明シート部分981と、で膜状態が異なるように制御することができる。すなわち、加熱圧着時において、透明シート部分980はヒートロールの熱が伝わりやすいため、エマルジョンE2の一部が膜化して一部粒子が残存した状態(図71)、あるいは透明シートのエマルジョンE2が完全に皮膜化した状態(図71)になる。一方、透明シート部分981はヒートロールの熱が伝わらないため、エマルジョンE2を粒子状態のままにすることができる。これにより剥離工程では、境界部982を基点としてクラックが入りやすくなる。   With this range, as shown in FIG. 71, the transparent sheet portion 980 of the portion 963 where the image support 55 and the color material receiving layer are bonded to each other and the image support and the color material receiving layer are bonded to each other at the time of thermocompression bonding. It can be controlled so that the film state differs between the transparent sheet portion 981 of the portion 964 that is not. That is, at the time of thermocompression bonding, since the heat of the heat roll is easily transmitted to the transparent sheet portion 980, a part of the emulsion E2 is formed into a film and some particles remain (FIG. 71), or the emulsion E2 of the transparent sheet is completely In this state, a film is formed (FIG. 71). On the other hand, since the heat of the heat roll is not transmitted to the transparent sheet portion 981, the emulsion E2 can be left in a particle state. Thereby, in a peeling process, it becomes easy to enter a crack on the boundary part 982.

さらに上記範囲にすることで、エマルジョンE2の樹脂は伸びにくくなり、さらに手の油脂や汗になじみにくくなるため、透明シートのべたつきが防止できる。加えて、上記範囲にすることでアルコール等の薬品に対する溶解性が低下し、耐薬品性が向上する。また、エマルジョンのガラス転移温度Tgを120℃以下、より好ましくは115℃以下、さらにより好ましくは110℃以下にすることで、加熱圧着における熱エネルギーを低エネルギーで効率的に制御して、画像支持体への過剰な熱エネルギーの付加による熱変形を防止することができる。本発明においては、色材受容層の水溶性樹脂のポリビニルアルコール(PVA)をガラス転移温度の約90℃以上にすることで、色材受容層を画像支持体に転写できる。このため上記温度範囲であれば、色材受容層を画像支持体に加熱圧着するときに、色材受容層が約90℃まで加熱される過程で、ヒートロール側に近い透明シートはTg2以上に加熱されるため、転写時に過剰な熱エネルギーを与えることなく、エマルジョンE2を膜化させて転写することができる。Tg2が90℃より小さくなると、手の油脂や汗になじみやすくなるためべたつきやすくなり、ブロッキング性も発生しやすい。さらにクラックが入りにくくなり、箔切れ性も低下する。Tg2が120より大きくなると、加熱圧着における熱エネルギーを高エネルギーが必要となり、画像支持体への過剰な熱エネルギーの付加による熱変形が発生しやすくなる。   Furthermore, by making it into the said range, since the resin of emulsion E2 becomes difficult to extend | expand and it becomes difficult to become familiar with fats and oils and sweat of a hand, the stickiness of a transparent sheet can be prevented. In addition, by making it in the above range, the solubility in chemicals such as alcohol is lowered, and the chemical resistance is improved. In addition, by setting the glass transition temperature Tg of the emulsion to 120 ° C. or lower, more preferably 115 ° C. or lower, and even more preferably 110 ° C. or lower, the thermal energy in thermocompression bonding can be controlled efficiently with low energy to support the image. Thermal deformation due to the addition of excessive heat energy to the body can be prevented. In the present invention, the colorant-receiving layer can be transferred to the image support by setting the water-soluble resin polyvinyl alcohol (PVA) of the colorant-receiving layer to a glass transition temperature of about 90 ° C. or higher. Therefore, within the above temperature range, when the colorant receiving layer is heated and pressure-bonded to the image support, the transparent sheet close to the heat roll side becomes Tg2 or higher in the process of heating the colorant receiving layer to about 90 ° C. Since it is heated, the emulsion E2 can be transferred into a film without giving excessive thermal energy during transfer. When Tg2 is smaller than 90 ° C., it becomes easy to become familiar with hand oils and fats and sweat, so that it becomes sticky and blocking properties are likely to occur. Furthermore, cracks are less likely to occur, and the foil breakability also decreases. When Tg2 is greater than 120, high energy is required for thermal compression in thermocompression bonding, and thermal deformation due to addition of excessive thermal energy to the image support tends to occur.

[1−2−4−9]エマルジョンE2の材質
エマルジョンE2を構成する高分子物質としては、エマルジョンE1と同等のものを使用できる。ただし、アクリル系樹脂やウレタン系樹脂は、透明シートと基材シートのSPの差SP1を1.1以上に制御でき、基材シートからの剥離性が向上するため、好ましく用いられる。エマルジョンE2に、特に好ましいのはウレタン系樹脂である。ウレタン系樹脂とすることで適度なやわらかさを持ち、べたつきが抑えられる。さらには、膜の脆さや薬品への溶解性を改善して、アルコールなど薬品に浸漬しても割れやはがれ等が起きにくくなり、耐薬品性が向上できる。エマルジョンE2は、エマルジョンE1と異なる種類の樹脂を用いることが好ましく、種類の異なる樹脂を用いることで樹脂同士の相溶が起こりにくくなり、転写前の状態で膜と粒子の共存状態が維持しやすい。エマルジョンE1としてアクリル系樹脂を用いた場合、エマルジョンE2として特に好ましくはウレタン系樹脂である。
[1-2-4-9] Material of Emulsion E2 As the polymer substance constituting the emulsion E2, the same material as the emulsion E1 can be used. However, acrylic resins and urethane resins are preferably used because the SP difference SP1 between the transparent sheet and the base sheet can be controlled to 1.1 or more and the peelability from the base sheet is improved. Particularly preferred for the emulsion E2 is a urethane resin. By using urethane resin, it has moderate softness and stickiness is suppressed. Furthermore, the brittleness of the film and the solubility in chemicals are improved, and even when immersed in chemicals such as alcohol, cracking and peeling are less likely to occur, and chemical resistance can be improved. Emulsion E2 preferably uses a different type of resin from emulsion E1, and the use of different types of resin makes it difficult for the resins to be compatible with each other, making it easy to maintain the coexistence state of the film and particles before transfer. . When an acrylic resin is used as the emulsion E1, the urethane resin is particularly preferable as the emulsion E2.

ウレタン系樹脂としては、例えば、以下に挙げるポリオール化合物とジイソシアネート化合物とを種々組み合わせて、重付加反応により合成されたウレタン系樹脂を挙げることができる。ウレタン系樹脂は特に限定されないが、好ましくポリエーテル系のポリオール化合物とジイソシアネート化合物から合成されるポリエーテルウレタン系樹脂が好ましい。ポリエーテルウレタン系樹脂は加水分解しにくいので、記録物の耐水性を含む耐久性が向上する。   Examples of the urethane resin include urethane resins synthesized by a polyaddition reaction using various combinations of the following polyol compounds and diisocyanate compounds. The urethane resin is not particularly limited, but a polyether urethane resin synthesized from a polyether polyol compound and a diisocyanate compound is preferable. Since the polyether urethane resin is hardly hydrolyzed, the durability including the water resistance of the recorded matter is improved.

ポリオール化合物としては、2つの水酸基を含有するジオール、若しくは3以上の水酸基を含有するポリオールであれば特に限定されずに用いることができる。例えば、ポリエーテル系、ポリエステル系、ポリカーボネート系、アクリル系、ポリブタジエン系若しくはポリオレフィン系等のポリオール、カプロラクトン変性ポリオール、ポリエステルアミドポリオール、ポリウレタンポリオール、エポキシポリオール、エポキシ変性ポリオール、アルキド変性ポリオール、ひまし油、フッ素含有ポリオール等のポリオールを単独で用いてもよいし、これらを併用しても良い。   As the polyol compound, any diol containing two hydroxyl groups or a polyol containing three or more hydroxyl groups can be used without particular limitation. For example, polyether, polyester, polycarbonate, acrylic, polybutadiene or polyolefin polyols, caprolactone modified polyol, polyester amide polyol, polyurethane polyol, epoxy polyol, epoxy modified polyol, alkyd modified polyol, castor oil, fluorine-containing Polyols such as polyols may be used alone or in combination.

ポリエーテル系ポリオールとしては、具体的には、例えば、エチレングリコール、プロピレングリコール、ブチレングリコール、テトラメチレングリコール、グリセリン、トリメチロールプロパン、ペンタエリスリトール、ソルビトール、シュークロース等の多価アルコール類、エチレンジアミン等の脂肪族アミン化合物類、トルエンジアミン、ジフェニルメタンー4,4−ジアミン等の芳香族アミン化合物、エタノールアミンおよびジエタノールアミン等のようなアルカノールアミン類のような少なくとも2個以上の活性水素基を有する化合物を出発原料として、これにエチレンオキサイド、プロピレンオキサイド、ブチレンオキサイド若しくはポリオキシテトラメチレンオキサイドに代表されるアルキレンオキサイドを付加させて得られるポリオール等が挙げられる。   Specific examples of polyether polyols include polyhydric alcohols such as ethylene glycol, propylene glycol, butylene glycol, tetramethylene glycol, glycerin, trimethylolpropane, pentaerythritol, sorbitol, sucrose, and ethylenediamine. Starting with compounds having at least two active hydrogen groups such as aliphatic amine compounds, aromatic amine compounds such as toluenediamine and diphenylmethane-4,4-diamine, and alkanolamines such as ethanolamine and diethanolamine It is obtained by adding an alkylene oxide typified by ethylene oxide, propylene oxide, butylene oxide or polyoxytetramethylene oxide as a raw material. Polyol, and the like.

ポリエステル系ポリオールとしては、具体的には、例えば、エチレングリコール、プロピレングリコール、ブタンジオールペンタンジオール、ヘキサンジオール、グリセリン、1,1,1−トリメチロールプロパンおよびその他の低分子ポリオールなどから選ばれる少なくとも1種と、グルタル酸、アジピン酸、ピメリン酸、スベリン酸、セバシン酸、ダイマー酸、その他の低分子脂肪族カルボン酸およびオリゴマー酸などから選ばれる少なくとも1種との縮合重合体;プロピオンラクトンまたはバレロラクトン等の開環重合体;等が挙げられる。   Specific examples of the polyester polyol include at least one selected from, for example, ethylene glycol, propylene glycol, butanediol pentanediol, hexanediol, glycerin, 1,1,1-trimethylolpropane, and other low molecular polyols. A condensation polymer of a seed and at least one selected from glutaric acid, adipic acid, pimelic acid, suberic acid, sebacic acid, dimer acid, other low molecular weight aliphatic carboxylic acid and oligomeric acid; propionlactone or valerolactone Ring-opening polymers such as;

その他のポリオールとしては、たとえば、ポリマーポリオール、ポリカーボネートポリオール;ポリブタジエンポリオール;水素添加されたポリブタジエンポリオール;アクリルポリオール;エチレングリコール、ジエチレングリコール、プロピレングリコール、ジプロピレングリコール、ブタンジオール、ペンタンジオール、ヘキサンジオール等の低分子ポリオールが挙げられる。   Other polyols include, for example, polymer polyols, polycarbonate polyols, polybutadiene polyols, hydrogenated polybutadiene polyols, acrylic polyols, ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, butanediol, pentanediol, hexanediol Examples include molecular polyols.

ジイソシアネート化合物は、特に限定されずに用いることができる。ジイソシアネート化合物としては、メチレンジイソシアネート、エチレンジイソシアネート、イソホロンジイソシアネート、ヘキサメチレンジイソシアネート,1,4−シクロヘキサンジイソシアネート、2,4−トルエンジイソシアネート、2,6−トルエンジイソシアネート、1,3−キシリレンジイソシアネート、1,5−ナフタレンジイソシアネート,m−フェニレンジイソシアネート、p−フェニレンジイソシアネート、3,3’−ジメチル−4,4’―ジフェニルメタンジイソシアネート、3,3’−ジメチルビフェニレンジイソシアネート、4,4’−ビフェニレンジイソシアネート、ジシクロヘキシルメタンジイソシアネート、メチレンビス(4−シクロヘキシルイソシアネート)等を挙げることができる。   The diisocyanate compound can be used without any particular limitation. Diisocyanate compounds include methylene diisocyanate, ethylene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, 1,4-cyclohexane diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 1,3-xylylene diisocyanate, 1,5. -Naphthalene diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, 3,3'-dimethyl-4,4'-diphenylmethane diisocyanate, 3,3'-dimethylbiphenylene diisocyanate, 4,4'-biphenylene diisocyanate, dicyclohexylmethane diisocyanate, And methylene bis (4-cyclohexyl isocyanate).

[1−2−4−10]エマルジョンE2の平均粒子径
エマルジョンE2の平均粒径としては特に制限はないが、好ましくは1〜200nm、より好ましくは5〜150nm、さらにより好ましくは10〜50nmである。平均粒子径を、好ましくは1nm以上、より好ましくは5nm以上、さらにより好ましくは10nm以上とすることで、加熱圧着時において、画像支持体と色材受容層が接着していない部分964の透明シート部分980の、エマルジョンE2を粒子状態にすることが容易になる。したがって、画像支持体55と色材受容層が接着している部分963の透明シート部分980の境界部で、クラックが入りやすくなり、転写後の剥離工程において、端部にバリの発生がなく箔切れ性を良好にすることができる。本発明の転写材では、エマルジョンE2を粒子状態に維持させるため、そのエマルジョンE2の粒径は透明シートの透明性に大きく影響する。エマルジョンE2の平均粒子径を、好ましくは200nm以下、より好ましくは150nm以下、さらにより好ましくは50nm以下とすることで、透明シートの透明性を良好にすることができる。さらには、粒子径が上記以下の場合は、細かいクラックがはいりやすくなり、端部の切れ性も良好となる。E2の平均粒径が1nmより小さいと粒子が小さ過ぎるため、透明シートが膜に近い状態となって、転写時にクラックが入りにくくなって箔切れ性が低下する。E2の平均粒径が200nmより大きいと透明性が低下するおそれがある。
[1-2-4-10] Average particle size of emulsion E2 The average particle size of emulsion E2 is not particularly limited, but is preferably 1 to 200 nm, more preferably 5 to 150 nm, and even more preferably 10 to 50 nm. is there. By setting the average particle size to preferably 1 nm or more, more preferably 5 nm or more, and even more preferably 10 nm or more, the transparent sheet of the portion 964 where the image support and the colorant receiving layer are not adhered at the time of thermocompression bonding It becomes easy to make emulsion E2 into the particle state of the part 980. Therefore, cracks are likely to occur at the boundary between the transparent sheet portion 980 of the portion 963 where the image support 55 and the colorant receiving layer are bonded, and there is no occurrence of burrs at the edges in the peeling process after transfer. Cutting performance can be improved. In the transfer material of the present invention, since the emulsion E2 is maintained in a particle state, the particle size of the emulsion E2 greatly affects the transparency of the transparent sheet. By setting the average particle size of the emulsion E2 to 200 nm or less, more preferably 150 nm or less, and even more preferably 50 nm or less, the transparency of the transparent sheet can be improved. Furthermore, when the particle diameter is equal to or smaller than the above, fine cracks are likely to occur, and the edge cutability is also improved. If the average particle diameter of E2 is smaller than 1 nm, the particles are too small, so that the transparent sheet is close to a film, cracks are difficult to occur during transfer, and the foil breakage is reduced. If the average particle diameter of E2 is larger than 200 nm, the transparency may be lowered.

[1−2−4−11]エマルジョンE1、E2の混合比率
本発明においては、エマルジョンE1とエマルジョンE2の比率(E1/E2)は下記式(3)を満たすことが好ましく、より好ましくは5.0≦E1/E2≦50.0、さらにより好ましくは10.0≦E1/E2≦35.0を満たすことが好ましい。E1/E2を65.0以下、さらに好ましくは50.0以下、より好ましくは35.0以下にすることで、E2が増加し、粒子成分が増えることで、エマルジョンE2を粒子状態で残存させることが容易になり、画像支持体55と色材受容層が接着している部分963の透明シート部分980との境界部で、クラックが入りやすくなり、端部にバリの発生がなく箔切れ性を良好にすることができる。
[1-2-4-11] Mixing ratio of emulsions E1 and E2 In the present invention, the ratio of emulsion E1 to emulsion E2 (E1 / E2) preferably satisfies the following formula (3), more preferably 5. It is preferable that 0 ≦ E1 / E2 ≦ 50.0, still more preferably 10.0 ≦ E1 / E2 ≦ 35.0. By setting E1 / E2 to 65.0 or less, more preferably 50.0 or less, more preferably 35.0 or less, E2 increases, and the particle component increases, so that emulsion E2 remains in a particle state. Is easy to crack, and cracks easily occur at the boundary between the image support 55 and the transparent sheet portion 980 of the portion 963 where the colorant receiving layer is adhered, and there is no occurrence of burrs at the end portion, resulting in the ability to break the foil. Can be good.

すなわち、この範囲にすることで、図71に示すように加熱圧着時に、画像支持体55と色材受容層が接着している部分963の透明シート部分980と、画像支持体と色材受容層が接着していない部分964の透明シート部分981と、で膜状態が異なるように制御することができる。加熱圧着時において、透明シート部分980はヒートロールの熱が伝わりやすいため、エマルジョンE2の一部が膜化して一部粒子が残存した状態(図40(b))、あるいは透明シートのエマルジョンE2が完全に皮膜化した状態(図40(c))になる。   That is, by setting this range, as shown in FIG. 71, the transparent sheet portion 980 of the portion 963 where the image support 55 and the color material receiving layer are bonded, and the image support and the color material receiving layer as shown in FIG. It can be controlled so that the film state is different between the transparent sheet portion 981 of the portion 964 where the film is not bonded. At the time of thermocompression bonding, since the heat of the heat roll is easily transmitted to the transparent sheet portion 980, a part of the emulsion E2 is formed into a film and a part of the particles remains (FIG. 40 (b)), or the emulsion E2 of the transparent sheet is formed. A completely filmed state (FIG. 40C) is obtained.

一方、E1/E2が3.0以上、より好ましくは5.0以上、さらにより好ましくは10.0以上とすることで、E1が増加し、造膜成分が増えることで膜強度が向上し、さらに色材受容層との接触面積が大きくなり、色材受容層と透明シートの接着性を向上させることができる。特に、10.0≦E1/E2≦35.0の範囲にすることで、接着性と端部の切れ性の向上、およびひび割れ防止を高レベルで両立できる。E1/E2が65.0より大きくなると、粒子成分が少なくなって膜の状態に近づくため、クラックが入りにくくなり、箔切れ性を得ることが難しくなる。また、E1/E2が3.0より小さいと、E2のバインダーとなるE1が少なくなるため、色材受容層形成時に、透明シートのエマルジョンのはがれや粉落ちが発生する場合があり、色材受容層が均一に形成できなくなるおそれがある。さらには、膜成分が少なくなるため、色材受容層との接着性が低下して、透明シートのはがれが発生しやすくなる。
3.0≦E1/E2≦65.0 (3)
On the other hand, when E1 / E2 is 3.0 or more, more preferably 5.0 or more, and even more preferably 10.0 or more, E1 is increased, and the film-forming component is increased to improve the film strength. Furthermore, a contact area with a color material receiving layer becomes large, and the adhesiveness of a color material receiving layer and a transparent sheet can be improved. In particular, by setting the range of 10.0 ≦ E1 / E2 ≦ 35.0, it is possible to achieve both a high level of improvement in adhesiveness, edge cutability, and crack prevention. When E1 / E2 is larger than 65.0, the particle component is reduced and approaches the state of the film, so that it becomes difficult for cracks to occur and it becomes difficult to obtain the foil breakability. Further, when E1 / E2 is smaller than 3.0, since E1 serving as a binder for E2 is reduced, the emulsion of the transparent sheet may be peeled off or powdered off at the time of forming the colorant receiving layer. There is a possibility that the layer cannot be formed uniformly. Furthermore, since the film component is reduced, the adhesiveness with the colorant receiving layer is lowered and peeling of the transparent sheet is likely to occur.
3.0 ≦ E1 / E2 ≦ 65.0 (3)

エマルジョンE1とE2の割合(E1/E2)が10より小さい(エマルジョンE2の割合が9.1%より多い)と、透明シートと色材受容層を含む転写材の透明シートにエマルジョンを使用して、一部は造膜、一部は粒子状態にすると、透明シート上に色材受容層を塗工する際の色材受容層が乾燥していくときの収縮に耐え切れず、透明シートのひび割れが発生しやすくなる場合がある。この現象は、色材受容層を含有するタイプの転写材特有の現象であって、水溶性化合物と無機微粒子を含む水性塗工液を透明シート上に塗工する場合にのみ発生する。基材と保護層のみで構成されている転写材では発生しない。特に、本発明のようにインクジェット方式に好ましく用いられる転写材の場合は、色材受容層に大量のインクを吸収させる必要があるため、色材受容層の厚みが大きくなり、塗工量と乾燥時の収縮量も合わせて大きくなるため、塗工時のひび割れが発生しやすい。さらに本発明のように接着性、白切れ性、耐薬品性、べたつき防止を考慮して、透明シート中で膜化しているエマルジョンとして、ガラス転移温度Tg1が50℃より大きいエマルジョン樹脂E1を用いる場合は、エマルジョン樹脂が硬く伸びにくくなり、収縮によってひび割れの現象が非常に発生しやすい傾向にある。以上のことから、本発明のように、基材、色材受容層、透明シートが順次積層され、透明シートがエマルジョンE1とE2を含み、膜化しているエマルジョンE1のガラス転移温度Tg1が50℃より大きく、エマルジョンE2を粒子として残存させている場合は、E1とE2の比率を精密に制御することが重要である。   When the ratio of emulsions E1 and E2 (E1 / E2) is less than 10 (the ratio of emulsion E2 is more than 9.1%), the emulsion is used for the transparent sheet of the transfer material including the transparent sheet and the colorant receiving layer. When part of the film is formed into a film and partly in the form of particles, the colorant receiving layer applied to the transparent sheet cannot withstand the shrinkage caused by drying, and the transparent sheet is cracked. May be more likely to occur. This phenomenon is a phenomenon peculiar to the type of transfer material containing a color material receiving layer, and occurs only when an aqueous coating liquid containing a water-soluble compound and inorganic fine particles is applied on a transparent sheet. It does not occur with transfer materials that consist only of a substrate and a protective layer. In particular, in the case of a transfer material that is preferably used in an ink jet system as in the present invention, since it is necessary to absorb a large amount of ink in the color material receiving layer, the thickness of the color material receiving layer is increased, and the coating amount and the drying amount are increased. Since the amount of shrinkage at the time also increases, cracking during coating tends to occur. Further, in the case of using an emulsion resin E1 having a glass transition temperature Tg1 higher than 50 ° C. as an emulsion formed into a film in a transparent sheet in consideration of adhesiveness, whiteness, chemical resistance, and stickiness prevention as in the present invention. The emulsion resin is hard and difficult to stretch, and the phenomenon of cracking tends to occur very easily due to shrinkage. From the above, as in the present invention, the base material, the colorant receiving layer, and the transparent sheet are sequentially laminated, and the transparent sheet contains the emulsions E1 and E2, and the glass transition temperature Tg1 of the emulsion E1 formed into a film is 50 ° C. If the emulsion E2 remains larger as particles, it is important to precisely control the ratio of E1 and E2.

本実施形態の透明シートが基材シートに当接する場合、基材シートのSP値と透明シートのSP値との差の絶対値|SP1|が下式(10)を満たすように、それらの材料を選択することが好ましい。差の絶対値|SP1|が下式(10)の関係を満たすことにより、透明シートと基材シートは比較的弱い接着状態で積層されることなる。これにより、転写時においては、基材シートが透明シートから剥離しやすくなり、一方、色材受容層と画像支持体との接着性をより強くすることできるため、転写時の転写性を高めることができる。
1.1≦|SP1|≦3 (10)
When the transparent sheet of the present embodiment abuts on the base sheet, those materials are set so that the absolute value | SP1 | of the difference between the SP value of the base sheet and the SP value of the transparent sheet satisfies the following expression (10). Is preferably selected. When the absolute value | SP1 | of the difference satisfies the relationship of the following expression (10), the transparent sheet and the base sheet are laminated with a relatively weak adhesive state. Thereby, at the time of transfer, the base material sheet is easily peeled off from the transparent sheet, and on the other hand, the adhesion between the colorant receiving layer and the image support can be strengthened, so that the transferability at the time of transfer is improved. Can do.
1.1 ≦ | SP1 | ≦ 3 (10)

また、本実施形態の転写材を画像支持体に加熱圧着させて、基材シートを剥離することにより、透明シートを介して、色材受容層に記録された画像を本来の画像として視認することができる。また、転写材を画像支持体に加熱圧着させた場合に、透明シートは色材受容層に記録された画像の保護層として機能する。   In addition, the image recorded on the colorant receiving layer is visually recognized as an original image through the transparent sheet by heat-pressing the transfer material of the present embodiment to the image support and peeling the base sheet. Can do. Further, when the transfer material is heat-pressed to the image support, the transparent sheet functions as a protective layer for the image recorded on the color material receiving layer.

透明シートは、JIS K7375に準拠して測定される全光線透過率が50%以上、好ましくは90%以上のシートである。したがって透明シートには、無色透明シートの他、半透明シートおよび着色透明シート等も含まれる。色材受容層に画像を記録するインクとして染料インクを用いる場合には、紫外線による染料の分解(光劣化)を防止するために、透明シートがUVカット剤を含有するものであることが好ましい。UVカット剤としては、例えば、ベンゾトリアゾール系化合物、ベンゾフェノン系化合物等の紫外線吸収剤;酸化チタン、酸化亜鉛等の紫外線散乱剤;等を挙げることができる。   The transparent sheet is a sheet having a total light transmittance measured in accordance with JIS K7375 of 50% or more, preferably 90% or more. Accordingly, the transparent sheet includes a semi-transparent sheet and a colored transparent sheet in addition to the colorless transparent sheet. When a dye ink is used as an ink for recording an image on the colorant-receiving layer, the transparent sheet preferably contains a UV cut agent in order to prevent the dye from being decomposed (photodegraded) by ultraviolet rays. Examples of the UV-cutting agent include ultraviolet absorbers such as benzotriazole compounds and benzophenone compounds; ultraviolet scattering agents such as titanium oxide and zinc oxide;

[1−2−5]細孔の形成方法
透明シートが樹脂を主成分とするものであって、基材シート上に製膜される場合、透明シートに細孔を形成する方法としては、種々の方式を適用可能である。例えば、透明シートの製膜工程中、もしくは、その後の工程において、透明シートの構成材料中に含まれる成分によって、図36、図37、および図38のように連泡構造の細孔を構成するようにしてもよい。後述するように、図36、図37、および図38においては、それぞれ発泡剤、多孔質粒子、および中空粒子を用いて連泡構造の細孔を構成する。また、図39および図40のように、予め細孔構造を有する透明シートを作成しておき、それを基材シート上にラミネートないしは積層接着させてもよい。その詳細については後述する。さらに、図41および図42のように、基材シート上に透明シートを製膜した後に、別の手段により、透明シートに所望の細孔を形成する細孔処理を施してもよい。その詳細については後述する。このように透明シートの細孔は、基材シートと色材受容層との間を貫通する細孔構造となっていればよく、もちろん公知の方法を用いて形成することも可能であり、目的および用途に応じて最適な形成方法を選択することができる。
[1-2-5] Method for forming pores When the transparent sheet is mainly composed of a resin and is formed on a substrate sheet, there are various methods for forming pores in the transparent sheet. This method can be applied. For example, in the film forming process of the transparent sheet or in the subsequent process, the pores of the open cell structure are configured as shown in FIGS. 36, 37, and 38 by the components contained in the constituent material of the transparent sheet. You may do it. As will be described later, in FIG. 36, FIG. 37, and FIG. 38, pores having an open cell structure are formed using a foaming agent, porous particles, and hollow particles, respectively. Further, as shown in FIGS. 39 and 40, a transparent sheet having a pore structure may be prepared in advance, and may be laminated or laminated and adhered on the base sheet. Details thereof will be described later. Furthermore, as shown in FIG. 41 and FIG. 42, after forming a transparent sheet on a base sheet, a pore treatment for forming desired pores in the transparent sheet may be performed by another means. Details thereof will be described later. Thus, the pores of the transparent sheet need only have a pore structure that penetrates between the base material sheet and the colorant receiving layer, and can be formed using a known method. The optimum forming method can be selected according to the application.

[1−2−6]発泡剤
発泡剤を用いて透明シート内に連泡構造を構成する場合には、エマルジョンを含有する塗工液に機械的撹拌を施して、その塗工液に多数の微細な気泡を形成して分散させて、透明シートを形成する。
[1-2-6] Foaming agent In the case of forming a continuous cell structure in a transparent sheet using a foaming agent, mechanical stirring is applied to the coating solution containing the emulsion, Fine bubbles are formed and dispersed to form a transparent sheet.

具体的には、図36のように、エマルジョンを含有する塗工液を攪拌して多数の微細の気泡553が分散させた塗工液を用意し、ダイコーター655Aを用いて、その塗工液から薄膜の透明シート52を形成する。図36(a)の場合は、その透明シート52に対して、ダイコーター655Bを用いて色材受容層53を形成してから、ダイコーター65Cを用いて基準シート50を形成する。図36(b)の場合は、透明シート52に対して、ダイコーター65Cを用いて基準シート50を形成してから、ダイコーター655Bを用いて色材受容層53を形成する。図36(c)の場合は、予め用意した基準シート50に対して、ダイコーター655Aを用いて透明シート52を形成してから、ダイコーター655Bを用いて色材受容層53を形成する。この結果、図20(f)のように、気泡553が連なる連泡構造の透明シート52を含む転写材1が製造される。   Specifically, as shown in FIG. 36, the coating liquid containing the emulsion is stirred to prepare a coating liquid in which a large number of fine bubbles 553 are dispersed, and the coating liquid is prepared using a die coater 655A. Then, a thin transparent sheet 52 is formed. In the case of FIG. 36A, after forming the color material receiving layer 53 on the transparent sheet 52 using the die coater 655B, the reference sheet 50 is formed using the die coater 65C. In the case of FIG. 36B, after the reference sheet 50 is formed on the transparent sheet 52 using the die coater 65C, the color material receiving layer 53 is formed using the die coater 655B. In the case of FIG. 36C, the transparent sheet 52 is formed on the reference sheet 50 prepared in advance using the die coater 655A, and then the color material receiving layer 53 is formed using the die coater 655B. As a result, as shown in FIG. 20F, the transfer material 1 including the transparent sheet 52 having the continuous bubble structure in which the bubbles 553 are continuous is manufactured.

透明シート52を形成する塗工液の機械的撹拌方法は特に制限はされず、公知の撹拌翼を有する発泡機、乳化分散等に利用されているホモミキサー、カウレスディゾルバー等の撹拌機、および連続発泡機等を用いて行うことができる。エマルジョンを含有する塗工液には、発泡による皮膜形成性を安定化させるために、さらに樹脂を添加することが望ましい。その樹脂としては、色材受容層に添加する水溶性樹脂と同等のものが使用できるが、これらに限定されるものではない。これらの樹脂は必要に応じて、単独あるいは2種類以上混合して使用することができる。   The mechanical stirring method of the coating liquid for forming the transparent sheet 52 is not particularly limited, and is a foaming machine having a known stirring blade, a homomixer used for emulsification dispersion, etc., a stirring machine such as a cowless dissolver, and the like. It can be performed using a continuous foaming machine or the like. In order to stabilize the film-forming property by foaming, it is desirable to add a resin to the coating liquid containing the emulsion. As the resin, those equivalent to the water-soluble resin added to the colorant receiving layer can be used, but are not limited thereto. These resins can be used alone or in combination of two or more as required.

このようなエマルジョンおよび樹脂を含む塗工液には、気泡の安定性を向上させるために、整泡剤あるいは発泡剤と称されている、界面活性作用のある材料を適宜選定して配合してもよい。例えば、高級脂肪酸、高級脂肪酸変性物、高級脂肪族のアルカリ塩、高級脂肪酸のアミン塩等の陰イオン性の界面活性剤を配当することにより、特に、樹脂液の発泡性、および分散含有させた気泡の安定性を高めることができる。これら整泡剤あるいは発泡剤の材料は限定はされず、樹脂液の流動性や塗工作業性を考慮して選択することができる。   In such a coating liquid containing an emulsion and a resin, in order to improve the stability of the bubbles, a material having a surface active action called a foam stabilizer or a foaming agent is appropriately selected and blended. Also good. For example, by paying out anionic surfactants such as higher fatty acids, higher fatty acid modified products, higher aliphatic alkali salts, higher fatty acid amine salts, etc. The stability of bubbles can be increased. The material of these foam stabilizers or foaming agents is not limited, and can be selected in consideration of the fluidity of the resin liquid and the coating workability.

このような整泡剤あるいは発泡剤の樹脂液に対する配合比率は、樹脂液の固形分100重量部に対して、好ましくは固形分で0〜30重量部、より好ましくは1〜20重量部である。その配合比率が30重量部を越えると、多くの気泡を小さく制御できるものの、その気泡により作製した透明シートの透明性が低下して、記録画像の視認性が低下するため好ましくない。   The blending ratio of the foam stabilizer or the foaming agent to the resin liquid is preferably 0 to 30 parts by weight, more preferably 1 to 20 parts by weight, based on 100 parts by weight of the solid content of the resin liquid. . If the blending ratio exceeds 30 parts by weight, many bubbles can be controlled to be small, but the transparency of the transparent sheet produced by the bubbles is lowered and the visibility of the recorded image is lowered, which is not preferable.

また、エマルジョンおよび樹脂を含む塗工液に関して、その発泡前の体積に対する発泡後の体積の体積比(以下、発泡倍率という)は、樹脂液の組成とのバランスを考慮して設定すればよい。その発泡倍率は、好ましくは0.5倍を越えかつ10倍以下、より好ましくは1.0倍以上かつ5倍以下である。発泡倍率は、気泡を含有する水分散型樹脂の塗布液中の気泡含有率を示す尺度である。発泡倍率が0.5倍以下では、透明シートが水分透過性もしくは透湿性を示すための十分な連泡構造を得ることが困難になるため、好ましくない。一方、発泡倍率が10倍以上になると、気泡を構成する樹脂液膜(壁)の厚さが薄くなって、耐水性以外の保護層としての機能が低下するため、好ましくない。また、その場合には、内包する空気の量が増加して透明シートの断熱性が高くなり、転写性能が低下するおそれがある。さらに、発泡前の水分散型樹脂液の固形分濃度が低いほど、気孔含有樹脂層の気孔を囲む樹脂膜(壁)が薄くなるため、保護層としての機能が低下する。   Moreover, regarding the coating liquid containing the emulsion and the resin, the volume ratio of the volume after foaming to the volume before foaming (hereinafter referred to as foaming ratio) may be set in consideration of the balance with the composition of the resin liquid. The expansion ratio is preferably more than 0.5 times and not more than 10 times, more preferably not less than 1.0 times and not more than 5 times. The expansion ratio is a scale indicating the bubble content in the coating liquid of the water-dispersed resin containing bubbles. When the expansion ratio is 0.5 times or less, it is difficult to obtain a sufficient open cell structure for the transparent sheet to exhibit moisture permeability or moisture permeability, which is not preferable. On the other hand, if the expansion ratio is 10 times or more, the thickness of the resin liquid film (wall) constituting the bubbles becomes thin, and the function as a protective layer other than water resistance is lowered, which is not preferable. In that case, the amount of air to be included increases and the heat insulating property of the transparent sheet becomes high, and there is a possibility that the transfer performance is lowered. Furthermore, since the resin film (wall) surrounding the pores of the pore-containing resin layer becomes thinner as the solid content concentration of the water-dispersed resin liquid before foaming is lower, the function as a protective layer is lowered.

[1−2−7]多孔質粒子
多孔質粒子を用いて透明シート内に連泡構造を構成する場合には、多孔質粒子を含有する樹脂を主成分とする透明シートを基材シート上に製膜し、多孔質粒子の連結によって、基材シートと色材受容層との間を貫通する細孔を形成する。例えば、図37のように、ダイコーター655Aを用いて、多孔質粒子554を含有する樹脂材料から透明シート52を形成する。
[1-2-7] Porous particles When the open cell structure is formed in the transparent sheet using the porous particles, a transparent sheet mainly composed of a resin containing porous particles is formed on the base sheet. Film formation is performed, and pores penetrating between the base material sheet and the colorant receiving layer are formed by connecting the porous particles. For example, as shown in FIG. 37, a transparent sheet 52 is formed from a resin material containing porous particles 554 using a die coater 655A.

図37(a)の場合は、その透明シート52に対して、ダイコーター655Bを用いて色材受容層53を形成してから、ダイコーター65Cを用いて基準シート50を形成する。図37(b)の場合は、透明シート52に対して、ダイコーター65Cを用いて基準シート50を形成してから、ダイコーター655Bを用いて色材受容層53を形成する。図37(c)の場合は、予め用意した基準シート50に対して、ダイコーター655Aを用いて透明シート52を形成してから、ダイコーター655Bを用いて色材受容層53を形成する。この結果、図22(g)のように、多孔質粒子554の多孔質部分が連なる連泡構造の透明シート52を含む転写材1が製造される。   In the case of FIG. 37 (a), the colorant receiving layer 53 is formed on the transparent sheet 52 using the die coater 655B, and then the reference sheet 50 is formed using the die coater 65C. In the case of FIG. 37B, the reference sheet 50 is formed on the transparent sheet 52 using the die coater 65C, and then the colorant receiving layer 53 is formed using the die coater 655B. In the case of FIG. 37 (c), the transparent sheet 52 is formed on the reference sheet 50 prepared in advance using the die coater 655A, and then the color material receiving layer 53 is formed using the die coater 655B. As a result, as shown in FIG. 22G, the transfer material 1 including the transparent sheet 52 having the open cell structure in which the porous portions of the porous particles 554 are continuous is manufactured.

多孔質粒子の材料は特に制限されず、有機物および無機物の両方を用いることがきる。ただし、耐熱性の観点から、多孔質の無機微粒子を用いることが好ましい。例えば、炭酸カルシウム、炭酸マグネシウム、カオリン、クレー、タルク、ハイドロタルサイト、珪酸アルミニウム、珪酸カルシウム、珪酸マグネシウム、ケイソウ土、アルミナ、コロイダルアルミナ、水酸化アルミニウム、ベーマイト構造のアルミナ水和物、擬ベーマイト構造のアルミナ水和物、リトポン(硫酸バリウムと硫化亜鉛の混合物)、ゼオライト等を挙げることができる。多孔質粒子の含有量に応じて、細孔の密度を制御できる。多孔質粒子の含有量は、エマルジョンの合計量に対して1%〜30%程度が好ましい。その含有量が1%以下になると、水の透過性が低下して、ひび割れが起こりやすくなる。それが30%以上になると、水の透過性が増大し、過剰に液体を吸収して透明シートとしての保護性能が低下する。   The material of the porous particles is not particularly limited, and both organic and inorganic materials can be used. However, it is preferable to use porous inorganic fine particles from the viewpoint of heat resistance. For example, calcium carbonate, magnesium carbonate, kaolin, clay, talc, hydrotalcite, aluminum silicate, calcium silicate, magnesium silicate, diatomaceous earth, alumina, colloidal alumina, aluminum hydroxide, boehmite structure alumina hydrate, pseudo boehmite structure And alumina hydrate, lithopone (a mixture of barium sulfate and zinc sulfide), zeolite and the like. The density of the pores can be controlled according to the content of the porous particles. The content of the porous particles is preferably about 1% to 30% with respect to the total amount of the emulsion. When the content is 1% or less, the water permeability is lowered and cracking is likely to occur. If it is 30% or more, the water permeability increases, the liquid is excessively absorbed, and the protective performance as a transparent sheet is lowered.

[1−2−8]中空樹脂粒子
中空粒子を用いて透明シート内に連泡構造を構成する場合には、中空粒子を含有する樹脂を主成分とする透明シートを基材シート上に製膜し、中空粒子の連結によって、基材シートと色材受容層との間を貫通する細孔を形成する。例えば、図38のように、ダイコーター655Aを用いて、中空粒子555を含有する樹脂材料から透明シート52を形成する。
[1-2-8] Hollow resin particles When the open cell structure is formed in the transparent sheet using the hollow particles, a transparent sheet mainly composed of a resin containing hollow particles is formed on the base sheet. Then, pores penetrating between the base material sheet and the colorant receiving layer are formed by the connection of the hollow particles. For example, as shown in FIG. 38, a transparent sheet 52 is formed from a resin material containing hollow particles 555 using a die coater 655A.

図38(a)の場合は、その透明シート52に対して、ダイコーター655Bを用いて色材受容層53を形成してから、ダイコーター65Cを用いて基準シート50を形成する。図38(b)の場合は、透明シート52に対して、ダイコーター65Cを用いて基準シート50を形成してから、ダイコーター655Bを用いて色材受容層53を形成する。図38(c)の場合は、予め用意した基準シート50に対して、ダイコーター655Aを用いて透明シート52を形成してから、ダイコーター655Bを用いて色材受容層53を形成する。この結果、図22(h)のように、中空粒子555の中空部分が連なる連泡構造の透明シート52を含む転写材1が製造される。   In the case of FIG. 38A, after forming the color material receiving layer 53 on the transparent sheet 52 using the die coater 655B, the reference sheet 50 is formed using the die coater 65C. In the case of FIG. 38B, the reference sheet 50 is formed on the transparent sheet 52 using the die coater 65C, and then the colorant receiving layer 53 is formed using the die coater 655B. In the case of FIG. 38C, the transparent sheet 52 is formed on the reference sheet 50 prepared in advance using the die coater 655A, and then the color material receiving layer 53 is formed using the die coater 655B. As a result, as shown in FIG. 22 (h), the transfer material 1 including the transparent sheet 52 having the open cell structure in which the hollow portions of the hollow particles 555 are continuous is manufactured.

中空樹脂粒子の材料は特に制限されず、有機物および無機物の両方用いることがきる。ただし、耐熱性の観点から、中空無機微粒子を用いることが好ましい。例えば、ガラス、シラス、シリカ、アルミナ、セラミックなどが挙げられる。中空粒子の含有量に応じて、細孔の密度が制御できる。中空粒子の含有量は、エマルジョンの合計量に対して1%〜30%程度が好ましい。それが1%以下になると、水の透過性が低下して、ひび割れが起こりやすくなる。それが30%以上になると、水の透過性が増加し、過剰に液体を吸収して透明シートとしての保護性能が低下する。   The material of the hollow resin particles is not particularly limited, and both organic and inorganic materials can be used. However, it is preferable to use hollow inorganic fine particles from the viewpoint of heat resistance. Examples thereof include glass, shirasu, silica, alumina, and ceramic. The density of the pores can be controlled according to the content of the hollow particles. The content of the hollow particles is preferably about 1% to 30% with respect to the total amount of the emulsion. If it is 1% or less, the water permeability decreases and cracking is likely to occur. When it becomes 30% or more, the water permeability increases, the liquid is excessively absorbed, and the protective performance as a transparent sheet is lowered.

中空粒子の材料は特に制限されず、無機物および有機物の両方を用いることができる。中空無機微粒子は耐熱性に優れており、例えば、ガラス、シラス、シリカ、アルミナ、セラミックなどを用いることができる。中空樹脂微粒子は、その製造方法によっていくつかの種類が存在し、例えば、下記(1)〜(5)の方法が挙げられる。
(1)ポリマー粒子中に発泡剤を含有させておき、後でこれを発泡させて、中空の粒子を得る方法。
(2)ポリマーにブタン等の揮発性物質を封入しておき、後にこれをガス化膨張させて中空の粒子を得る方法。
(3)ポリマーを溶融し、これに空気等のジェットを吹き付け、気泡を封入する方法。
(4)重合性モノマー成分を水中に分散して水中油滴型エマルジョンを作成し、重合して中空の粒子を得る方法。
(5)ポリマー粒子の内部にアルカリ膨潤性の物質を含有させておき、このポリマー粒子にアルカリ性液体を浸透させてアルカリ膨潤性物質を膨張させて中空の粒子を得る方法。
The material of the hollow particles is not particularly limited, and both inorganic and organic materials can be used. The hollow inorganic fine particles are excellent in heat resistance, and for example, glass, shirasu, silica, alumina, ceramic and the like can be used. There are several types of hollow resin fine particles depending on the production method, and examples thereof include the following methods (1) to (5).
(1) A method in which a foaming agent is contained in polymer particles, and this is subsequently foamed to obtain hollow particles.
(2) A method in which a volatile substance such as butane is encapsulated in a polymer, which is then gasified and expanded to obtain hollow particles.
(3) A method in which a polymer is melted, a jet of air or the like is sprayed thereon, and bubbles are enclosed.
(4) A method in which a polymerizable monomer component is dispersed in water to form an oil-in-water emulsion and polymerized to obtain hollow particles.
(5) A method in which an alkali-swellable substance is contained in the polymer particles, and an alkaline liquid is infiltrated into the polymer particles to expand the alkali-swellable substance to obtain hollow particles.

色材受容層を大気に連通させる細孔を基材シートと透明シートに形成するために、中空樹脂粒子を用いる場合には、その細孔を連泡構造とする必要がある。そのために使用する中空粒子としては、シェルに微細な穴があるものが好ましく、上記(1)〜(5)の中でも(4)または(5)の方法により製造された中空粒子が好ましい。上記(1)〜(3)により製造された中空粒子は、そのシェルに微細な穴がなく、透明シートに入れた場合に、水を系外に放出しにくい。中空粒子の含有量に応じて、細孔の密度が制御できる。中空粒子の含有量は、エマルジョンの合計量に対して1%〜30%程度が好ましい。それが1%以下になると、水の透過性が低下して、ひび割れが起こりやすくなる。それが30%以上になると、空隙に内容される空気の量が増加し、基材シートの断熱性が高くなり転写性能が低下するおそれがある。   When hollow resin particles are used to form pores that allow the colorant-receiving layer to communicate with the atmosphere in the base sheet and the transparent sheet, the pores must have a continuous cell structure. The hollow particles used for this purpose are preferably those having fine holes in the shell, and among the above (1) to (5), hollow particles produced by the method (4) or (5) are preferred. The hollow particles produced by the above (1) to (3) do not have fine holes in the shell, and are difficult to release water out of the system when placed in a transparent sheet. The density of the pores can be controlled according to the content of the hollow particles. The content of the hollow particles is preferably about 1% to 30% with respect to the total amount of the emulsion. If it is 1% or less, the water permeability decreases and cracking is likely to occur. If it becomes 30% or more, the amount of air contained in the voids increases, the heat insulating property of the base sheet becomes high, and the transfer performance may be lowered.

[1−2−9]延伸処理
透明フィルムとして、予め細孔構造を有するフィルムを用いてもよく、そのフィルムには、延伸処理を施すことによって細孔を形成することができる。例えば、図43のように、延伸加工装置656によって、透明シート52の素材となるフィルムを延伸させることによって、細孔521を形成することができる。
[1-2-9] Stretching Treatment A film having a pore structure in advance may be used as the transparent film, and pores can be formed on the film by subjecting it to a stretching treatment. For example, as illustrated in FIG. 43, the pores 521 can be formed by stretching a film that is a material of the transparent sheet 52 by a stretching apparatus 656.

透明シート52用のフィルムとしては、ポリテトラフルオロエチレン(PTFE)を延伸加工したePTFEフィルムと、ポリウレタンポリマーと、を複合化して作成された防水透湿フィルムを用いることができる。この場合には、1平方センチメートルに14億個の微細な孔を形成して、防水性と透湿性とを両立させることができる。そのフィルムの耐水圧は45000mm以上、透湿性は、JIS L1099B−2法の測定で13500g/m2/24hrsである。このようなフィルムは単層として用いることも可能であり、また透水性の他のフィルムと複層化して用いてもよく、透明シートとして基材シートに積層させることができる。すなわち、表裏を貫通する細孔構造が構成されている透明のフィルムであれば、転写材の透明シートとして用いることができる。そのフィルムとしては、ポリエチレンを主成分として、炭酸カルシウムを分散させたフィルムを延伸加工して得られる多孔質フィルム、およびポリオレフィンを主成分として無機フィラーレスで延伸加工した多孔質フィルムなどを用いることができる。これらのフィルムによっても安定した細孔構造が得られるため、それを、透水性もしくは防水透湿性の透明シートとして用いることができる。 As the film for the transparent sheet 52, a waterproof and moisture permeable film produced by combining an ePTFE film obtained by stretching polytetrafluoroethylene (PTFE) and a polyurethane polymer can be used. In this case, 1.4 billion fine holes can be formed in one square centimeter to achieve both waterproofness and moisture permeability. Its water pressure resistance of the film is 45000mm above, moisture permeability is 13500g / m 2 / 24hrs as measured in JIS L1099B-2 method. Such a film can be used as a single layer, or may be used as a multilayer with other water-permeable films, and can be laminated on a base sheet as a transparent sheet. That is, any transparent film having a pore structure penetrating the front and back can be used as a transparent sheet for a transfer material. As the film, it is possible to use a porous film obtained by stretching a film in which calcium carbonate is dispersed with polyethylene as a main component, and a porous film having a polyolefin as a main component and stretched without an inorganic filler. it can. Since these films can provide a stable pore structure, it can be used as a water-permeable or waterproof moisture-permeable transparent sheet.

[1−2−10]クレイズ処理
樹脂フィルムに細孔構造を構成する加工法は、上記の延伸処理に特定されず、クレイズ加工を用いてもよい。
[1-2-10] Crazing treatment The processing method for forming the pore structure in the resin film is not limited to the above-described stretching treatment, and crazing may be used.

例えば、図44のようなクレイズ加工装置651を用いて、樹脂フィルムに細孔構造を構成することができる。すなわちクレイズ処理部653によって、透明なポリフッ化ビニリデンのフィルム、つまり透明シート52の素材となるフィルム、その分子配向方向に対して略並行に所定の角度652で折り曲げ、その上面および下面に圧力を掛けながら矢印a方向に引っ張る。これにより、透明シート52の素材となるフィルムには、図45(a)のように、分子配向方向と略平行に、細かな連続的なひび状の模様を成す縞状のクレイズが形成され、そのクレイズによって細孔52Aが形成される。図45(b)のように、透明シート52の素材となるフィルムに、基材シート50を接合してから、それらをクレイズ処理した場合には、細孔52A,40Aが形成される。また図45(c)のように、透明シート52の素材となるフィルムに、基材シート50と色材受容層53とを接合してから、それらをクレイズ処理した場合には、細孔52A,40A,53Aが形成される。   For example, a pore structure can be formed in the resin film using a crazing apparatus 651 as shown in FIG. In other words, a transparent polyvinylidene fluoride film, that is, a film as a material of the transparent sheet 52, is bent at a predetermined angle 652 substantially in parallel with the molecular orientation direction by the craze processing unit 653, and pressure is applied to the upper and lower surfaces thereof. While pulling in the direction of arrow a. Thereby, in the film as the material of the transparent sheet 52, as shown in FIG. 45 (a), striped crazes forming a fine continuous cracked pattern are formed substantially parallel to the molecular orientation direction, The crazes form pores 52A. As shown in FIG. 45 (b), when the base sheet 50 is bonded to the film that is the material of the transparent sheet 52 and then subjected to crazing treatment, the pores 52A and 40A are formed. In addition, as shown in FIG. 45 (c), when the base material sheet 50 and the colorant receiving layer 53 are bonded to a film that is a material of the transparent sheet 52 and then subjected to a craze treatment, the pores 52A, 40A and 53A are formed.

クレイズには、樹脂フィルムの表面に現れる表面クレイズと、その内部に発生する内部クレイズがある。透明シート52には、それらのクレイズが連結して、透明シート52を貫通する細孔52Aが形成されればよい。つまり、クレイズ加工により、透明シート52用のフィルムには分子束(フィブリル)と孔(ボイド)とが形成され、それらが部分的に連結して、全体としてスポンジ構造を成すように貫通する細孔52Aが形成されればよい。このような細孔52Aが形成されたフィルムは、透水性もしくは防湿透湿性の透明シート52として使用することができる。また、クレイズは、熱処理等により緩和されて消失する場合もある。しかし、再度引っ張ることにより再び現れるため、クレイズ加工した透明シート52に適切な張力を掛けながら、それを基材シート50に積層することにより、透明シート52の細孔構造を調整することができる。また、細孔52Aの大きさは、クレイズ加工の際にフィルムを引っ張る力、およびフィルムの上面および下面に掛ける圧力などによって、調整することができる。また、ポリフッ化ビニリデンのフィルムをクレイズ加工することによって、細孔構造を構成することが可能であり、例えば、ポリスチレン、ポリエチレン、ポリプロピレン、ポリエステル、ポリアミド等のフィルムを用いることもできる。   The craze includes a surface craze that appears on the surface of the resin film and an internal craze that is generated inside. The transparent sheet 52 may be formed by connecting these crazes to form the pores 52 </ b> A penetrating the transparent sheet 52. In other words, molecular bundles (fibrils) and pores (voids) are formed in the film for the transparent sheet 52 by craze processing, and these are partially connected to each other so as to form a sponge structure as a whole. 52A may be formed. The film in which such pores 52A are formed can be used as a water-permeable or moisture-proof and moisture-permeable transparent sheet 52. In addition, the craze may be lost by being relaxed by heat treatment or the like. However, since it appears again by being pulled again, the pore structure of the transparent sheet 52 can be adjusted by laminating it on the base sheet 50 while applying an appropriate tension to the crazed transparent sheet 52. Further, the size of the pores 52A can be adjusted by the force of pulling the film during craze processing, the pressure applied to the upper and lower surfaces of the film, and the like. In addition, a pore structure can be formed by craze processing a polyvinylidene fluoride film. For example, films of polystyrene, polyethylene, polypropylene, polyester, polyamide, and the like can be used.

《透明シート製膜後に細孔処理》
[1−2−11]穿孔加工
図1(b)のように透明シート52が細孔構造を持たない場合には、種々の穿孔処理によって、透明シート52に細孔52Aを形成することができる。穿孔処理としては、図46(a),(b)のような針657、拍車650、および刃型などの機械的穿孔加工、あるいは図46(c)のようなレーザ加工装置658によるレーザ加工を用いることができる。
《Pore treatment after forming transparent sheet》
[1-2-11] Perforation Processing When the transparent sheet 52 does not have a pore structure as shown in FIG. 1B, the pores 52A can be formed in the transparent sheet 52 by various perforation processes. . As the drilling process, mechanical drilling such as a needle 657, a spur 650, and a blade shape as shown in FIGS. 46A and 46B, or laser processing using a laser processing device 658 as shown in FIG. 46C is performed. Can be used.

図39のように透明シート52単体に穿孔処理を施した後、同図(a)または(b)のように、その透明シート52に基材シート50と色材転写層53を積層してもよい。また、図40(a)または(b)のように、透明シート52と色材転写層53とを積層してから、透明シート52側または色材転写層53側から穿孔処理を施した後に、基材シート50を積層してもよい。また、図41のように透明シート52と基材シート50とを積層した後、同図(a),(b),(c)のように穿孔処理を施してから、色材転写層53を積層してもよい。図41(a)の場合は、透明シート52が穿孔処理され、図41(b)の場合は、透明シート52と基材シート50が透明シート52側から穿孔処理され、図41(c)の場合は、透明シート52と基材シート50が基材シート50側から穿孔処理される。また、図42のように透明シート52と基材シート50と色材転写層53とを積層した後、同図(a),(b),(c),(d)のように穿孔処理を施してもよい。図42(a)の場合は、透明シート52と基材シート50が基材シート50側から穿孔処理され、図42(b)の場合は、透明シート52と基材シート50と色材転写層53が基材シート50側から穿孔処理される。図42(c)の場合は、透明シート52と色材転写層53が色材転写層53側から穿孔処理され、図42(d)の場合は、透明シート52と基材シート50と色材転写層53が色材転写層53側から穿孔処理される。   After perforating the transparent sheet 52 as shown in FIG. 39, the base sheet 50 and the color material transfer layer 53 may be laminated on the transparent sheet 52 as shown in FIG. Good. Further, as shown in FIG. 40 (a) or (b), after laminating the transparent sheet 52 and the color material transfer layer 53, after performing a perforating process from the transparent sheet 52 side or the color material transfer layer 53 side, The base sheet 50 may be laminated. In addition, after laminating the transparent sheet 52 and the base sheet 50 as shown in FIG. 41, a perforation process is performed as shown in FIGS. You may laminate. In the case of FIG. 41 (a), the transparent sheet 52 is punched, and in the case of FIG. 41 (b), the transparent sheet 52 and the base sheet 50 are punched from the transparent sheet 52 side. In this case, the transparent sheet 52 and the base sheet 50 are perforated from the base sheet 50 side. Further, after laminating the transparent sheet 52, the base material sheet 50, and the color material transfer layer 53 as shown in FIG. 42, the punching process is performed as shown in FIGS. 42 (a), (b), (c), and (d). You may give it. In the case of FIG. 42 (a), the transparent sheet 52 and the base sheet 50 are perforated from the base sheet 50 side, and in the case of FIG. 42 (b), the transparent sheet 52, the base sheet 50, and the color material transfer layer. 53 is perforated from the substrate sheet 50 side. In the case of FIG. 42 (c), the transparent sheet 52 and the color material transfer layer 53 are perforated from the color material transfer layer 53 side, and in the case of FIG. 42 (d), the transparent sheet 52, the base sheet 50, and the color material. The transfer layer 53 is perforated from the color material transfer layer 53 side.

図42の例においては、反転画像72が形成される前の転写材1に対して、穿孔処理が施される。しかし、図24から図26のように、転写材1に反転画像72を記録(工程1)してから、穿孔処理を施してもよい。図24の場合は、同図(a),(b),(c),(d)のように、反転画像72が記録された転写材1に穿孔処理(穿孔工程)を施してから、色材転写層53を記録物の画像支持体55に転写(工程2)して、基材シート50を剥離(工程3)する。図25の場合は、色材転写層53を画像支持体55に転写(工程2)した後、穿孔処理(穿孔工程)を施してから、基材シート50を剥離(工程3)する。図26の場合は、色材転写層53を画像支持体55に転写(工程2)して、基材シート50を剥離(工程3)した後に、穿孔処理(穿孔工程)を施す。   In the example of FIG. 42, a punching process is performed on the transfer material 1 before the reverse image 72 is formed. However, as shown in FIGS. 24 to 26, the reverse image 72 may be recorded on the transfer material 1 (step 1) and then the punching process may be performed. In the case of FIG. 24, the transfer material 1 on which the reverse image 72 is recorded is subjected to a punching process (a punching process) as shown in FIGS. The material transfer layer 53 is transferred to the recorded image support 55 (step 2), and the base sheet 50 is peeled off (step 3). In the case of FIG. 25, after transferring the color material transfer layer 53 to the image support 55 (step 2), the substrate sheet 50 is peeled off (step 3) after being subjected to perforation processing (perforation step). In the case of FIG. 26, the color material transfer layer 53 is transferred to the image support 55 (step 2), the substrate sheet 50 is peeled off (step 3), and then a perforation process (perforation step) is performed.

このように、少なくとも記録物が実際に使用される前に、その表面を覆う透明シート52に貫通する細孔52Aが形成されていればよい。   Thus, at least before the recorded material is actually used, it is only necessary to form the pores 52A penetrating the transparent sheet 52 covering the surface.

[1−2−12]穿孔加工(針)
図46(a),(b)のように、透明シートに細孔構造を付与する簡単な加工方法としては、先端が鋭利に尖った針や刃型を押し付けて、透明シートを貫通する細孔を形成する方法がある。
[1-2-12] Drilling (needle)
As shown in FIGS. 46 (a) and 46 (b), as a simple processing method for imparting a pore structure to the transparent sheet, pores penetrating the transparent sheet by pressing a sharp-pointed needle or blade shape. There is a method of forming.

透明シートが薄膜の樹脂フィルムの場合は、小さく圧力による押し付け加工によって穿孔することが可能である。やや厚手の樹脂フィルムの場合は、ガラス転移温度の前後にまで樹脂フィルムを加熱した状態で機械的な穿孔加工を施すことによって、より安定した細孔構造を与えることが可能である。金属やセラミックスなどの先端を鋭利に加工した針列、針ローラ、拍車列、刃型、刃型ロールを用いることにより、好適な細孔構造を連続的に付与し、効率よく穿孔することができる。さらに、鋭利な先端に、ダイヤモンド加工などを施すことにより、その耐久性を向上させることができる。透明シートの穿孔加工は、前述したように、透明シート単体の他、基材シート上に積層された状態、色材受容層と積層された状態、または基材シート、透明シート、および色材受容層が順次積層された状態の透明シートに対して、行うことができる。透明シートが表面に露出した状態であれば、透明シートの表面側から機械的な穿孔加工を行うことが好ましい。透明シートが基材シートや色材受容層など他の層に挟まれている場合には、他の層の厚みや材質など機械的強度を考慮して、他の層側を介して透明シートを貫通する機械的な穿孔加工を施せばよい。この場合には、基材シートや色材受容層などにも微細な細孔が形成される。しかし、転写材の搬送性やインクジェット記録特性に影響がないよう留意して、細孔の径や密度を調整すればよい。   When the transparent sheet is a thin resin film, it can be perforated by pressing with a small pressure. In the case of a slightly thick resin film, it is possible to give a more stable pore structure by performing mechanical perforation while the resin film is heated to around the glass transition temperature. By using a needle row, needle roller, spur row, blade shape, blade shape roll with sharply machined tips of metal, ceramics, etc., a suitable pore structure can be continuously provided and drilled efficiently. . Furthermore, the durability can be improved by applying diamond processing or the like to the sharp tip. As described above, the perforation processing of the transparent sheet is performed in the state of being laminated on the base material sheet, the state of being laminated with the color material receiving layer, or the base material sheet, the transparent sheet, and the color material receiving as well as the transparent sheet alone. It can carry out with respect to the transparent sheet in the state where the layers were sequentially laminated. If the transparent sheet is exposed on the surface, it is preferable to perform mechanical perforation from the surface side of the transparent sheet. When the transparent sheet is sandwiched between other layers such as a base sheet or a colorant receiving layer, the transparent sheet is inserted through the other layer side in consideration of mechanical strength such as the thickness and material of the other layer. What is necessary is just to perform the mechanical drilling which penetrates. In this case, fine pores are also formed in the base material sheet and the color material receiving layer. However, the diameter and density of the pores may be adjusted taking care not to affect the transferability of the transfer material and the inkjet recording characteristics.

前述したように、画像支持体に色材受容層と透明シートが転写された後に、透明シートに穿孔加工を施すことも可能である。上記のように、透明シートが加熱された状態で機械的な穿孔加工を行うことが好ましいため、転写材を画像支持体に加熱圧着してから基材シートを剥離した直後に、機械的な穿孔加工を行うことが好ましい。先端が鋭利な拍車列によって穿孔加工を行う場合には、画像支持体の搬送排出機能を拍車列に持たせることも可能である。同様に、透明シートや転写材の製膜・積層工程中、および画像記録装置の中において、拍車列や針ローラなどを用いて穿孔加工を行う場合には、それらの拍車列や針ローラなどにフィルムの搬送機能を合わせて持たせることが可能である。このように、記録物に対して、透明シートを貫通する細孔構造を機械的に設けてもよく、その方法、装置構成は特に制限されない。   As described above, it is also possible to perforate the transparent sheet after the colorant receiving layer and the transparent sheet have been transferred to the image support. As described above, since it is preferable to perform mechanical perforation processing in a state where the transparent sheet is heated, mechanical perforation is performed immediately after the base material sheet is peeled off after heat-pressing the transfer material to the image support. It is preferable to perform processing. When punching is performed by a spur train having a sharp tip, the spur train can be provided with a function of conveying and discharging the image support. Similarly, when drilling is performed using spur trains, needle rollers, etc. during the film forming / laminating process of transparent sheets and transfer materials and in image recording devices, the spur trains, needle rollers, etc. It is possible to have a film transport function. As described above, the recorded material may be mechanically provided with a pore structure penetrating the transparent sheet, and the method and apparatus configuration are not particularly limited.

[1−2−13]穿孔加工(レーザ)
図46(c)のように、透明シートに細孔構造を付与する簡単な加工方法としては、レーザ加工装置658を用いる方法がある。
[1-2-13] Drilling (laser)
As shown in FIG. 46C, as a simple processing method for imparting a pore structure to the transparent sheet, there is a method using a laser processing apparatus 658.

透明シートが薄膜の樹脂フィルムの場合には、公知のレーザ加工装置を用いて、良好で安定した細孔構造を生産性良く付与することができる。例えば、特許公報第2706498号には、ワーク表面からの反射レーザ光のレベルを検知して、次の細孔の加工に移行するレーザ加工方法が記載されており、この加工方法を透明シートに細孔構造を付与する方法として適用可能である。透明シートに設けられる細孔の孔径は、レーザ光源の選定およびレーザ光の集光レンズなどの光学系の調整によって設定可能であり、また細孔の間隔は、反射ミラーなどによる光学走査系によって設定可能である。レーザ加工による穿孔加工は、機械的な穿孔加工と同様に、透明シート単体の他、基材シート上に積層された状態、色材受容層と積層された状態、または基材シート、透明シート、および色材受容層が順次積層された状態の透明シートに対して、行うことができる。透明シートが表面に露出した状態であれば、透明シートの表面側からレーザ光を照射して穿孔加工を行うことが好ましい。また、透明シートが基材シートや色材受容層など他の層に挟まれている場合には、透明シートの光吸収特性と、他の層の厚みや材質などの光学的特性と、を考慮して、他の層側からレーザ光を照射することにより透明シートの穿孔加工が可能である。この場合には、基材シートや色材受容層などにも微細な細孔が形成されることがある。しかし、転写材の搬送性やインクジェット記録特性に影響がないように留意して、細孔の径や密度を調整すればよい。また、必要に応じて、レーザ光の照射側とは反対側になる他の層の表面に、レーザ光の反射膜などを設けて、透明シートが効率的にレーザ光を吸収できるようにしてもよい。さらに、透明シートの樹脂に、予め、レーザ光を吸収しやすい微粒子を分散させておいて、レーザ光による穿孔加工性を向上させてもよい。   When the transparent sheet is a thin resin film, a well-known and stable pore structure can be imparted with high productivity using a known laser processing apparatus. For example, Japanese Patent Publication No. 2706498 describes a laser processing method in which the level of reflected laser light from the workpiece surface is detected and the processing proceeds to processing of the next pore, and this processing method is detailed on a transparent sheet. It can be applied as a method for imparting a pore structure. The hole diameter of the pores provided in the transparent sheet can be set by selecting the laser light source and adjusting the optical system such as the laser beam condenser lens, and the interval between the pores is set by the optical scanning system such as a reflection mirror Is possible. The drilling process by laser processing is the same as the mechanical drilling process, in addition to the transparent sheet alone, the state laminated on the base sheet, the state laminated with the colorant receiving layer, or the base sheet, transparent sheet, And the transparent sheet in which the colorant receiving layers are sequentially laminated. If the transparent sheet is exposed on the surface, it is preferable to perform perforation by irradiating laser light from the surface side of the transparent sheet. In addition, when the transparent sheet is sandwiched between other layers such as a base sheet or a colorant receiving layer, the light absorption characteristics of the transparent sheet and the optical characteristics such as the thickness and material of the other layers are considered. Then, the transparent sheet can be perforated by irradiating laser light from the other layer side. In this case, fine pores may be formed in the base material sheet and the colorant receiving layer. However, the diameter and density of the pores may be adjusted taking care not to affect the transferability of the transfer material and the ink jet recording characteristics. In addition, if necessary, a laser light reflection film or the like may be provided on the surface of the other layer opposite to the laser light irradiation side so that the transparent sheet can efficiently absorb the laser light. Good. In addition, fine particles that easily absorb laser light may be dispersed in the resin of the transparent sheet in advance to improve the drilling workability by laser light.

[1−3]基材シート
本実施形態の転写材は、図1(b)の転写材1と同様に基材シート50を備えている。基材シート(「剥離ライナー」、「セパレータ」とも称される。)は、後述する離型層または色材受容層の支持体となるシート体である。
[1-3] Base Material Sheet The transfer material of this embodiment includes a base material sheet 50 as in the case of the transfer material 1 in FIG. A base sheet (also referred to as “release liner” or “separator”) is a sheet body that serves as a support for a release layer or a colorant receiving layer described later.

基材シートの材質については、前述したように、基材シートのSP値と色材受容層のSP値との差SP1が式(10)を満たす材料であることが好ましく、また基材シートの材料としては樹脂フィルム等を挙げることができる。例えば、基材シートとして、従来の熱転写シートの基材フィルムとして利用されていた樹脂フィルム等をそのまま利用することができる。   As for the material of the base sheet, as described above, it is preferable that the difference SP1 between the SP value of the base sheet and the SP value of the colorant receiving layer satisfies the formula (10). Examples of the material include a resin film. For example, a resin film that has been used as a base film of a conventional thermal transfer sheet can be used as it is as the base sheet.

基材シートの形成材料としては、例えば、ポリエステル(PET等)、ナイロン(脂肪族ポリアミド)、ポリイミド、酢酸セルロース、セロハン、ポリエチレン、ポリプロピレン、ポリスチレン、ポリカーボネート、ポリビニルアルコール、ポリ塩化ビニル、ポリ塩化ビニリデン、塩化ゴム、フッ素樹脂、アイオノマー等の樹脂からなる樹脂フィルム;等が好ましい。これらの中でも、耐熱性に優れるPETフィルムが好ましい。樹脂フィルムは、1種を単独で用いること、または2種以上を複合あるいは積層して用いることができる。   Examples of the material for forming the base sheet include polyester (PET, etc.), nylon (aliphatic polyamide), polyimide, cellulose acetate, cellophane, polyethylene, polypropylene, polystyrene, polycarbonate, polyvinyl alcohol, polyvinyl chloride, polyvinylidene chloride, A resin film made of a resin such as chlorinated rubber, fluororesin, or ionomer is preferred. Among these, a PET film having excellent heat resistance is preferable. The resin film can be used alone or in combination of two or more.

基材シートの厚さは、材料強度等を考慮して適宜決定すればよく、特に制限はない。ただし、基材シートの厚さは、5〜200μmであることが好ましい。基材シートの厚さを好ましくは5μm以上、さらに好ましくは10μm以上とすることにより、色材受容層を積層した際に、その積層体のカールを防止することができる。転写材をロール状とする場合には、転写材の製造装置上での搬送性を向上させるために、転写材の厚さを15μm以上とすることが好ましい。転写材をカットシート状とする場合には、カットシートのカールを防止する観点から、転写材の厚さを30μm以上とすることが好ましい。   The thickness of the substrate sheet may be appropriately determined in consideration of material strength and the like, and is not particularly limited. However, the thickness of the base sheet is preferably 5 to 200 μm. By setting the thickness of the base sheet to preferably 5 μm or more, and more preferably 10 μm or more, curling of the laminate can be prevented when the colorant receiving layer is laminated. When the transfer material is in a roll shape, it is preferable that the thickness of the transfer material is 15 μm or more in order to improve transportability on the transfer material manufacturing apparatus. When the transfer material is cut sheet, the thickness of the transfer material is preferably 30 μm or more from the viewpoint of preventing curling of the cut sheet.

一方、基材シートの厚さを200μm以下、好ましくは60μm以下、さらに好ましくは50μm以下とすることにより、転写材を画像支持体に加熱圧着させる場合の熱伝達性を良好とすることができる。   On the other hand, when the thickness of the substrate sheet is 200 μm or less, preferably 60 μm or less, more preferably 50 μm or less, the heat transfer property when the transfer material is heat-pressed to the image support can be improved.

[1−4]離型層
転写材は、図1(c)の転写材1のように離型層51を備えていてもよい。離型層51は、離型剤を含有する組成物からなる層であり、基材シート50と透明シート52との間に設けられる。離型層51を備えることによって、透明シート52から基材シート50を容易に剥離することができる。
[1-4] Release Layer The transfer material may include a release layer 51 like the transfer material 1 in FIG. The release layer 51 is a layer made of a composition containing a release agent, and is provided between the base sheet 50 and the transparent sheet 52. By providing the release layer 51, the base sheet 50 can be easily peeled from the transparent sheet 52.

離型剤の種類としては特に制限はなく、離型性に優れ、ヒートローラやサーマル式のインクジェット記録ヘッドが発生する熱で容易に溶融しない材料であることが好ましい。例えば、シリコーンワックス等のワックス類に代表されるシリコーンワックス、シリコーン樹脂等のシリコーン系材料;フッ素樹脂等のフッ素系材料;は、離型性に優れる点において好ましい。   The type of release agent is not particularly limited, and is preferably a material that is excellent in releasability and is not easily melted by heat generated by a heat roller or a thermal ink jet recording head. For example, silicone waxes typified by waxes such as silicone wax, silicone-based materials such as silicone resins, and fluorine-based materials such as fluororesins are preferable in terms of excellent releasability.

離型層の厚さは、剥離性等を考慮して適宜決定すればよく、特に制限はない。ただし、離型層の厚さは、乾燥状態で0.1〜10μmであることが好ましい。離型層の厚さを好ましくは0.1μm以上、さらに好ましくは1μm以上とすることにより、基材シートと透明シートとの融着を抑制することができる。一方、離型層の厚さを好ましくは10μm以下、さらに好ましくは5μm以下とすることにより、転写材を画像支持体に加熱圧着させる場合の熱伝達性を良好とすることができる。   The thickness of the release layer may be appropriately determined in consideration of peelability and the like, and is not particularly limited. However, the thickness of the release layer is preferably 0.1 to 10 μm in a dry state. By setting the thickness of the release layer to preferably 0.1 μm or more, more preferably 1 μm or more, it is possible to suppress the fusion between the base sheet and the transparent sheet. On the other hand, when the thickness of the release layer is preferably 10 μm or less, more preferably 5 μm or less, the heat transfer property when the transfer material is heat-pressed to the image support can be improved.

なお、透明シートの表面に艶消し(マット)加工を行う場合には、離型層に各種粒子を含有させること、または透明シートに当接する側の離型層の表面をマット処理しておくことが好ましい。マット加工は、透明シートの光沢感を適度に制御することができる点において有である。   In addition, when matte (matte) processing is performed on the surface of the transparent sheet, the release layer contains various particles, or the surface of the release layer on the side in contact with the transparent sheet is matted. Is preferred. The mat processing is advantageous in that the glossiness of the transparent sheet can be appropriately controlled.

[1−5]アンカー層
転写材は、図1(c)の転写材1のようにアンカー層59をさらに備えてもよい。
[1-5] Anchor Layer The transfer material may further include an anchor layer 59 like the transfer material 1 in FIG.

アンカー層59は、透明シート52と色材受容層53との間に配置される。アンカー層を備えることにより、透明シートと色材受容層との接着強度を向上させて、それらの接着強度の不足による透明シートからの色材受容層の剥離を抑制することができる。アンカー層は、色材受容層の水溶性樹脂のけん化度や分子量を上述した範囲にすることにより、色材受容層と透明シートの接着性を向上させ、その相乗効果により高い接着性を得ることができる。透明シートと色材受容層の間に設けられるアンカー層は、透明シートと同様に水分を系外に放出する必要がある。そのため、透明シートに細孔構造を付与するための処理をアンカー層に対しても行って、透明シートとアンカー層を貫通する細孔を形成することが好ましい。   The anchor layer 59 is disposed between the transparent sheet 52 and the color material receiving layer 53. By providing the anchor layer, the adhesive strength between the transparent sheet and the color material receiving layer can be improved, and peeling of the color material receiving layer from the transparent sheet due to a lack of the adhesive strength can be suppressed. The anchor layer improves the adhesiveness between the colorant-receiving layer and the transparent sheet by setting the saponification degree and molecular weight of the water-soluble resin of the colorant-receiving layer to the above-mentioned ranges, and obtains high adhesiveness due to its synergistic effect. Can do. The anchor layer provided between the transparent sheet and the colorant receiving layer needs to release moisture out of the system in the same manner as the transparent sheet. Therefore, it is preferable to perform the treatment for imparting a pore structure to the transparent sheet also on the anchor layer to form pores penetrating the transparent sheet and the anchor layer.

また、表面改質処理として、色材受容層を塗工する透明シート52の表面に、予めコロナ放電処理やプラズマ放電処理を施したり、IPAやアセトン等の有機溶剤を塗工して透明シート52の表面をあらしたりしてもよい。このようなアンカー層の処理により、塗れ性を改良して密着性を向上させることができる。このように、アンカー層の形成や表面処理により、色材受容層53と透明シート52との結着性を高めて、膜強度を上げ、透明シート52の剥がれを防止することができる。   Further, as the surface modification treatment, the surface of the transparent sheet 52 to be coated with the colorant receiving layer is previously subjected to corona discharge treatment or plasma discharge treatment, or an organic solvent such as IPA or acetone is applied to the transparent sheet 52. Or the surface of the By such treatment of the anchor layer, paintability can be improved and adhesion can be improved. Thus, by forming the anchor layer or performing the surface treatment, the binding property between the colorant receiving layer 53 and the transparent sheet 52 can be increased, the film strength can be increased, and the peeling of the transparent sheet 52 can be prevented.

このような、アンカー層59としては、結着性を高めるものとして、例えば、熱可塑性の合成樹脂、天然樹脂、ゴム、ワックス等を用いて形成することができる。より具体的には、エチルセルロース、セルロースアセテートプロピオネート等のセルロース誘導体、ポリスチレン、ポリα−メチルスチレン等のスチレン系樹脂、ポリメタクリル酸メチル、ポリアクリル酸エチル等のアクリル系樹脂、ポリ塩化ビニル、ポリ酢酸ビニル、塩化ビニル−酢酸ビニル共重合体、ポリビニルブチラール、ポリビニルアセタール等のビニル系樹脂、ポリエステル樹脂、ポリアミド樹脂、エポキシ樹脂、ポリウレタン樹脂、アイオノマー、エチレンアクリル酸共重合体、エチレン−アクリル酸エステル共重合体等の合成樹脂、粘着性付与剤としてのロジン、ロジン変性マレイン酸樹脂、エステルガム、ポリイソブチレンゴム、ブチルゴム、スチレンブタジエンゴム、ブタジエンアクリロニトリルゴム、ポリアミド樹脂、ポリ塩素化オレフィン等の天然樹脂や合成ゴムの誘導体等を挙げることができる。   Such an anchor layer 59 can be formed using, for example, a thermoplastic synthetic resin, a natural resin, rubber, wax, or the like as a material that enhances the binding property. More specifically, cellulose derivatives such as ethyl cellulose, cellulose acetate propionate, styrene resins such as polystyrene and poly α-methylstyrene, acrylic resins such as polymethyl methacrylate and polyethyl acrylate, polyvinyl chloride, Polyvinyl acetate, vinyl chloride-vinyl acetate copolymer, polyvinyl resins such as polyvinyl butyral, polyvinyl acetal, polyester resin, polyamide resin, epoxy resin, polyurethane resin, ionomer, ethylene acrylic acid copolymer, ethylene-acrylic acid ester Synthetic resins such as copolymers, rosin as tackifier, rosin modified maleic resin, ester gum, polyisobutylene rubber, butyl rubber, styrene butadiene rubber, butadiene acrylonitrile rubber, polyamide resin, It can be mentioned derivatives of natural resins and synthetic rubber such as Li chlorinated olefins.

アンカー層59は、後述する付着工程時のヒートローラによる熱処理によって、溶融させることが好ましい。アンカー層59の溶融により、色材受容層53及び透明シート52の表面の凹凸の影響を受けることなく、色材受容層53と透明シート52の結着性をより強固なものとすることができる。そのためアンカー層59は、ガラス転移温度(Tg)が好ましくは60〜160℃、さらに好ましくは70〜140℃、特に好ましくは70〜100℃の熱可塑性樹脂によって形成することが好ましい。一方、その温度範囲が160℃以上の場合には、過剰な熱エネルギーにより熱可塑性樹脂が熱変形するため、良好な接着が行われなくなる。   The anchor layer 59 is preferably melted by heat treatment with a heat roller during an adhesion process described later. Due to the melting of the anchor layer 59, the binding property between the color material receiving layer 53 and the transparent sheet 52 can be made stronger without being affected by the unevenness of the surfaces of the color material receiving layer 53 and the transparent sheet 52. . Therefore, the anchor layer 59 is preferably formed of a thermoplastic resin having a glass transition temperature (Tg) of preferably 60 to 160 ° C, more preferably 70 to 140 ° C, and particularly preferably 70 to 100 ° C. On the other hand, when the temperature range is 160 ° C. or higher, the thermoplastic resin is thermally deformed by excessive thermal energy, and thus good adhesion cannot be performed.

[1−6]ホログラム層
転写材は、図1(c)の転写材1のようにホログラム層58をさらに備えてもよい。ホログラム層58は、三次元像が記録された層であり、透明シート52と色材受容層53との間に配置される。透明シートと色材受容層との間に設けられるホログラム層は、透明シートと同様に水分を系外に放出する必要がある。そのため、透明シートに細孔構造を付与するための処理をホログラム層に対しても行って、透明シートとホログラム層を貫通する細孔を形成することが好ましい。ホログラム層を備えることにより、記録物(クレジットカード等)の偽造を防止する効果が得られる。ホログラム層の構成に特に制限はなく、従来公知の構成を採用することができる。例えば、レリーフホログラム等を挙げることができる。
[1-6] Hologram Layer The transfer material may further include a hologram layer 58 like the transfer material 1 in FIG. The hologram layer 58 is a layer in which a three-dimensional image is recorded, and is disposed between the transparent sheet 52 and the color material receiving layer 53. The hologram layer provided between the transparent sheet and the colorant receiving layer needs to release moisture out of the system in the same manner as the transparent sheet. Therefore, it is preferable to perform a process for imparting a pore structure to the transparent sheet also on the hologram layer to form pores penetrating the transparent sheet and the hologram layer. By providing the hologram layer, an effect of preventing forgery of recorded matter (credit card or the like) can be obtained. There is no restriction | limiting in particular in the structure of a hologram layer, A conventionally well-known structure is employable. For example, a relief hologram can be mentioned.

アンカー層59を設けられる場合には、図1(c)のように、アンカー層59と透明シート52の間にホログラム層58を設けることができる。ホログラム層58は、一般に樹脂層によって構成され、その層自体は単一構造でもよく、また多層構造でもよい。また、ホログラム層は、平面型ホログラムおよび体積型ホログラムのいずれでもよく、平面型ホログラムの場合、なかでもレリーフホログラムの場合には量産性及びコストの面から好ましい。   When the anchor layer 59 is provided, the hologram layer 58 can be provided between the anchor layer 59 and the transparent sheet 52 as shown in FIG. The hologram layer 58 is generally composed of a resin layer, and the layer itself may have a single structure or a multilayer structure. The hologram layer may be either a planar hologram or a volume hologram, and is preferably a planar hologram, particularly a relief hologram, from the viewpoints of mass productivity and cost.

その他、フレネルホログラム、フラウンホーファーホログラム、レンズレスフーリエ変換ホログラム、イメージホログラム等のレーザ再生ホログラム、及び、レインボーホログラム等の白色光再生ホログラム、さらにそれらの原理を利用したカラーホログラム、コンピュータホログラム、ホログラムディスプレイ、マルチプレックスホログラム、ホログラフィックステレオグラム、ホログラフィック回折格子等を用いることができる。   In addition, Fresnel holograms, Fraunhofer holograms, lensless Fourier transform holograms, laser reproduction holograms such as image holograms, and white light reproduction holograms such as rainbow holograms, color holograms using these principles, computer holograms, hologram displays, Multiplex holograms, holographic stereograms, holographic diffraction gratings and the like can be used.

干渉縞を記録するためのホログラム形成用の感光材料としては、銀塩、重クロム酸ゼラチン、サーモプラスチックス、ジアゾ系感光材料フォトレジスト、強誘電体、フォトクロミックス材料、カルコゲンガラス等が使用できる。また、ホログラム形成層の材質として、ポリ塩化ビニル、アクリル樹脂(例えば、ポリメチルメタアクリレート)、ポリスチレン、ポリカーボネート等の熱可塑性樹脂、そして、不飽和ポリエステル、メラミン、エポキシ、ポリエステル(メタ)アクリレート、ウレタン(メタ)アクリレート、エポキシ(メタ)アクリレート、ポリエーテル(メタ)アクリレート、ポリオール(メタ)アクリレート、メラミン(メタ)アクリレート、トリアジン系アクリレート等の熱硬化性樹脂を硬化させたもの、又は、上記熱可塑性樹脂と熱硬化性樹脂との混合物が使用可能である。   As a photosensitive material for forming a hologram for recording interference fringes, silver salt, dichromated gelatin, thermoplastics, diazo photosensitive material photoresist, ferroelectric, photochromic material, chalcogen glass, and the like can be used. Moreover, as a material of the hologram forming layer, thermoplastic resins such as polyvinyl chloride, acrylic resin (for example, polymethyl methacrylate), polystyrene, polycarbonate, and unsaturated polyester, melamine, epoxy, polyester (meth) acrylate, urethane Cured thermosetting resins such as (meth) acrylate, epoxy (meth) acrylate, polyether (meth) acrylate, polyol (meth) acrylate, melamine (meth) acrylate, triazine acrylate, or the above thermoplastics A mixture of a resin and a thermosetting resin can be used.

さらに、ホログラム層58の材質として、ラジカル重合性不飽和基を有する熱成形性物質の使用が可能である。ホログラム層58は、従来既知の方法によって形成することができる。例えば、透明型ホログラムがレリーフホログラムである場合には、干渉縞が凹凸の形で記録されたホログラム原版をプレス型として用いる。そして、このホログラム原版上にホログラム形成用樹脂シートを置いて、加熱ロール等の手段によって両者を加熱圧着し、ホログラム形成用の樹脂シートの表面にホログラム原版の凹凸模様を複製する。このような方法によって、レリーフ形成面を有するホログラム形成層を得ることができる。   Further, as the material of the hologram layer 58, a thermoformable substance having a radical polymerizable unsaturated group can be used. The hologram layer 58 can be formed by a conventionally known method. For example, when the transparent hologram is a relief hologram, a hologram master on which interference fringes are recorded in an uneven shape is used as a press die. Then, a hologram forming resin sheet is placed on the hologram original plate, and both are heat-pressed by means of a heating roll or the like, and the uneven pattern of the hologram original plate is replicated on the surface of the hologram forming resin sheet. By such a method, a hologram forming layer having a relief forming surface can be obtained.

[1−7]積層構造
転写材は、基本的には、図1(b)および図22の転写材1のように、基材シート50、透明シート52、及び色材受容層53が順次積層された積層構造である。「基材シート、透明シート、及び色材受容層が順次積層」とは、基材シート、透明シート、および色材受容層の相互間に他の層が介在するか否かに拘わらず、基材シート、透明シート、および色材受容層がその順序に従って積層されていることを意味する。そのため、図1(c)の転写材1のように、透明シート52と色材受容層53との間にアンカー層59やホログラム層58が存在する構造も、「基材シート、透明シート、及び色材受容層が順次積層」された積層構造に含まれる。
[1-7] Laminated Structure Basically, the transfer material is formed by sequentially laminating the base material sheet 50, the transparent sheet 52, and the color material receiving layer 53 as in the transfer material 1 of FIGS. It is the laminated structure made. “Substrate sheet, transparent sheet, and color material receiving layer are sequentially laminated” means that the base sheet, transparent sheet, and color material receiving layer are stacked regardless of whether or not another layer is interposed between them. It means that the material sheet, the transparent sheet, and the color material receiving layer are laminated in that order. Therefore, as in the transfer material 1 in FIG. 1C, the structure in which the anchor layer 59 and the hologram layer 58 exist between the transparent sheet 52 and the color material receiving layer 53 is also “base material sheet, transparent sheet, and It is included in the laminated structure in which the color material receiving layers are sequentially laminated.

転写材は、図1(c)および図22の転写材1のように、基材シート50、透明シート52、色材受容層53が相互に当接された積層構造であることが好ましい。すなわち、基材シート50と透明シート52、透明シート52と色材受容層53の間に、他の層(シートも含む。)が介在していない構造が好ましい。記録物の対象物となるクレジットカード等は厚さの制限が厳格であるため、積層される層やシートの数を減じて、記録物を薄厚化することが望ましいからである。   The transfer material preferably has a laminated structure in which the base material sheet 50, the transparent sheet 52, and the color material receiving layer 53 are in contact with each other as in the transfer material 1 of FIGS. That is, a structure in which other layers (including sheets) are not interposed between the base sheet 50 and the transparent sheet 52 and between the transparent sheet 52 and the colorant receiving layer 53 is preferable. This is because the thickness of a credit card or the like, which is an object of the recorded material, is strict, and it is desirable to reduce the thickness of the recorded material by reducing the number of stacked layers and sheets.

図1(c)のように、転写材1が離型層51、アンカー層59、ホログラム層58を備える場合には、色材受容層53、アンカー層59、ホログラム層58、透明シート52、離型層51、及び基材シート50が順次積層された積層構造とすることが好ましい。   As shown in FIG. 1C, when the transfer material 1 includes a release layer 51, an anchor layer 59, and a hologram layer 58, a color material receiving layer 53, an anchor layer 59, a hologram layer 58, a transparent sheet 52, a release sheet 52, It is preferable to have a laminated structure in which the mold layer 51 and the base sheet 50 are sequentially laminated.

[1−8]転写材の形状と厚さ
転写材は、後述する画像記録装置や記録物の製造装置の構造に合わせて、ロール状又はシート状(カットシート状)であってもよい。ロール状の転写材の場合、色材受容層は外側にしても内側にしてもよい。しかし、後述する画像記録装置の搬送機構に最適に対応するように、色材受容層を外側とし、基材シートを内側とするロール状が好ましい。
[1-8] Shape and Thickness of Transfer Material The transfer material may be in a roll shape or a sheet shape (cut sheet shape) according to the structure of an image recording apparatus or a recorded product manufacturing apparatus described later. In the case of a roll-shaped transfer material, the color material receiving layer may be on the outside or the inside. However, a roll shape in which the color material receiving layer is on the outside and the base sheet is on the inside is preferable so as to optimally correspond to the conveyance mechanism of the image recording apparatus described later.

基材シートの厚さは、色材受容層の厚さの1.5〜5倍であることが好ましい。それを1.5倍以上とすることにより、シート状(カットシート状)の転写材のカールを防止して、画像記録装置や記録物の製造装置における転写材の搬送性を良好にすることができる。一方、それを5倍以下とすることにより、画像支持体に転写材を加熱圧着させる際の熱伝達性を良好にすることができる。   The thickness of the base sheet is preferably 1.5 to 5 times the thickness of the colorant receiving layer. By making it 1.5 times or more, curling of a sheet-like (cut sheet-like) transfer material can be prevented, and transferability of the transfer material in an image recording apparatus or recorded product manufacturing apparatus can be improved. it can. On the other hand, by making it 5 times or less, it is possible to improve the heat transfer property when the transfer material is heat-pressed on the image support.

転写材は、熱時剥離型であってもよいし、冷時剥離型であってもよい。熱時剥離型の転写材は、画像支持体と転写材を加熱圧着させた後、それら両部材の積層体の温度が高い状態のまま、基材シートを剥離することが最適な転写材である。一方、冷時剥離型の転写材は、画像支持体と転写材を加熱圧着させた後、それら両部材の積層体の温度が低下した状態で基材シートを剥離することが最適な転写材である。   The transfer material may be a hot peeling type or a cold peeling type. The heat-peelable transfer material is an optimal transfer material for exfoliating the base sheet while the temperature of the laminate of both members is high after the image support and the transfer material are heat-pressed. . On the other hand, the cold-peeling transfer material is an optimal transfer material in which after the image support and the transfer material are heat-bonded, the base sheet is peeled in a state where the temperature of the laminate of these two members is lowered. is there.

熱時剥離型の転写材は、画像支持体に転写材を加熱圧着させた後、直ぐに基材シートを剥離することができるため、生産性の面で優れている。例えば、ロール状の転写材を用いて、基材シートの剥離をロール・ツー・ロール(roll to roll)で行うことにより、生産性を向上させることができる。一方、冷時剥離型の転写材は、画像支持体と転写材を加熱圧着させた後、両部材の積層体の温度が低下してからの基材シートの剥離が可能である。そのため、シート状(カットシート状)の転写材を用いる場合等には、画像支持体と転写材を加熱圧着させた後、基材シートを剥離する際のハンドリングが容易になる。   The heat-peeling transfer material is excellent in productivity because the substrate sheet can be peeled immediately after the transfer material is heat-pressed on the image support. For example, productivity can be improved by performing peeling of a base material sheet by a roll-to-roll (roll to roll) using a roll-shaped transfer material. On the other hand, the cold-peeling transfer material can peel the substrate sheet after the temperature of the laminate of both members is lowered after the image support and the transfer material are heat-pressed. For this reason, when a sheet-like (cut sheet-like) transfer material is used, handling when the substrate sheet is peeled after the image support and the transfer material are heat-pressed is facilitated.

[1−9]製造方法
転写材は、前述したように、透明シートの製膜工程中もしくはその後工程において、透明シートの構成材料中に成分として含まれる材料が連泡構造の細孔を構成(発泡(図36)、多孔質粒子(図37)、中空粒子(図38))することができる。また、穿孔(図39,図40)によって連泡構造の細孔を構成することもできる。このような透明シートを基材シート上にラミネート(図39,図40)または積層接着させ、その後、色材受容層を形成する塗工液を塗工することによって、転写材を製造することができる。また、基材シート上に透明シートの製膜した後、別の手段により透明シートに所望の細孔処理を施して、その後、色材受容層を形成する塗工液を塗工することによって、転写材を製造することができる。また、基材シート及び透明シートが順次積層された積層体に、色材受容層を形成する塗工液を塗工した後に、別の手段により透明シートに所望の細孔処理(図41,図42)を施すことによって、転写材を製造することができる。また、基材シート及び透明シートが順次積層された積層体に、色材受容層を形成する塗工液を塗工した後に、色材受容層に画像を記録してから、別の手段により透明シートに所望の細孔処理(図41,図42)を施すこともできる。なお、以下の記載においては、転写材の項等で既に説明した事項については割愛し、製造方法固有の事項のみ説明する。
[1-9] Manufacturing Method As described above, in the transfer material, the material contained as a component in the constituent material of the transparent sheet constitutes the pores of the open cell structure in the film forming process of the transparent sheet or in the subsequent process ( Foaming (FIG. 36), porous particles (FIG. 37), and hollow particles (FIG. 38)). In addition, pores having an open cell structure can be formed by perforation (FIGS. 39 and 40). A transfer material can be produced by laminating (FIG. 39, FIG. 40) or laminating and bonding such a transparent sheet on a base sheet, and then applying a coating liquid for forming a colorant receiving layer. it can. In addition, after forming a transparent sheet on the substrate sheet, by applying a desired pore treatment to the transparent sheet by another means, and then coating a coating liquid for forming a colorant receiving layer, A transfer material can be manufactured. In addition, after applying a coating liquid for forming a colorant receiving layer to a laminate in which a base sheet and a transparent sheet are sequentially laminated, a desired pore treatment (FIG. 41, FIG. By applying 42), a transfer material can be manufactured. In addition, after applying a coating solution for forming a color material receiving layer to a laminate in which a base sheet and a transparent sheet are sequentially laminated, an image is recorded on the color material receiving layer and then transparent by another means. Desired pore processing (FIGS. 41 and 42) can be applied to the sheet. In the following description, items already described in the transfer material section are omitted, and only items specific to the manufacturing method are described.

[1−9−1]透明シート
透明シートとしては、予め表面改質が行われたものを用いてもよい。透明シートの表面を粗面化する表面改質を行うことにより、透明シートの濡れ性が向上し、色材受容層やアンカー層との密着性を向上させることができる場合がある。表面改質の方法は、特に制限されない。例えば、透明シートの表面に、予めコロナ放電処理やプラズマ放電処理を行う方法;透明シートの表面にIPAやアセトン等の有機溶剤を塗工する方法;等を挙げることができる。これらの表面処理により、色材受容層と透明シートとの結着性が高まり、強度が向上し、透明シートからの材受容層の剥離を抑制することができる。
[1-9-1] Transparent sheet As the transparent sheet, a sheet that has been surface-modified in advance may be used. By performing surface modification that roughens the surface of the transparent sheet, the wettability of the transparent sheet may be improved, and the adhesion to the colorant receiving layer or the anchor layer may be improved. The method for surface modification is not particularly limited. For example, a method of previously performing corona discharge treatment or plasma discharge treatment on the surface of the transparent sheet; a method of applying an organic solvent such as IPA or acetone on the surface of the transparent sheet; By these surface treatments, the binding property between the color material receiving layer and the transparent sheet is increased, the strength is improved, and the peeling of the material receiving layer from the transparent sheet can be suppressed.

透明シートは、他の層やシートとの積層体とした状態で用いてもよい。例えば、アンカー層、透明シート、離型剤を含有する組成物からなる離型層、および基材シートが順次積層された積層シートを用いることが好ましい。   You may use a transparent sheet in the state made into the laminated body with another layer and a sheet | seat. For example, it is preferable to use a laminated sheet in which an anchor layer, a transparent sheet, a release layer composed of a composition containing a release agent, and a base sheet are sequentially laminated.

透明シートの形成は、透明シートに2種類のエマルション溶液および、前記エマルション溶液に発泡材や中空粒子、多孔質粒子を含有させた塗工液を、ロールコーティング法、ロッドバーコーティング法、スプレーコーティング法、エアナイフコーティング法、スロットダイコーティング法等により基材上に塗工し、乾燥させることで行なうことができる。このとき、塗工後の乾燥温度をエマルジョンE1のTg以上、エマルジョンE2のTg未満とすることが好ましい。この温度で透明シートを作成することにより、エマルジョンの一方を造膜し、他方が粒子として残存している透明シートを製造することができる。透明シート形成時に、Tg2以上の温度で加熱乾燥するとE1とE2が両方とも造膜した状態となり、剥離工程において、クラックが入りにくくなり、十分な端部の切れ性、基材シートからの剥離性、べたつき防止が得られない。一方、透明シート形成時にTg1より小さい温度で加熱してしまうと、エマルジョンE1,E2が両方とも粒子状態となり、膜が形成しにくくなると共に、膜形成ができたとしても平滑性が低下し、色材受容層への十分な接着性が得られなくなる。また、透明シートの強度が著しく低下し、薬品などに浸漬したときの剥がれなども発生しやすくなる。透明シート形成時の乾燥温度が高いと、塗工スピードをあげることができるので、生産性の面において、透明シート形成時の乾燥温度は、上記範囲内においてできるだけ高いほうが好ましい。また、前述した透明シートを形成する材料に延伸加工を施して、透明シートを形成してよい。なお、透明シートは、透明シートを形成する過程で、[1−1−2]細孔の形成方法に記載した方法により細孔を形成することが好ましい。   The transparent sheet is formed by using a roll coating method, a rod bar coating method, or a spray coating method with two types of emulsion solution in the transparent sheet and a coating solution containing the foam solution, hollow particles, and porous particles in the emulsion solution. It can be carried out by coating on a substrate by an air knife coating method, a slot die coating method or the like and drying. At this time, it is preferable that the drying temperature after coating is not less than the Tg of the emulsion E1 and less than the Tg of the emulsion E2. By producing a transparent sheet at this temperature, it is possible to produce a transparent sheet in which one of the emulsions is formed and the other remains as particles. At the time of forming the transparent sheet, when it is heated and dried at a temperature of Tg2 or higher, both E1 and E2 are formed into a film, and in the peeling process, cracks are difficult to occur, sufficient edge cutability, peelability from the base sheet. , Stickiness prevention is not obtained. On the other hand, if the transparent sheet is heated at a temperature lower than Tg1, both emulsions E1 and E2 are in a particle state, and it becomes difficult to form a film. Sufficient adhesion to the material receiving layer cannot be obtained. Further, the strength of the transparent sheet is remarkably lowered, and peeling when immersed in a chemical or the like is likely to occur. When the drying temperature at the time of forming the transparent sheet is high, the coating speed can be increased. Therefore, in terms of productivity, the drying temperature at the time of forming the transparent sheet is preferably as high as possible within the above range. In addition, the transparent sheet may be formed by subjecting the material forming the transparent sheet described above to stretching. In addition, it is preferable that a transparent sheet forms a pore by the method described in the formation method of [1-1-2] pore in the process of forming a transparent sheet.

離型層は、基材シートを構成する樹脂フィルム等に、離型層を構成する樹脂やワックスを含有する塗工液を塗工し、乾燥することにより形成することができる。塗工方法としては、従来公知の塗工方法、例えばグラビア記録法、スクリーン記録法、グラビア版を用いたリバースロールコーティング法等の塗工方法を挙げることができる。   The release layer can be formed by applying a coating liquid containing a resin or wax constituting the release layer to a resin film or the like constituting the base sheet and drying. Examples of the coating method include conventionally known coating methods such as a gravure recording method, a screen recording method, and a reverse roll coating method using a gravure plate.

[1−9−2]塗工液
色材受容層は、少なくとも水溶性樹脂を、適当な媒体と混合して塗工液を調製し、これを透明シートの表面に塗布し、乾燥させて色材受容層を形成することで得られる。尚、色材受容層を空隙吸収型とする場合は、少なくとも水溶性樹脂、無機微粒子、水溶性樹脂及びカチオン性樹脂を、適当な媒体と混合して塗工液を調製する。
[1-9-2] Coating liquid The colorant-receiving layer is prepared by mixing at least a water-soluble resin with an appropriate medium to prepare a coating liquid, applying the coating liquid to the surface of the transparent sheet, and drying it. It is obtained by forming a material receiving layer. When the colorant receiving layer is a void absorption type, at least a water-soluble resin, inorganic fine particles, a water-soluble resin and a cationic resin are mixed with an appropriate medium to prepare a coating solution.

塗工液の媒体としては、水性媒体を用いることが好ましい。水性媒体としては、水;水と水溶性有機溶剤との混合溶媒;等を挙げることができる。水溶性有機溶剤としては、例えば、
メタノール、エタノール、プロパノール等のアルコール類;
エチレングリコールモノメチルエーテル、エチレングリコールジメチルエーテル等の多価アルコールの低級アルキルエーテル類;
アセトン、メチルエチルケトン等のケトン類;
テトラヒドロフラン等のエーテル類;等を挙げることができる。
As a medium for the coating liquid, an aqueous medium is preferably used. Examples of the aqueous medium include water; a mixed solvent of water and a water-soluble organic solvent; Examples of water-soluble organic solvents include:
Alcohols such as methanol, ethanol, propanol;
Lower alkyl ethers of polyhydric alcohols such as ethylene glycol monomethyl ether and ethylene glycol dimethyl ether;
Ketones such as acetone and methyl ethyl ketone;
And ethers such as tetrahydrofuran;

塗工液には、本発明の効果を妨げない限り、各種添加剤を含有させることができる。反転画像を記録するインクとして染料インクを用いる場合には、染料固着剤を含有させることが好ましい。染料固着剤は染料分子のアニオン性基と結合して塩を形成して、染料を水に対して不溶化させることにより、マイグレーションを防止することができる。   Various additives can be contained in the coating liquid as long as the effects of the present invention are not hindered. When a dye ink is used as an ink for recording a reverse image, it is preferable to contain a dye fixing agent. The dye fixing agent can be bonded to the anionic group of the dye molecule to form a salt, thereby making the dye insoluble in water, thereby preventing migration.

その他の添加剤としては、例えば、界面活性剤、顔料分散剤、増粘剤、消泡剤、インク定着剤、ドット調整剤、着色剤、蛍光増白剤、酸化防止剤、紫外線吸収剤、防腐剤、pH調整剤等を挙げることができる。   Other additives include, for example, surfactants, pigment dispersants, thickeners, antifoaming agents, ink fixing agents, dot adjusting agents, colorants, fluorescent whitening agents, antioxidants, ultraviolet absorbers, antiseptics Agents, pH adjusters and the like.

塗工液中の無機微粒子の濃度は塗工液の塗工性等を考慮して適宜決定すればよく、特に制限はない。ただし、塗工液の全質量に対し、10〜30質量%とすることが好ましい。   The concentration of the inorganic fine particles in the coating solution may be appropriately determined in consideration of the coating property of the coating solution, and there is no particular limitation. However, it is preferable to set it as 10-30 mass% with respect to the total mass of a coating liquid.

[1−9−3]塗工
色材受容層の形成は、例えば、基材シート及び透明シートの積層体を構成する透明シートの表面に、塗工液を塗工することにより行う。塗工後は、必要に応じて塗工液の乾燥を行う。これにより、図1(b)または図18のように、基材シート50、透明シート52、及び色材受容層53が順次積層された積層構造の転写材1を得ることができる。
[1-9-3] Coating The colorant receiving layer is formed, for example, by applying a coating liquid on the surface of the transparent sheet constituting the laminate of the base sheet and the transparent sheet. After coating, the coating solution is dried as necessary. Thereby, as shown in FIG. 1B or FIG. 18, the transfer material 1 having a laminated structure in which the base sheet 50, the transparent sheet 52, and the color material receiving layer 53 are sequentially laminated can be obtained.

アンカー層、透明シート、離型層、及び基材シートが順次積層された積層シートを用いる場合には、積層シートを構成する透明シートの表面に、塗工液を塗工すればよい。これにより、図1(c)のように、色材受容層53、アンカー層59、透明シート52、離型層51、及び基材シート50が順次積層された積層構造を有する転写材1を得ることができる。   In the case of using a laminated sheet in which an anchor layer, a transparent sheet, a release layer, and a base sheet are sequentially laminated, a coating liquid may be applied to the surface of the transparent sheet constituting the laminated sheet. As a result, as shown in FIG. 1C, the transfer material 1 having a laminated structure in which the color material receiving layer 53, the anchor layer 59, the transparent sheet 52, the release layer 51, and the base sheet 50 are sequentially laminated is obtained. be able to.

塗工方法としては、従来公知の塗工方法を用いることができる。例えば、ブレードコーティング法、エアーナイフコーティング法、カーテンコーティング法、スロットダイコーティング法、バーコーティング法、グラビアコーティング法、ロールコーティング法等を挙げることができる。   As a coating method, a conventionally known coating method can be used. For example, blade coating method, air knife coating method, curtain coating method, slot die coating method, bar coating method, gravure coating method, roll coating method and the like can be mentioned.

塗工液の塗工量は、固形分換算で10〜40g/m2とすることが好ましい。塗工量を好ましくは10g/m2以上、さらに好ましくは15g/m2以上とすることにより、インク中の水分吸収性に優れた色材受容層を形成することができる。これにより、記録された反転画像中のインクが流れ、および反転画像の滲みを抑制することができる。一方、塗工量を好ましくは40g/m2以下、さらに好ましくは20g/m2以下とすることにより、塗工層を乾燥させる際に、転写材にカールが発生し難くなる。また、色材受容層の厚さを薄くすることにより、最終的に形成される記録物の厚さを薄厚化することができる。画像支持体がクレジットカード等のプラスチックカードである場合には、日本工業規格(JIS−X−6305)により厚さが厳格に規定されているため、塗工量とすることが有効である。なお、色材受容層用塗工液の塗工時に乾燥工程を設ける場合は、乾燥温度をエマルジョンE2のTg2未満にする必要がある。透明シート形成時の乾燥工程によって、色材受容層用塗工液を塗工するときにはエマルジョンE1が造膜し、エマルジョンE2が粒子状態となっている。色材受容層塗工時の乾燥温度がTg2以上になるとエマルジョンE2が造膜し、透明シート全体でE1とE2の両方が膜化した状態になり、転写材を転写するときにクラックが入りにくくなって、端部の切れ性が低下する。 The coating amount of the coating liquid is preferably 10 to 40 g / m 2 in terms of solid content. When the coating amount is preferably 10 g / m 2 or more, more preferably 15 g / m 2 or more, a colorant receiving layer having excellent water absorption in the ink can be formed. Thereby, the ink in the recorded reverse image flows and bleeding of the reverse image can be suppressed. On the other hand, when the coating amount is preferably 40 g / m 2 or less, more preferably 20 g / m 2 or less, the transfer material is less likely to curl when the coating layer is dried. Further, by reducing the thickness of the color material receiving layer, it is possible to reduce the thickness of the finally formed recorded matter. When the image support is a plastic card such as a credit card, the coating amount is effective because the thickness is strictly defined by the Japanese Industrial Standard (JIS-X-6305). In addition, when providing a drying process at the time of application | coating of the coating liquid for color material receiving layers, it is necessary to make drying temperature less than Tg2 of emulsion E2. When the colorant-receiving layer coating solution is applied by the drying process at the time of forming the transparent sheet, the emulsion E1 forms a film and the emulsion E2 is in a particle state. When the drying temperature at the time of coating the colorant receiving layer becomes Tg2 or more, the emulsion E2 is formed into a film, and both E1 and E2 are formed into a film on the entire transparent sheet, and cracks are not easily generated when the transfer material is transferred. As a result, the edge cutability is reduced.

[1−10]画像
図2(a)は、転写材を模式的に示す斜視図である。転写材は、その色材受容層に画像が記録される。図2(a)のように、色材受容層53には、色材受容層53の側から見ると鏡像となり、透明シート52の側から見ると正像となる反転画像72が記録されることが好ましい。反転画像72は、透明シート52が積層されていない色材受容層53の面に記録される。インクジェット記録方式は、従来の熱転写方式と比較して、記録物の生産性及び情報セキュリティーが向上して、記録コストの低減を図ることが可能となる。
[1-10] Image FIG. 2A is a perspective view schematically showing a transfer material. An image is recorded on the color material receiving layer of the transfer material. As shown in FIG. 2A, a reverse image 72 is recorded on the color material receiving layer 53 as a mirror image when viewed from the color material receiving layer 53 side and as a normal image when viewed from the transparent sheet 52 side. Is preferred. The reverse image 72 is recorded on the surface of the color material receiving layer 53 on which the transparent sheet 52 is not laminated. The ink jet recording method can improve the productivity of recorded matter and information security and can reduce the recording cost as compared with the conventional thermal transfer method.

転写材に記録される画像は、染料インクにより形成された画像であってもよいし、顔料インクにより形成された画像であってもよい。ただし、画像は、顔料インクにより形成されることが好ましい。顔料インクにより反転画像を形成することにより、色材受容層の表面にインク中の水分や溶媒が残存し難くなり、乾燥が容易となる。この結果、水分や溶媒に起因する画像支持体と転写材(具体的には、色材受容層)との接着不良、およびマイグレーション(インクの移動)を効果的に抑制することができる。さらに、顔料インクにより反転画像を形成することにより、その反転画像の耐光性を向上させることができる。   The image recorded on the transfer material may be an image formed with dye ink or an image formed with pigment ink. However, the image is preferably formed with pigment ink. By forming a reversal image with pigment ink, moisture and solvent in the ink hardly remain on the surface of the colorant receiving layer, and drying becomes easy. As a result, poor adhesion between the image support and the transfer material (specifically, the colorant receiving layer) and migration (ink movement) due to moisture or solvent can be effectively suppressed. Furthermore, by forming a reversal image with pigment ink, the light resistance of the reversal image can be improved.

顔料インクは、図2(b)のように、その顔料インク中の顔料成分63は粒子径が大きい。そのため顔料成分63は、空隙吸収型の色材受容層64においては、その色材受容層64を形成する無機微粒子65によって構成される細孔の内部までは浸透せずに、色材受容層64の記録表面で定着する。また、空隙吸収型の色材受容層64は、膨潤型の色材受容層とは異なり、色材受容層64が膨潤することなく平滑に保たれる。一方、膨潤吸収型の色材受容層の場合は、図3(a)のように、インク中の水分により色材受容層67が膨潤して、色材受容層67の表面に凹凸が発生するため、画像支持体に対する色材受容層67の接着性を低下させてしまう。また、インク中の残存水分や溶媒は、色材受容層66の表面に残って、付着工程における残存水分及び溶媒の蒸発により画像支持体と色材受容層66との密着性を低下させる可能性があるため、好ましくない。   As shown in FIG. 2B, the pigment component 63 in the pigment ink has a large particle diameter. Therefore, the pigment component 63 does not penetrate into the pores constituted by the inorganic fine particles 65 forming the color material receiving layer 64 in the space absorption type color material receiving layer 64, and the color material receiving layer 64. Fix on the recording surface. Further, unlike the swelling type color material receiving layer, the space absorption type color material receiving layer 64 is kept smooth without swelling the color material receiving layer 64. On the other hand, in the case of a swelling absorption type color material receiving layer, as shown in FIG. 3A, the color material receiving layer 67 is swollen by moisture in the ink, and irregularities are generated on the surface of the color material receiving layer 67. Therefore, the adhesion of the color material receiving layer 67 to the image support is lowered. Further, residual moisture and solvent in the ink may remain on the surface of the color material receiving layer 66, and the adhesion between the image support and the color material receiving layer 66 may be reduced by evaporation of the residual water and solvent in the adhesion process. This is not preferable.

また、空隙吸収型の色材受容層64においては、図2(b)のように、顔料インク中の顔料成分63は色材受容層64の表面で定着し、一方、インク中の水分及び溶媒成分62は、色材受容層64の内部まで浸透して、顔料成分63と分離(固液分離)する。そのため、転写時には色材受容層64の表面が乾燥した状態になるため、水分の蒸発に起因する接着不良を抑制して、接着性を向上することができる。また、残存水分及び溶媒成分62は色材受容層64の内部に留まるため、顔料成分63は、再度、残存水分及び溶媒成分62が接触することがなく、インクの移動(マイグレーション)を抑制することができる。一方、染料インクの場合には、図3(b)のように、残存水分の影響により、染料成分68が溶媒成分69のように移動(マイグレーション)してしまい、にじみが発生する。   In the void absorption type color material receiving layer 64, as shown in FIG. 2B, the pigment component 63 in the pigment ink is fixed on the surface of the color material receiving layer 64, while the moisture and solvent in the ink are used. The component 62 penetrates to the inside of the colorant receiving layer 64 and separates (solid-liquid separation) from the pigment component 63. Therefore, since the surface of the color material receiving layer 64 is in a dry state at the time of transfer, adhesion failure due to evaporation of moisture can be suppressed and adhesion can be improved. Further, since the residual moisture and the solvent component 62 remain inside the color material receiving layer 64, the pigment component 63 does not come into contact with the residual moisture and the solvent component 62 again, thereby suppressing ink migration. Can do. On the other hand, in the case of dye ink, as shown in FIG. 3B, the dye component 68 moves (migrate) like the solvent component 69 due to the influence of residual moisture, and bleeding occurs.

顔料インク中の顔料成分としては、カルボニル基、カルボキシル基、ヒドロキシル基、およびスルホン基のうちの少なくとも1種の官能基またはその塩を結合された自己分散顔料、あるいは顔料粒子の周りを樹脂で被覆した樹脂分散型の顔料を用いることができる。それらの中でも後者の樹脂分散型の顔料は、記録画像の擦過性が向上するため好ましい。また、樹脂分散型顔料を用いることによって、インク媒体と分離した後の顔料粒子同士の結着力を高めて、色材受容層の表面に顔料膜を形成することができる。この場合、顔料膜の表面上の水分は少量となる。これは、顔料膜が色材受容層中の下層の水分をほぼ遮断し、さらに下層からの水分補給もほぼ遮断するからである。そのため、樹脂分散型の顔料成分は、インクの高速定着および高速記録に適しており、好ましい。なお、色材受容層にカチオン性樹脂を含有させることにより、一般的にマイナス帯電している顔料粒子は、カチオン性樹脂と静電気的に結合して、色材受容層と顔料インクとの接着性を強固にする。また、顔料インクとして樹脂分散型顔料を使用する場合には、その分散樹脂と色材受容層中のカチオン性樹脂のSP値を近い値にすることが好ましい。これにより、樹脂分散型顔料の色材受容層への接着性が向上する。このような分散樹脂としては、(メタ)アクリル酸エステル共重合体等のアクリル樹脂を用いることが好ましい。   The pigment component in the pigment ink includes a self-dispersing pigment to which at least one functional group of carbonyl group, carboxyl group, hydroxyl group, and sulfone group or a salt thereof is bonded, or a coating around a pigment particle with a resin. Resin dispersion type pigments can be used. Among these, the latter resin-dispersed pigment is preferred because it improves the scratching of the recorded image. Further, by using a resin-dispersed pigment, it is possible to increase the binding force between the pigment particles after being separated from the ink medium, and to form a pigment film on the surface of the colorant receiving layer. In this case, the amount of water on the surface of the pigment film is small. This is because the pigment film substantially blocks water in the lower layer in the colorant receiving layer and further blocks water supply from the lower layer. Therefore, the resin-dispersed pigment component is suitable and suitable for high-speed fixing and high-speed recording of ink. In addition, by incorporating a cationic resin into the color material receiving layer, generally negatively charged pigment particles are electrostatically bonded to the cationic resin, and the adhesion between the color material receiving layer and the pigment ink. To strengthen. Moreover, when using a resin dispersion type pigment as a pigment ink, it is preferable to make the SP value of the dispersion resin and the cationic resin in the colorant receiving layer close to each other. Thereby, the adhesiveness of the resin dispersed pigment to the colorant receiving layer is improved. As such a dispersion resin, it is preferable to use an acrylic resin such as a (meth) acrylic acid ester copolymer.

また、分散樹脂は、色材受容層の水溶性樹脂のポリビニルアルコールなどのSP値と値が近いため、転写時の熱で分散樹脂および水溶性樹脂が溶融すると、両者の相溶性が高まり、樹脂分散顔料は色材受容層にも強固に接着される。そのため、記録画像の表面が顔料膜で覆われても、色材受容層との結着性を高めることができる。さらに、分散樹脂のSP値は、画像支持体のPVC、PET−GなどのSP値と値が近いため、転写時の熱で分散樹脂および画像支持体表面の構成成分(PVC、PET−Gなど)が溶融すると、両者の相溶性が高まり、樹脂分散顔料は画像支持体に強固に接着される。これにより、記録画像の色材受容層表面が顔料膜で覆われても、画像支持体との結着性を高めることができる。よって、画像支持体に対する色材受容層の転写性能を向上させることができる。   In addition, since the dispersion resin is close to the SP value of the water-soluble resin such as polyvinyl alcohol of the colorant receiving layer, when the dispersion resin and the water-soluble resin are melted by heat during transfer, the compatibility between the two increases. The dispersed pigment is firmly adhered to the colorant receiving layer. Therefore, even when the surface of the recorded image is covered with a pigment film, the binding property with the colorant receiving layer can be improved. Furthermore, since the SP value of the dispersion resin is close to the SP value of PVC, PET-G, etc. of the image support, the constituent components of the dispersion resin and the image support surface (PVC, PET-G, etc.) by heat during transfer ) Melts, the compatibility of both increases, and the resin-dispersed pigment is firmly adhered to the image support. Thereby, even if the color material receiving layer surface of the recorded image is covered with the pigment film, the binding property with the image support can be enhanced. Therefore, the transfer performance of the color material receiving layer to the image support can be improved.

顔料粒子の周りを被覆する樹脂としては、酸価100〜160mgKOH/gである(メタ)アクリル酸エステル系共重合体が好ましい。酸価を100mgKOH/g以上とすると、サーマル方式でインクを吐出するインクジェット記録方式において、インクの吐出安定性が向上する。一方、酸価を160mgKOH/g以下とすると、顔料粒子に対して相対的に疎水性を有するようになり、インクの定着性及び耐滲み性が良好となる。したがって、インクの高速定着および高速記録に適する。   As the resin covering the periphery of the pigment particles, a (meth) acrylic acid ester copolymer having an acid value of 100 to 160 mgKOH / g is preferable. When the acid value is 100 mgKOH / g or more, the ink ejection stability is improved in the ink jet recording system in which the ink is ejected by the thermal system. On the other hand, when the acid value is 160 mgKOH / g or less, the ink particles have a relatively hydrophobic property with respect to the pigment particles, and the fixing property and bleeding resistance of the ink are improved. Therefore, it is suitable for high-speed ink fixing and high-speed recording.

ここで酸価とは、1gの樹脂を中和するのに必要となるKOHの量(mg)であり、その親水性を示す指標となり得るものである。また、この場合の酸価は、樹脂分散剤を構成する各モノマーの組成比から計算により求めることもできる。具体的な顔料分散体の酸価の測定方法としては、電位差滴定により酸価を求める、Titrino(Metrohm製)等を使用することができる。   Here, the acid value is the amount (mg) of KOH required to neutralize 1 g of resin and can serve as an index indicating the hydrophilicity. Moreover, the acid value in this case can also be calculated | required by calculation from the composition ratio of each monomer which comprises a resin dispersing agent. As a specific method for measuring the acid value of the pigment dispersion, Titrino (manufactured by Metrohm) or the like for obtaining an acid value by potentiometric titration can be used.

顔料分散体で使用する樹脂は、疎水性の顔料を水系液媒体中に良好に分散させる分散機能を有するものであることが好ましく、ランダムコポリマーが使用される。ランダムコポリマー以外、例えばブロックコポリマー等は、顔料の親水性が高くなるものが多く、印字画像の耐水性が劣るものが多いため好ましくない。顔料分散体で使用する樹脂の製法は、常法によるものであり、例えば、特許4956917号に開示されている方法を用いることができる。なお、顔料インクの各成分と物性の好ましい範囲については、例えば、特開2015−110321号公報に記載されているものを使用することができる。   The resin used in the pigment dispersion preferably has a dispersing function for satisfactorily dispersing the hydrophobic pigment in the aqueous liquid medium, and a random copolymer is used. Other than the random copolymer, for example, a block copolymer or the like is not preferred because many pigments have high hydrophilicity and many printed images have poor water resistance. The production method of the resin used in the pigment dispersion is a conventional method, and for example, the method disclosed in Japanese Patent No. 4956917 can be used. In addition, about the preferable range of each component and physical property of a pigment ink, what is described in Unexamined-Japanese-Patent No. 2015-110321 can be used, for example.

[1−11]画像の記録
転写材に対しては、前述したように、透明シートが積層されていない色材受容層の面に画像を記録する。その画像は、色材受容層の側から見ると鏡像となり、透明シートの側から見ると正像となる反転画像である。その結果、図2(a)のように、転写材1の色材受容層53に反転画像72が記録されて、記録媒体(画像が記録された転写材)が形成される。
[1-11] Image Recording As described above, an image is recorded on the surface of the color material receiving layer on which the transparent sheet is not laminated. The image is a reverse image that is a mirror image when viewed from the colorant-receiving layer side and a normal image when viewed from the transparent sheet side. As a result, as shown in FIG. 2A, the reverse image 72 is recorded on the color material receiving layer 53 of the transfer material 1 to form a recording medium (transfer material on which the image is recorded).

インクジェット記録方式とは、記録ヘッドに形成された複数のノズルから、転写材に対してインク(インク滴)を吐出して画像を記録する方式である。インクジェット記録方式の種類は、特に制限されない。例えば、駆動パルスに応じてヒータが発する熱エネルギーによって、ノズル内のインクを発泡させ、その発泡エネルギーを利用してノズルからインク滴を吐出させる、サーマルインクジェット記録方式が好ましい。   The inkjet recording method is a method of recording an image by ejecting ink (ink droplets) to a transfer material from a plurality of nozzles formed on a recording head. The type of the ink jet recording method is not particularly limited. For example, a thermal ink jet recording method in which ink in a nozzle is foamed by thermal energy generated by a heater in response to a driving pulse and ink droplets are ejected from the nozzle using the foaming energy is preferable.

インクジェット記録方式による画像の記録は、インクジェット記録装置(インクジェットプリンタ)により実施することができる。インクジェットプリンタは、画像の記録時に、記録ヘッドと転写材とが接触しないため、画像を極めて安定して記録することができる点において好ましい。インクジェットプリンタの種類は、特に制限されない。例えば、インク吐出口及びインク流路等からなるノズルを複数集積したマルチノズルヘッドを、転写材の搬送方向と直交するように多数配列させたラインヘッドを備えた、フルライン型のインクジェットプリンタを用いることが好ましい。フルライン型のインクジェットプリンタは、転写材の搬送に合わせて、複数のノズルのインク吐出口から同時にインクを吐出させて画像の記録を行う。そのため、高品位で高解像度の画像を高速で記録することができる。   Image recording by the ink jet recording method can be performed by an ink jet recording apparatus (ink jet printer). The ink jet printer is preferable in that the image can be recorded extremely stably because the recording head and the transfer material do not contact each other during image recording. The type of ink jet printer is not particularly limited. For example, a full-line type ink jet printer having a line head in which a multi-nozzle head in which a plurality of nozzles including ink discharge ports and ink flow paths are integrated is arranged so as to be orthogonal to the transfer material conveyance direction is used. It is preferable. A full-line type ink jet printer records an image by simultaneously ejecting ink from ink ejection ports of a plurality of nozzles in accordance with conveyance of a transfer material. Therefore, high-quality and high-resolution images can be recorded at high speed.

記録ヘッドのインクの吐出量としては、20pl以下であることが好ましい。インクの吐出量を好ましくは20pl以下、さらに好ましくは10pl以下、特に好ましくは5pl以下とすることにより、転写材と画像支持体との加熱圧着工程において、インクの水分量を適切なレベルにコントロールすることができる。また、吐出量を小さくするほど、色材受容層でのインクの広がりを抑えて、稠密で十分な濃度の反転画像を記録することができる。さらには、画像層(インク層)の厚さを抑えることが可能となる。   The ink discharge amount of the recording head is preferably 20 pl or less. By setting the ink discharge amount to preferably 20 pl or less, more preferably 10 pl or less, and particularly preferably 5 pl or less, the water content of the ink is controlled to an appropriate level in the heat-pressing step between the transfer material and the image support. be able to. Further, as the ejection amount is reduced, the spread of ink in the color material receiving layer can be suppressed, and a dense and sufficiently reversed image can be recorded. Furthermore, the thickness of the image layer (ink layer) can be suppressed.

また、記録方式として、記録面に対する記録ヘッドの相対的な移動走査と、画像が記録された転写材の搬送と、を繰り返す、シリアルヘッド型のインクジェット記録方式を用いてもよい。このような記録方式は、熱転写方式の記録速度に比べて十分な優位性があり、また液滴を小さくして高品位な画像を容易に記録することができる。   Further, as a recording method, a serial head type ink jet recording method may be used in which the relative scanning of the recording head with respect to the recording surface and the transfer of the transfer material on which the image is recorded are repeated. Such a recording method is sufficiently superior to the recording speed of the thermal transfer method, and it is possible to easily record a high-quality image by reducing the droplets.

また画像は、画像支持体よりも大きなサイズで転写材に記録することが好ましい。これにより、転写材の記録画像を記録物の画像支持体に転写して、結果的に、その画像支持体に対して、良好な画像をふち無し記録することができる。仮に、インクジェット方式によって、直接、画像支持体にふち無し記録を行った場合には、その画像支持体のエッジ部分にインクが吸収されて、そのエッジ部分に記録される画像の品位が低下するおそれがある。しかし、本実施形態のように、画像支持体よりも大きなサイズの画像を転写材に記録して、その画像を画像支持体に転写することにより、画像支持体のエッジ部に対しても良好な画像を記録することができる。   The image is preferably recorded on the transfer material with a size larger than that of the image support. Thereby, the recorded image of the transfer material can be transferred to the image support of the recorded material, and as a result, a good image can be recorded on the image support without any margins. If borderless recording is performed directly on the image support by the inkjet method, the ink is absorbed by the edge portion of the image support, and the quality of the image recorded on the edge portion may be degraded. There is. However, as in the present embodiment, an image having a size larger than that of the image support is recorded on the transfer material, and the image is transferred to the image support. Images can be recorded.

[1−11−1]マーキング処理
また、画像を記録する際に、後述する転写工程における自動ラミネート機(転写部)に転写材を位置合わせするために、図4(a)のように、マーキング162を印刷することが好ましい。転写材に対して、記録物の画像支持体のサイズに対応する記録領域161と、その外側の領域160と、を含む範囲に画像を記録して、それを転写することにより、上記のように画像支持体にふち無し記録を行うことができる。位置合わせようのマーキング162は、これらの領域160,161の外側に印刷される。このマーキング162を後述する透過または反射型のセンサで読み取ることにより、転写時における貼り合わせ位置を正確に規制することができる。また、図4(b)のように、転写材がカットシート形状である場合には、記録領域161の外側に、マーキング162に加えて、貼り合わせガイド163を印字することにより、転写時における貼り合わせの位置調整を容易に行うことができる。
[1-11-1] Marking Processing Also, as shown in FIG. 4A, in order to align the transfer material with an automatic laminating machine (transfer section) in a transfer process, which will be described later, when an image is recorded. It is preferable to print 162. As described above, an image is recorded on a transfer material in a range including a recording area 161 corresponding to the size of the image support of the recorded material and an outer area 160, and transferred. Borderless recording can be performed on the image support. An alignment marking 162 is printed outside these areas 160 and 161. By reading this marking 162 with a transmission or reflection type sensor, which will be described later, the bonding position at the time of transfer can be accurately regulated. As shown in FIG. 4B, when the transfer material has a cut sheet shape, a bonding guide 163 is printed on the outside of the recording area 161 in addition to the marking 162, thereby attaching the transfer material at the time of transfer. The alignment position can be easily adjusted.

[1−11−2]インクの乾燥
画像が記録された転写材は、画像を形成しているインクジェット記録用のインクの水分量が、インクの総打ち込み量に対して70質量%以下となるまで乾燥することが好ましい。インクの水分量を好ましくは70%質量%以下、さらに好ましくは50質量%以下とすることにより、画像支持体と転写材とを加熱圧着させる際に、インク成分の急激な蒸発を抑制することができる。この結果、画像支持体と転写材との密着強度の低下、および色材受容層における気泡残り等の発生を抑制することができる。なお、ここにいう水分量とは、色材を除く水及び不揮発性溶媒等の総量を意味するものとする。
[1-11-2] Drying of ink In the transfer material on which the image is recorded, the water content of the ink for ink-jet recording forming the image is 70% by mass or less with respect to the total amount of ink to be deposited. It is preferable to dry. By setting the water content of the ink to preferably 70% by mass or less, more preferably 50% by mass or less, rapid evaporation of the ink components can be suppressed when the image support and the transfer material are thermocompression bonded. it can. As a result, it is possible to suppress the decrease in the adhesion strength between the image support and the transfer material and the generation of bubbles remaining in the color material receiving layer. In addition, the amount of water here means the total amount of water, non-volatile solvent, and the like excluding the coloring material.

インクの総打ち込み量は、記録ヘッドのインク吐出量により調整することができる。水分量の制御を容易に行えるように、予め、画像記録時に形成するインクのドット数を間引く等して、打ち込み量を制限してもよい。   The total ink ejection amount can be adjusted by the ink ejection amount of the recording head. In order to easily control the amount of moisture, the amount of ink may be limited in advance by thinning out the number of dots of ink formed during image recording.

乾燥は、ハロゲンヒータ等のヒータ(熱源)、ファン等の排気装置等により行うことができる。ただし、ヒータ等の特別な乾燥手段を設けずに、十分な長さの搬送路を搬送させることによって、自然乾燥を促してもよい。   Drying can be performed by a heater (heat source) such as a halogen heater or an exhaust device such as a fan. However, natural drying may be promoted by transporting a sufficiently long transport path without providing a special drying means such as a heater.

[1−12]細孔処理
前述したように、透明シートに予め細孔が形成されていない転写材を用いる場合には、画像記録後の転写材に所望の細孔処理手段を用いて、透明シートに細孔を形成することができる。この場合には、図24のように、細孔を色材受容層53の表面側から形成してもよく、基材シート50の表面側から形成してもよい。画像品位を良好に保つためには、基材シート50の表面から細孔を形成することが好ましい。
[1-12] Pore Treatment As described above, when using a transfer material in which pores are not formed in advance on the transparent sheet, a desired pore treatment means is used for the transfer material after image recording. It is possible to form pores in the sheet. In this case, as shown in FIG. 24, the pores may be formed from the surface side of the colorant receiving layer 53 or from the surface side of the base material sheet 50. In order to maintain good image quality, it is preferable to form pores from the surface of the base sheet 50.

[1−13]プライマー層
本実施の形態においては、図5および図66のように、画像記録後の転写材1の色材受容層53の表面に、プライマー層56をさらに備えてもよい。プライマー層として、例えば、特開2015−110321号公報に記載されているものを好ましく使用することができる。
[1-13] Primer Layer In this embodiment, as shown in FIGS. 5 and 66, a primer layer 56 may be further provided on the surface of the color material receiving layer 53 of the transfer material 1 after image recording. As the primer layer, for example, those described in JP-A-2015-110321 can be preferably used.

[2]記録物
記録物は、前述した図33のように構成することができ、画像支持体55に、画像が記録された転写材1の色材受容層53が転写される。その色材受容層53を覆う透明シート52には、前述したように、細孔52Aが形成、または連泡構造553,554,555が構成される。また、画像支持体55のSP値と、画像支持体55に当接する転写材の層(図1(a)の例では、色材受容層53のSP値と、の差SP2が下式(12)の関係を満たすことが好ましい。これにより、画像支持体と色材受容層との相溶性が高くなり、画像支持体と色材受容層は高い接着性を示す。 0≦SP2≦1.0 (12)
[2] Recorded Material The recorded material can be configured as shown in FIG. 33 described above, and the color material receiving layer 53 of the transfer material 1 on which the image is recorded is transferred to the image support 55. In the transparent sheet 52 covering the color material receiving layer 53, as described above, the pores 52A are formed, or the open cell structures 553, 554, and 555 are formed. Further, the difference SP2 between the SP value of the image support 55 and the transfer material layer in contact with the image support 55 (in the example of FIG. 1A, the SP value of the color material receiving layer 53 is expressed by the following equation (12). In this case, the compatibility between the image support and the color material receiving layer is increased, and the image support and the color material receiving layer exhibit high adhesiveness: 0 ≦ SP2 ≦ 1.0 (12)

[3]記録物の製造方法
画像支持体、色材受容層、及び透明シート、を備えた記録物は、工程1,2,3を含む製造方法によって製造される。工程1においては、基材シートと、透明シートと、少なくとも水溶性樹脂を含有する色材受容層と、が積層された転写材の色材受容層に、インクジェット記録方式などにより画像を記録して、画像が記録された転写材(記録媒体)を得る。工程2においては、その記録媒体の色材受容層を画像支持体に加熱圧着する。工程3においては、記録媒体から基材シートを剥離して記録物を得る。透明シートには、図23および図47から図49のように予め細孔が形成されていてもよい。また、前述しように穿孔工程によって透明シートに細孔を形成してもよく、図24の場合には工程2の前、図25の場合は工程2の後、図26の場合には工程3の後に、穿孔工程によって細孔が形成される。
[3] Manufacturing method of recorded matter A recorded matter provided with an image support, a colorant receiving layer, and a transparent sheet is manufactured by a manufacturing method including steps 1, 2, and 3. In step 1, an image is recorded by an inkjet recording method or the like on a color material receiving layer of a transfer material in which a base material sheet, a transparent sheet, and a color material receiving layer containing at least a water-soluble resin are laminated. A transfer material (recording medium) on which an image is recorded is obtained. In step 2, the color material receiving layer of the recording medium is heat-pressed to the image support. In step 3, the substrate sheet is peeled from the recording medium to obtain a recorded matter. In the transparent sheet, pores may be formed in advance as shown in FIGS. 23 and 47 to 49. Further, as described above, pores may be formed in the transparent sheet by a perforating process. In the case of FIG. 24, before the process 2, in the case of FIG. 25, after the process 2, and in the case of FIG. Later, pores are formed by a perforation process.

以下、具体的に、記録物の製造方法における工程2および工程3について説明する。   Hereinafter, step 2 and step 3 in the method for manufacturing a recorded matter will be specifically described.

図6(a)は、転写材1を画像支持体55に貼付した積層体84を模式的に示す断面図である。図6(b)および図67は、図6(a)の積層体84から基材シート50を剥離した記録物73を模式的に示す斜視図である。   FIG. 6A is a cross-sectional view schematically showing a laminate 84 in which the transfer material 1 is attached to the image support 55. FIGS. 6B and 67 are perspective views schematically showing a recorded matter 73 from which the base sheet 50 has been peeled from the laminate 84 of FIG.

転写材1は、図6(a)のように、その色材受容層53が画像支持体55に貼り付けられる。これにより、画像支持体55、色材受容層53、及び透明シート52が順次積層された積層体84が形成されて、色材受容層53に記録された反転画像が画像支持体55に貼り付けられる。   As shown in FIG. 6A, the color material receiving layer 53 of the transfer material 1 is attached to the image support 55. As a result, a laminate 84 in which the image support 55, the color material receiving layer 53, and the transparent sheet 52 are sequentially laminated is formed, and the reverse image recorded on the color material receiving layer 53 is attached to the image support 55. It is done.

図6(b)のように、透明シート52に予め細孔が形成されていない転写材1を用いる場合には、前述したように、積層体84が形成された後に、基材シート50の表面側から透明シート52に細孔を形成することができる。その場合には、図25のように、基材シート50と透明シート52に細孔50A,52Aを形成することができ、また基材シート50、透明シート52、色材受容層53に細孔50A,52A,53Aを形成することもできる。これらの細孔は、前述したように、図46(a),(b)の針657、拍車650、または刃型などの機械的穿孔加工、あるいは図46(c)のようなレーザ加工装置658などによって形成することができる。画像の記録品位を良好に保つにためには、基材シート50と透明シート52に対して細孔50A,52Aが形成することが好ましい。   As shown in FIG. 6B, when the transfer material 1 in which pores are not previously formed in the transparent sheet 52 is used, the surface of the base sheet 50 is formed after the laminate 84 is formed as described above. Fine pores can be formed in the transparent sheet 52 from the side. In that case, as shown in FIG. 25, the pores 50A and 52A can be formed in the base sheet 50 and the transparent sheet 52, and the pores are formed in the base sheet 50, the transparent sheet 52, and the colorant receiving layer 53. 50A, 52A, and 53A can also be formed. As described above, these pores are formed by mechanical drilling such as the needle 657, the spur 650, or the blade shape of FIGS. 46A and 46B, or the laser processing apparatus 658 as shown in FIG. Etc. can be formed. In order to maintain good image recording quality, it is preferable to form the pores 50 </ b> A and 52 </ b> A in the base sheet 50 and the transparent sheet 52.

図6(b)および図67のように、積層体84から基材シート50を剥離することにより記録物73が得られる。図6(b)のように、透明シート52に細孔が形成されていない場合には、後述するように、記録物73を形成後に、図46のような穿孔処理を施すことによって、透明シート52に細孔52Aを形成することができる。   As shown in FIGS. 6B and 67, the recorded material 73 is obtained by peeling the base sheet 50 from the laminate 84. As shown in FIG. 6B, when no pores are formed in the transparent sheet 52, the transparent sheet 52 is subjected to perforation as shown in FIG. 52 can be formed with pores 52A.

[3−1]画像支持体
画像支持体の構成は、特に制限されない。画像支持体としては、例えば、樹脂を構成材料とする画像支持体(樹脂ベース支持体)、紙を構成材料とする画像支持体(紙ベース支持体)等を挙げることができる。樹脂べース支持体としては、例えば、クレジットカード、ICカード等の樹脂製カードを挙げることができる。紙ベース基材としては、例えば、パスポート等の紙製冊子、および紙製カード等を挙げることができる。
[3-1] Image support The configuration of the image support is not particularly limited. Examples of the image support include an image support using a resin as a constituent material (resin base support), an image support using paper as a constituent material (paper base support), and the like. Examples of the resin base support include resin cards such as credit cards and IC cards. Examples of the paper base material include a paper booklet such as a passport, a paper card, and the like.

[3−1−1]樹脂ベース支持体
樹脂ベース支持体を構成する樹脂は、画像支持体の用途に応じて適宜選択すればよく、特に制限されない。例えば、
ポリエチレンテレフタレート、ポリブチレンテレフタレート、ポリエチレンテレフタレート/イソフタレート共重合体等のポリエステル樹脂;
ポリエチレン、ポリプロピレン、ポリメチルペンテン等のポリオレフィン樹脂;
ポリフッ化ビニル、ポリフッ化ビニリデン、ポリ4フッ化エチレン、エチレン−4フッ化エチレン共重合体等のポリフッ化エチレン系樹脂;
ナイロン6、ナイロン6,6等の脂肪族ポリアミド樹脂;
ポリ塩化ビニル、塩化ビニル/酢酸ビニル共重合体、エチレン/酢酸ビニル共重合体、エチレン/ビニルアルコール共重合体、ポリビニルアルコール、ビニロン等のビニル重合体樹脂;
三酢酸セルロース、セロハン等のセルロース系樹脂;
ポリメタアクリル酸メチル、ポリメタアクリル酸エチル、ポリアクリル酸エチル、ポリアクリル酸ブチル等のアクリル系樹脂;
ポリスチレン、ポリカーボネート、ポリアリレート、ポリイミド等の、その他の合成樹脂;を挙げることができる。
[3-1-1] Resin Base Support The resin constituting the resin base support may be appropriately selected according to the use of the image support, and is not particularly limited. For example,
Polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene terephthalate / isophthalate copolymer;
Polyolefin resins such as polyethylene, polypropylene and polymethylpentene;
Polyfluorinated ethylene resins such as polyvinyl fluoride, polyvinylidene fluoride, polytetrafluoroethylene, ethylene-tetrafluoroethylene copolymer;
Aliphatic polyamide resins such as nylon 6 and nylon 6 and 6;
Vinyl polymer resins such as polyvinyl chloride, vinyl chloride / vinyl acetate copolymer, ethylene / vinyl acetate copolymer, ethylene / vinyl alcohol copolymer, polyvinyl alcohol, vinylon;
Cellulosic resins such as cellulose triacetate and cellophane;
Acrylic resins such as methyl polymethacrylate, ethyl polymethacrylate, polyethyl acrylate, polybutyl acrylate;
And other synthetic resins such as polystyrene, polycarbonate, polyarylate, and polyimide.

樹脂ベース支持体を構成する樹脂は、例えば、脂肪族ポリエステル、ポリカーボネート、ポリ乳酸、ポリビニルアルコール、セルロースアセテート、ポリカプロラクトン等の生分解性樹脂であってもよい。また、樹脂ベース支持体は、樹脂を主たる構成材料としているものであればよく、例えば、属箔等の樹脂以外の材料を含むものであってもよい。   The resin constituting the resin base support may be, for example, a biodegradable resin such as aliphatic polyester, polycarbonate, polylactic acid, polyvinyl alcohol, cellulose acetate, and polycaprolactone. Moreover, the resin base support body should just be what uses resin as the main structural material, for example, may contain materials other than resin, such as a metal foil.

[3−1−2]紙ベース支持体
紙ベース支持体を構成する紙の種類は、特に制限されない。例えば、コンデンサーペーパー、グラシン紙、硫酸紙、サイズ度の高い紙、合成紙(ポリオレフィン系、ポリスチレン系)、上質紙、アート紙、コート紙、キャストコート紙、壁紙、裏打用紙、合成樹脂又はエマルジョン含浸紙、合成ゴムラテックス含浸紙、合成樹脂内添紙、板紙、セルロース繊維紙等を挙げることができる。
[3-1-2] Paper base support The type of paper constituting the paper base support is not particularly limited. For example, condenser paper, glassine paper, sulfuric acid paper, high-size paper, synthetic paper (polyolefin, polystyrene), fine paper, art paper, coated paper, cast coated paper, wallpaper, backing paper, synthetic resin or emulsion impregnation Examples thereof include paper, synthetic rubber latex-impregnated paper, synthetic resin-added paper, paperboard, and cellulose fiber paper.

[3−1−3]その他
樹脂ベース支持体及び紙ベース支持体は、必要に応じて、エンボス、サイン、ICメモリ(ICチップ)、光メモリ、磁気記録層、偽変造防止用記録層(パール顔料層、透かし記録層、マイクロ文字等)、エンボス記録層、ICチップ隠蔽層等を備えてもよい。また、樹脂ベース支持体及び紙ベース支持体は、上述の材質からなる単層体として構成してもよいし、材質や厚さの異なるシートやフィルムを2層以上貼り合わせた複層体として構成してもよい。
[3-1-3] Other Resin base support and paper base support may be embossed, signed, IC memory (IC chip), optical memory, magnetic recording layer, anti-counterfeit recording layer (pearl pigment, if necessary) Layer, watermark recording layer, micro characters, etc.), embossed recording layer, IC chip concealing layer, and the like. In addition, the resin base support and the paper base support may be configured as a single layer made of the above-described materials, or may be configured as a multilayer body in which two or more sheets or films having different materials and thicknesses are bonded together. May be.

さらに、画像支持体の全体の厚さは、30〜800μmであることが好ましい。画像支持体の厚さを好ましくは30μm以上、さらに好ましくは500μm以上、特に好ましくは650μm以上とする。一方、画像支持体の厚さを好ましくは800μm以下、さらに好ましくは770μm以下とする。画像支持体としてプラスチックカードを用いた場合には、インクジェット記録物全体の厚さをJIS6301に記載される総厚さ0.68〜0.84mmに制御することができる。   Furthermore, the total thickness of the image support is preferably 30 to 800 μm. The thickness of the image support is preferably 30 μm or more, more preferably 500 μm or more, and particularly preferably 650 μm or more. On the other hand, the thickness of the image support is preferably 800 μm or less, more preferably 770 μm or less. When a plastic card is used as the image support, the total thickness of the inkjet recording can be controlled to a total thickness of 0.68 to 0.84 mm described in JIS6301.

[3−2]積層構造
記録物73は、図6(b)および図67のように、画像支持体55、色材受容層53、及び透明シート52が順次積層された積層構造を有している。また、図67の記録物73における透明シート52は、貫通する細孔52Aを有している。
[3-2] Laminated Structure The recorded matter 73 has a laminated structure in which the image support 55, the color material receiving layer 53, and the transparent sheet 52 are sequentially laminated as shown in FIGS. Yes. In addition, the transparent sheet 52 in the recorded matter 73 in FIG. 67 has a through-hole 52A.

[3−3]記録媒体と画像支持体との加熱圧着
図6(a)のように、画像支持体と、画像が記録された転写材(記録媒体)1と、が重ねた状態で加熱圧着されることにより、積層体84が得られる。
[3-3] Thermocompression bonding between recording medium and image support As shown in FIG. 6 (a), thermocompression bonding is performed in a state where the image support and the transfer material (recording medium) 1 on which the image is recorded are overlapped. As a result, a laminate 84 is obtained.

加熱圧着の温度は、60〜160℃に制御することが好ましい。加熱圧着の温度を好ましくは60℃以上とすることにより、色材受容層中のカチオン性樹脂、水溶性樹脂等の樹脂やプライマー層(又はアンカー層)に含まれる熱可塑性樹脂を接着に十分な程度に溶融させて、画像支持体と転写材とを圧着させることができる。一方、加熱圧着の温度を好ましくは160℃以下とすることにより、画像支持体と記録媒体とを加熱圧着させる際に、インク成分の急激な蒸発を抑制して、画像支持体と記録媒体との密着強度の低下、色材受容層における気泡残り等の発生を抑制することができる。   It is preferable to control the temperature of thermocompression bonding to 60-160 degreeC. When the temperature of thermocompression bonding is preferably 60 ° C. or higher, a resin such as a cationic resin or a water-soluble resin in the colorant receiving layer or a thermoplastic resin contained in the primer layer (or anchor layer) is sufficient for adhesion. The image support and the transfer material can be pressure-bonded by being melted to the extent. On the other hand, when the temperature of the thermocompression bonding is preferably 160 ° C. or less, when the image support and the recording medium are thermocompression bonded, the rapid evaporation of the ink component is suppressed, and the image support and the recording medium It is possible to suppress the decrease in the adhesion strength and the generation of bubbles remaining in the colorant receiving layer.

記録物におけるエマルジョンE2は、転写条件(例えば、転写温度や転写速度)を調整することにより、十分に皮膜化した状態で転写することもでき、または、一部粒子が残った状態で転写することもできる。図71に示すように加熱圧着時に、画像支持体55と色材受容層が接着している部分963の透明シート部分980と、画像支持体と色材受容層が接着していない部分964の透明シート部分981と、で膜状態が異なるように制御することができる。すなわち、加熱圧着時において、透明シート部分980はヒートロールの熱が伝わりやすいため、エマルジョンE2の一部が膜化して一部粒子が残存した状態(図71(b))、あるいは透明シートのエマルジョンE2が完全に皮膜化した状態(図71(c))になる。このとき、一部あるいは完全に膜化したエマルジョンE2は、予め膜化しているエマルジョンE1と結合力が強化されて透明シートの膜強度を強化することができる。一方、透明シート部分981はヒートロールの熱が伝わらないため、エマルジョンE2を粒子状態のままにすることができる。透明シート部分980と透明シート部分981では膜の状態が異なるため、剥離工程では、境界部982を基点としてクラックが入りやすくなる。以上から、2種類のエマルジョンを用いて、エマルジョンE2の膜状態を、加熱圧着時の温度を利用して変化させることにより、箔切れを良好することができる。使用者の要求する性能に応じて、エマルジョンE2の一部粒子が皮膜化した状態と、エマルジョンE2が完全に膜化した状態と、を使い分けることができる。   The emulsion E2 in the recorded matter can be transferred in a sufficiently filmed state by adjusting transfer conditions (for example, transfer temperature and transfer speed), or transferred with some particles remaining. You can also. As shown in FIG. 71, at the time of thermocompression bonding, the transparent sheet portion 980 of the portion 963 where the image support 55 and the color material receiving layer are bonded and the transparent portion 964 where the image support and the color material receiving layer are not bonded are transparent. The sheet portion 981 can be controlled to have a different film state. That is, at the time of thermocompression bonding, since the heat of the heat roll is easily transmitted to the transparent sheet portion 980, a state in which a part of the emulsion E2 is formed into a film and some particles remain (FIG. 71 (b)), or an emulsion of the transparent sheet E2 is completely filmed (FIG. 71 (c)). At this time, the emulsion E2 that is partially or completely formed into a film can strengthen the bonding strength with the emulsion E1 that has been formed into a film in advance, thereby enhancing the film strength of the transparent sheet. On the other hand, since the heat of the heat roll is not transmitted to the transparent sheet portion 981, the emulsion E2 can be left in a particle state. Since the film state is different between the transparent sheet portion 980 and the transparent sheet portion 981, in the peeling process, cracks are easily generated with the boundary portion 982 as a base point. From the above, the foil breakage can be improved by using two types of emulsions and changing the film state of the emulsion E2 using the temperature at the time of thermocompression bonding. Depending on the performance required by the user, the state in which some particles of the emulsion E2 are formed into a film and the state in which the emulsion E2 is completely formed into a film can be properly used.

加熱圧着の方法は、特に制限されない。例えば、画像支持体に記録媒体を積層して積層体とし、その積層体を一対のヒートローラ間に挟み込んで加熱圧着する方法等を挙げることができる。その場合、ヒートローラの表面温度は、100〜180℃とすることが好ましい。これにより、積層体の搬送速度が速くて加熱時間が十分にとれない場合でも、積層体を60〜160℃に加熱することができる。   The method for thermocompression bonding is not particularly limited. For example, a method of laminating a recording medium on an image support to form a laminated body, and sandwiching the laminated body between a pair of heat rollers can be used. In that case, the surface temperature of the heat roller is preferably 100 to 180 ° C. Thereby, even when the conveyance speed of a laminated body is quick and heating time cannot fully be taken, a laminated body can be heated at 60-160 degreeC.

図9、図28から図31のような後述する製造装置25を用いる場合には、画像支持体55側に接するヒートローラ22として、シリコーンローラを使用することが好ましい。シリコーンローラはSP値が8.7付近になるため、ヒートロータ21,22の間に画像支持体55が存在しないとき、つまり色材受容層53がヒートローラ22に接するときに、ヒートローラ22に対して色材受容層53が付着し難くなる。したがって、ヒートローラ22への色材受容層53の転写を防止することができる。ヒートローラ21は、基材シート50側から記録媒体を加熱する。   When using the manufacturing apparatus 25 described later as shown in FIGS. 9 and 28 to 31, it is preferable to use a silicone roller as the heat roller 22 in contact with the image support 55 side. Since the SP value of the silicone roller is around 8.7, when the image support 55 is not present between the heat rotors 21 and 22, that is, when the color material receiving layer 53 is in contact with the heat roller 22, As a result, the colorant receiving layer 53 becomes difficult to adhere. Therefore, transfer of the color material receiving layer 53 to the heat roller 22 can be prevented. The heat roller 21 heats the recording medium from the base material sheet 50 side.

[3−4]基材シート及び離型層の剥離
図6(a)の積層体84から基材シート50を剥離することにより、インクジェット記録物73が得られる。この記録物73において、最上層に位置する透明シート52は、その下層側の色材受容層53に記録された反転画像72を保護する。プライマー層を備える場合、画像支持体55は、プライマー層を介して色材受容層53に十分に密着固定される。
[3-4] Peeling of base material sheet and release layer By peeling the base material sheet 50 from the laminate 84 of FIG. 6A, an ink jet recorded product 73 is obtained. In the recorded matter 73, the transparent sheet 52 positioned at the uppermost layer protects the reverse image 72 recorded on the color material receiving layer 53 on the lower layer side. When the primer layer is provided, the image support 55 is sufficiently closely fixed to the color material receiving layer 53 through the primer layer.

転写材が熱時剥離である場合には、加熱圧着後、温度が下がらないうちに、直ちに基材シートを剥離することが好ましい。熱時剥離タイプの場合は、図7(a)のような分離爪86を備えた剥離機構、または図7(b)のような剥離ロール88を用いて、基材シートを剥離することが好ましい。このような剥離方法は、転写材をロール・ツー・ロール(roll to roll)によって供給する場合、つまりロール状の転写材を繰り出して供給し、その転写材の基材シートをロール状に巻き取る場合に、生産性を高める上において有効である。   In the case where the transfer material is peeled off when heated, it is preferable that the substrate sheet is peeled immediately after the thermocompression bonding and before the temperature is lowered. In the case of a hot peeling type, it is preferable to peel the base sheet using a peeling mechanism having a separation claw 86 as shown in FIG. 7A or a peeling roll 88 as shown in FIG. 7B. . In such a peeling method, when the transfer material is supplied by roll-to-roll, that is, the roll-shaped transfer material is fed out and supplied, and the base material sheet of the transfer material is wound into a roll shape. In this case, it is effective in increasing productivity.

転写材が冷時剥離型の場合は、温度が下がっても基材シートを剥離することができる。そのため、ロールやピール機構による剥離だけでなく、手動による剥離も可能になるため、特に、基材シートがカットシート状に加工されている場合に好適である。転写材をロール・ツー・ロール(roll to roll)によって供給する場合の剥離角度θは0〜165°であり、さらに好ましくは90°〜165°である。この剥離角度θを設定することにより、後述する転写材のプレカット処理により分離されたパッチ部分が不用意に剥がれたり、めくれたりすることが防止できる。図7(b)における搬送角度θは、上記の角度のみに限定されない。   When the transfer material is a cold release type, the substrate sheet can be released even when the temperature is lowered. Therefore, since not only peeling by a roll or a peel mechanism but also manual peeling is possible, it is particularly suitable when the base sheet is processed into a cut sheet. In the case where the transfer material is supplied by roll to roll, the peeling angle θ is 0 to 165 °, more preferably 90 ° to 165 °. By setting the peeling angle θ, it is possible to prevent the patch portion separated by the pre-cut processing of the transfer material described later from being inadvertently peeled off or turned up. The conveyance angle θ in FIG. 7B is not limited to the above angle.

加熱圧着および剥離工程においては、公知の2本ロールタイプ、あるいは4本ロールタイプのラミネート機を使用してもよい。4本ロールタイプは、2本ロールタイプに比べて、加熱圧着時の熱が伝わりやすく、剥離工程を容易に行うことができるため、好ましく使用される。   In the thermocompression bonding and peeling step, a known two-roll type or four-roll type laminating machine may be used. The 4-roll type is preferably used because the heat at the time of thermocompression bonding can be easily transmitted and the peeling process can be easily performed as compared with the 2-roll type.

[3−5]両面同時剥離
画像支持体の両面のそれぞれに、画像が記録された転写材を同時に転写する場合には、図8のように、上面転写材92と下面転写材94における画像の記録位置をずらすことが好ましい。これにより、熱ローラ転写において膨潤型色材受容層を用いた場合には、SP値が同じであるため色材受容層同士の接着する場合があるが、これを防止して、表裏同時の転写が可能となる。また、ピール部90によって、基材シートを容易に引き剥がすことができる。
[3-5] Double-sided simultaneous peeling When transferring the transfer material on which the image is recorded on both sides of the image support simultaneously, the images on the upper transfer material 92 and the lower transfer material 94 are transferred as shown in FIG. It is preferable to shift the recording position. As a result, when the swelling type color material receiving layer is used in the heat roller transfer, the SP value is the same, so the color material receiving layers may adhere to each other. Is possible. Further, the base material sheet can be easily peeled off by the peel part 90.

[3−6]透明シートに対する細孔形成
前述したように、透明シート52に予め細孔が形成されていない転写材1を用いる場合には、積層体84が形成された後に、基材シート50の表面側から透明シート52に細孔を形成することができる。すなわち、図25のように、基材シート50と透明シート52に細孔50A,52Aを形成することができ、また基材シート50、透明シート52、色材受容層53に細孔50A,52A,53Aを形成することもできる。これらの細孔は、前述したように、図46(a),(b)の針657、拍車650、または刃型などの機械的穿孔加工、あるいは図46(c)のようなレーザ加工装置658などによって形成することができる。画像の記録品位を良好に保つにためには、基材シート50と透明シート52に対して細孔50A,52Aが形成することが好ましい。
[3-6] Formation of pores in transparent sheet As described above, when the transfer material 1 in which pores are not previously formed in the transparent sheet 52 is used, the base material sheet 50 is formed after the laminate 84 is formed. It is possible to form pores in the transparent sheet 52 from the front surface side. That is, as shown in FIG. 25, the pores 50A and 52A can be formed in the base sheet 50 and the transparent sheet 52, and the pores 50A and 52A are formed in the base sheet 50, the transparent sheet 52, and the colorant receiving layer 53. , 53A can also be formed. As described above, these pores are formed by mechanical drilling such as the needle 657, the spur 650, or the blade shape of FIGS. 46A and 46B, or the laser processing apparatus 658 as shown in FIG. 46C. Etc. can be formed. In order to maintain good image recording quality, it is preferable to form the pores 50 </ b> A and 52 </ b> A in the base sheet 50 and the transparent sheet 52.

[4]インクジェット記録装置
図27の記録装置は、転写材を搬送経路に送り出す供給部と、その搬送経路に送り出された転写材の色材受容層に、色材を付与して画像を記録する記録部6と、を備える。尚、透明シートに細孔が形成されていない転写材を用いる場合には、前述したように、工程2の前工程(図24)、工程2の後工程(図25)、または工程3の後工程(図26)において、透明シートに細孔を形成するための穿孔加工部659を備える。図27における穿孔加工部659は、工程1の前工程において透明シートに細孔を形成するように、備えられている。
[4] Inkjet recording apparatus The recording apparatus in FIG. 27 records an image by applying a coloring material to a supply unit that feeds a transfer material to a conveyance path and a coloring material receiving layer of the transfer material that is fed to the conveyance path. And a recording unit 6. In addition, when using the transfer material in which pores are not formed in the transparent sheet, as described above, after the step 2 (FIG. 24), after the step 2 (FIG. 25), or after the step 3 In the step (FIG. 26), a perforation processing part 659 for forming pores in the transparent sheet is provided. 27 is provided so as to form pores in the transparent sheet in the previous step of step 1.

[4−1]インクジェット記録装置
具体的に、記録装置としては、記録ヘッドに形成された複数のノズルから、転写材にインク(インク滴)を吐出して画像を記録するインクジェット方式の記録装置(インクジェットプリンタ)を用いることができる。このような記録装置は、画像の記録時に記録ヘッドと転写材とが接触しないため、極めて安定的に画像を記録することができて好ましい。インクジェットの記録方式は特に限定されず、サーマル方式およびピエゾ方式は、いずれも好適に使用できる。駆動パルスに応じて発熱するヒータの熱エネルギーによってノズル内のインクを発泡させ、その発泡エネルギーを利用して、ノズルからインク滴を吐出させるサーマルインクジェット記録方式は、他の記録方式に比して高解像度であるため好ましい。また、インク吐出口およびインク流路などからなるノズルを複数集積したマルチノズルヘッドを、転写材の搬送方向と直交するように多数配列させたラインヘッドを備えた、フルライン型のインクジェットプリンタを用いることが好ましい。このフルライン型のインクジェットプリンタは、転写材の搬送に合わせて、複数のノズルのインク吐出口から同時にインクを吐出させて画像を記録する。そのため、高品位で高解像度の画像を高速に記録することができる。
[4-1] Inkjet recording apparatus Specifically, the recording apparatus includes an inkjet recording apparatus that records an image by ejecting ink (ink droplets) onto a transfer material from a plurality of nozzles formed on a recording head. Inkjet printers can be used. Such a recording apparatus is preferable because an image can be recorded extremely stably because the recording head and the transfer material do not come into contact with each other during image recording. The inkjet recording method is not particularly limited, and both the thermal method and the piezo method can be suitably used. The thermal ink jet recording method, in which the ink in the nozzle is foamed by the heat energy of the heater that generates heat in response to the drive pulse and ink droplets are ejected from the nozzle using the foaming energy, is higher than other recording methods. The resolution is preferable. In addition, a full-line type ink jet printer having a line head in which a multi-nozzle head in which a plurality of nozzles including ink discharge ports and ink flow paths are integrated is arranged so as to be orthogonal to the transfer material conveyance direction is used. It is preferable. This full-line type ink jet printer records an image by simultaneously ejecting ink from the ink ejection ports of a plurality of nozzles in accordance with the transfer of the transfer material. Therefore, high-quality and high-resolution images can be recorded at high speed.

[4−2]透明シートへの細孔形成
前述したように、透明シートに予め細孔構造が構成されていない図1(b)の転写材1を用いる場合には、図27の記録装置において、機械的穿孔加工あるいはレーザ加工によって、透明シートに細孔を形成することができる。
[4-2] Formation of pores in transparent sheet As described above, when the transfer material 1 in FIG. 1B in which the pore structure is not previously formed is used in the transparent sheet, the recording apparatus in FIG. Fine pores can be formed in the transparent sheet by mechanical drilling or laser processing.

[5]記録物の製造装置
記録物の製造装置は、図27のような記録装置と、画像支持体を搬送経路に送り出す画像支持体供給部と、搬送経路に送り出された画像支持体に転写材を付着させる付着部と、転写材から基材シートを剥離する剥離部と、を備える。透明シートに予め細孔構造が構成されていない転写材を用いる場合には、図24から図26のような穿孔工程に対応する穿孔加工部659を備える。
[5] Recorded Product Manufacturing Apparatus The recorded product manufacturing apparatus includes a recording apparatus as shown in FIG. 27, an image support supply unit that sends the image support to the transport path, and a transfer to the image support sent to the transport path. An attachment portion for attaching the material and a peeling portion for peeling the base sheet from the transfer material are provided. In the case of using a transfer material in which the pore structure is not previously configured for the transparent sheet, a punching processing unit 659 corresponding to the punching process as shown in FIGS. 24 to 26 is provided.

[5−1]第1の製造装置
図9は、透明シートに予め細孔が形成されている転写材を用いて、記録物を製造する製造装置25の第1の構成例(以下、「第1の製造装置」ともいう。)を模式的に示す側面図である。
[5-1] First Manufacturing Apparatus FIG. 9 shows a first configuration example of a manufacturing apparatus 25 (hereinafter referred to as “first”) for manufacturing a recorded matter using a transfer material in which pores are previously formed in a transparent sheet. 1 is a side view schematically showing a manufacturing apparatus 1).

[5−1−1]主要な構成
製造装置25は、供給部4と、記録部6と、を備える。供給部4は、透明シートに予め細孔が形成されていてロール状に巻かれた転写材1を、搬送経路へと送り出す。記録部6は、搬送経路へ送り出された転写材1に、色材、水、および不揮発性の有機溶媒等を含有する水系インクを直接吐出して、反転画像を記録する。
[5-1-1] Main Configuration The manufacturing apparatus 25 includes a supply unit 4 and a recording unit 6. The supply unit 4 sends the transfer material 1 in which pores are formed in advance in a transparent sheet and wound in a roll shape, to the conveyance path. The recording unit 6 directly discharges water-based ink containing a color material, water, a non-volatile organic solvent, and the like onto the transfer material 1 sent to the conveyance path, and records a reversed image.

また、製造装置25は、インクが付与された転写材1の中の水分を蒸発させて、画像支持体55との密着性を向上させるための乾燥部7と、蒸発した水分によって、装置内の結露を防止するファン10と、を備える。さらに、製造装置25は、画像支持体55を加熱して転写材1との密着性を向上させるための予備加熱部19と、反転画像が記録された色材受容層および透明シートを画像支持体55に付着させる付着部29と、を備える。さらに、付着後の画像支持体55のカールを矯正するカール矯正部150、基材シートを剥離する剥離部151、両面記録を行う際に画像支持体55を反転させる画像反転部152、および画像が記録された画像支持体55を排出して集積する排出部26を備える。   Further, the manufacturing apparatus 25 evaporates moisture in the transfer material 1 to which ink has been applied, and the drying unit 7 for improving the adhesion to the image support 55 and the evaporated moisture in the apparatus. And a fan 10 for preventing condensation. Further, the manufacturing apparatus 25 includes the preheating unit 19 for heating the image support 55 to improve the adhesion to the transfer material 1, the color material receiving layer on which the reverse image is recorded, and the transparent sheet. And an attaching portion 29 to be attached to 55. Furthermore, a curl correction unit 150 that corrects the curl of the image support 55 after being attached, a peeling unit 151 that peels the base sheet, an image reversing unit 152 that reverses the image support 55 when performing double-sided recording, and an image A discharge unit 26 for discharging and accumulating the recorded image support 55 is provided.

[5−1−2]動作
供給部4は、色材受容層が外側に位置するように巻かれたロール状の転写材1を、図中の矢印に示す方向に回転させることにより、転写材1を記録部6へ送り出す。転写材1は、不図示のガイド板によって案内されると共に、グリップローラ3とニップローラ2により挟持されて、平坦な状態で記録部6へと搬送される。
[5-1-2] Operation The supply unit 4 rotates the roll-shaped transfer material 1 wound so that the color material receiving layer is positioned on the outside in the direction indicated by the arrow in the drawing, thereby transferring the transfer material. 1 is sent to the recording unit 6. The transfer material 1 is guided by a guide plate (not shown), is sandwiched between the grip roller 3 and the nip roller 2, and is transported to the recording unit 6 in a flat state.

供給部4から転写材1の搬送が開始されると、マーキングをセンサ部31が検出し、その転写材1の色材受容層に記録部6が反転画像を記録する。その後、転写材1は乾燥部7を通過する。乾燥部7は、反転画像を形成するインク中の水などを蒸発させ、ファン10は蒸発した水分を排気する。これにより、色材受容層に反転画像が記録された転写材1が得られる。このとき、前述したマーキング印刷も行う。   When conveyance of the transfer material 1 is started from the supply unit 4, the sensor unit 31 detects the marking, and the recording unit 6 records a reverse image on the color material receiving layer of the transfer material 1. Thereafter, the transfer material 1 passes through the drying unit 7. The drying unit 7 evaporates water or the like in the ink that forms the reverse image, and the fan 10 exhausts the evaporated water. Thereby, the transfer material 1 in which the reverse image is recorded on the color material receiving layer is obtained. At this time, the above-described marking printing is also performed.

一方、供給部12は、付着部に画像支持体55を1枚ずつ供給する。レジストガイド14が画像支持体55と転写材1とを位置合わせし、その画像支持体55の上に転写材1が積層される。画像支持体55と転写材1との積層体は、付着部29に搬送される。付着部29は一対のヒートローラ21,22を備えており、それらのローラ間を積層体が通過する際に、画像支持体55と転写材1とが加熱圧着される。   On the other hand, the supply unit 12 supplies the image supports 55 one by one to the attachment part. The resist guide 14 aligns the image support 55 and the transfer material 1, and the transfer material 1 is laminated on the image support 55. The laminated body of the image support 55 and the transfer material 1 is conveyed to the attaching portion 29. The adhering portion 29 includes a pair of heat rollers 21 and 22, and the image support 55 and the transfer material 1 are heat-pressed when the laminate passes between the rollers.

その後、画像支持体55と転写材1との積層体は、カール矯正部150に搬送されてカールが矯正されてから、剥離部151において、転写材1の基材シート及び離型層が剥離されて巻取りロール24に巻き取られる。また、両面記録を行う場合には、画像反転部152によって画像支持体55を反転させて、それをレジストガイド14までバックフィードさせる。そして記録部6において、表面記録時と同様に、画像支持体55の裏面に転写すべき反転画像を転写材1の色材受容層に記録し、レジストガイド14までバックフィードさせた画像支持体55の裏面に、その反転画像を転写させる。このようにして、画像支持体55に転写材1が加熱圧着された記録物を得ることができる。   Thereafter, the laminate of the image support 55 and the transfer material 1 is conveyed to the curl correction unit 150 to correct the curl, and then the base material sheet and the release layer of the transfer material 1 are peeled off at the peeling unit 151. Then, it is wound on the winding roll 24. When performing double-sided recording, the image inverting unit 152 inverts the image support 55 and back-feeds it to the registration guide 14. Then, in the recording unit 6, the reverse image to be transferred to the back surface of the image support 55 is recorded on the color material receiving layer of the transfer material 1 and back-fed to the resist guide 14 in the same manner as when recording on the front surface. The reverse image is transferred to the back surface of. In this way, a recorded matter in which the transfer material 1 is heat-pressed to the image support 55 can be obtained.

[5−1−3]第1の製造装置とコントローラとの接続
製造装置25は、図10のように、ネットワーク47を経由してコントローラ41に接続される。この製造装置25は、ネットワーク47を介さずに、シリアル・ポート、パラレル・ポート、またはUSBポート等を介して、コントローラ41に接続することも可能である。製造装置25の制御部44に備わるCPUは、記録部、乾燥部、付着部、カール矯正部、剥離部、画像反転部に接続されていて、それらの動作を制御する。
[5-1-3] Connection between First Manufacturing Apparatus and Controller The manufacturing apparatus 25 is connected to the controller 41 via the network 47 as shown in FIG. The manufacturing apparatus 25 can also be connected to the controller 41 via a serial port, a parallel port, a USB port, or the like without using the network 47. The CPU provided in the control unit 44 of the manufacturing apparatus 25 is connected to the recording unit, the drying unit, the adhering unit, the curl correcting unit, the peeling unit, and the image inverting unit, and controls their operations.

ネットワーク47は、インターネット、ローカルエリアネットワーク(LAN)等のネットワークであり、有線、無線を問わない。コントローラ41は、製造装置25を制御するためのコンピュータである。コントローラ41において、制御部44、表示部45、入出力部46、記憶部42、および通信部43は、システム・バス48を介して互いに接続されている。コントローラ41には、デジタルカメラ、画像データ等を読み込むためのドライブ装置、および製版装置等を接続してもよい。   The network 47 is a network such as the Internet or a local area network (LAN), and may be wired or wireless. The controller 41 is a computer for controlling the manufacturing apparatus 25. In the controller 41, the control unit 44, the display unit 45, the input / output unit 46, the storage unit 42, and the communication unit 43 are connected to each other via a system bus 48. The controller 41 may be connected to a digital camera, a drive device for reading image data, and a plate making device.

制御部44は、CPU、RAM、およびROM等を有する。CPUは、ROM等に格納されるプログラムをRAM上のワークメモリ領域に呼び出して実行し、演算処理および動作制御を行って、システム全体を制御する。ROMは不揮発性メモリであり、プログラムおよびデータ等を恒久的に保持する。RAMは揮発性メモリであり、プログラム、およびデータ等を一時的に保持する。   The control unit 44 includes a CPU, a RAM, a ROM, and the like. The CPU calls and executes a program stored in the ROM or the like in a work memory area on the RAM, performs arithmetic processing and operation control, and controls the entire system. The ROM is a non-volatile memory and permanently stores programs, data, and the like. The RAM is a volatile memory, and temporarily stores programs, data, and the like.

表示部45は、CRTモニタ、または液晶パネル等のディスプレイ装置であり、ディスプレイ装置と連携してコンピュータのビデオ機能を実現するための論理回路等(ビデオアダプタ等)を含む。入出力部46は、データの入出力を行う部分である。データの入力を行うものとしては、例えば、キーボード、マウス等のポインティングデバイス、テンキー等であり、これらの入力部を介して、コントローラ41に対して、操作指示、動作指示、データ入力、維持管理等を行うことができる。また、入出力部46に不図示のスキャナやドライブ装置等を接続することにより、これらの外部装置からの入力データを制御部44に転送したり、データを外部装置に出力したりすることができる。   The display unit 45 is a display device such as a CRT monitor or a liquid crystal panel, and includes a logic circuit or the like (video adapter or the like) for realizing a video function of a computer in cooperation with the display device. The input / output unit 46 is a part that inputs and outputs data. Examples of data input include a keyboard, a pointing device such as a mouse, a numeric keypad, and the like. Through these input units, operation instructions, operation instructions, data input, maintenance management, etc. It can be performed. Further, by connecting a scanner, a drive device (not shown) or the like to the input / output unit 46, input data from these external devices can be transferred to the control unit 44, and data can be output to the external device. .

記憶部42はデータを記憶する装置であり、磁気ディスク、メモリ、光ディスク装置等を用いることができる。記憶部42には、制御部44が実行するプログラム、プログラム実行に必要なデータ、OS(Operating System)等が格納される。また、製造装置25の記録部6によって記録されるパターンを格納することもできる。通信部43は、コントローラ41とネットワーク47間の通信を媒介する通信インターフェースであり、通信制御装置および通信ポート等を有する。コントローラ41の代りに、パーソナルコンピュータ等を用いることも可能である。   The storage unit 42 is a device that stores data, and a magnetic disk, a memory, an optical disk device, or the like can be used. The storage unit 42 stores a program executed by the control unit 44, data necessary for program execution, an OS (Operating System), and the like. Moreover, the pattern recorded by the recording part 6 of the manufacturing apparatus 25 can also be stored. The communication unit 43 is a communication interface that mediates communication between the controller 41 and the network 47, and includes a communication control device, a communication port, and the like. A personal computer or the like can be used instead of the controller 41.

[5−1−4]制御系
図11は、図9の記録部6に備わる制御系の構成を示すブロック図である。ホストPC120から送信された記録データやコマンドは、インターフェイスコントローラ102を介してCPU100に受信される。CPU100は、記録部6の記録データの受信、記録動作、転写材1のハンドリング等、全般的な制御を司る演算処理装置である。CPU100は、受信したコマンドを解析した後、記録データの各色成分の画像データをイメージメモリ106にビットマップ展開する。画像の記録前に、出力ポート114およびモータ駆動部116を介してキャッピングモータ122とヘッドアップダウンモータ118を駆動し、記録ヘッド22(22K、22C、22M、22Y)をキャッピング位置(待機位置)から記録位置(画像形成位置)に移動させる。記録ヘッド22K、22C、22M、22Yは、それぞれブラック(Bk)、シアン(C),マゼンタ(M)、イエロー(Y)のインクを吐出する記録ヘッドである。その後、一定速度で搬送される転写材に対して、インクを吐出し始めるタイミング(記録タイミング)を決定するために、センサ部31(先端検出センサ)によって転写材の位置を検出する。その後、転写材の搬送に同期して、CPU100は、イメージメモリ106から各インク色に対応する記録データを順次に読み出し、その記録データを、記録ヘッド制御回路112を介して対応する記録ヘッド22K、22C、22M、22Yに転送する。これにより、記録ヘッドの各ノズルに設けられた吐出エネルギー発生素子(ヒータやピエゾ素子など)が記録データに基づいて駆動され、駆動された吐出エネルギー発生素子に対応するノズルからインク滴が吐出される。吐出されたインク滴は、記録ヘッドの対向位置にある転写材の色材受容層(インク受容部)へ着弾して、ドットを形成する。このドットの集合によって、所望の画像が記録される。
[5-1-4] Control System FIG. 11 is a block diagram showing a configuration of a control system provided in the recording unit 6 of FIG. Recording data and commands transmitted from the host PC 120 are received by the CPU 100 via the interface controller 102. The CPU 100 is an arithmetic processing unit that performs overall control such as reception of recording data of the recording unit 6, recording operation, and handling of the transfer material 1. After analyzing the received command, the CPU 100 develops the image data of each color component of the recording data in the image memory 106 as a bitmap. Before the image recording, the capping motor 122 and the head up / down motor 118 are driven via the output port 114 and the motor driving unit 116, and the recording head 22 (22K, 22C, 22M, 22Y) is moved from the capping position (standby position). Move to the recording position (image forming position). The recording heads 22K, 22C, 22M, and 22Y are recording heads that eject black (Bk), cyan (C), magenta (M), and yellow (Y) inks, respectively. Thereafter, the position of the transfer material is detected by the sensor unit 31 (tip detection sensor) in order to determine the timing (recording timing) at which ink starts to be ejected from the transfer material conveyed at a constant speed. Thereafter, in synchronism with the transfer of the transfer material, the CPU 100 sequentially reads out the recording data corresponding to each ink color from the image memory 106, and the recording data is transferred to the corresponding recording head 22 </ b> K via the recording head control circuit 112. Transfer to 22C, 22M, 22Y. As a result, the ejection energy generating elements (such as heaters and piezo elements) provided in each nozzle of the recording head are driven based on the recording data, and ink droplets are ejected from the nozzles corresponding to the driven ejection energy generating elements. . The ejected ink droplets land on the color material receiving layer (ink receiving portion) of the transfer material at the position facing the recording head to form dots. A desired image is recorded by the set of dots.

このようなCPU100の動作は、プログラムROM104に記憶された処理プログラムに基づいて実行される。プログラムROM104には、制御フローに対応する処理プログラム及びテーブル等が記憶されている。また、作業用のメモリとしてワークRAM108が使用される。   Such an operation of the CPU 100 is executed based on a processing program stored in the program ROM 104. The program ROM 104 stores a processing program corresponding to the control flow, a table, and the like. A work RAM 108 is used as a working memory.

[5−1−5]第1の製造装置の動作フロー
次に、図2のフローチャートにしたがって、図9の製造装置(第1の製造装置)25の動作フローについて説明する。この動作フローにしたがう処理は、図11の記録部のCPU100によって実行される。
[5-1-5] Operation Flow of First Manufacturing Apparatus Next, the operation flow of the manufacturing apparatus (first manufacturing apparatus) 25 of FIG. 9 will be described according to the flowchart of FIG. The processing according to this operation flow is executed by the CPU 100 of the recording unit in FIG.

記録部のCPUは、記録データがコントローラからネットワークまたは各種ポートを介して送信されたか否かを判定し(ステップS101)、記録データが送信されたときに、供給部からの画像が未記録の転写材の供給を開始させる(ステップS102)。そして、マーキングをセンサ部が検出していなければ、つまりセンサ部がOFFであれば、記録部が転写材に対する記録動作を開始する(ステップS103,S104)。記録動作の終了後(ステップS105)、乾燥部の乾燥処理によって、画像が記録された転写材から余分な水分を蒸発させる(ステップS106)。その後、レジストガイドにおいて、画像支持体と転写材とを位置合わせする(ステップS107)。その位置合わせの完了後、付着部において転写材と画像支持体とを接着させる(ステップS108,S109)。以上の動作は、いずれもセンサ部がマーキングを検出した時点を基準としている。   The CPU of the recording unit determines whether or not the recording data is transmitted from the controller via the network or various ports (step S101), and when the recording data is transmitted, the image from the supply unit is not transferred. The material supply is started (step S102). If the marking is not detected by the sensor unit, that is, if the sensor unit is OFF, the recording unit starts a recording operation on the transfer material (steps S103 and S104). After the recording operation is completed (step S105), excess moisture is evaporated from the transfer material on which the image is recorded by the drying process of the drying unit (step S106). Thereafter, the image support and the transfer material are aligned in the resist guide (step S107). After completion of the alignment, the transfer material and the image support are bonded at the attachment portion (steps S108 and S109). The above operations are all based on the time point when the sensor unit detects the marking.

一方、CPUによって、記録データが送信されたと判定されたときに、画像支持体の供給部から付着部へ画像支持体が給送される(ステップS107,S108)。レジストガイドにおいて、画像支持体と転写材とを位置合わせする(ステップS111)。その位置合わせの完了後、付着部において転写材と画像支持体とを接着させる(ステップS112,S113)。その後、剥離部へと搬送されるに伴って、転写材の基材シートが剥離され、記録物(最終記録物)を排出部に排出して積載させる(ステップS114)。   On the other hand, when the CPU determines that the recording data has been transmitted, the image support is fed from the supply portion of the image support to the attachment portion (steps S107 and S108). In the resist guide, the image support and the transfer material are aligned (step S111). After completion of the alignment, the transfer material and the image support are bonded at the attachment portion (steps S112 and S113). Thereafter, the substrate sheet of the transfer material is peeled off as it is conveyed to the peeling portion, and the recorded matter (final recorded matter) is discharged and stacked on the discharge portion (step S114).

[5−1−6]第1の製造装置により実行される処理
[5−1−6−1]転写材の位置検出
図9のセンサ部31は、付着部の動作の同期をとるために転写材1の位置を検出し、CPUは、その検出結果に基づいて各部の制御を行う。マーキングの検出には、反射型又は透過型の光センサを用いる。
[5-1-6] Process Executed by First Manufacturing Apparatus [5-1-6-1] Position Detection of Transfer Material The sensor unit 31 in FIG. 9 performs transfer in order to synchronize the operation of the adhesion portion. The position of the material 1 is detected, and the CPU controls each part based on the detection result. A reflective or transmissive optical sensor is used to detect the marking.

[5−1−6−2]プレカット処理
必要に応じて、転写材に色材受容層を形成した後に、色材受容層の側から、色材受容層と透明シートの一部に切り込みを入れるプレカット処理を行ってもよい。プレカット処理は、反転画像が記録された転写材と画像支持体とを接着した後に、切り込みを起点にして透明シートを綺麗に切断することができる。これにより、均一な厚さの透明シートによって強固な保護層を形成して、色材受容層に形成された反転画像に十分な耐久性を付与することができる。好ましいプレカット処理としては、特開2015−110321号公報に処理方法が挙げられる。
[5-1-6-2] Pre-cut treatment If necessary, after forming the color material receiving layer on the transfer material, cut the color material receiving layer and a part of the transparent sheet from the color material receiving layer side. You may perform a precut process. In the precut process, after the transfer material on which the reverse image is recorded and the image support are bonded, the transparent sheet can be cut cleanly from the notch. Thereby, a strong protective layer can be formed with a transparent sheet having a uniform thickness, and sufficient durability can be imparted to the reverse image formed on the colorant receiving layer. As a preferable precut treatment, a treatment method is disclosed in JP-A No. 2015-110321.

[5−1−6−3]記録処理
前述したように、インクジェット方式の記録装置によれば、記録ヘッドと転写材とが非接触であるため画像を安定的に記録することができ、またフルライン型の場合には、高解像度の高品位の画像を高速に記録することができる。
[5-1-6-3] Recording Process As described above, according to the ink jet recording apparatus, the recording head and the transfer material are not in contact with each other, so that an image can be stably recorded. In the case of the line type, a high-resolution and high-quality image can be recorded at high speed.

図9の製造装置25において、転写材1は、グリップローラ3とニップローラ2とに挟持されつつ、不図示のガイド板上を通過して記録部6に入る。記録部6は、画像データに応じて記録ヘッド6からインクを吐出することにより、転写材1の色材受容層に画像を記録する。   In the manufacturing apparatus 25 of FIG. 9, the transfer material 1 passes through a guide plate (not shown) and enters the recording unit 6 while being sandwiched between the grip roller 3 and the nip roller 2. The recording unit 6 records an image on the color material receiving layer of the transfer material 1 by ejecting ink from the recording head 6 according to the image data.

[5−1−6−4]水分蒸発制御
画像の転写時に、インクを含む色材受容層の表面にインクが残存していると、その色材受容層と画像支持体との密着不良が生じるおそれがある。その転写時の加熱により、色材受容層の表面に残るインク成分やインクが急激に蒸発して、密着不良や色材受容層の部分的な気泡残り等が生じるおそれがある。そのため、画像が記録されてから転写されるまでの間の転写材の搬送路において、その転写材を乾燥させることが好ましい。その場合、ヒータ等の特別な乾燥手段を設けずに、転写前の転写材の搬送路を十分に長くして自然乾燥を促してもよい。また、蒸発したインク成分を考慮して、記録装置内部の気流制御および排気手段が必要となる場合もある。図9の製造装置25においては、インク画像が記録された転写材1が乾燥部7と不図示のガイド板との間を通る際に、ハロゲンなどの熱源、送風機、またはそれら組み合わせた乾燥部7によって、インクの主成分である水や若干の揮発性溶剤成分を蒸発させる。また、その蒸発した気体の記録装置内における結露等を防ぐために、ファン10によって気流および排気を制御する。気流の制御を併用することによって、色材受容層の表面の飽和蒸気圧を改善して乾燥を促進させることもできる。
[5-1-6-4] Water Evaporation Control If the ink remains on the surface of the color material receiving layer containing ink during image transfer, poor adhesion between the color material receiving layer and the image support occurs. There is a fear. Due to the heating during the transfer, the ink component and ink remaining on the surface of the color material receiving layer may be rapidly evaporated, resulting in poor adhesion and partial remaining of bubbles in the color material receiving layer. Therefore, it is preferable to dry the transfer material in the transfer material conveyance path from when the image is recorded to when the image is transferred. In that case, natural drying may be promoted by sufficiently lengthening the conveyance path of the transfer material before transfer without providing a special drying means such as a heater. Further, in consideration of the evaporated ink component, air flow control and exhaust means inside the recording apparatus may be required. In the manufacturing apparatus 25 of FIG. 9, when the transfer material 1 on which an ink image is recorded passes between the drying unit 7 and a guide plate (not shown), a heat source such as a halogen, a blower, or a drying unit 7 combining them. As a result, water, which is the main component of the ink, and some volatile solvent components are evaporated. Further, the air flow and exhaust are controlled by the fan 10 in order to prevent condensation of the evaporated gas in the recording apparatus. By using the control of the airflow in combination, it is possible to improve the saturated vapor pressure on the surface of the colorant receiving layer and promote drying.

このようなインクの水分制御によって、付着部29における付着工程時に、色材受容層中のインクの水分量(色材を除く水と不揮発性溶媒等の総量)をインクの総打ち込み量に対して、好ましくは70%以下、さらに好ましくは50%以下に制御する。インクの水分量が70%以上残る場合には、色材受容層の厚さにもよるが、色材受容層の表面に残るインク成分やインクの急激な蒸発により、密着不良や色材受容層の部分的な気泡残り等が生じるおそれがある。また、インクの総打ち込み量は、記録ヘッドの吐出量により異なるが、上記のような水分制御が適切に行われるように、予め、画像の記録時にドット数を間引く等して適正な量に設定することができる。   By such ink moisture control, the amount of ink moisture (total amount of water, non-volatile solvent, etc. excluding the color material) in the coloring material receiving layer during the adhesion process in the adhesion portion 29 is compared to the total ink deposition amount. , Preferably 70% or less, more preferably 50% or less. When the water content of the ink remains 70% or more, although depending on the thickness of the color material receiving layer, the ink component remaining on the surface of the color material receiving layer or the rapid evaporation of the ink causes poor adhesion or the color material receiving layer. There is a possibility that partial bubble remaining or the like may occur. Although the total ink ejection amount varies depending on the ejection amount of the recording head, it is set in advance to an appropriate amount by thinning out the number of dots during image recording so that the moisture control as described above is appropriately performed. can do.

[5−1−6−5]付着工程
図9のように、画像が記録された転写材1は不図示のガイド板に案内されて、ヒートローラ21,22を含む付着部29に移動する。枚葉状のシート形態の画像支持体55は、供給部12に積載されており、レジストガイド14によって位置を補正されてから、転写材1の搬送に合わせて付着部29に供給される。供給部12は、画像支持体55における画像の転写面へのゴミ付着、およびピックアップ時によるゴムロールからの汚染を防止するため、下側に位置するものから供給される。
[5-1-6-5] Adhering Step As shown in FIG. 9, the transfer material 1 on which an image is recorded is guided by a guide plate (not shown) and moves to the attaching portion 29 including the heat rollers 21 and 22. The sheet-like sheet-shaped image support 55 is stacked on the supply unit 12, the position of which is corrected by the registration guide 14, and then supplied to the attachment unit 29 in accordance with the transfer of the transfer material 1. The supply unit 12 is supplied from the lower side in order to prevent dust from adhering to the image transfer surface of the image support 55 and contamination from the rubber roll during pickup.

画像が記録された転写材1の色材受容層と、画像支持体55と、が当接するように、転写材1と画像支持体55とを重ねてヒートローラ21,22間に搬送して、加熱することにより、画像支持体55と転写材1とが接着される。その後、転写材1の基材シートを剥離する。これにより、画像支持体55は、画像が記録された色材受容層と共に透明シートが付着した状態となる。つまり、画像支持体55上には、透明シートが保護膜として最上層に位置し、その保護膜の下に画像が位置する。   The transfer material 1 and the image support 55 are stacked and conveyed between the heat rollers 21 and 22 so that the color material receiving layer of the transfer material 1 on which the image is recorded and the image support 55 are in contact with each other. By heating, the image support 55 and the transfer material 1 are bonded. Thereafter, the base material sheet of the transfer material 1 is peeled off. As a result, the image support 55 is in a state in which the transparent sheet is attached together with the color material receiving layer on which the image is recorded. That is, on the image support 55, the transparent sheet is positioned in the uppermost layer as a protective film, and the image is positioned under the protective film.

加熱圧着時における転写材への加熱は、プラスチックカード等の厚めの画像支持体側からでなく、主として転写材の基材シート側からの熱伝達によって行う。付着部29による付着工程において、色材受容層の最大到達温度は、色材受容層の水溶性樹脂成分をガラス転移温度以上で、かつインクの主成分たる水の蒸発温度を超えないように制御すればよい。つまり、転写材1と画像支持体55とを接着させる際のヒートローラの表面温度は、色材受容層の水溶性樹脂が十分に溶融し、かつ水が蒸発して転写材1と画像支持体55との間に気泡を生じさせない温度であればよい。また、搬送速度等が速くて、熱源による加熱時間が十分に確保できない場合には、熱源と色材受容層とに温度差が生じるおそれがある。この場合には、ヒートローラの表面温度は、100〜180℃等、通常よりも高くなるように制御してもよい。また、閉空間内において加熱した場合には、圧力上昇によって沸点が上昇して、プライマー層と透明シート層とに挟まれた色材受容層では水の蒸発温度は上昇するため、密着性および端部の箔切れ性に考慮してさらに高い温度となるように制御してもよい。   Heating to the transfer material at the time of thermocompression bonding is performed mainly by heat transfer from the side of the base material sheet of the transfer material, not from the side of the thick image support such as a plastic card. In the adhesion process by the adhesion part 29, the maximum temperature reached by the color material receiving layer is controlled so that the water-soluble resin component of the color material receiving layer is not less than the glass transition temperature and does not exceed the evaporation temperature of water, which is the main component of the ink. do it. That is, the surface temperature of the heat roller when the transfer material 1 and the image support 55 are bonded is such that the water-soluble resin of the color material receiving layer is sufficiently melted and the water is evaporated to transfer the transfer material 1 and the image support. The temperature may be any temperature that does not cause bubbles to be generated between the temperature and 55. In addition, when the conveyance speed is high and the heating time by the heat source cannot be secured sufficiently, there is a possibility that a temperature difference occurs between the heat source and the color material receiving layer. In this case, the surface temperature of the heat roller may be controlled to be higher than usual, such as 100 to 180 ° C. In addition, when heated in a closed space, the boiling point rises due to an increase in pressure, and the water evaporation temperature rises in the colorant receiving layer sandwiched between the primer layer and the transparent sheet layer. The temperature may be controlled to be higher in consideration of the foil breakability of the part.

[5−1−6−6]予備加熱
必要に応じて、画像支持体55を加熱して転写材1との密着性を向上させるために、予備加熱部を供給部12と付着部との間に設けてもよい。予備加熱により、転写材1が付着される前の画像支持体(カード等)55の表面を適度に加熱することができる。
[5-1-6-6] Preheating If necessary, the preheating unit is provided between the supply unit 12 and the adhering unit in order to improve the adhesion to the transfer material 1 by heating the image support 55. May be provided. By the preheating, the surface of the image support (card etc.) 55 before the transfer material 1 is attached can be appropriately heated.

[5−1−6−7]カール矯正
図9のように、画像支持体55と転写材1とを付着させた後に、カール矯正部150によって画像支持体55のカールを矯正して、それをフラットにする。画像支持体55が温かいうちに、それをカール矯正部150における加熱プレートと支持プレートとの間に挟み込むことにより、その画像支持体55のカールを矯正することができる。
[5-1-6-7] Curling Correction As shown in FIG. 9, after the image support 55 and the transfer material 1 are attached, the curling of the image support 55 is corrected by the curl correction unit 150. Make it flat. While the image support 55 is warm, the curl of the image support 55 can be corrected by sandwiching it between the heating plate and the support plate in the curl correction unit 150.

[5−1−6−8]剥離処理
図9のように、付着部29を通過した転写材1における基材シート50は、画像の記録領域以外の部分が剥がされて、巻取りロール24に巻き取られる。また画像が転写された画像支持体55は、排出部26に搬送されて一枚ずつ集積される。
[5-1-6-8] Peeling Process As shown in FIG. 9, the base material sheet 50 in the transfer material 1 that has passed through the adhering portion 29 is peeled off at portions other than the image recording area, and is taken up by the take-up roll 24. It is wound up. Further, the image support 55 to which the image is transferred is conveyed to the discharge unit 26 and accumulated one by one.

[5−1−6−9]画像反転装置
画像支持体55の両面に画像を転写する場合には、図9のように、製造装置25に画像反転部152を備えることが好ましい。画像支持体55の一方の面(表面)に画像が転写されて、その面から基材シート50が剥離された後の画像支持体55(記録物)は、反転装置152により上下が反転される。その記録物は、他方の面(裏面)に画像を転写するために、レジストガイド14までフィードバックされる。これと同時に転写材1もフィードバックされ、そのフィードバック後、記録部、付着部、カール矯正部、および剥離部において表面の画像記録時と同様の処理を行なって、記録物の裏面に画像が転写される。
[5-1-6-9] Image Inversion Device When images are transferred to both sides of the image support 55, it is preferable that the manufacturing apparatus 25 includes an image inversion unit 152 as shown in FIG. The image support 55 (recorded material) after the image is transferred to one surface (front surface) of the image support 55 and the base sheet 50 is peeled from the surface is inverted by the reversing device 152. . The recorded matter is fed back to the resist guide 14 in order to transfer the image to the other side (back side). At the same time, the transfer material 1 is also fed back, and after that feedback, the image is transferred to the back side of the recorded material by performing the same processing as the front side image recording in the recording unit, the adhesion unit, the curl correction unit, and the peeling unit. The

製造装置25には、図13のように、転写材1の搬送経路上のインクジェト画像記録後に、転写材1にプライマーを転写するための転写部13を備えてもよい。プライマーは、レジストガイド14において位置合わせされた画像支持体55を転写材1に接着させるためのものである。   As shown in FIG. 13, the manufacturing apparatus 25 may include a transfer unit 13 for transferring a primer to the transfer material 1 after recording an inkjet image on the transfer path of the transfer material 1. The primer is for adhering the image support 55 aligned in the resist guide 14 to the transfer material 1.

転写部13には、転写材1が1枚ずつ供給される。転写部13において、プライマーシートは、供給ロール15(プライマー供給ロール)から供給され、サーマルヘッド30と転写材1との間を通り、ガイドロール16を経由して巻上げロール17(プライマー巻上げロール)に巻き取られる。サーマルヘッド30によって、転写材1にプライマーが転写される。サーマルヘッド30は、プライマーの厚さや材質等により変化する熱容量に応じたエネルギーが印加されることにより、発熱して、プライマーを転写材1に移行させて接着層を形成する。サーマルヘッド30がプライマーシートを部分的に加熱(選択的加熱)することにより、IC部等、表面コートを施したくない特殊な部分に対しては、プライマーを転写させない選択的なプライマー転写が可能となる。転写材1の全面にプライマー層を付与する場合には、ヒートローラ等の安価な加熱手段を用いてプライマー転写を行うことが可能である。   The transfer material 1 is supplied to the transfer unit 13 one by one. In the transfer unit 13, the primer sheet is supplied from a supply roll 15 (primer supply roll), passes between the thermal head 30 and the transfer material 1, and passes through a guide roll 16 to a winding roll 17 (primer winding roll). It is wound up. The primer is transferred to the transfer material 1 by the thermal head 30. The thermal head 30 generates heat by applying energy corresponding to the heat capacity that varies depending on the thickness and material of the primer, and the primer is transferred to the transfer material 1 to form an adhesive layer. When the thermal head 30 partially heats the primer sheet (selective heating), it is possible to perform selective primer transfer that does not transfer the primer to special parts that do not require surface coating, such as IC parts. Become. When a primer layer is applied to the entire surface of the transfer material 1, primer transfer can be performed using an inexpensive heating means such as a heat roller.

[5−2]第2の製造装置
図28は、記録物の製造装置の第2の構成例(以下、「第2の製造装置」ともいう)の説明図である。第2の製造装置25は、透明シートに予め細孔構造が構成されていない転写材1を用いる。この第2の製造装置は、前述した第1の製造装置に対して、透明シートに細孔を付与するための穿孔加工部659を備えた構成となっている。この穿孔加工部659は、画像記録前の転写材1の透明シートに対して細孔を付与する。第1の製造装置と同様の部分についての説明は省略する。
[5-2] Second Manufacturing Apparatus FIG. 28 is an explanatory diagram of a second configuration example (hereinafter, also referred to as “second manufacturing apparatus”) of a recorded matter manufacturing apparatus. The second manufacturing apparatus 25 uses the transfer material 1 in which the pore structure is not previously configured in the transparent sheet. This 2nd manufacturing apparatus is the structure provided with the punching process part 659 for providing a pore to a transparent sheet with respect to the 1st manufacturing apparatus mentioned above. This perforation processing part 659 gives pores to the transparent sheet of the transfer material 1 before image recording. A description of the same parts as those of the first manufacturing apparatus is omitted.

穿孔加工部659は、転写材の色材受容層側もしく基材シート側のどちら側からでも透明シートに細孔を形成することができる。記録画像の品位を良好に保つためには、図28のように、基材シート側から穿孔することが好ましい。また、このような穿孔加工は、図24のように、少なくとも透明シートに細孔が形成できればよい。その穿孔加工は、図46(a),(b)のような針657、拍車650、刃型などの機械的の穿孔加工、あるいは図46(c)のようなレーザ加工装置658によるレーザ加工であってもよい。   The perforating part 659 can form pores in the transparent sheet from either the colorant receiving layer side or the base sheet side of the transfer material. In order to maintain the quality of the recorded image, it is preferable to perforate from the base sheet side as shown in FIG. Moreover, such a perforation process should just form a pore at least in a transparent sheet like FIG. The drilling is performed by mechanical drilling such as a needle 657, a spur 650, and a blade shape as shown in FIGS. 46 (a) and 46 (b), or laser processing by a laser processing device 658 as shown in FIG. 46 (c). There may be.

[5−3]第3の製造装置
図29は、記録物の製造装置の第3の構成例(以下、「第3の製造装置」ともいう)の説明図である。第3の製造装置25は、透明シートに予め細孔構造が構成されていない転写材1を用いる。この第3の製造装置は、穿孔加工部659の配備位置が第2の製造装置と異なる。すなわち、第3の製造装置における穿孔加工部659は、画像記録後の転写材1の透明シートに対して細孔を付与するように配備されている。第2の製造装置と同様の部分についての説明は省略する。
[5-3] Third Manufacturing Apparatus FIG. 29 is an explanatory diagram of a third configuration example (hereinafter, also referred to as “third manufacturing apparatus”) of a recorded matter manufacturing apparatus. The 3rd manufacturing apparatus 25 uses the transfer material 1 by which the pore structure is not previously comprised by the transparent sheet. This third manufacturing apparatus is different from the second manufacturing apparatus in the position where the drilling unit 659 is provided. That is, the perforation processing unit 659 in the third manufacturing apparatus is arranged so as to give pores to the transparent sheet of the transfer material 1 after image recording. A description of the same parts as those of the second manufacturing apparatus is omitted.

[5−4]第4の製造装置
図30は、記録物の製造装置の第4の構成例(以下、「第4の製造装置」ともいう)の説明図である。第4の製造装置25は、透明シートに予め細孔構造が構成されていない転写材1を用いる。この第4の製造装置は、穿孔加工部659の配備位置が第2および第3の製造装置と異なる。すなわち、第4の製造装置における穿孔加工部659は、図25のように、画像が転写されたた後、かつ基材シートの剥離前における転写材1の透明シートに対して、細孔を付与するように配備されている。第2の製造装置と同様の部分についての説明は省略する。
[5-4] Fourth Manufacturing Apparatus FIG. 30 is an explanatory diagram of a fourth configuration example (hereinafter also referred to as “fourth manufacturing apparatus”) of a recorded matter manufacturing apparatus. The 4th manufacturing apparatus 25 uses the transfer material 1 by which the pore structure is not previously comprised by the transparent sheet. This fourth manufacturing apparatus is different from the second and third manufacturing apparatuses in the position where the drilling unit 659 is disposed. That is, as shown in FIG. 25, the punching unit 659 in the fourth manufacturing apparatus gives pores to the transparent sheet of the transfer material 1 after the image is transferred and before the substrate sheet is peeled off. Have been deployed. A description of the same parts as those of the second manufacturing apparatus is omitted.

[5−5]第5の製造装置
図31は、記録物の製造装置の第5の構成例(以下、「第5の製造装置」ともいう)の説明図である。第5の製造装置25は、透明シートに予め細孔構造が構成されていない転写材1を用いる。この第5の製造装置は、穿孔加工部659の配備位置が第2,第3,および第4の製造装置と異なる。すなわち、第5の製造装置における穿孔加工部659は、図26のように、画像が転写され、かつ基材シートの剥離された後における転写材1の透明シートに対して、細孔を付与するように配備されている。第2の製造装置と同様の部分についての説明は省略する。
[5-5] Fifth Manufacturing Apparatus FIG. 31 is an explanatory diagram of a fifth configuration example (hereinafter also referred to as “fifth manufacturing apparatus”) of a recorded matter manufacturing apparatus. The fifth manufacturing apparatus 25 uses the transfer material 1 in which the pore structure is not previously configured in the transparent sheet. This fifth manufacturing apparatus is different from the second, third, and fourth manufacturing apparatuses in the position where the drilling unit 659 is disposed. That is, as shown in FIG. 26, the punching unit 659 in the fifth manufacturing apparatus gives pores to the transparent sheet of the transfer material 1 after the image is transferred and the base material sheet is peeled off. Have been deployed. A description of the same parts as those of the second manufacturing apparatus is omitted.

[5−6]第6の製造装置
記録物の製造装置の第6の構成例(以下、「第6の製造装置」ともいう)においては、プリンタ部と転写部とが分離独立して構成されている。
[5-6] Sixth Manufacturing Apparatus In the sixth configuration example (hereinafter also referred to as “sixth manufacturing apparatus”) of the recorded product manufacturing apparatus, the printer unit and the transfer unit are configured separately and independently. ing.

図14(a)は、転写材1に画像を記録するプリンタ301の斜視図であり、図14(b)および図15(a)は、転写材1を搬送する搬送機構302の説明図である。まず、図15(a)の巻き出しロール313に、図15(b)のように色材受容層53が外側にして巻かれたロール状(外巻きロール)の転写材1をセットする。転写材1は、搬送ベルト310によって記録ヘッド311と対向する記録位置に搬送され、反転画像が記録されてから、巻き取りロール314によって記録媒体として巻き取られる。   14A is a perspective view of the printer 301 that records an image on the transfer material 1, and FIGS. 14B and 15A are explanatory views of a conveyance mechanism 302 that conveys the transfer material 1. FIG. . First, the roll-shaped transfer material 1 in which the color material receiving layer 53 is wound outward as shown in FIG. 15B is set on the unwinding roll 313 in FIG. The transfer material 1 is transported to a recording position facing the recording head 311 by the transport belt 310 and a reverse image is recorded, and then is wound as a recording medium by a winding roll 314.

次に、画像が記録済みのロール状の転写材(記録媒体)1を、図16のラミネート機の巻き出しロール201にセットする。画像支持体55が供給部206から供給され、転写材1は巻き出しロール201から転写部203へ搬送される。転写材は、センサ208によってマーキングが検知され、画像支持体55と位置合わせされてから、転写ロール204によって画像支持体55と加熱圧着される。その後、転写材1の基材シート50が剥離ロール207によって剥離されてから、巻き取りロール202によって巻き取られる。なお、図17(a)のように、基材シート50を外側にし、色材受容層53を内側にして巻かれたロール状(内巻きロール)の転写材1を用いる場合には、図17(b)のように構成された搬送パスを用いる。このような内巻きのロール形態においては、色材受容層の表面に対するゴミの付着を防止することができる。   Next, a roll-shaped transfer material (recording medium) 1 on which an image has been recorded is set on the unwinding roll 201 of the laminating machine shown in FIG. The image support 55 is supplied from the supply unit 206, and the transfer material 1 is conveyed from the unwinding roll 201 to the transfer unit 203. Marking of the transfer material is detected by the sensor 208 and is aligned with the image support 55, and then the transfer material is heat-pressed with the image support 55 by the transfer roll 204. Then, after the base material sheet 50 of the transfer material 1 is peeled off by the peeling roll 207, it is wound up by the winding roll 202. As shown in FIG. 17A, when the roll-shaped (inner winding roll) transfer material 1 wound with the base sheet 50 outside and the color material receiving layer 53 inside is used, FIG. The conveyance path configured as shown in (b) is used. In such an inner roll form, dust can be prevented from adhering to the surface of the colorant receiving layer.

透明シートに予め細孔構造が構成されていない転写材を用いる場合には、図50(a),(b)のように記録ヘッド311による画像の記録工程の前後において、穿孔加工部659により透明シートに細孔を形成することができる。または、図51(a),(b),(c)のようにラミネート機による転写工程の前、基材シートの剥離工程の後、基材シートの剥離工程の前において、穿孔加工部659により透明シートに細孔を形成してもよい。また、穿孔加工部659は、プリンタ部と転写部から独立させた穿孔加工装置を構成するものであってもよい。この場合、転写材の状態において細孔を形成するためには、プリンタ部と転写部の間に、図56(a)のような独立した穿孔加工部を設けることが好ましい。また、基材シートの剥離後に細孔を形成するためには、図56(b)のように、画像の転写工程の後に穿孔加工をする独立した穿孔加工部を設けることが好ましい。   When a transfer material having a pore structure not previously formed is used for the transparent sheet, as shown in FIGS. 50A and 50B, before and after the image recording process by the recording head 311, the punching processing unit 659 makes the transparent sheet transparent. It is possible to form pores in the sheet. Alternatively, as shown in FIGS. 51 (a), 51 (b), and 51 (c), before the transfer process by the laminator, after the peeling process of the base material sheet, and before the peeling process of the base material sheet, the perforation processing unit 659 You may form a pore in a transparent sheet. Further, the punching unit 659 may constitute a punching device that is independent from the printer unit and the transfer unit. In this case, in order to form the pores in the state of the transfer material, it is preferable to provide an independent punching portion as shown in FIG. 56 (a) between the printer portion and the transfer portion. Further, in order to form pores after the substrate sheet is peeled off, it is preferable to provide an independent perforating part for perforating after the image transfer step as shown in FIG.

[5−7]第7の製造装置
記録物の製造装置の第7の構成例(以下、「第7の製造装置」ともいう)においては、プリンタ部と転写部とが分離独立して構成されている。この製造装置は、図18のように、転写材1に画像が記録した後に、その転写材1をカット機構315によってシート状にカットしてから、排出部316に排出するように構成されている。カットされた転写材1は、その後、図19のように、手動によって画像支持体55と位置合わせされた後、転写部203を構成する転写ロール204によって加熱圧着されてから、排出部205に排出される。その後、基材シートを手動で引き剥がして記録物を得る。また、転写材に画像する記録するときに張り合わせガイドを同時に記録することにより、その張り合わせガイドに画像支持体55が沿うように目視により確認しつつ、それらを手動により位置合わせすることができる。
[5-7] Seventh Manufacturing Apparatus In a seventh configuration example (hereinafter also referred to as “seventh manufacturing apparatus”) of a recorded product manufacturing apparatus, a printer unit and a transfer unit are configured separately and independently. ing. As shown in FIG. 18, the manufacturing apparatus is configured such that after an image is recorded on the transfer material 1, the transfer material 1 is cut into a sheet shape by a cutting mechanism 315 and then discharged to a discharge unit 316. . Thereafter, the cut transfer material 1 is manually aligned with the image support 55 as shown in FIG. 19, and then heat-pressed by the transfer roll 204 constituting the transfer unit 203 and then discharged to the discharge unit 205. Is done. Thereafter, the substrate sheet is manually peeled off to obtain a recorded matter. Further, by simultaneously recording the bonding guide when recording an image on the transfer material, it is possible to manually align them while visually confirming that the image support 55 is along the bonding guide.

透明シートに予め細孔構造が構成されていない転写材を用いる場合には、図52(a),(b)のようにカット機構315による転写材1のカット工程の前後において、穿孔加工部659により透明シートに細孔を形成することができる。または、図53(a),(b)のようにラミネート機による転写工程の前後において、穿孔加工部659により透明シートに細孔を形成してもよい。また、穿孔加工部659は、プリンタ部と転写部から独立させた穿孔加工装置を構成するものであってもよい。この場合、転写材の状態において細孔を形成するためには、プリンタ部と転写部の間に、図57のような独立した穿孔加工部を設けることが好ましい。また、基材シートの剥離後に細孔を形成するためには、図58のように、画像の転写工程の後に穿孔加工をする独立した穿孔加工部を設けることが好ましい。   When using a transfer material in which the pore structure is not previously configured for the transparent sheet, the punching section 659 is used before and after the cutting process of the transfer material 1 by the cutting mechanism 315 as shown in FIGS. 52 (a) and 52 (b). Thus, pores can be formed in the transparent sheet. Alternatively, as shown in FIGS. 53 (a) and 53 (b), before and after the transfer process by the laminating machine, pores may be formed in the transparent sheet by the perforating part 659. Further, the punching unit 659 may constitute a punching device that is independent from the printer unit and the transfer unit. In this case, in order to form the pores in the state of the transfer material, it is preferable to provide an independent punching portion as shown in FIG. 57 between the printer portion and the transfer portion. In order to form the pores after the substrate sheet is peeled off, it is preferable to provide an independent perforation processing part for perforating after the image transfer step as shown in FIG.

[5−8]第8の製造装置
記録物の製造装置の第8の構成例(以下、「第8の製造装置」ともいう)においては、プリンタ部と転写部とが分離独立して構成されている。
[5-8] Eighth Manufacturing Apparatus In an eighth configuration example (hereinafter also referred to as “eighth manufacturing apparatus”) of a recorded product manufacturing apparatus, a printer unit and a transfer unit are configured separately and independently. ing.

図20(a)は、カットシート状に加工された転写材1に画像を記録するプリンタ401の斜視図であり、図20(b)は、プリンタ401における搬送機構402の概略構成図である。プリンタ401の供給部にセットされた転写材1は、搬送ベルト310によって記録ヘッド311と対向する記録位置に搬送され、反転画像が記録されてから、記録媒体として排出部414に排出される。その後、画像が記録済みの転写材1と画像支持体55とを図19のラミネート機より加熱圧着してから、手動により基材シートを引き剥がすことにより、記録物を得る。また、転写材に画像する記録するときに張り合わせガイドを同時に記録することにより、その張り合わせガイドに画像支持体55が沿うように目視により確認しつつ、それらを手動により位置合わせすることができる。   20A is a perspective view of the printer 401 that records an image on the transfer material 1 processed into a cut sheet shape, and FIG. 20B is a schematic configuration diagram of the transport mechanism 402 in the printer 401. The transfer material 1 set in the supply unit of the printer 401 is conveyed to a recording position facing the recording head 311 by the conveyance belt 310, and after a reverse image is recorded, it is discharged as a recording medium to the discharge unit 414. Thereafter, the transfer material 1 on which the image has been recorded and the image support 55 are heat-pressed by the laminating machine shown in FIG. 19, and then the base material sheet is manually peeled off to obtain a recorded matter. Further, by simultaneously recording the bonding guide when recording an image on the transfer material, it is possible to manually align them while visually confirming that the image support 55 is along the bonding guide.

透明シートに予め細孔構造が構成されていない転写材を用いる場合には、図54(a),(b)のように記録ヘッド311による画像の記録工程の前後において、穿孔加工部659により透明シートに細孔を形成することができる。または、図53(a),(b)のようにラミネート機による転写工程の前後において、穿孔加工部659により透明シートに細孔を形成してもよい。また、穿孔加工部659は、プリンタ部と転写部から独立させた穿孔加工装置を構成するものであってもよい。この場合、転写材の状態において細孔を形成するためには、プリンタ部と転写部の間に、図58のような独立した穿孔加工部を設けることが好ましい。また、基材シートの剥離後に細孔を形成するためには、図56(b)のように、画像の転写工程の後に穿孔加工をする独立した穿孔加工部を設けることが好ましい。   When a transfer material that does not have a pore structure formed in advance is used for the transparent sheet, as shown in FIGS. 54A and 54B, before and after the image recording process by the recording head 311, the punching processing unit 659 makes the transparent sheet transparent. It is possible to form pores in the sheet. Alternatively, as shown in FIGS. 53 (a) and 53 (b), before and after the transfer process by the laminating machine, pores may be formed in the transparent sheet by the perforating part 659. Further, the punching unit 659 may constitute a punching device that is independent from the printer unit and the transfer unit. In this case, in order to form pores in the state of the transfer material, it is preferable to provide an independent perforating portion as shown in FIG. 58 between the printer portion and the transfer portion. Further, in order to form pores after the substrate sheet is peeled off, it is preferable to provide an independent perforating part for perforating after the image transfer step as shown in FIG.

[5−9]第9の製造装置
記録物の製造装置の第9の構成例(以下、「第9の製造装置」ともいう)においては、プリンタ部と転写部とが分離独立して構成されている。
[5-9] Ninth Manufacturing Apparatus In a ninth configuration example (hereinafter also referred to as “ninth manufacturing apparatus”) of a recorded product manufacturing apparatus, the printer unit and the transfer unit are configured separately and independently. ing.

図13のようなプリンタ部と転写部とが一体の製造装置において、シリアル型のインクジェットプリンタを用いる場合には、プリント部と転写部との間において、転写材および画像支持体の搬送速度に差を生じる場合があるため、このような速度差を吸収及び調節するためには、転写材および画像支持体に弛みをもたせる必要がある。プリント部と転写部とを独立させた分離型の場合には、プリント部と転写部における処理を各々の最適な速度で実施することができるため好ましい。   In a manufacturing apparatus in which the printer unit and the transfer unit are integrated as shown in FIG. 13, when a serial type ink jet printer is used, there is a difference in the transfer speed of the transfer material and the image support between the print unit and the transfer unit. In order to absorb and adjust such a speed difference, it is necessary to make the transfer material and the image support slack. In the case of a separation type in which the print unit and the transfer unit are made independent, it is preferable because the processing in the print unit and the transfer unit can be carried out at the respective optimum speeds.

図21(a)は、転写材1に画像を記録するシリアルプリンタ501の斜視図であり、供給部513に転写材1がセットされる。転写材1は、搬送ロール510によって記録ヘッド502と対向する記録位置に搬送され、反転画像が記録されてから排出される。記録ヘッド502を矢印a,b方向に移動させつつ、記録ヘッド502のノズル511(図21(b)からインクを吐出する動作と、矢印a,b方向と交差(本例の場合は、直交)する方向に転写材1を搬送する動作と、繰り返すことによって、画像を記録する。その後、画像が記録済みの転写材と画像支持体とを図19のラミネート機により加熱圧着させてから、手動で基材シートを引き剥がすことにより、記録物を得る。また、転写材に画像する記録するときに張り合わせガイドを同時に記録することにより、その張り合わせガイドに画像支持体55が沿うように目視により確認しつつ、それらを手動により位置合わせすることができる。   FIG. 21A is a perspective view of a serial printer 501 that records an image on the transfer material 1, and the transfer material 1 is set in the supply unit 513. The transfer material 1 is transported to a recording position facing the recording head 502 by a transport roller 510, and is discharged after a reverse image is recorded. While moving the recording head 502 in the directions of arrows a and b, the nozzle 511 of the recording head 502 (the operation of ejecting ink from FIG. 21B) intersects the directions of arrows a and b (in this example, orthogonal). The image is recorded by repeating the operation of transporting the transfer material 1 in the direction in which the image is recorded.Then, the transfer material on which the image has been recorded and the image support are heat-pressed by the laminating machine of FIG. A recorded material is obtained by peeling off the base material sheet, and a recording guide is simultaneously recorded when an image is recorded on a transfer material, so that the image support 55 is visually confirmed to be along the bonding guide. However, they can be manually aligned.

透明シートに予め細孔構造が構成されていない転写材を用いる場合には、図55(a),(b)のように記録ヘッド502による画像の記録工程の前後において、穿孔加工部659により透明シートに細孔を形成することができる。または、図53(a),(b)のようにラミネート機による転写工程の前後において、穿孔加工部659により透明シートに細孔を形成してもよい。また、穿孔加工部659は、プリンタ部と転写部から独立させた穿孔加工装置を構成するものであってもよい。この場合、転写材の状態において細孔を形成するためには、プリンタ部と転写部の間に、図58のような独立した穿孔加工部を設けることが好ましい。また、基材シートの剥離後に細孔を形成するためには、図56(b)のように、画像の転写工程の後に穿孔加工をする独立した穿孔加工部を設けることが好ましい。   In the case where a transfer material that does not have a pore structure formed in advance is used for the transparent sheet, as shown in FIGS. It is possible to form pores in the sheet. Alternatively, as shown in FIGS. 53 (a) and 53 (b), before and after the transfer process by the laminating machine, pores may be formed in the transparent sheet by the perforating part 659. Further, the punching unit 659 may constitute a punching device that is independent from the printer unit and the transfer unit. In this case, in order to form pores in the state of the transfer material, it is preferable to provide an independent perforating portion as shown in FIG. 58 between the printer portion and the transfer portion. Further, in order to form pores after the substrate sheet is peeled off, it is preferable to provide an independent perforating part for perforating after the image transfer step as shown in FIG.

以上の第1から第9の製造装置においては、転写材が基材上に少なくとも透明シートと色材受容層を有している場合に、転写材を画像支持体に付着させる工程において、色材受容層のインク水分量の制御と付着時の温度制御とが行われる。これにより、転写材の透明シートと画像支持体との密着性を向上させて、耐候性、耐水性、耐薬品性、および耐ガス性等の各種耐久性に優れた記録物を提供することができる。   In the first to ninth manufacturing apparatuses described above, in the step of attaching the transfer material to the image support when the transfer material has at least a transparent sheet and a color material receiving layer on the base material, Control of the ink moisture content of the receiving layer and temperature control at the time of adhesion are performed. Thereby, it is possible to improve the adhesion between the transparent sheet of the transfer material and the image support, and to provide a recorded material excellent in various durability such as weather resistance, water resistance, chemical resistance, and gas resistance. it can.

(第2の発明)
次に、第2の発明について説明する
(Second invention)
Next, the second invention will be described.

[6]第2の発明の転写材
図68は、第2の発明における転写材1の断面図である。その転写材1は、基材シート50、透明シート52及び色材受容層53がこの順で積層された積層構造であり、透明シート52は水分を系外に水を排する機構を有する。色材受容層53は水溶性樹脂を含有し、また透明シート52は膨潤性樹脂を含有している。
[6] Transfer Material of Second Invention FIG. 68 is a sectional view of the transfer material 1 in the second invention. The transfer material 1 has a laminated structure in which a base sheet 50, a transparent sheet 52, and a color material receiving layer 53 are laminated in this order, and the transparent sheet 52 has a mechanism for draining water out of the system. The color material receiving layer 53 contains a water-soluble resin, and the transparent sheet 52 contains a swellable resin.

図60は、画像支持体55に、転写材1の色材受容層53と透明シート52を転写して作成した記録物73の断面図である。透明シート52は膨潤性樹脂を有するため、色材受容層53に含まれる不要な水分を吸収して、その表面から水蒸気550として蒸発させることができる。図59は、図69の記録物73を長時間、水に浸漬させた後、水から取り出した状態における記録物73の断面図である。記録物73を水から取り出すと、色材受容層53に吸収された水分は色材受容層53の端部からだけでなく、膨潤性樹脂を介して透明シート52の表面全体からも蒸発する。このように、透明シートの表面全体から色材受容層内の水分を蒸発させることにより、色材受容層の収縮の応力は、矢印Bのように透明シートの表面全体に広く分散され、この結果、透明シートのひび割れを抑制することができる。   60 is a cross-sectional view of a recorded matter 73 created by transferring the color material receiving layer 53 of the transfer material 1 and the transparent sheet 52 to the image support 55. FIG. Since the transparent sheet 52 has a swellable resin, it can absorb unnecessary moisture contained in the color material receiving layer 53 and evaporate from the surface as water vapor 550. 59 is a cross-sectional view of the recorded matter 73 in a state where the recorded matter 73 of FIG. 69 is immersed in water for a long time and then taken out from the water. When the recorded matter 73 is taken out of the water, the water absorbed in the color material receiving layer 53 evaporates not only from the end portion of the color material receiving layer 53 but also from the entire surface of the transparent sheet 52 through the swelling resin. In this way, by evaporating the water in the color material receiving layer from the entire surface of the transparent sheet, the shrinkage stress of the color material receiving layer is widely dispersed over the entire surface of the transparent sheet as indicated by the arrow B. As a result, The crack of a transparent sheet can be suppressed.

第2の発明と前述した第1の発明との相違点について説明する。第1の発明において、透明シートは、基材シートと色材受容層との間を貫通する細孔を有し、その物理的な穴(細孔)を通して色材受容層の水分が系外に排出される。この第1の発明においては、水が通過する細孔を他の分子が通る可能性がある。例えば、オゾンの分子などである。気体の水分子の大きさは0.4nm、オゾン分子の大きさは0.44nmであり、水が通ることのできる大きさの細孔であればオゾンも通過する可能性がある。そのため、第1の発明における透明シートは、第2の発明における無孔質の透明シートと比較すると、耐ガス性に関しては少し低下するおそれがある。しかしながら、色材として耐候性に優れた顔料を使用することにより、実用的に耐ガス性の低下は問題にならない。   Differences between the second invention and the first invention will be described. In the first invention, the transparent sheet has pores penetrating between the base material sheet and the color material receiving layer, and moisture of the color material receiving layer is exposed outside the system through the physical holes (pores). Discharged. In the first invention, there is a possibility that other molecules pass through the pores through which water passes. For example, ozone molecules. The size of gaseous water molecules is 0.4 nm, the size of ozone molecules is 0.44 nm, and ozone may pass if the pores are large enough to allow water to pass through. For this reason, the transparent sheet in the first invention may be slightly reduced in terms of gas resistance as compared to the nonporous transparent sheet in the second invention. However, by using a pigment having excellent weather resistance as a color material, a decrease in gas resistance is not a problem in practice.

第2の発明における透明シートは膨潤性樹脂を含むものであって、透明シートの物理的な細孔ではなく、透明シートの膨潤性樹脂の分子内を通過して、水が系外に排出される。透明シートが貫通する細孔を持っていないため、水以外の気体は通過し難く、耐ガス性に優れている。一方、透明シートに含まれる膨潤性樹脂は液体の水も吸収するため、汚染水等が透明シートの表面に長時間付着した場合に、それが透明シートの表面からも吸収される。そのため、第1の発明における透明シートと比較すると、薬品、および汚染水など液体状の汚れからの保護性能は劣るおそれがある。しかし、膨潤性樹脂を含む透明シートにおける水の吸収速度は、細孔を含む空隙吸収型の色材受容層における水の吸収速度の数十分の1程度であるため、短時間で液体状の汚れをふき取れば色材受容層の汚染までには至らない。   The transparent sheet in the second invention contains a swellable resin, and passes through the molecules of the swellable resin of the transparent sheet, not physical pores of the transparent sheet, and water is discharged out of the system. The Since the transparent sheet does not have through-holes, gases other than water do not easily pass through and are excellent in gas resistance. On the other hand, since the swellable resin contained in the transparent sheet also absorbs liquid water, when contaminated water or the like adheres to the surface of the transparent sheet for a long time, it is also absorbed from the surface of the transparent sheet. Therefore, compared with the transparent sheet in the first invention, the protection performance from liquid stains such as chemicals and contaminated water may be inferior. However, the water absorption rate in the transparent sheet containing the swellable resin is about several tenths of the water absorption rate in the void-absorbing type colorant receiving layer containing pores. Wiping off the stain will not lead to contamination of the colorant receiving layer.

第2の発明における記録物73を製造する際には、図70のように、まず、転写材1の色材受容層53に、記録ヘッド607によって反転画像72を記録する(工程1)。次に、ヒートローラ21を用いて転写材1と画像支持体55とを加熱圧着して、画像支持体55に色材受容層53を転写させる(工程2)。最後に、剥離ロール88を用いて基材シート50を剥離(工程3)することにより、インクジェット記録物73を得る。   When manufacturing the recorded matter 73 according to the second invention, as shown in FIG. 70, first, the reverse image 72 is recorded on the color material receiving layer 53 of the transfer material 1 by the recording head 607 (step 1). Next, the transfer material 1 and the image support 55 are heat-pressed using the heat roller 21, and the color material receiving layer 53 is transferred to the image support 55 (step 2). Finally, the base material sheet 50 is peeled using the peeling roll 88 (step 3), thereby obtaining an ink jet recorded matter 73.

上述したように、第2の発明における転写材は、基材シート、透明シート及び色材受容層がこの順で積層された積層構造を有し、色材受容層は水溶性樹脂を含有し、透明シートは膨潤性樹脂を含有する。   As described above, the transfer material in the second invention has a laminated structure in which the base material sheet, the transparent sheet, and the color material receiving layer are laminated in this order, and the color material receiving layer contains a water-soluble resin, The transparent sheet contains a swellable resin.

[6−1]色材受容層
色材受容層については、上述した第1の発明と同様に、膨潤吸収型および空隙吸収型のいずれの色材受容層も使用できる。
[6-1] Color Material Receiving Layer As for the color material receiving layer, any of the swelling absorption type and void absorption type color material receiving layers can be used as in the first invention described above.

[6−1−1]無機微粒子
色材受容層を形成する無機微粒子としては、上述した[1−1−1]と同様のものが使用できる。
[6-1-1] Inorganic fine particles As the inorganic fine particles forming the colorant receiving layer, those similar to the above-mentioned [1-1-1] can be used.

[6−1−2]水溶性樹脂
色材受容層を形成する水溶性樹脂としては、上述した[1−1−2]と同様のものが使用できる。
[6-1-2] Water-soluble resin As the water-soluble resin for forming the colorant receiving layer, the same as [1-1-2] described above can be used.

[6−1−3]カチオン性樹脂
色材受容層を形成するカチオン性樹脂としては、上述した[1−1−3]と同様のものが使用できる。
[6-1-3] Cationic resin As the cationic resin for forming the colorant receiving layer, the same ones as described in [1-1-3] can be used.

[6−1−4]その他の添加物
色材受容層を形成するその他添加物としては、上述した[1−1−4]と同様のものが使用できる。
[6-1-4] Other Additives As other additives for forming the colorant receiving layer, the same ones as described in [1-1-4] can be used.

[6−1−5]厚さ
色材受容層の厚さは、上述した[1−1−5]と同様に設定できる。
[6-1-5] Thickness The thickness of the color material receiving layer can be set in the same manner as [1-1-5] described above.

[6−2]透明シート
転写材1は、図68のように透明シート52を備えている。透明シート52は、膨潤性樹脂660を含有しており、色材受容層53から透明シート52の表面まで膨潤性樹脂が均一に分散して、それらの間を連通する構造を持っている。膨潤性樹脂は分子内に多数の親水基を有しており、図59のように、その多数の親水基が水分子663を捕らえることによって水を吸収する性質を持っている。そのため透明シートは、それが無孔質であっても膨潤性樹脂が存在することによって、色材受容層の過剰な水分を吸収して表面から蒸発させることができる。透明シートは、その表面から蒸発した分だけ、新たに色材受容層から水分を吸収して蒸発させる。すなわち、透明シートに膨潤性樹脂を含有させることによって、透明シートに、記録物の系内の水分を系外に排出するポンプとしての機能を持たせることができる。このように、透明シートに膨潤性樹脂を含有させることにより、その膨潤性樹脂は、細孔と同様に記録物内の水分を外部に放出可能な通路を形成する。したがって、記録物の耐水性試験をして、色材受容層に多量の水分を吸水させた後に乾燥させた場合に、吸収された水分を記録物の端部のみならず、透明シートの全表面からも蒸発放散させて、応力集中に起因するひび割れの発生を抑制することができる。
[6-2] Transparent Sheet The transfer material 1 includes a transparent sheet 52 as shown in FIG. The transparent sheet 52 contains a swellable resin 660 and has a structure in which the swellable resin is uniformly dispersed from the colorant receiving layer 53 to the surface of the transparent sheet 52 and communicates therebetween. The swellable resin has a number of hydrophilic groups in the molecule, and has a property of absorbing water by capturing the water molecules 663 as shown in FIG. Therefore, even if the transparent sheet is nonporous, due to the presence of the swellable resin, the transparent sheet can absorb the excess moisture of the colorant receiving layer and evaporate from the surface. The transparent sheet newly absorbs moisture from the colorant receiving layer and evaporates it by the amount evaporated from the surface. That is, by adding a swellable resin to the transparent sheet, the transparent sheet can have a function as a pump for discharging moisture in the system of the recorded matter out of the system. As described above, when the swellable resin is contained in the transparent sheet, the swellable resin forms a passage through which moisture in the recorded matter can be released to the outside in the same manner as the pores. Therefore, when the recorded material is subjected to a water resistance test and a colorant receiving layer absorbs a large amount of water and then dried, the absorbed water is not only absorbed at the edges of the recorded material but also on the entire surface of the transparent sheet. It is also possible to suppress the occurrence of cracks caused by stress concentration by evaporating and evaporating from the substrate.

透明シートが系内の水分を系外に放出するためには、透明シートの表面から色材受容層までの間に存在する全ての層内に、膨潤性樹脂を含有させることが好ましい。例えば、透明シートの表面の平滑性の向上、あるいは色材受容層との接着性の向上などの目的のために、透明シートにおける基材シート側もしくは色材受容層側に層を追加して、複数の層からなる透明シートを用いることもできる。この場合、透明シートが水分を系外に放出するためには、図61(b)のように、複数の層661,662からなる透明シート52の全ての層に膨潤性樹脂を含有させることが必要となる。仮に、透明シートと色材受容層との間に水の排出機構を持たない場合には、図61(a)のように、系外への水の排出が著しく阻害される。この結果、透明シートの表面からの水分の蒸発量が減少し、透明シートに応力が集中してひび割れが発生しやすくなる。   In order for the transparent sheet to release moisture in the system to the outside of the system, it is preferable to include a swellable resin in all layers existing between the surface of the transparent sheet and the colorant receiving layer. For example, for the purpose of improving the smoothness of the surface of the transparent sheet or improving the adhesion with the colorant receiving layer, a layer is added to the base material sheet side or the colorant receiving layer side in the transparent sheet, A transparent sheet comprising a plurality of layers can also be used. In this case, in order for the transparent sheet to release moisture to the outside of the system, as shown in FIG. Necessary. If there is no water discharge mechanism between the transparent sheet and the colorant receiving layer, the discharge of water to the outside of the system is remarkably inhibited as shown in FIG. As a result, the amount of water evaporated from the surface of the transparent sheet is reduced, stress is concentrated on the transparent sheet, and cracks are likely to occur.

透明コートと色材受容層との間に、それらの接着性などを高めるためのアンカー層、あるいはセキュリティー性および意匠性を高めるためのホログラム層などを設けることもできる。この場合には、図62(a),(b)のように、透明シートの表面から色材受容層までに存在する透明シートの全ての層161,162,58,59に、水溶性樹脂あるいは吸水性樹脂を含有させることが好ましい。   Between the transparent coat and the colorant-receiving layer, an anchor layer for enhancing their adhesion or a hologram layer for enhancing security and design can be provided. In this case, as shown in FIGS. 62A and 62B, all the layers 161, 162, 58, and 59 of the transparent sheet existing from the surface of the transparent sheet to the colorant receiving layer have a water-soluble resin or It is preferable to contain a water absorbent resin.

[6−2−1]厚さ
透明シートの厚さは、特に制限されない。透明シートの水の排水効果に加えて、色材受容層の厚みに対する透明シートの厚みを制御することにより、耐水性をより向上させることができる。すなわち、透明シートの厚みが色材受容層の厚みに対して十分に大きければ、透明シートは十分な強度を持って収縮の応力を吸収することができるため、透明シートのひび割れは発生しにくい。一方、透明シートの厚みが色材受容層の厚みに対して小さくなると、透明シートの強度が相対的に弱くなり、色材受容層の収縮が相対的に大きくなるため、透明シートのひび割れは発生しやすくなり、透明シートの透湿性および水透過性を大きくする必要がある。水透過性および透湿性の度合いは、後述するように、水溶性樹脂の種類、ポリビニルアルコールにおいてはけん化度と重合度によって、制御できる。透明シートの厚み(A)と前記色材受容層の厚み(B)の比率(A/B)は、0.07≦(A/B)≦3.00.0の範囲であることが好ましい。
[6-2-1] Thickness The thickness of the transparent sheet is not particularly limited. In addition to the water draining effect of the transparent sheet, the water resistance can be further improved by controlling the thickness of the transparent sheet relative to the thickness of the colorant receiving layer. That is, if the thickness of the transparent sheet is sufficiently larger than the thickness of the colorant receiving layer, the transparent sheet can absorb the shrinkage stress with sufficient strength, and thus the transparent sheet is hardly cracked. On the other hand, when the thickness of the transparent sheet becomes smaller than the thickness of the color material receiving layer, the strength of the transparent sheet becomes relatively weak and the shrinkage of the color material receiving layer becomes relatively large, so the crack of the transparent sheet occurs. It is necessary to increase the moisture permeability and water permeability of the transparent sheet. As will be described later, the degree of water permeability and moisture permeability can be controlled by the type of water-soluble resin, and in the case of polyvinyl alcohol, the degree of saponification and the degree of polymerization. The ratio (A / B) of the thickness (A) of the transparent sheet and the thickness (B) of the colorant receiving layer is preferably in the range of 0.07 ≦ (A / B) ≦ 3.00.0.

比率(A/B)が大きくて、透明シートの厚みが色材受容層の厚みに対して十分大きければ、透明シートは、十分な強度を持って収縮の応力をある程度吸収するため、透明シートにひび割れは起こりにくい。記録物の利用目的によっては、画像の長期保存性や耐候性、あるいはセキュリティー性の観点から、保護層である透明シートの厚みを数十μm以上にする必要が生じる場合もある。この場合でも、画像支持体と色材受容層との間の接着力、および色材受容層と透明シートとの間の接着力に応じて、水溶性樹脂を含む色材受容層の吸水膨張および乾燥収縮に対応するように、透明シートの細孔構造を設定することにより応力を緩和することができる。すなわち、透明シートが厚い場合には、透明シート中の膨潤性樹脂の含有量を減らすことができる。一方、比率(A/B)が小さければ、透明シートの厚みが色材受容層の厚みに対して小さくなり、透明シートの強度は相対的に弱くなり、色材受容層の収縮は相対的に大きくなるため、透明シートのひび割れは起こりやすくなる。この場合には、透明シートの水透過性および透湿性を大きくしなければならない。   If the ratio (A / B) is large and the thickness of the transparent sheet is sufficiently large relative to the thickness of the colorant receiving layer, the transparent sheet absorbs the shrinkage stress to some extent with sufficient strength. Cracks are unlikely to occur. Depending on the purpose of use of the recorded matter, it may be necessary to make the thickness of the transparent sheet, which is a protective layer, several tens of μm or more from the viewpoint of long-term storage stability, weather resistance, and security. Even in this case, depending on the adhesive force between the image support and the color material receiving layer and the adhesive force between the color material receiving layer and the transparent sheet, the water absorption expansion of the color material receiving layer containing the water-soluble resin and The stress can be relieved by setting the pore structure of the transparent sheet so as to correspond to the drying shrinkage. That is, when the transparent sheet is thick, the content of the swellable resin in the transparent sheet can be reduced. On the other hand, if the ratio (A / B) is small, the thickness of the transparent sheet is smaller than the thickness of the color material receiving layer, the strength of the transparent sheet is relatively weak, and the shrinkage of the color material receiving layer is relatively small. Since it becomes large, the transparent sheet is likely to crack. In this case, the water permeability and moisture permeability of the transparent sheet must be increased.

透明シートの厚さは、実用的には、2〜40μmであることが好ましい。透明シートの厚さをさらに好ましくは5μm以上とすることにより、透明シートの耐水性や耐擦過性をさらに向上させることができる。一方、透明シートの厚みが小さくなり過ぎると、記録支持体への加熱圧着時における熱伝達に大きなエネルギーが必要となり、また透明シートの膨潤性樹脂を介した色材受容層からの水分の蒸発が進みにくくなる。したがって、透明シートの厚さは40μm以下とすることが望ましい。さらに好ましくは、20μ以下とすることにより、透明シートとしての基本機能である透明性、および保護機能に加えて、転写接着時におけるエネルギーおよび水分透過性など付随的な機能とのバランスも得られやすくなる。   Practically, the thickness of the transparent sheet is preferably 2 to 40 μm. By making the thickness of the transparent sheet more preferably 5 μm or more, the water resistance and scratch resistance of the transparent sheet can be further improved. On the other hand, if the thickness of the transparent sheet becomes too small, a large amount of energy is required for heat transfer at the time of thermocompression bonding to the recording support, and the evaporation of moisture from the colorant receiving layer via the swellable resin of the transparent sheet It becomes difficult to advance. Therefore, the thickness of the transparent sheet is desirably 40 μm or less. More preferably, by setting the thickness to 20 μm or less, in addition to the transparency and protection functions that are basic functions as a transparent sheet, it is easy to obtain a balance with incidental functions such as energy and moisture permeability during transfer adhesion. Become.

[6−2−2]透湿度
通常の環境下であれば、水分を吸収した記録物は30分程度で乾燥されるため、透明シートの透湿度が(5g/m2・h)以上であれば、耐水性をより向上させることができる。すなわち、透明シートの透湿度を上記の値以上に設定することにより、吸水後の色材受容層の収縮時の応力がより広く分散されて、ひび割れの発生をより抑制することができる。
[6-2-2] Moisture permeability Since the recorded matter that has absorbed moisture is dried in about 30 minutes under normal circumstances, the moisture permeability of the transparent sheet should be (5 g / m 2 · h) or more. In this case, the water resistance can be further improved. That is, by setting the moisture permeability of the transparent sheet to the above value or more, the stress at the time of contraction of the colorant receiving layer after water absorption is more widely dispersed, and the occurrence of cracks can be further suppressed.

[6−2−3]膨潤性樹脂
膨潤性樹脂としては、水により膨潤して、水に溶解するタイプの水溶性樹脂、および水に不溶なタイプの吸水性樹脂が含まれる。
[6-2-3] Swellable Resin Swellable resins include water-soluble resins that swell with water and dissolve in water, and water-absorbent resins that are insoluble in water.

水溶性樹脂とは、25℃において水と十分に混和する樹脂、あるいは水に対する溶解度が1(g/100g)以上の樹脂である。水溶性樹脂の種類は、特に限定されない。例えば、項目[1−1−2]に記載した色材受容層の水溶性樹脂と同じものを用いることができる。中でもポリビニルアルコールとして、完全けん化、部分ケン化、低けん化等、又はこれらの変性物(カチオン変性物、アニオン変性物、シラノール変性物等)は特に好ましく用いることができる。特に、ポリ酢酸ビニルを加水分解(けん化)することにより得られる、けん化ポリビニルアルコールが好ましい。後述する色材受容層にもけん化ポリビニルアルコールが好ましく用いられており、透明シートにもけん化ポリビニルアルコールを用いることにより、透明シートと色材受容層との接着性(転写性能)を向上させることもできる。その他に、分子内に親水性基を付与して水溶性樹脂としたアクリル系、ポリエステル系、ポリウレタン系、ポリアミド系、ナイロン系等の単独、あるいは共重合体なども使用することができる。膨潤性樹脂とは、膨潤性でかつ水不溶性の樹脂であって、無加圧下吸水倍率(CRC)が0.1g/g以上であるものとする。膨潤性樹脂は、その全量(100%)が重合体でることに限定されず、上記の性能を維持する範囲において、後述する添加剤を含んでもよい。すなわち本発明においては、膨潤性樹脂および添加剤を含む膨潤性樹脂の組成物も、膨潤性樹脂と総称する。膨潤性樹脂は特に限定されない。例えば、(メタ)アクリル酸塩系、(メタ)アクリルアミド系、ビニルアルコール系、無水マレイン酸(塩)系、ポリウレタン系等の単独、あるいは共重合体、(メタ)アクリルアミド−(メタ)アクリル酸塩共重合体、スルホン酸基含有(メタ)アクリル酸塩系単独あるいは共重合体、酢酸ビニル−無水マレイン酸共重合体、酢酸ビニル−アクリル酸エステル共重合体等、澱粉系あるいはセルロース系高分子、それらの部分架橋重合体やグラフト変性重合体等、を例示することができる。   The water-soluble resin is a resin that is sufficiently mixed with water at 25 ° C. or a resin having a solubility in water of 1 (g / 100 g) or more. The kind of water-soluble resin is not particularly limited. For example, the same water-soluble resin as the colorant-receiving layer described in item [1-1-2] can be used. Among these, as the polyvinyl alcohol, complete saponification, partial saponification, low saponification and the like, or modified products thereof (cation modified product, anion modified product, silanol modified product, etc.) can be used particularly preferably. In particular, saponified polyvinyl alcohol obtained by hydrolyzing (saponifying) polyvinyl acetate is preferred. Saponified polyvinyl alcohol is also preferably used in the color material receiving layer described later, and by using saponified polyvinyl alcohol also in the transparent sheet, the adhesiveness (transfer performance) between the transparent sheet and the color material receiving layer may be improved. it can. In addition, acrylic, polyester-based, polyurethane-based, polyamide-based, nylon-based, or the like, which is a water-soluble resin by adding a hydrophilic group in the molecule, or a copolymer can also be used. The swellable resin is a swellable and water-insoluble resin having a water absorption capacity (CRC) of 0.1 g / g or more under no pressure. The total amount (100%) of the swellable resin is not limited to being a polymer, and may contain additives to be described later as long as the above performance is maintained. That is, in the present invention, the composition of the swellable resin containing the swellable resin and the additive is also collectively referred to as the swellable resin. The swelling resin is not particularly limited. For example, (meth) acrylate-based, (meth) acrylamide-based, vinyl alcohol-based, maleic anhydride (salt) -based, polyurethane-based alone or copolymer, (meth) acrylamide- (meth) acrylate Copolymer, sulfonic acid group-containing (meth) acrylate-based homopolymer or copolymer, vinyl acetate-maleic anhydride copolymer, vinyl acetate-acrylate copolymer, starch-based or cellulose-based polymer, Examples thereof include partially crosslinked polymers and graft-modified polymers.

膨潤性樹脂は、1種を単独で用いてもよく、または2種以上を混合して用いることもできる。「2種以上」とは、けん化度および平均重合度等の特性が異なるものも含まれる。   Swelling resin may be used individually by 1 type, or can mix and use 2 or more types. “Two or more” includes those having different characteristics such as saponification degree and average degree of polymerization.

[6−2−4]膨潤性樹脂の量
膨潤性樹脂の量は、透明シート全体の0.05質量%以上、2.00質量%以下とすることが好ましい。より好ましくは0.09質量%以上、1.00質量%以下であって、さらにより好ましくは0.15質量%以上、0.60質量%以下である。膨潤性樹脂の量を0.05質量%以上、好ましくは0.09質量%以上、さらに好ましくは0.15質量%以上とすることにより、膨潤性樹脂が透明シート内に均一に分散された状態、かつ十分な量で透明シートの表面と色材受容層とが連通された状態となる。この結果、透明シートの表面からより多くの水分を蒸発させ、収縮の応力を広く分散させて、透明シートのひび割れの発生を抑制することができる。また、膨潤性樹脂の量を2.00質量%以下、好ましくは1.00質量%以下、さらに好ましくは0.6質量%以下とすることにより、溶解や過剰な膨潤によって透明シートの機械的強度を低下させることなく、透明シートのひび割れの発生を抑制することができる。一方で膨潤性樹脂が2.00質量%より大きいと透明シートの機械的強度が低下し、収縮の応力によってひびが入りやすくなり、また擦過性が低下するおそれもある。また、透明シートが粒子状のエマルジョンを含有する場合、膨潤性樹脂が多いと、膨潤性樹脂がエマルションの分散に寄与して、エマルションの粒径が大きく変化し、透明シートの透明性が低下するおそれがある。さらには、透明シートの吸水性が高すぎて、液体状の汚れが付いたときに汚染されやすくなる場合がある。反対に膨潤性樹脂が0.05質量%より小さいと透明シートからの水分蒸発が不十分となって、透明シートのひび割れが発生しやすくなる場合がある。
[6-2-4] Amount of swellable resin The amount of the swellable resin is preferably 0.05% by mass or more and 2.00% by mass or less of the entire transparent sheet. More preferably, they are 0.09 mass% or more and 1.00 mass% or less, More preferably, they are 0.15 mass% or more and 0.60 mass% or less. A state in which the swellable resin is uniformly dispersed in the transparent sheet by setting the amount of the swellable resin to 0.05% by mass or more, preferably 0.09% by mass or more, and more preferably 0.15% by mass or more. In addition, the surface of the transparent sheet and the color material receiving layer are communicated with each other in a sufficient amount. As a result, more water can be evaporated from the surface of the transparent sheet, and the shrinkage stress can be widely dispersed, thereby suppressing the occurrence of cracks in the transparent sheet. In addition, the amount of the swellable resin is 2.00% by mass or less, preferably 1.00% by mass or less, more preferably 0.6% by mass or less, so that the mechanical strength of the transparent sheet can be improved by dissolution or excessive swelling. The generation of cracks in the transparent sheet can be suppressed without lowering the thickness. On the other hand, if the swellable resin is larger than 2.00% by mass, the mechanical strength of the transparent sheet is lowered, cracking is likely to occur due to shrinkage stress, and the scratching property may be lowered. Further, when the transparent sheet contains a particulate emulsion, if there is a large amount of the swellable resin, the swellable resin contributes to the dispersion of the emulsion, the emulsion particle size changes greatly, and the transparency of the transparent sheet decreases. There is a fear. Furthermore, the water absorption of the transparent sheet may be too high, and the liquid may be easily contaminated when it is stained with liquid. On the other hand, if the swellable resin is less than 0.05% by mass, moisture evaporation from the transparent sheet becomes insufficient, and cracking of the transparent sheet is likely to occur.

膨潤性樹脂は、膨潤性樹脂が吸水により膨潤する割合(以下吸水膨潤率という)が高すぎると、記録物を水に浸漬した場合に、透明シート内で膨潤した分のひずみによって透明シートにひびが入りやすくなるおそれがある。   If the swelling ratio of the swellable resin due to water absorption (hereinafter referred to as the water absorption swelling ratio) is too high, the recording sheet will be cracked in the transparent sheet due to the strain swelled in the transparent sheet when immersed in water. May be easy to enter.

本発明においては、膨潤性樹脂が吸水により膨潤する割合のバランスを考慮して、膨潤性樹脂として、けん化度と重合度を厳密に制御したポリビニルアルコール(PVA)を含有することが特に好ましい。PVAは、分子内に大量の水酸基を有しており、それらがPVA分子内、あるいは、PVA分子間で水素結合を生成している。重合度とけん化度が高い場合には、ポリビニルアルコール同士がより多くの水素結合により結合が強固であるため、吸水により膨潤する体積は低く抑えられる。
また、高重合度かつ高けん化度のポリビニルアルコールは、分子内の水素結合によって、水溶性樹脂の中では硬い樹脂となるため、透明シートの耐擦過性を向上させる上において効果的である。さらに、ポリビニルアルコールは色材受容層にも好ましく用いられており、透明シートにもポリビニルアルコールを含有することによって、色材受容層との接着性を向上させることもできる。
In the present invention, considering the balance of the ratio of swelling of the swellable resin by water absorption, it is particularly preferable to contain polyvinyl alcohol (PVA) whose saponification degree and polymerization degree are strictly controlled as the swellable resin. PVA has a large amount of hydroxyl groups in the molecule, and these generate hydrogen bonds within the PVA molecule or between PVA molecules. When the degree of polymerization and the degree of saponification are high, since the polyvinyl alcohols are strongly bonded by more hydrogen bonds, the volume swollen by water absorption can be kept low.
In addition, polyvinyl alcohol having a high polymerization degree and a high saponification degree is effective in improving the scratch resistance of the transparent sheet because it becomes a hard resin among water-soluble resins due to hydrogen bonding in the molecule. Furthermore, polyvinyl alcohol is also preferably used in the color material receiving layer, and the adhesiveness with the color material receiving layer can also be improved by including polyvinyl alcohol in the transparent sheet.

ここで、透明シートの膨潤性樹脂が大量に水を吸収するものであった場合には、液体汚れによる保護性能がやや低下するおそれがある。すなわち、図63のように、透明シート52の表面に汚染水552などの液体状の汚れが付着した場合には、透明シート52の膨潤性樹脂が汚染水552を吸収して、汚染水552が色材受容層53に接触して吸収されるおそれがある。汚染水552が着色されている場合には、反転画像72による記録情報が背景側から液体水552によって着色され、その記録情報の一部が消えてしまうおそれがある。   Here, when the swellable resin of the transparent sheet absorbs a large amount of water, there is a possibility that the protection performance due to the liquid stain is slightly lowered. That is, as shown in FIG. 63, when liquid dirt such as contaminated water 552 adheres to the surface of the transparent sheet 52, the swellable resin of the transparent sheet 52 absorbs the contaminated water 552, and the contaminated water 552 There is a risk of being absorbed by contact with the colorant receiving layer 53. When the contaminated water 552 is colored, the recorded information by the reverse image 72 is colored by the liquid water 552 from the background side, and a part of the recorded information may disappear.

しかしながら、好ましい範囲の高けん化度および高重合度のポリビニルアルコールを含有することにより、保護性能の低下を抑えることができる。高けん化度かつ高重合度のポリビニルアルコールの場合、ポリビニルアルコール同士の水素結合の量が多く、水を水和するためには非常に長い時間を要する。したがって、図64のように透明シート52の表面に汚染水552が付着した場合には、その汚染水の吸収速度も抑えられるため、透明シート52および色材受容層53内に汚染が広がりにくい。   However, by containing polyvinyl alcohol having a high saponification degree and a high polymerization degree in a preferable range, it is possible to suppress a decrease in protective performance. In the case of polyvinyl alcohol having a high degree of saponification and a high degree of polymerization, the amount of hydrogen bonds between the polyvinyl alcohols is large, and it takes a very long time to hydrate water. Therefore, when the contaminated water 552 adheres to the surface of the transparent sheet 52 as shown in FIG. 64, the absorption rate of the contaminated water is also suppressed, so that the contamination hardly spreads in the transparent sheet 52 and the colorant receiving layer 53.

[6−2−5]ポリビニルアルコールけん化度と重合度
透明シートに用いるポリビニルアルコールは、けん化度75〜100mol%のポリビニルアルコールを含有する組成物からなることが好ましい。
[6-2-5] Polyvinyl alcohol saponification degree and polymerization degree The polyvinyl alcohol used for the transparent sheet is preferably composed of a composition containing polyvinyl alcohol having a saponification degree of 75 to 100 mol%.

けん化度を好ましくは86mol%以上、より好ましくは98mol%以上とすることにより、ポリビニルアルコールが吸水により膨潤する量を最適にすることができ、透明シート表面から水分を蒸発させて、ひび割れの発生をより抑制することができる。さらに、水分の吸収速度を抑えて、液体汚れからの記録情報の汚染を防止することもできる。86mol%より小さいと、記録物を水に浸漬した時にポリビニルアルコールの吸水により膨潤する量が大きくなるため、ひび割れが発生しやすくなる。また、水分の吸収速度が速くなり、液体汚れによる汚染が起こりやすくなる。さらに、ポリビニルアルコールの強度が低下し、透明シートの擦過性が低下するおそれがある。   By setting the degree of saponification to preferably 86 mol% or more, more preferably 98 mol% or more, the amount of polyvinyl alcohol that swells due to water absorption can be optimized, and moisture can be evaporated from the surface of the transparent sheet to generate cracks. It can be suppressed more. Furthermore, the moisture absorption rate can be suppressed to prevent contamination of recorded information from liquid stains. If it is less than 86 mol%, the amount of swelling due to the water absorption of polyvinyl alcohol when the recorded material is immersed in water becomes large, so that cracking tends to occur. In addition, the moisture absorption rate is increased, and contamination with liquid stains is likely to occur. Further, the strength of the polyvinyl alcohol is lowered, and the scratchability of the transparent sheet may be lowered.

けん化度の範囲を満たす、けん化ポリビニルアルコールとしては、完全けん化ポリビニルアルコール(けん化度98〜100mol%)、部分けん化ポリビニルアルコール(けん化度87〜89mol%)、低けん化ポリビニルアルコール(けん化度78〜82mol%)等を挙げることができる。中でも、完全けん化ポリビニルアルコールが好ましい。   As saponified polyvinyl alcohol satisfying the range of saponification degree, completely saponified polyvinyl alcohol (saponification degree 98-100 mol%), partially saponified polyvinyl alcohol (saponification degree 87-89 mol%), low saponified polyvinyl alcohol (saponification degree 78-82 mol%). And the like. Of these, completely saponified polyvinyl alcohol is preferred.

透明シートは、平均重合度が1,500〜5,000のポリビニルアルコールを含有する組成物からなることが好ましい。   The transparent sheet is preferably made of a composition containing polyvinyl alcohol having an average degree of polymerization of 1,500 to 5,000.

平均重合度を好ましくは1,500以上、さらに好ましくは2,000以上とすることにより、ポリビニルアルコールが吸水により膨潤する量を最適にすることができ、透明シートの表面から水分を蒸発させて、ひび割れの発生をより抑制することができる。さらに、水分の吸収速度を抑えて、液体汚れからの記録情報の汚染を防止することもできる。一方、平均重合度を好ましくは5,000以下、さらに好ましくは4,500以下とすることにより、透明シートを過度に硬くすることなく、透明シートに応力が掛ったときにもひび割れを起こりにくくすることができる。平均重合度の値は、JIS−K−6726に記載の方法に準拠して算出された値である。平均重合度が1500より小さいと、記録物を水に浸漬した時にポリビニルアルコールの吸水により膨潤する量が大きくなるため、ひび割れが発生しやすくなる。また、水分の吸収速度が速くなり、液体汚れによる汚染が起こりやすくなる。さらにはポリビニルアルコールの強度が低下し、透明シートの擦過性が低下するおそれがある。平均重合度が5000より大きいと、ポリビニルアルコール分子内の水素結合量が多くなるため、吸水により膨潤しづらくなり、水分を排出するためのポンプのとしての作用が低下するため、透明シートに応力がかかったときにひび割れが起こりやすくなる恐れがある。   By making the average degree of polymerization preferably 1,500 or more, more preferably 2,000 or more, it is possible to optimize the amount of polyvinyl alcohol swelled by water absorption, evaporate moisture from the surface of the transparent sheet, The occurrence of cracks can be further suppressed. Furthermore, the moisture absorption rate can be suppressed to prevent contamination of recorded information from liquid stains. On the other hand, by making the average degree of polymerization preferably 5,000 or less, more preferably 4,500 or less, the transparent sheet is not excessively hardened, and cracking is less likely to occur when the transparent sheet is stressed. be able to. The average degree of polymerization is a value calculated according to the method described in JIS-K-6726. If the average degree of polymerization is less than 1500, the amount of swelling due to water absorption of polyvinyl alcohol when the recorded material is immersed in water becomes large, so that cracking is likely to occur. In addition, the moisture absorption rate is increased, and contamination with liquid stains is likely to occur. Further, the strength of the polyvinyl alcohol is lowered, and the scratchability of the transparent sheet may be lowered. When the average degree of polymerization is greater than 5000, the amount of hydrogen bonds in the polyvinyl alcohol molecule increases, so that it becomes difficult to swell due to water absorption, and the action as a pump for discharging water is reduced, so that stress is applied to the transparent sheet. There is a risk of cracking when applied.

[6−2−6]エマルジョン
透明シートを構成するエマルションとしては、上述した[1−2−4]と同様のものが使用できる。
[6-2-6] Emulsion As the emulsion constituting the transparent sheet, the same as [1-2-4] described above can be used.

[6−2−7]厚さ
透明シートの厚さは特に制限されず、上述した[1−2−2]と同様のものが使用できる。ただし、この第2の発明においては、透明シートの厚み(A)と色材受容層の厚み(B)との比率(A/B)が下式(1)の範囲であることが好ましい。
0.07≦(A/B)≦3.00 (1)
A/Bが0.07以上であれば、透明シートの厚みが色材受容層の厚みに対して十分に大きく十分な強度を持つため、水透過性および透湿性は少なくてもひび割れは起こりにくい。また、A/Bが3.00以下であれば、透明シートの厚みが色材受容層の厚みに対して小さくなり、加熱圧着させる際に熱伝導を良好にできるため、透明シートと色材受容層との接着性(転写性能)を向上させることができる。一方、A/Bが0.07より小さい場合、透明シートの厚みが色材受容層の厚みに対して小さく、色材受容層の収縮に耐えうる十分な強度を持たないため、水透過性および透湿性は少ないときにひび割れは起こりやすい。また、A/Bが3より大きい場合、透明シートの厚みが色材受容層の厚みに対して大きくなり、加熱圧着させる際に熱伝導が低下し、透明シートと色材受容層との転写性能が低下する。
[6-2-7] Thickness The thickness of the transparent sheet is not particularly limited, and those similar to [1-2-2] described above can be used. However, in the second invention, the ratio (A / B) between the thickness (A) of the transparent sheet and the thickness (B) of the colorant receiving layer is preferably in the range of the following formula (1).
0.07 ≦ (A / B) ≦ 3.00 (1)
If A / B is 0.07 or more, the thickness of the transparent sheet is sufficiently large with respect to the thickness of the colorant receiving layer and has sufficient strength, so that even if water permeability and moisture permeability are small, cracks are unlikely to occur. . Moreover, if A / B is 3.00 or less, the thickness of the transparent sheet is smaller than the thickness of the color material receiving layer, and heat conduction can be improved when thermocompression bonding is performed. Adhesiveness (transfer performance) with the layer can be improved. On the other hand, when A / B is smaller than 0.07, the thickness of the transparent sheet is small relative to the thickness of the color material receiving layer and does not have sufficient strength to withstand the shrinkage of the color material receiving layer. Cracks tend to occur when moisture permeability is low. Further, when A / B is larger than 3, the thickness of the transparent sheet becomes larger than the thickness of the color material receiving layer, and the heat conduction is lowered when heat-pressing, and the transfer performance between the transparent sheet and the color material receiving layer. Decreases.

前述したように、比率(A/B)が大きくて、透明シートの厚みが色材受容層の厚みに対して十分大きければ、透明シートは、十分な強度を持って収縮の応力をある程度吸収するため、透明シートにひび割れは起こりにくい。   As described above, if the ratio (A / B) is large and the thickness of the transparent sheet is sufficiently large with respect to the thickness of the colorant receiving layer, the transparent sheet has sufficient strength and absorbs the shrinkage stress to some extent. Therefore, cracks are unlikely to occur in the transparent sheet.

[6−3]基材シート
基材シートについては[1−3]で前述したものと同様のものが使用できる
[6-3] Base sheet The same base sheet as described in [1-3] can be used.

[6−4]離型シート
離型シートとしては、前述した[1−4]と同様のものが使用できる。
[6-4] Release Sheet As the release sheet, the same as [1-4] described above can be used.

[6−4]アンカー層
アンカー層としては、前述した[1−5]と同様のものが使用できる。但し、第2の発明においては、透明シートが水分を系外に放出するために、図61(b)のように、アンカー層59が膨潤性樹脂を含有することが必要である。
[6-4] Anchor layer As the anchor layer, those similar to the above-mentioned [1-5] can be used. However, in the second invention, since the transparent sheet releases moisture out of the system, the anchor layer 59 needs to contain a swellable resin as shown in FIG.

[6−6]ホログラム層
ホログラム層としては、前述した[1−6]と同様のものが使用できる。但し、第2の発明においては、透明シートが水分を系外に放出するために、図61(b)のように、ホログラム層58が膨潤性樹脂を含有することが必要である。
[6-6] Hologram Layer As the hologram layer, the same as [1-6] described above can be used. However, in the second invention, since the transparent sheet releases moisture out of the system, the hologram layer 58 needs to contain a swellable resin as shown in FIG.

[6−7]積層構造
転写材1は、図68のように、基材シート50、透明シート52及び色材受容層53が順次積層された積層構造を有している。「基材シート、透明シート及び色材受容層が順次積層」とは、基材シート、透明シート、色材受容層の間に他の層が介在するか否かに拘わらず、基材シート、透明シート、色材受容層がその順序に従って積層されていることを意味する。すなわち、図62(a),(b)の転写材1のように、透明シート52と色材受容層53との間に、アンカー層59やホログラム層58が存在する構造も、「基材シート、透明シート及び色材受容層が順次積層」された積層構造に含まれる。
[6-7] Laminated Structure The transfer material 1 has a laminated structure in which a base sheet 50, a transparent sheet 52, and a color material receiving layer 53 are sequentially laminated as shown in FIG. “Substrate sheet, transparent sheet and color material receiving layer are sequentially laminated” means that the base sheet, transparent sheet, color material receiving layer, regardless of whether or not other layers are interposed, It means that the transparent sheet and the color material receiving layer are laminated according to the order. That is, the structure in which the anchor layer 59 and the hologram layer 58 exist between the transparent sheet 52 and the color material receiving layer 53 as in the transfer material 1 in FIGS. , A transparent sheet and a colorant-receiving layer are included in the laminated structure.

転写材1は、図68のように、基材シート50、透明シート52、色材受容層53が相互に当接された積層構造を有することが好ましい。すなわち、基材シート50と透明シート52との間、および透明シート52と色材受容層53との間に、他の層(シートも含む)が介在していない構造が好ましい。記録物の対象物となるクレジットカード等は厚さが厳格に制限されるため、積層される層やシートの数を減らして、記録物を薄厚化することが望ましいからである。   As shown in FIG. 68, the transfer material 1 preferably has a laminated structure in which a base sheet 50, a transparent sheet 52, and a color material receiving layer 53 are in contact with each other. That is, a structure in which no other layer (including a sheet) is interposed between the base sheet 50 and the transparent sheet 52 and between the transparent sheet 52 and the color material receiving layer 53 is preferable. This is because the thickness of a credit card or the like, which is an object of the recorded material, is strictly limited, so that it is desirable to reduce the number of layers and sheets to be stacked to reduce the thickness of the recorded material.

転写材が離型層51、アンカー層59、ホログラム層58をさらに備える場合には、色材受容層53、アンカー層59、ホログラム層58、透明シート52、離型層51及び基材シート50が順次積層された積層構造とすることが好ましい。   When the transfer material further includes a release layer 51, an anchor layer 59, and a hologram layer 58, the color material receiving layer 53, the anchor layer 59, the hologram layer 58, the transparent sheet 52, the release layer 51, and the base material sheet 50 are provided. A stacked structure in which layers are sequentially stacked is preferable.

[6−8]転写材の形状と厚さ
転写材の形状と厚さは、前述した[1−8]と同様に設定することができる
[6-8] Shape and thickness of transfer material The shape and thickness of the transfer material can be set in the same manner as [1-8] described above.

[6−9]製造方法
転写材は、前述した[1−9]と同様の方法で製造することができる。すなわち、基材シートに、透明シートを形成するための水溶性樹脂もしくは吸水性樹脂を含む塗工液を塗工して、基材シートに透明シートを積層する。その後、この積層体に、少なくとも水溶性樹脂を含有する塗工液を塗工することにより、転写材を製造することができる。尚、空隙吸収型の構成とする場合は、少なくとも無機微粒子、水溶性樹脂及びカチオン性樹脂を含有する塗工液を塗工することにより、転写材を製造することができる。
[6-9] Manufacturing Method The transfer material can be manufactured by the same method as [1-9] described above. That is, a coating liquid containing a water-soluble resin or a water-absorbing resin for forming a transparent sheet is applied to the base sheet, and the transparent sheet is laminated on the base sheet. Thereafter, a transfer material can be produced by coating the laminate with a coating solution containing at least a water-soluble resin. In addition, when setting it as a space | gap absorption type structure, a transfer material can be manufactured by applying the coating liquid containing an inorganic fine particle, water-soluble resin, and cationic resin at least.

[6−10]画像
画像としては、前述した[1−10]と同様ものが記録できる。
[6-10] Image As the image, the same image as [1-10] described above can be recorded.

[6−11]画像の記録
画像の記録は、前述した[1−11]と同様に記録することができる。
[6-11] Image Recording Image recording can be performed in the same manner as [1-11] described above.

[6−12]プライマー層
プライマー層としては、前述した[1−12]と同様のものが使用できる。
[6-12] Primer layer As the primer layer, those similar to [1-12] described above can be used.

[7]記録物
第2の発明における記録物は、図68のように、画像支持体、色材受容層、及び透明シートを備えた記録物である。基材シート、透明シートと、少なくとも膨潤性樹脂を含有する色材受容層と、が積層された転写材の色材受容層に、画像を記録してから、その転写材を画像支持体に積層して基材シートを剥離することによって、記録物が得られる。画像が記録された転写材(記録媒体)は、前述した[6]に記載の転写材により得られたものである。
[7] Recorded matter The recorded matter in the second invention is a recorded matter comprising an image support, a colorant receiving layer, and a transparent sheet as shown in FIG. An image is recorded on a color material receiving layer of a transfer material in which a base material sheet, a transparent sheet, and a color material receiving layer containing at least a swellable resin are laminated, and then the transfer material is laminated on an image support. Then, the recorded material is obtained by peeling the substrate sheet. The transfer material (recording medium) on which the image is recorded is obtained by the transfer material described in [6] above.

[8]第2の発明における記録物の製造方法
第2の発明における記録物は、図70のように、工程5,6,7を経て製造される。工程5では、前述した[6]に記載の転写材の色材受容層に画像を記録して記録媒体とし、工程6では、記録媒体の色材受容層に画像支持体に加熱圧着し、工程7では基材シートを剥離する。
[8] Method for Producing Recorded Material in Second Invention The recorded material in the second invention is produced through steps 5, 6, and 7 as shown in FIG. In step 5, an image is recorded on the color material receiving layer of the transfer material described in [6] above to obtain a recording medium. In step 6, the color material receiving layer of the recording medium is heated and pressure-bonded to an image support, In 7, the base sheet is peeled off.

[8−1]画像支持体
画像支持体としては、前述した[3−1]と同様のものが使用できる。
[8-1] Image support As the image support, the same one as described in [3-1] can be used.

[8−2]積層構造
記録物は、図6(b)の記録物73と同様に、画像支持体55、色材受容層53及び透明シート52が順次積層された積層構造を有する。
[8-2] Laminated Structure The recorded matter has a laminated structure in which the image support 55, the color material receiving layer 53, and the transparent sheet 52 are sequentially laminated in the same manner as the recorded matter 73 in FIG.

[8−3]転写材と画像支持体との加熱圧着
転写材と画像支持体との加熱圧着は、図9の製造装置25を用いて、[3−3]と同様に行うことができる
[8-3] Thermocompression bonding between the transfer material and the image support The thermocompression bonding between the transfer material and the image support can be performed in the same manner as [3-3] using the manufacturing apparatus 25 of FIG.

[8−4]基材シート及び離型層の剥離
記録物は、図6(b)の記録物73と同様に、基材シート50を剥離することにより、画像支持体55、色材受容層53及び透明シート52が順次積層された構造を有する。基材シート50は、前述した[3−4]と同様に剥離することができる。
[8-4] Peeling of base material sheet and release layer The recorded material is peeled off the base material sheet 50 in the same manner as the recorded material 73 of FIG. 53 and a transparent sheet 52 are sequentially laminated. The base material sheet 50 can be peeled in the same manner as [3-4] described above.

[8−5]両面同時剥離
両面同時剥離は、前述した[3−5]と同様に実施することができる。
[8-5] Double-sided simultaneous peeling Double-sided simultaneous peeling can be carried out in the same manner as [3-5] described above.

[9]第2の発明における記録装置
第2の発明における記録装置は、図65のように、前述した[6]に記載の転写材1を搬送経路に送り出す供給部4と、その転写1材の色材受容層に色材を付与して画像を記録する記録部6と、を備える。記録装置としては、前述した[4−1]と同様のものが使用できる。
[9] Recording apparatus in the second invention As shown in FIG. 65, the recording apparatus in the second invention is a supply unit 4 for feeding the transfer material 1 described in [6] above to the transport path, and the transfer material 1 And a recording unit 6 for recording an image by applying a color material to the color material receiving layer. As the recording apparatus, the same recording apparatus as described in [4-1] can be used.

[10]第2の発明における記録物の製造装置
前述した[7]の記録物の製造装置は、前述した[9]に記載の記録装置と、画像支持体を搬送経路に送り出す供給部と、画像支持体に記録媒体を付着させる付着部と、記録媒体から基材シートを剥離する剥離部と、を備える。
[10] Recorded matter manufacturing apparatus according to the second aspect [7] The recorded matter manufacturing apparatus of [7] described above, the recording device according to [9] described above, a supply unit for feeding the image support to the conveyance path, An attachment portion for attaching the recording medium to the image support and a peeling portion for peeling the base sheet from the recording medium are provided.

[10−1]第10の製造装置
第10の製造装置は、前述した図9または図13の第1の製造装置25と同様に構成することができる。水分を系外に放出できる膨潤性樹脂を含有した転写材を用いる点においてのみ、第1の製造装置と相違する。
[10-1] Tenth Manufacturing Apparatus The tenth manufacturing apparatus can be configured in the same manner as the first manufacturing apparatus 25 in FIG. 9 or FIG. 13 described above. It differs from the first manufacturing apparatus only in that a transfer material containing a swellable resin capable of releasing moisture out of the system is used.

[10−2]第11の製造装置
第11の製造装置は、前述した第6の製造装置と同様に、プリンタ部と転写部が分離独立して構成されている。水分を系外に放出できる膨潤性樹脂を含有したロール状の転写材を用いる点においてのみ、第6の製造装置と相違する。
[10-2] Eleventh Manufacturing Apparatus In the eleventh manufacturing apparatus, similarly to the above-described sixth manufacturing apparatus, the printer unit and the transfer unit are configured separately and independently. It differs from the sixth manufacturing apparatus only in that a roll-shaped transfer material containing a swellable resin capable of releasing moisture out of the system is used.

[10−3]第12の製造装置
第12の製造装置は、前述した第7の製造装置と同様に、プリンタ部と転写部が分離独立して構成されている。水分を系外に放出できる膨潤性樹脂を含有したロール状の転写材を用いる点においてのみ、第7の製造装置と相違する。
[10-3] Twelfth Manufacturing Apparatus In the twelfth manufacturing apparatus, similarly to the seventh manufacturing apparatus described above, the printer unit and the transfer unit are configured separately and independently. It differs from the seventh manufacturing apparatus only in that a roll-shaped transfer material containing a swellable resin capable of releasing moisture out of the system is used.

[10−4]第13の製造装置
第13の製造装置は、前述した第8の製造装置と同様に、プリンタ部と転写部が分離独立して構成されている。水分を系外に放出できる膨潤性樹脂を含有したロール状の転写材を用いる点においてのみ、第8の製造装置と相違する。
[10-4] Thirteenth Manufacturing Apparatus In the thirteenth manufacturing apparatus, similarly to the above-described eighth manufacturing apparatus, the printer unit and the transfer unit are configured separately and independently. It differs from the eighth manufacturing apparatus only in that a roll-shaped transfer material containing a swellable resin capable of releasing moisture out of the system is used.

[10−5]第14の製造装置
第14の製造装置は、前述した第9の製造装置と同様に、プリンタ部と転写部が分離独立して構成されている。水分を系外に放出できる膨潤性樹脂を含有したロール状の転写材を用いる点においてのみ、第9の製造装置と相違する。
[10-5] Fourteenth Manufacturing Apparatus In the fourteenth manufacturing apparatus, similarly to the ninth manufacturing apparatus described above, the printer unit and the transfer unit are configured separately and independently. It differs from the ninth manufacturing apparatus only in that a roll-shaped transfer material containing a swellable resin capable of releasing moisture out of the system is used.

以上の第10から第15の製造装置においては、転写材が基材上に少なくとも、膨潤性樹脂を含有する透明シートと色材受容層を有している場合に、転写材を画像支持体に付着させる工程にて、色材受容層のインク水分量の制御と付着時の温度制御とが行われる。これにより、転写材の透明シートと画像支持体との密着性を向上させて、耐候性、耐水性、耐薬品性、および耐ガス性等の各種耐久性に優れた記録物を提供することができる。   In the above tenth to fifteenth manufacturing apparatuses, when the transfer material has at least a transparent sheet containing a swellable resin and a color material receiving layer on the base material, the transfer material is used as an image support. In the adhering step, control of the ink moisture content of the color material receiving layer and temperature control during adhering are performed. Thereby, it is possible to improve the adhesion between the transparent sheet of the transfer material and the image support, and to provide a recorded material excellent in various durability such as weather resistance, water resistance, chemical resistance, and gas resistance. it can.

以下、本発明の具体的な実施例について説明する。ただし、本発明は、下記の実施例によっていかなる制限を受けるものではない。なお、以下の記載における「部」、「%」は特に断らない限り質量基準である。   Hereinafter, specific examples of the present invention will be described. However, the present invention is not limited in any way by the following examples. In the following description, “parts” and “%” are based on mass unless otherwise specified.

(実施例1)
[透明シート形成用塗工液の合成]
アクリルエマルジョン水溶液(BASF社製ジョンクリル352D、Tg56℃、固形分濃度45%)を9部と、ウレタンエマルジョン水溶液(第一工業製薬社製スーパーフレックス130、Tg101℃、固形分濃度35%)1部と、を加えて5分攪拌混合し、積層シート用塗工液を得た。
Example 1
[Synthesis of coating liquid for forming transparent sheet]
9 parts of an acrylic emulsion aqueous solution (BASF Co., Ltd. Jonkrill 352D, Tg 56 ° C., solid content concentration 45%) and urethane emulsion aqueous solution (Daiichi Kogyo Seiyaku Co., Ltd. Superflex 130, Tg 101 ° C., solid content concentration 35%) 1 part And stirring and mixing for 5 minutes to obtain a coating solution for laminated sheets.

[積層シート(転写材の構成素材)の製造]
透明シート形成用の塗工液をPET基材シートの表面(厚さ25μm)に塗工した後、乾燥することにより、細孔が形成されていない透明シートと、基材シートと、を含む転写材の構成素材としての積層シートを製造した。塗工にはダイコーターを用い、塗工速度は5m/分、乾燥後の塗工量は5g/m2とした。乾燥温度は90℃とした。透明シートの厚さ(B)は5μmであった。
[Manufacture of laminated sheets (component materials for transfer materials)]
A transfer containing a transparent sheet on which no pores are formed and a base sheet by applying a coating liquid for forming a transparent sheet on the surface (thickness 25 μm) of the PET base sheet and drying it. A laminated sheet as a constituent material of the material was manufactured. A die coater was used for coating, the coating speed was 5 m / min, and the coating amount after drying was 5 g / m 2 . The drying temperature was 90 ° C. The thickness (B) of the transparent sheet was 5 μm.

[細孔の形成]
積層シートに、図60中の(a)の細孔形成方法によって機械的な穿孔処理を行い、細孔が形成された透明シートを含む転写材を製造した。穿孔処理には、図46(a)のような針657を用いた。細孔の分布密度は、1平方mm当たり1つの孔が存在する密度とし、細孔径は0.02μmとした。細孔が形成された層(実施例1では保護シート(透明シート))については、表内の通路場所に○をつけている。表内に○が付いていない場合はその層には細孔は形成されていないことを示す。
[Formation of pores]
The laminated sheet was mechanically perforated by the pore formation method (a) in FIG. 60 to produce a transfer material including a transparent sheet having pores formed therein. A needle 657 as shown in FIG. 46A was used for the drilling process. The distribution density of the pores was such that one pore per square mm was present, and the pore diameter was 0.02 μm. For the layer in which the pores are formed (the protective sheet (transparent sheet) in Example 1), the passage locations in the table are circled. If the circle is not shown in the table, it indicates that no pores are formed in the layer.

[アルミナ水和物分散液の調製]
ベーマイト構造(擬ベーマイト構造)を有するアルミナ水和物A(商品名「Disperal HP14」、サソール製)20部を純水中に添加し、さらに酢酸0.4部を添加して解膠処理を行うことにより、アルミナ水和物分散液を得た。アルミナ水和物分散液におけるアルミナ水和物微粒子の平均粒子径は、140nmであった。次いで、分散液に対して、ホウ酸0.3部を添加して、ホウ酸添加アルミナ水和物分散液を得た。
[Preparation of Alumina Hydrate Dispersion]
20 parts of alumina hydrate A having a boehmite structure (pseudo boehmite structure) (trade name “Disperal HP14”, manufactured by Sasol) is added to pure water, and 0.4 part of acetic acid is further added to perform peptization. As a result, an alumina hydrate dispersion was obtained. The average particle diameter of the alumina hydrate fine particles in the alumina hydrate dispersion was 140 nm. Next, 0.3 parts of boric acid was added to the dispersion to obtain a boric acid-added alumina hydrate dispersion.

[ポリビニルアルコール水溶液の調製]
ポリビニルアルコール(商品名「PVA235」、クラレ製)をイオン交換水に溶解して、固形分含量が8%のポリビニルアルコール水溶液を調製した。ポリビニルアルコールは、平均重合度が3,500、けん化度が87〜89mol%、SP値は9.4であった。
[Preparation of aqueous polyvinyl alcohol solution]
Polyvinyl alcohol (trade name “PVA235”, manufactured by Kuraray Co., Ltd.) was dissolved in ion-exchanged water to prepare a polyvinyl alcohol aqueous solution having a solid content of 8%. Polyvinyl alcohol had an average degree of polymerization of 3,500, a degree of saponification of 87 to 89 mol%, and an SP value of 9.4.

[色材受容層形成用の塗工液の調製]
ホウ酸添加アルミナ水和物分散液100部に、ポリビニルアルコール水溶液27.8部を加え、さらにカチオン性樹脂としてポリアリルアミン3.0部を加えてスタティックミキサーにより混合し、色材受容層形成用の塗工液を得た。ポリアリルアミンとしては、融点が83.3℃、平均重合度が1,600のポリアリルアミン(商品名「PAA−01」、日東紡製)を用いた。
[Preparation of coating solution for forming colorant receiving layer]
Add 27.8 parts of polyvinyl alcohol aqueous solution to 100 parts of boric acid-added alumina hydrate dispersion, and then add 3.0 parts of polyallylamine as a cationic resin and mix with a static mixer to form a colorant receiving layer. A coating solution was obtained. As the polyallylamine, polyallylamine (trade name “PAA-01”, manufactured by Nittobo) having a melting point of 83.3 ° C. and an average degree of polymerization of 1,600 was used.

[転写材の製造]
細孔が形成された積層シートの透明シートの表面に、混合直後の色材受容層形成用の塗工液を塗工して、乾燥することにより、空隙吸収型の色材受容層を備えた転写材を製造した。塗工液の塗工にはダイコーターを用い、塗工速度は5m/分、乾燥後の塗工量は15g/m2とした。乾燥温度は60℃とした。転写材は、色材受容層を外側、基材シートを内側にしてロール状に巻くことにより、ロール状転写材とした。色材受容層の厚さAは10μmであった。色材受容層の厚みAと透明シートの厚みBの比率(A/B)は0.5であった。
[Manufacture of transfer material]
On the surface of the transparent sheet of the laminated sheet in which the pores were formed, a coating material for forming a color material receiving layer immediately after mixing was applied and dried to provide a void absorption type color material receiving layer A transfer material was produced. A die coater was used for coating the coating solution, the coating speed was 5 m / min, and the coating amount after drying was 15 g / m 2 . The drying temperature was 60 ° C. The transfer material was made into a roll-shaped transfer material by winding in a roll shape with the color material receiving layer on the outside and the base material sheet on the inside. The thickness A of the colorant receiving layer was 10 μm. The ratio (A / B) between the thickness A of the colorant receiving layer and the thickness B of the transparent sheet was 0.5.

[透湿度の測定]
転写材の透明シートの透湿度をJIS L1099B−2に規定される方法で測定した。透明シートの透湿度は10g/m2・hであった。
[Measurement of moisture permeability]
The moisture permeability of the transparent sheet of the transfer material was measured by the method defined in JIS L1099B-2. The moisture permeability of the transparent sheet was 10 g / m 2 · h.

このようにして得られた実施例1の転写材に、上述した第1の製造装置を用いて、顔料インクにより記録デューティー60%の60%ベタ画像を記録した。その後、その転写材を画像支持体に加熱圧着させた後、基材シートを剥離することにより、実施例1の記録物を得た。顔料インクの調製法については、後述する。製造装置の記録部としては、ラインヘッドを搭載したプリントモジュール(商品名「PM−200Z」、キヤノンファインテック製)を用い、画像支持体としては、塩化ビニル製のカード(商品名「C−4002」、エボリス製)を用いた。加熱圧着の条件は、温度160℃、圧力3.9Kg/cm、搬送速度50mm/secとした。基材シートを剥離する際の引き剥がし角度は90°とした。色材受容層のSP値と、画像支持体のSP値と、の差SP2は0.1であった。   A 60% solid image with a recording duty of 60% was recorded with the pigment ink on the transfer material of Example 1 thus obtained using the first manufacturing apparatus described above. Then, the recorded material of Example 1 was obtained by heat-pressing the transfer material on the image support and then peeling the substrate sheet. The method for preparing the pigment ink will be described later. As a recording unit of the manufacturing apparatus, a print module (trade name “PM-200Z”, manufactured by Canon Finetech) equipped with a line head is used, and a card made of vinyl chloride (trade name “C-4002” is used as an image support. “Evolis”). The thermocompression bonding conditions were a temperature of 160 ° C., a pressure of 3.9 Kg / cm, and a conveyance speed of 50 mm / sec. The peeling angle when peeling the base sheet was 90 °. The difference SP2 between the SP value of the color material receiving layer and the SP value of the image support was 0.1.

[顔料インクの調製]
<(メタ)アクリル酸エステル系共重合体の合成>
撹拌装置と、滴下装置と、温度センサと、上部に窒素導入装置を有する還流装置と、を取り付けた反応容器に、メチルエチルケトン1,000部を仕込み、そのメチルエチルケトンを撹拌しながら反応容器内を窒素置換した。反応容器内を窒素雰囲気に保ちながら80℃に昇温させた後、滴下装置よりメタクリル酸2−ヒドロキシエチル63部、メタクリル酸141部、スチレン417部、メタクリル酸ベンジル188部、メタクリル酸グリシジル25部、重合度調整剤(商品名「ブレンマーTGL」、日本油脂社製)33部、及びペルオキシ−2−エチルヘキサン酸−t−ブチル 67部を混合して得た混合液を4時間かけて滴下した。滴下終了後、さらに同温度で10時間反応を継続させて、酸価110mgKOH/g、ガラス転移点(Tg)89℃、重量平均分子量8,000の(メタ)アクリル酸エステル系共重合体(A−1)の溶液(樹脂分:45.4%)を得た。
[Preparation of pigment ink]
<Synthesis of (meth) acrylic ester copolymer>
1,000 parts of methyl ethyl ketone was charged into a reaction vessel equipped with a stirring device, a dropping device, a temperature sensor, and a reflux device having a nitrogen introducing device at the top, and the inside of the reaction vessel was purged with nitrogen while stirring the methyl ethyl ketone. did. The temperature inside the reaction vessel was raised to 80 ° C. while maintaining a nitrogen atmosphere, and then from a dropping device, 63 parts of 2-hydroxyethyl methacrylate, 141 parts of methacrylic acid, 417 parts of styrene, 188 parts of benzyl methacrylate, and 25 parts of glycidyl methacrylate. , 33 parts of a polymerization degree modifier (trade name “Blenmer TGL”, manufactured by NOF Corporation) and 67 parts of peroxy-2-ethylhexanoic acid-t-butyl were added dropwise over 4 hours. . After completion of the dropwise addition, the reaction was further continued at the same temperature for 10 hours, and a (meth) acrylic acid ester copolymer (A) having an acid value of 110 mgKOH / g, a glass transition point (Tg) of 89 ° C., and a weight average molecular weight of 8,000 (A -1) solution (resin content: 45.4%).

<水性顔料分散体の調製1>
冷却機能を備えた混合槽に、フタロシアニン系ブルー顔料1,000部、上記の合成により得られた(メタ)アクリル酸エステル系共重合体(A−1)の溶液、25%水酸化カリウム水溶液、及び水を仕込み、撹拌及び混合して混合液を得た。なお、(メタ)アクリル酸エステル系共重合体(A−1)は、フタロシアニン系ブルー顔料に対して、不揮発分で40%の比率となる量を用いた。また、25%水酸化カリウム水溶液としては、(メタ)アクリル酸エステル系共重合体(A−1)が100%中和される量を用いた。さらに、水は、得られる混合液の不揮発分を27%とする量を用いた。得られた混合液は、直径0.3mmのジルコニアビーズを充填した分散装置に通し、循環方式により4時間分散させた。分散液の温度は40℃以下に保持した。
<Preparation 1 of aqueous pigment dispersion>
In a mixing tank equipped with a cooling function, 1,000 parts of a phthalocyanine blue pigment, a solution of the (meth) acrylic ester copolymer (A-1) obtained by the above synthesis, a 25% aqueous potassium hydroxide solution, And water were charged, stirred and mixed to obtain a mixed solution. The (meth) acrylic acid ester copolymer (A-1) was used in an amount of 40% in terms of nonvolatile content with respect to the phthalocyanine blue pigment. Moreover, as 25% potassium hydroxide aqueous solution, the quantity by which (meth) acrylic acid ester type copolymer (A-1) is neutralized 100% was used. Furthermore, the water used the quantity which makes the non volatile matter of the obtained liquid mixture 27%. The obtained mixed solution was passed through a dispersing apparatus filled with zirconia beads having a diameter of 0.3 mm, and dispersed for 4 hours by a circulation method. The temperature of the dispersion was kept below 40 ° C.

混合槽から分散液を抜き取った後、水10,000部で混合槽と分散装置との流路を洗浄し、洗浄液と分散液とを混合して希釈分散液を得た。得られた希釈分散液を蒸留装置に入れ、メチルエチルケトンの全量と水の一部を留去して、濃縮分散液を得た。室温まで放冷した濃縮分散液を撹拌しながら2%塩酸を滴下して、pH4.5に調整した後、ヌッチェ式濾過装置にて固形分を濾過して水洗した。得られた固形分(ケーキ)を容器に入れ、水を加えた後、分散撹拌機を使用して再分散させ、25%水酸化カリウム水溶液によってpH9.5に調整した。その後、遠心分離器を使用し、6000Gで30分間かけて粗大粒子を除去した後、不揮発分を調整して水性シアン顔料分散体(顔料分:14% 酸価110)を得た。   After the dispersion liquid was extracted from the mixing tank, the flow path between the mixing tank and the dispersion apparatus was washed with 10,000 parts of water, and the cleaning liquid and the dispersion liquid were mixed to obtain a diluted dispersion liquid. The obtained diluted dispersion was put into a distillation apparatus, and the whole amount of methyl ethyl ketone and a part of water were distilled off to obtain a concentrated dispersion. 2% hydrochloric acid was added dropwise with stirring to the concentrated dispersion which had been allowed to cool to room temperature, and the pH was adjusted to 4.5. Then, the solid content was filtered and washed with a Nutsche filter. The obtained solid (cake) was put in a container, water was added, and then redispersed using a dispersion stirrer, and the pH was adjusted to 9.5 with a 25% aqueous potassium hydroxide solution. Thereafter, using a centrifugal separator, coarse particles were removed at 6000 G for 30 minutes, and then the non-volatile content was adjusted to obtain an aqueous cyan pigment dispersion (pigment content: 14% acid value 110).

フタロシアニン系ブルー顔料を、カーボンブラック系ブラック顔料、キナクリドン系マゼンタ顔料又はジアゾ系イエロー顔料に変更したことを除いては、水性シアン顔料分散体と同様にして、水性ブラック顔料分散体、水性マゼンタ顔料分散体、又は水性イエロー顔料分散体を得た。   Except for changing the phthalocyanine blue pigment to carbon black black pigment, quinacridone magenta pigment or diazo yellow pigment, the same as the aqueous cyan pigment dispersion, the aqueous black pigment dispersion, the aqueous magenta pigment dispersion Or an aqueous yellow pigment dispersion was obtained.

<インクの調製>
下表3に示す組成(合計:100部)となるように、水性顔料分散体及び表3に示す各成分を容器に投入し、プロペラ撹拌機を使用して30分以上撹拌した。その後、孔径0.2μmのフィルター(日本ポール社製)で濾過して、顔料インクを調製した。なお、表3中の「AE−100」は、アセチレングリコール10モルエチレンオキサイド付加物(商品名「アセチレノールE100」、川研ファインケミカル製)を示す。
<Preparation of ink>
The aqueous pigment dispersion and each component shown in Table 3 were put into a container so as to have the composition shown in Table 3 below (total: 100 parts), and stirred for 30 minutes or more using a propeller stirrer. Thereafter, the mixture was filtered with a filter having a pore size of 0.2 μm (manufactured by Nippon Pole Co., Ltd.) to prepare pigment ink. “AE-100” in Table 3 represents an acetylene glycol 10-mole ethylene oxide adduct (trade name “acetylenol E100”, manufactured by Kawaken Fine Chemicals).

(実施例2)
色材受容層形成用の塗工液を高松油脂製NS625XCに変更して、膨潤型の色材受容層を形成した以外は、実施例1と同様にして転写材および記録物を得た。実施例2における細孔径、透湿度、厚み比率A/Bは、後述する表4に記載した。
(Example 2)
A transfer material and a recorded material were obtained in the same manner as in Example 1 except that the coating material for forming the color material receiving layer was changed to NS625XC made of Takamatsu Oil and Fat and a swollen color material receiving layer was formed. The pore diameter, moisture permeability, and thickness ratio A / B in Example 2 are shown in Table 4 described later.

(実施例3)
透明シートの細孔径を0.02μmから0.002μmに変更した以外は、実施例1と同様にして転写材および記録物を得た。実施例3における透湿度、厚み比率A/Bは、後述する表4に記載した。
(Example 3)
A transfer material and recorded matter were obtained in the same manner as in Example 1 except that the pore diameter of the transparent sheet was changed from 0.02 μm to 0.002 μm. The moisture permeability and thickness ratio A / B in Example 3 are shown in Table 4 described later.

(実施例4)
透明シートの細孔径を0.02μmから0.7μmに変更した以外は、実施例1と同様にして転写材および記録物を得た。実施例4における透湿度、厚み比率A/Bは、後述する表4に記載した。
(Example 4)
A transfer material and a recorded matter were obtained in the same manner as in Example 1 except that the pore diameter of the transparent sheet was changed from 0.02 μm to 0.7 μm. The moisture permeability and thickness ratio A / B in Example 4 are shown in Table 4 described later.

(実施例5)
透明シートの細孔径を0.02μmから0.001μmに変更した以外は、実施例1と同様にして転写材および記録物を得た。実施例5における透湿度、厚み比率A/Bは、後述する表4に記載した。
(Example 5)
A transfer material and a recorded matter were obtained in the same manner as in Example 1 except that the pore diameter of the transparent sheet was changed from 0.02 μm to 0.001 μm. The moisture permeability and thickness ratio A / B in Example 5 are shown in Table 4 described later.

(実施例6)
透明シートの細孔径を0.02μmから1μmに変更した以外は、実施例1と同様にして転写材および記録物を得た。実施例6における透湿度、厚み比率A/Bは、後述する表4に記載した。
(Example 6)
A transfer material and a recorded matter were obtained in the same manner as in Example 1 except that the pore diameter of the transparent sheet was changed from 0.02 μm to 1 μm. The moisture permeability and thickness ratio A / B in Example 6 are shown in Table 4 described later.

(実施例7)
透明シートの細孔径を0.02μmから10μmに変更した以外は実施例1と同様にして、転写材さらには記録物を得た。実施例7における透湿度、厚み比率A/Bは、後述する表4に記載した。
(Example 7)
A transfer material and a recorded matter were obtained in the same manner as in Example 1 except that the pore diameter of the transparent sheet was changed from 0.02 μm to 10 μm. The moisture permeability and thickness ratio A / B in Example 7 are shown in Table 4 described later.

(実施例8)
透明シートの細孔径を0.02μmから100μmに変更した以外は、実施例1と同様にして転写材および記録物を得た。実施例8における透湿度、厚み比率A/Bは、後述する表4に記載した。
(Example 8)
A transfer material and a recorded material were obtained in the same manner as in Example 1 except that the pore diameter of the transparent sheet was changed from 0.02 μm to 100 μm. The moisture permeability and thickness ratio A / B in Example 8 are shown in Table 4 described later.

(実施例9)
透明シートの細孔分布密度を1平方mm当たり1孔から5平方mm当たり1孔に変更した以外は、実施例1と同様にして転写材および記録物を得た。実施例3における細孔径、透湿度、厚み比率A/Bは、後述する表4に記載した。
Example 9
A transfer material and recorded matter were obtained in the same manner as in Example 1 except that the pore distribution density of the transparent sheet was changed from 1 hole per 1 square mm to 1 hole per 5 square mm. The pore diameter, moisture permeability, and thickness ratio A / B in Example 3 are shown in Table 4 described later.

(実施例10)
透明シートの細孔分布密度を1平方mm当たり1孔から10平方mm当たり1孔に変更した以外は、実施例1と同様にして転写材および記録物を得た。透湿度は2g/m2・hであった。実施例3における細孔径、厚み比率A/Bは、後述する表4に記載した。
(Example 10)
A transfer material and recorded matter were obtained in the same manner as in Example 1 except that the pore distribution density of the transparent sheet was changed from 1 hole per square mm to 1 hole per 10 square mm. The moisture permeability was 2 g / m 2 · h. The pore diameter and thickness ratio A / B in Example 3 are shown in Table 4 described later.

(実施例11)
透明シートの厚みAを5μmから15μmに変更し、色材受容層の厚みを10μmから5μmに変更した以外は、実施例1と同様にして転写材および記録物を得た。色材受容層の厚みAと透明シートの厚みBの比率(A/B)は、3であった。
(Example 11)
A transfer material and a recorded material were obtained in the same manner as in Example 1 except that the thickness A of the transparent sheet was changed from 5 μm to 15 μm and the thickness of the colorant receiving layer was changed from 10 μm to 5 μm. The ratio (A / B) between the thickness A of the colorant receiving layer and the thickness B of the transparent sheet was 3.

(実施例12)
透明シートの厚みAを5μmから1μmに変更し、色材受容層の厚みBを10μmから15μmに変更した以外は、実施例1と同様にして転写材および記録物を得た。色材受容層の厚みAと透明シートの厚みBの比率(A/B)は、0.07であった。
Example 12
A transfer material and a recorded material were obtained in the same manner as in Example 1 except that the thickness A of the transparent sheet was changed from 5 μm to 1 μm and the thickness B of the colorant receiving layer was changed from 10 μm to 15 μm. The ratio (A / B) between the thickness A of the colorant receiving layer and the thickness B of the transparent sheet was 0.07.

(実施例13)
透明シートの厚みAを5μmから20μmに変更し、色材受容層の厚みを10μmから5μmに変更した以外は、実施例1と同様にして転写材および記録物を得た。色材受容層の厚みAと透明シートの厚みBの比率(A/B)は、4であった。
(Example 13)
A transfer material and a recorded material were obtained in the same manner as in Example 1 except that the thickness A of the transparent sheet was changed from 5 μm to 20 μm and the thickness of the colorant receiving layer was changed from 10 μm to 5 μm. The ratio (A / B) between the thickness A of the colorant receiving layer and the thickness B of the transparent sheet was 4.

(実施例14)
透明シートの厚みAを5μmから0.5μmに変更し、色材受容層の厚みを0.5μmに変更した以外は、実施例1と同様にして転写材および記録物を得た。色材受容層の厚みAと透明シートの厚みBの比率(A/B)は、0.03であった。
(Example 14)
A transfer material and a recorded material were obtained in the same manner as in Example 1 except that the thickness A of the transparent sheet was changed from 5 μm to 0.5 μm and the thickness of the colorant receiving layer was changed to 0.5 μm. The ratio (A / B) between the thickness A of the colorant receiving layer and the thickness B of the transparent sheet was 0.03.

(実施例15)
[積層シート(転写材の構成素材)の製造]
細孔構造を有するフィルムとして、ポリテトラフルオロエチレン(PTFE)を延伸加工したePTFEフィルムと、ポリウレタンポリマーと、を複合化して作成された厚さ5μmの防水透湿フィルムを、PET基材シート(厚さ25μm)にラミネートして、積層シートを製造した。積層シートの透明シートは、1平方センチメートルに14億個の微細な孔を含み、防水性と透湿性とが両立できる。耐水圧は45000mm以上、透湿性は、JIS L1099B−2法による測定で13500g/m2/24hrsである。
(Example 15)
[Manufacture of laminated sheets (component materials for transfer materials)]
As a film having a pore structure, a waterproof and moisture-permeable film having a thickness of 5 μm formed by combining an ePTFE film obtained by stretching polytetrafluoroethylene (PTFE) and a polyurethane polymer is used as a PET base sheet (thickness). 25 μm) to produce a laminated sheet. The transparent sheet of the laminated sheet includes 1.4 billion fine holes per square centimeter, and is compatible with waterproofness and moisture permeability. The water pressure resistance is 45000 mm or more, and the moisture permeability is 13500 g / m2 / 24 hrs as measured by the JIS L1099B-2 method.

[転写材の製造]
積層シートを変更した以外は、実施例1と同様にして転写材および記録物を得た。
[Manufacture of transfer material]
A transfer material and a recorded matter were obtained in the same manner as in Example 1 except that the laminated sheet was changed.

(実施例16)
[積層シート(転写材の構成素材)の製造]
細孔構造を有する透明フィルムとして、ポリフッ化ビニリデンをクレイズ加工して作成された厚さ5μmの防水透湿フィルムを、PET基材シート(厚さ25μm)にラミネートして、積層シートを製造した。積層シートの透明シートは、1平方センチメートルに4億個の微細な孔を含み、防水性と透湿性とが両立できる。透湿性は、JIS L1099B−2法による測定で3800g/m2/24hrsである。
(Example 16)
[Manufacture of laminated sheets (component materials for transfer materials)]
As a transparent film having a pore structure, a waterproof and moisture-permeable film having a thickness of 5 μm prepared by craze processing of polyvinylidene fluoride was laminated on a PET base sheet (thickness: 25 μm) to produce a laminated sheet. The transparent sheet of the laminated sheet includes 400 million fine holes in one square centimeter, and can achieve both waterproofness and moisture permeability. Moisture permeability is 3800g / m 2 / 24hrs as measured by JIS L1099B-2 method.

[転写材の製造]
積層シートを変更した以外は、実施例1と同様にして転写材および記録物を得た。
[Manufacture of transfer material]
A transfer material and a recorded matter were obtained in the same manner as in Example 1 except that the laminated sheet was changed.

(実施例17)
[透明シート形成用の塗工液の合成]
アクリルエマルジョン水溶液(BASF社製ジョンクリル352D、Tg56℃)を9部と、ウレタンエマルジョン水溶液(第一工業製薬社製スーパーフレックス130、Tg)を1部と、発泡剤1部と、を加えて5分攪拌混合し、積層シート用の塗工液を得た。
(Example 17)
[Synthesis of coating solution for forming transparent sheet]
9 parts of an acrylic emulsion aqueous solution (BASF Co., Ltd. Jonkrill 352D, Tg 56 ° C.), a urethane emulsion aqueous solution (Daiichi Kogyo Seiyaku Co., Ltd. Superflex 130, Tg), and 1 part of a foaming agent were added to add 5 parts. The mixture was stirred and mixed to obtain a coating solution for a laminated sheet.

[積層シートの製造]
図55(C)に記載の方法によって、透明シート形成用の塗工液をPET基材シートの表面(厚さ25μm)に塗工した後、乾燥させることにより積層シートを製造した。その塗工にはダイコーターを用い、塗工速度は5m/分、乾燥後の塗工量は5g/m2とした。乾燥温度は90℃とした。透明シートの厚さBは5μmであった。細孔の分布密度は、1平方mm当たり1万個の孔が存在する密度となり、細孔径は0.02μmであった。透湿度は10g/m2・hであった。
[Manufacture of laminated sheets]
A transparent sheet-forming coating solution was applied to the surface (thickness 25 μm) of the PET base sheet by the method described in FIG. 55 (C), and then dried to produce a laminated sheet. A die coater was used for the coating, the coating speed was 5 m / min, and the coating amount after drying was 5 g / m 2 . The drying temperature was 90 ° C. The thickness B of the transparent sheet was 5 μm. The distribution density of the pores was a density where 10,000 pores exist per square mm, and the pore diameter was 0.02 μm. The moisture permeability was 10 g / m 2 · h.

[転写材の製造]
積層シートを変更した以外は、実施例1と同様にして転写材および記録物を得た。
[Manufacture of transfer material]
A transfer material and a recorded matter were obtained in the same manner as in Example 1 except that the laminated sheet was changed.

(実施例18)
[透明シート形成用の塗工液の合成]
アクリルエマルジョン水溶液(BASF社製ジョンクリル352D、Tg56℃)を9部と、ウレタンエマルジョン水溶液(第一工業製薬社製スーパーフレックス130、Tg)を1部と、多孔質樹脂粒子を1部と、を加えて5分攪拌混合し、透明シート形成用の塗工液を得た。
(Example 18)
[Synthesis of coating solution for forming transparent sheet]
9 parts of an acrylic emulsion aqueous solution (BASF Co., Ltd. Jonkrill 352D, Tg56 ° C.), 1 part of urethane emulsion aqueous solution (Daiichi Kogyo Seiyaku Superflex 130, Tg), 1 part of porous resin particles, In addition, the mixture was stirred and mixed for 5 minutes to obtain a coating liquid for forming a transparent sheet.

[積層シートの製造]
図37の(c)に記載の方法により、透明シート形成用の塗工液をPET基材シートの表面(厚さ25μm)に塗工した後、乾燥することにより、積層シートを製造した。その塗工にはダイコーターを用い、塗工速度は5m/分、乾燥後の塗工量は5g/m2とした。乾燥温度は90℃とした。透明シートの厚さBは5μmであった。細孔の分布密度は、1平方mm当たりに1万個の孔が存在する密度となり、細孔径は0.02μmであった。透湿度は10g/m2・hであった。
[Manufacture of laminated sheets]
By applying the coating liquid for forming a transparent sheet to the surface (thickness 25 μm) of the PET base sheet by the method described in FIG. 37 (c), the laminate sheet was manufactured by drying. A die coater was used for the coating, the coating speed was 5 m / min, and the coating amount after drying was 5 g / m 2 . The drying temperature was 90 ° C. The thickness B of the transparent sheet was 5 μm. The distribution density of the pores was a density in which 10,000 pores exist per square mm, and the pore diameter was 0.02 μm. The moisture permeability was 10 g / m 2 · h.

[転写材の製造]
積層シートを変更した以外は、実施例1と同様にして転写材および記録物を得た。
[Manufacture of transfer material]
A transfer material and a recorded matter were obtained in the same manner as in Example 1 except that the laminated sheet was changed.

(実施例19)
[透明シート形成用の塗工液の合成]
アクリルエマルジョン水溶液(BASF社製ジョンクリル352D、Tg56℃)を9部と、ウレタンエマルジョン水溶液(第一工業製薬社製スーパーフレックス130、Tg)を1部と、中空樹脂粒子とを1部と、加えて5分攪拌混合し、透明シート形成用の塗工液を得た。
(Example 19)
[Synthesis of coating solution for forming transparent sheet]
Add 9 parts of an acrylic emulsion aqueous solution (BASF Co., Ltd. Joncrill 352D, Tg56 ° C), 1 part of urethane emulsion aqueous solution (Daiichi Kogyo Seiyaku Co., Ltd. Superflex 130, Tg), and 1 part of hollow resin particles. For 5 minutes to obtain a coating solution for forming a transparent sheet.

[積層シートの製造]
図38の(c)に記載の方法により、透明シート形成用の塗工液をPET基材シートの表面(厚さ25μm)に塗工した後、乾燥させることにより、積層シートを製造した。その塗工にはダイコーターを用い、塗工速度は5m/分、乾燥後の塗工量は5g/m2とした。乾燥温度は90℃とした。透明シートの厚さBは5μmであった。細孔の分布密度は、4平方mm当たりに1つの孔が存在する密度であった、細孔径は0.02μmであった。透湿度は10g/m2・hであった。
[Manufacture of laminated sheets]
By applying the coating liquid for forming the transparent sheet to the surface (thickness 25 μm) of the PET base sheet by the method described in FIG. 38 (c), the laminate sheet was manufactured by drying. A die coater was used for the coating, the coating speed was 5 m / min, and the coating amount after drying was 5 g / m 2 . The drying temperature was 90 ° C. The thickness B of the transparent sheet was 5 μm. The distribution density of the pores was such that one pore was present per 4 mm 2, and the pore diameter was 0.02 μm. The moisture permeability was 10 g / m 2 · h.

[転写材の製造]
積層シートを変更した以外は、実施例1と同様にして転写材および記録物を得た。
[Manufacture of transfer material]
A transfer material and a recorded matter were obtained in the same manner as in Example 1 except that the laminated sheet was changed.

(実施例20)
穿孔処理方法を図46(a)のような針657を用いる方法から、図46(b)のような拍車650を用いる方法に変更した以外は、実施例1と同様にして転写材および記録物を得た。
(Example 20)
The transfer material and recorded matter are the same as in Example 1 except that the punching method is changed from the method using the needle 657 as shown in FIG. 46A to the method using the spur 650 as shown in FIG. 46B. Got.

(実施例21)
穿孔処理方法を図46(a)のような針657を用いる方法から、図46(c)のようなレーザ加工装置658を用いる方法に変更した以外は、実施例1と同様にして転写材および記録物を得た。
(Example 21)
Except for changing the perforation processing method from the method using the needle 657 as shown in FIG. 46 (a) to the method using the laser processing device 658 as shown in FIG. 46 (c), the transfer material and A record was obtained.

(実施例22)
細孔の形成方法を図41の(a)に記載の方法から図42の(a)に記載に変更した以外は、実施例1と同様の方法により、透明シートおよび基材シートに細孔が形成された積層シートを製造した。その積載シートを用いて、実施例1と同様の方法により転写材および記録物を得た。
(Example 22)
Except for changing the formation method of the pores from the method described in FIG. 41A to the description in FIG. 42A, pores were formed in the transparent sheet and the base sheet in the same manner as in Example 1. The formed laminated sheet was manufactured. Using the stacked sheets, transfer materials and recorded matter were obtained in the same manner as in Example 1.

(実施例23)
細孔の形成方法を図41の(a)に記載の方法から図40の(a)に記載に変更した以外は、実施例1と同様の方法により、透明シートおよび色材受容層に細孔が形成された積層シートを製造した。その積載シートを用いて、実施例1と同様の方法により転写材および記録物を得た。
(Example 23)
Except for changing the formation method of the pores from the method shown in FIG. 41A to the description shown in FIG. 40A, pores were formed in the transparent sheet and the colorant receiving layer in the same manner as in Example 1. A laminated sheet in which was formed was manufactured. Using the stacked sheets, transfer materials and recorded matter were obtained in the same manner as in Example 1.

(実施例24)
細孔の形成方法を図41の(a)に記載の方法から図42の(b)に記載に変更した以外は、実施例1と同様の方法により、透明シート、色材受容層および基材シートに細孔が形成された積層シートを製造した。その積載シートを用いて、実施例1と同様の方法により転写材および記録物を得た。
(Example 24)
A transparent sheet, a colorant receiving layer, and a substrate were formed in the same manner as in Example 1 except that the pore formation method was changed from the method shown in FIG. 41 (a) to the one shown in FIG. 42 (b). A laminated sheet in which pores were formed in the sheet was produced. Using the stacked sheets, transfer materials and recorded matter were obtained in the same manner as in Example 1.

(実施例25)
[転写材25の製造]
積層シートに細孔形成を行わないことを除いては、実施例1と同様にして転写材を得た。
(Example 25)
[Manufacture of transfer material 25]
A transfer material was obtained in the same manner as in Example 1 except that pore formation was not performed on the laminated sheet.

[記録物の製造]
上述した第2の製造装置(図28の製造装置)を用いて、画像記録前の段階で上記の転写材25に機械的な穿孔処理を施し、基材シートおよび透明シートに細孔を形成してから、顔料インクにより記録デューティー60%の60%ベタ画像を記録した。その後、その転写材を画像支持体に加熱圧着させてから、基材シートを剥離することにより記録物を得た。製造装置の記録部としては、ラインヘッドを搭載したプリントモジュール(商品名「PM−200Z」、キヤノンファインテック製)を用い、画像支持体としては、塩化ビニル製のカード(商品名「C−4002」、エボリス製)を用いた。
[Manufacture of recorded materials]
Using the above-described second manufacturing apparatus (manufacturing apparatus in FIG. 28), the transfer material 25 is mechanically perforated in the stage before image recording to form pores in the base sheet and the transparent sheet. Thereafter, a 60% solid image with a recording duty of 60% was recorded with the pigment ink. Thereafter, the transfer material was heated and pressure-bonded to the image support, and then the base material sheet was peeled to obtain a recorded matter. As a recording unit of the manufacturing apparatus, a print module (trade name “PM-200Z”, manufactured by Canon Finetech) equipped with a line head is used, and a card made of vinyl chloride (trade name “C-4002” is used as an image support. “Evolis”).

(実施例26)
[記録物の製造]
上述した第3の製造装置(図29の製造装置)を用いて、転写材25に顔料インクにより記録デューティー60%の60%ベタ画像を記録し、その後の段階で機械的な穿孔処理を施し、基材シートおよび透明シートに細孔を形成した。その後、その転写材を画像支持体に加熱圧着させてから、基材シートを剥離することにより記録物を得た。製造装置の記録部としては、ラインヘッドを搭載したプリントモジュール(商品名「PM−200Z」、キヤノンファインテック製)を用い、画像支持体としては、塩化ビニル製のカード(商品名「C−4002」、エボリス製)を用いた。
(Example 26)
[Manufacture of recorded materials]
Using the above-described third manufacturing apparatus (manufacturing apparatus in FIG. 29), a 60% solid image with a recording duty of 60% is recorded on the transfer material 25 with pigment ink, and a mechanical perforation process is performed at a later stage. Pores were formed in the base sheet and the transparent sheet. Thereafter, the transfer material was heated and pressure-bonded to the image support, and then the substrate sheet was peeled off to obtain a recorded matter. As a recording unit of the manufacturing apparatus, a print module (trade name “PM-200Z”, manufactured by Canon Finetech) equipped with a line head is used, and a card made of vinyl chloride (trade name “C-4002” is used as an image support. “Evolis”).

(実施例27)
[記録物の製造]
上述した第4の製造装置(図30の製造装置)を用いて、転写材25に顔料インクにより記録デューティー60%の60%ベタ画像を記録し、その転写材を画像支持体に加熱圧着させた。その後の段階で機械的な穿孔処理を施し、基材シートおよび透明シートに細孔を形成し、その後、基材シートを剥離することにより記録物を得た。製造装置の記録部としては、ラインヘッドを搭載したプリントモジュール(商品名「PM−200Z」、キヤノンファインテック製)を用い、画像支持体としては、塩化ビニル製のカード(商品名「C−4002」、エボリス製)を用いた。
(Example 27)
[Manufacture of recorded materials]
Using the above-described fourth manufacturing apparatus (manufacturing apparatus in FIG. 30), a 60% solid image with a recording duty of 60% was recorded on the transfer material 25 with pigment ink, and the transfer material was heat-pressed to the image support. . At a later stage, a mechanical perforation treatment was performed to form pores in the base sheet and the transparent sheet, and then the base sheet was peeled to obtain a recorded matter. As a recording unit of the manufacturing apparatus, a print module (trade name “PM-200Z”, manufactured by Canon Finetech) equipped with a line head is used, and a card made of vinyl chloride (trade name “C-4002” is used as an image support. “Evolis”).

(実施例28)
[記録物の製造]
上述した第5の製造装置(図31の製造装置)を用いて、転写材25に顔料インクにより記録デューティー60%の60%ベタ画像を記録し、その転写材を画像支持体に加熱圧着させてから、基材シートを剥離した。基材シートを剥離した段階で機械的な穿孔処理を施し、透明シートに細孔を形成することにより記録物を得た。製造装置の記録部としては、ラインヘッドを搭載したプリントモジュール(商品名「PM−200Z」、キヤノンファインテック製)を用い、画像支持体としては、塩化ビニル製のカード(商品名「C−4002」、エボリス製)を用いた。
(Example 28)
[Manufacture of recorded materials]
Using the above-described fifth manufacturing apparatus (manufacturing apparatus in FIG. 31), a 60% solid image with a recording duty of 60% is recorded on the transfer material 25 with pigment ink, and the transfer material is heated and pressure-bonded to the image support. From this, the base sheet was peeled off. When the substrate sheet was peeled off, a mechanical punching process was performed to form pores in the transparent sheet to obtain a recorded matter. As a recording unit of the manufacturing apparatus, a print module (trade name “PM-200Z”, manufactured by Canon Finetech) equipped with a line head is used, and a card made of vinyl chloride (trade name “C-4002” is used as an image support. “Evolis”).

(実施例29)
[PVA水溶液1の合成]
ポリビニルアルコール(商品名「PVA123」、クラレ製)をイオン交換水に溶解し、固形分含量が8%のポリビニルアルコール水溶液を調製した。ポリビニルアルコールは、平均重合度が2300、けん化度が98〜99mol%であった。
(Example 29)
[Synthesis of PVA aqueous solution 1]
Polyvinyl alcohol (trade name “PVA123”, manufactured by Kuraray Co., Ltd.) was dissolved in ion-exchanged water to prepare a polyvinyl alcohol aqueous solution having a solid content of 8%. Polyvinyl alcohol had an average polymerization degree of 2300 and a saponification degree of 98 to 99 mol%.

[PVA水溶液2の合成]
ポリビニルアルコール(商品名「PVA235」、クラレ製)をイオン交換水に溶解し、固形分含量が8%のポリビニルアルコール水溶液を調製した。ポリビニルアルコールは、平均重合度が3500、けん化度が87〜89mol%であった。
[Synthesis of PVA aqueous solution 2]
Polyvinyl alcohol (trade name “PVA235”, manufactured by Kuraray Co., Ltd.) was dissolved in ion-exchanged water to prepare an aqueous polyvinyl alcohol solution having a solid content of 8%. Polyvinyl alcohol had an average polymerization degree of 3500 and a saponification degree of 87 to 89 mol%.

[PVA水溶液3の合成]
ポリビニルアルコール(商品名「PVA117」、クラレ製)をイオン交換水に溶解し、固形分含量が8%のポリビニルアルコール水溶液を調製した。ポリビニルアルコールは、平均重合度が1700、けん化度が98〜99mol%であった。
[Synthesis of PVA aqueous solution 3]
Polyvinyl alcohol (trade name “PVA117”, manufactured by Kuraray Co., Ltd.) was dissolved in ion-exchanged water to prepare a polyvinyl alcohol aqueous solution having a solid content of 8%. Polyvinyl alcohol had an average polymerization degree of 1700 and a saponification degree of 98 to 99 mol%.

[PVA水溶液4の合成]
ポリビニルアルコール(商品名「PVA110」、クラレ製)をイオン交換水に溶解し、固形分含量が8%のポリビニルアルコール水溶液を調製した。ポリビニルアルコールは、平均重合度が1100、けん化度が98〜99mol%であった。
[Synthesis of PVA aqueous solution 4]
Polyvinyl alcohol (trade name “PVA110”, manufactured by Kuraray Co., Ltd.) was dissolved in ion-exchanged water to prepare a polyvinyl alcohol aqueous solution having a solid content of 8%. Polyvinyl alcohol had an average degree of polymerization of 1100 and a degree of saponification of 98 to 99 mol%.

[PVA水溶液5の合成]
ポリビニルアルコール(商品名「PVA424H」、クラレ製)をイオン交換水に溶解し、固形分含量が8%のポリビニルアルコール水溶液を調製した。ポリビニルアルコールは、平均重合度が2400、けん化度が78.5〜80.5mol%であった。
[Synthesis of PVA aqueous solution 5]
Polyvinyl alcohol (trade name “PVA424H”, manufactured by Kuraray Co., Ltd.) was dissolved in ion-exchanged water to prepare a polyvinyl alcohol aqueous solution having a solid content of 8%. Polyvinyl alcohol had an average degree of polymerization of 2400 and a degree of saponification of 78.5 to 80.5 mol%.

[透明シート形成用の塗工液の合成]
アクリルエマルジョン水溶液(BASF社製ジョンクリル352D、Tg56℃、固形分濃度45%)を9部と、ウレタンエマルジョン水溶液(第一工業製薬社製スーパーフレックス130、Tg103℃、固形分濃度35%)を1部と、PVA水溶液1を0.5部と、加えて5分攪拌混合し、透明シート形成用の塗工液を得た。膨潤性樹脂の含有量は表6に記載した。
[Synthesis of coating solution for forming transparent sheet]
9 parts of an acrylic emulsion aqueous solution (BASF Co., Ltd. Jonkrill 352D, Tg 56 ° C., solid content concentration 45%) and urethane emulsion aqueous solution (Daiichi Kogyo Seiyaku Co., Ltd. Superflex 130, Tg 103 ° C., solid content concentration 35%) 1 Part and 0.5 part of PVA aqueous solution 1 were added and mixed with stirring for 5 minutes to obtain a coating liquid for forming a transparent sheet. The content of the swellable resin is shown in Table 6.

[積層シート(転写材の構成素材)の製造]
透明シート形成用の塗工液をPET基材シートの表面(厚さ25μm)に塗工した後、乾燥させることにより、積層シートを製造した。その塗工にはダイコーターを用い、塗工速度は5m/分、乾燥後の塗工量は5g/m2とした。乾燥温度は90℃とした。
[Manufacture of laminated sheets (component materials for transfer materials)]
After the coating liquid for forming the transparent sheet was applied to the surface (thickness 25 μm) of the PET base sheet, it was dried to produce a laminated sheet. A die coater was used for the coating, the coating speed was 5 m / min, and the coating amount after drying was 5 g / m 2 . The drying temperature was 90 ° C.

[転写材の製造]
積層シートにおける透明シートの表面に、混合直後の色材受容層形成用の塗工液を塗工して、乾燥させることにより、空隙吸収型の色材受容層を備えた実施例1の転写材を製造した。塗工液の塗工にはダイコーターを用い、塗工速度は5m/分、乾燥後の塗工量は15g/m2とした。乾燥温度は60℃とした。転写材は、色材受容層を外側、基材シートを内側としてロール状に巻くことにより、ロール状転写材とした。色材受容層の厚さAは10μmであった。色材受容層の厚みAと透明シートの厚みBの比率A/Bは0.5であった。
[Manufacture of transfer material]
The transfer material of Example 1 provided with a void-absorbing color material receiving layer by applying a coating liquid for forming a color material receiving layer immediately after mixing to the surface of the transparent sheet in the laminated sheet and drying it. Manufactured. A die coater was used for coating the coating solution, the coating speed was 5 m / min, and the coating amount after drying was 15 g / m 2 . The drying temperature was 60 ° C. The transfer material was made into a roll-shaped transfer material by winding in a roll shape with the color material receiving layer on the outside and the base sheet on the inside. The thickness A of the colorant receiving layer was 10 μm. The ratio A / B between the thickness A of the colorant receiving layer and the thickness B of the transparent sheet was 0.5.

上記のようにして得られた転写材に、上述した第1の製造装置を用いて、顔料インクにより記録デューティー60%の60%ベタ画像を記録し、その転写材を画像支持体に加熱圧着させてから、基材シートを剥離することにより記録物を得た。製造装置の記録部としては、ラインヘッドを搭載したプリントモジュール(商品名「PM−200Z」、キヤノンファインテック製)を用い、画像支持体としては、塩化ビニル製のカード(商品名「C−4002」、エボリス製)を用いた。加熱圧着の条件は、温度160℃、圧力3.9Kg/cm、搬送速度50mm/secである。基材シートを剥離する際の引き剥がし角度は90°とした。色材受容層のSP値と、画像支持体のSP値と、の差SP2は0.1であった。   A 60% solid image with a recording duty of 60% is recorded on the transfer material obtained as described above with the pigment ink using the first manufacturing apparatus described above, and the transfer material is heated and pressure-bonded to the image support. Then, the recorded material was obtained by peeling the base sheet. As a recording unit of the manufacturing apparatus, a print module (trade name “PM-200Z”, manufactured by Canon Finetech) equipped with a line head is used, and a card made of vinyl chloride (trade name “C-4002” is used as an image support. “Evolis”). The thermocompression bonding conditions are a temperature of 160 ° C., a pressure of 3.9 Kg / cm, and a conveyance speed of 50 mm / sec. The peeling angle when peeling the base sheet was 90 °. The difference SP2 between the SP value of the color material receiving layer and the SP value of the image support was 0.1.

(実施例30)
色材受容層形成用の塗工液を高松油脂製NS625XCに変更して、膨潤型の色材受容層を形成した以外は、実施例29と同様にして転写材および記録物を得た.
(Example 30)
A transfer material and a recorded material were obtained in the same manner as in Example 29 except that the coating material for forming the color material receiving layer was changed to NS625XC made of Takamatsu Oil and Fat and a swollen color material receiving layer was formed.

(実施例31)
透明シートの厚みAを5μmから15μmに変更し、色材受容層の厚みを10μmから5μmに変更した以外は、実施例29と同様にして転写材および記録物を得た。色材受容層の厚みAと、透明シートの厚みBと、の比率(A/B)は3であった。
(Example 31)
A transfer material and a recorded matter were obtained in the same manner as in Example 29 except that the thickness A of the transparent sheet was changed from 5 μm to 15 μm and the thickness of the colorant receiving layer was changed from 10 μm to 5 μm. The ratio (A / B) between the thickness A of the colorant receiving layer and the thickness B of the transparent sheet was 3.

(実施例32)
透明シートの厚みAを5μmから1μmに変更し、色材受容層の厚みを10μmから15μmに変更した以外は、実施例29と同様にして転写材および記録物を得た。色材受容層の厚みAと、透明シートの厚みBと、の比率(A/B)は0.07であった。
(Example 32)
A transfer material and a recorded matter were obtained in the same manner as in Example 29 except that the thickness A of the transparent sheet was changed from 5 μm to 1 μm and the thickness of the colorant receiving layer was changed from 10 μm to 15 μm. The ratio (A / B) between the thickness A of the colorant receiving layer and the thickness B of the transparent sheet was 0.07.

(実施例33)
透明シートの厚みAを5μmから20μmに変更し、色材受容層の厚みBを10μmから5μmに変更した以外は、実施例29と同様にして転写材および記録物を得た。色材受容層の厚みAと、透明シートの厚みBと、の比率(A/B)は4.0であった。
(Example 33)
A transfer material and a recorded material were obtained in the same manner as in Example 29 except that the thickness A of the transparent sheet was changed from 5 μm to 20 μm and the thickness B of the colorant receiving layer was changed from 10 μm to 5 μm. The ratio (A / B) between the thickness A of the colorant receiving layer and the thickness B of the transparent sheet was 4.0.

(実施例34)
透明シートの厚みAを5μmから0.5μmに変更し、色材受容層を10μmから15μmに変更した以外は、実施例29と同様にして転写材および記録物を得た。色材受容層の厚みAと、透明シートの厚みBと、の比率(A/B)は0.03であった。
(Example 34)
A transfer material and a recorded matter were obtained in the same manner as in Example 29 except that the thickness A of the transparent sheet was changed from 5 μm to 0.5 μm and the colorant receiving layer was changed from 10 μm to 15 μm. The ratio (A / B) between the thickness A of the colorant receiving layer and the thickness B of the transparent sheet was 0.03.

(実施例35)
[ポリエチレングリコール水溶液の調整]
ポリエチレングリコール(PEG,重合度1000)をイオン交換水に溶解して、固形分含量が8%のポリエチレングリコール水溶液を調製した。
(Example 35)
[Preparation of aqueous polyethylene glycol solution]
Polyethylene glycol (PEG, polymerization degree 1000) was dissolved in ion-exchanged water to prepare a polyethylene glycol aqueous solution having a solid content of 8%.

[転写材の製造]
透明シート形成用の塗工液の調製においてPVA水溶液1、0.5部をポリエチレングリコール(PEG)水溶液0.5部に変更した以外は、実施例29と同様にして転写材および記録物を得た。
[Manufacture of transfer material]
A transfer material and recorded matter were obtained in the same manner as in Example 29, except that in the preparation of the coating liquid for forming the transparent sheet, 0.5 part of PVA aqueous solution was changed to 0.5 part of polyethylene glycol (PEG) aqueous solution. It was.

(実施例36)
透明シート形成用の塗工液の調製においてPVA水溶液1、0.5部をポリエチレングリコール水溶液0.1部に変更した以外は、実施例29と同様にして転写材および記録物を得た。膨潤性樹脂の含有率は表6に記載した。
(Example 36)
A transfer material and a recorded matter were obtained in the same manner as in Example 29 except that in the preparation of the coating liquid for forming the transparent sheet, 0.5 part of the PVA aqueous solution was changed to 0.1 part of the aqueous polyethylene glycol solution. The content of the swellable resin is shown in Table 6.

(実施例37)
透明シート形成用の塗工液の調製においてPVA水溶液1、0.5部を1部に変更した以外は、実施例29と同様にして転写材および記録物を得た。透明シートの膨潤性樹脂の含有率は表6に記載した。
(Example 37)
A transfer material and recorded matter were obtained in the same manner as in Example 29, except that in the preparation of the coating liquid for forming the transparent sheet, 1 part of PVA aqueous solution was changed to 0.5 part. The content of the swellable resin in the transparent sheet is shown in Table 6.

(実施例38)
透明シート形成用の塗工液の調製においてPVA水溶液1、0.5部を0.1部に変更した以外は、実施例29と同様にして転写材および記録物を得た。透明シートの膨潤性樹脂の含有率は表6に記載した。
(Example 38)
A transfer material and recorded matter were obtained in the same manner as in Example 29 except that in the preparation of the coating liquid for forming the transparent sheet, 0.5 part of the PVA aqueous solution was changed to 0.1 part. The content of the swellable resin in the transparent sheet is shown in Table 6.

(実施例39)
透明シート形成用の塗工液の調製においてPVA水溶液1、0.5部を0.3部に変更した以外は、実施例29と同様にして転写材および記録物を得た。透明シートの膨潤性樹脂の含有率は表6に記載した。
(Example 39)
A transfer material and a recorded matter were obtained in the same manner as in Example 29 except that in the preparation of the coating liquid for forming the transparent sheet, 0.5 part of the PVA aqueous solution was changed to 0.3 part. The content of the swellable resin in the transparent sheet is shown in Table 6.

(実施例40)
透明シート形成用の塗工液の調製においてPVA水溶液1、0.5部を3部に変更した以外は、実施例29と同様にして転写材および記録物を得た。透明シートの膨潤性樹脂の含有率は表6に記載した。
(Example 40)
A transfer material and a recorded matter were obtained in the same manner as in Example 29 except that the PVA aqueous solution 1, 0.5 part was changed to 3 parts in the preparation of the coating liquid for forming the transparent sheet. The content of the swellable resin in the transparent sheet is shown in Table 6.

(実施例41)
透明シート形成用の塗工液の調製においてPVA水溶液1、0.5部を0.01部に変更した以外は、実施例29と同様にして転写材および記録物を得た。透明シートの膨潤性樹脂の含有率は表6に記載した。
(Example 41)
A transfer material and recorded matter were obtained in the same manner as in Example 29, except that in the preparation of the coating liquid for forming the transparent sheet, 0.5 part of the PVA aqueous solution was changed to 0.01 part. The content of the swellable resin in the transparent sheet is shown in Table 6.

(実施例42)
透明シート形成用の塗工液の調製においてPVA水溶液1を0.5部からPVA水溶液2を0.5部に変更した以外は、実施例29と同様にして転写材および記録物を得た。
(Example 42)
A transfer material and recorded matter were obtained in the same manner as in Example 29, except that in the preparation of the coating liquid for forming the transparent sheet, 0.5 part of the PVA aqueous solution 1 was changed to 0.5 part of the PVA aqueous solution 2.

(実施例43)
透明シート形成用の塗工液の調製においてPVA水溶液1を0.5部からPVA水溶液3を0.5部に変更した以外は、実施例29と同様にして転写材および記録物を得た。
(Example 43)
A transfer material and recorded matter were obtained in the same manner as in Example 29, except that in the preparation of the coating liquid for forming the transparent sheet, 0.5 part of the PVA aqueous solution 1 was changed to 0.5 part of the PVA aqueous solution 3.

(実施例44)
透明シート形成用の塗工液の調製においてPVA水溶液1を0.5部からPVA水溶液4を0.5部に変更した以外は、実施例29と同様にして転写材および記録物を得た。
(Example 44)
A transfer material and a recorded matter were obtained in the same manner as in Example 29 except that 0.5 part of the PVA aqueous solution 1 was changed to 0.5 part of the PVA aqueous solution 4 in the preparation of the coating liquid for forming the transparent sheet.

(実施例45)
透明シート形成用の塗工液の調製においてPVA水溶液1を0.5部からPVA水溶液5を0.5部に変更した以外は、実施例29と同様にして転写材および記録物を得た。
(Example 45)
A transfer material and a recorded matter were obtained in the same manner as in Example 29 except that 0.5 part of the PVA aqueous solution 1 was changed to 0.5 part of the PVA aqueous solution 5 in the preparation of the coating liquid for forming the transparent sheet.

(実施例46)
[転写材の製造]
透明シート形成用の塗工液の調製において、PVA水溶液1を0.5部から高松油脂製NS625XC水溶液(固形分濃度8%)を1部に変更した以外は、実施例29と同様にして転写材および記録物を得た。
(Example 46)
[Manufacture of transfer material]
Transfer in the same manner as in Example 29 except that 0.5 part of the PVA aqueous solution 1 was changed to 1 part of the NS625XC aqueous solution made of Takamatsu Yushi (solid content concentration 8%) in the preparation of the coating liquid for forming the transparent sheet. Materials and recorded materials were obtained.

以上の実施例に対して、下記のような評価を行った。   The following evaluation was performed on the above examples.

[評価<透明シートのひび割れ>]
記録物を水道水に48時間浸漬し、水中から取り出した後、表面を軽くふき取ってから、透明シートのひび割れを目視および顕微鏡で観察した。
◎:ひび割れがない。
○:ひび割れはないが、小さなシワ跡が確認できる。
△:ひび割れはないが、大きなシワ跡が確認できる。
×:シワ跡が残り、目視で大量のひび割れが確認できる。
[Evaluation <Crack of Transparent Sheet>]
The recorded material was immersed in tap water for 48 hours and taken out from the water, and then the surface was lightly wiped, and then the cracks of the transparent sheet were observed visually and with a microscope.
A: There is no crack.
○: Although there is no crack, small wrinkle marks can be confirmed.
(Triangle | delta): Although there is no crack, a big wrinkle trace can be confirmed.
X: Wrinkle marks remain and a large amount of cracks can be confirmed visually.

[評価<転写・剥離性>]
実施例または比較例の転写材を用いて、画像支持体に色材受容層を転写して記録物を作製し、その際における色材受容層の転写および基材シートの剥離の度合いを評価した。評価は目視により行った。その結果を下表3,4,5に示す。
○:画像支持体に対して、色材受容層が良好に転写されていて、基材シートも良好に剥離する。透明シートの剥離も見られない。
△:画像支持体に対して、色材受容層が転写されない部分があるか、透明シートの部分的な剥がれが見られる。または基材シートが剥離しない部分がある。
×:画像支持体に対して、色材受容層および透明シートが転写されない。
[Evaluation <Transfer / Peelability>]
Using the transfer material of Example or Comparative Example, a color material receiving layer was transferred to an image support to produce a recorded material, and the degree of transfer of the color material receiving layer and peeling of the base material sheet at that time was evaluated. . Evaluation was performed visually. The results are shown in Tables 3, 4, and 5 below.
◯: The colorant receiving layer is well transferred to the image support, and the base sheet is also peeled off well. There is no peeling of the transparent sheet.
Δ: There is a portion where the colorant receiving layer is not transferred to the image support, or partial peeling of the transparent sheet is observed. Alternatively, there is a portion where the base sheet does not peel.
X: The colorant receiving layer and the transparent sheet are not transferred to the image support.

[評価<汚染水>]
色材濃度5%の染料インクを透明シート上に一滴滴下し、滴下30秒後に染料インクをふき取り、透明シートの染色具合を目視で観察した。
○:透明シートに染色は見られない。
△:透明シートの一部が染色しているが、色材受容層の記録情報が認識可能である。
×:透明シートおよび色材受容層が染色され、色材受容層の記録情報が認識不可である。
[Evaluation <Contaminated Water>]
One drop of dye ink having a colorant concentration of 5% was dropped on the transparent sheet, and after 30 seconds of dropping, the dye ink was wiped off, and the dyeing condition of the transparent sheet was visually observed.
○: Dyeing is not seen on the transparent sheet.
Δ: A part of the transparent sheet is dyed, but the recording information of the colorant receiving layer can be recognized.
X: The transparent sheet and the color material receiving layer are dyed, and the recorded information of the color material receiving layer is unrecognizable.

1 転写材
50 基材シート
52 透明シート(保護シート)
52A 細孔
53 色材受容層
55 画像支持体
72 画像
73 記録物
650 拍車
657 針
658 レーザ加工装置
1 Transfer material 50 Base sheet 52 Transparent sheet (protective sheet)
52A pore 53 color material receiving layer 55 image support 72 image 73 recorded matter 650 spur 657 needle 658 laser processing apparatus

Claims (10)

基材シート、保護シート、および色材受容層が、この順に積層された転写材であって、
前記色材受容層は水溶性樹脂を含有し、
前記保護シートは、平均重合度が1,500以上5,000以下のポリビニルアルコールを含有し、
前記ポリビニルアルコールの含有量は、0.05質量%以上、2.0質量%以下であることを特徴とする転写材。
A base material sheet, a protective sheet, and a color material receiving layer are transfer materials laminated in this order,
The colorant receiving layer contains a water-soluble resin,
The protective sheet contains polyvinyl alcohol having an average degree of polymerization of 1,500 to 5,000 ,
Content of the said polyvinyl alcohol is 0.05 mass% or more and 2.0 mass% or less, The transfer material characterized by the above-mentioned.
前記ポリビニルアルコールのケン化度は、86 mol%以上であることを特徴とする請求項1に記載の転写材。  The transfer material according to claim 1, wherein the degree of saponification of the polyvinyl alcohol is 86 mol% or more. 前記保護シートの透湿度は5g/m2・h以上であることを特徴とする請求項1または2に記載の転写材。 The transfer material according to claim 1, wherein the moisture permeability of the protective sheet is 5 g / m 2 · h or more. 前記保護シートの厚みAと、前記色材受容層の厚みBと、の比率(A/B)が式(1)の範囲であることを特徴とする請求項1から3のいずれか1項に記載の転写材。
0.07≦(A/B)≦3.00 ・・・ (1)
The ratio (A / B) between the thickness A of the protective sheet and the thickness B of the colorant receiving layer is in the range of the formula (1), according to any one of claims 1 to 3. The transfer material described.
0.07 ≦ (A / B) ≦ 3.00 (1)
前記保護シートは、アクリル系および/またはウレタン系の樹脂を主成分として形成されることを特徴とする請求項1から4のいずれか1項に記載の転写材。   The transfer material according to any one of claims 1 to 4, wherein the protective sheet is formed mainly of an acrylic and / or urethane resin. 前記基材シートは、剥離可能であることを特徴とする請求項1からのいずれか1項に記載の転写材。 The base sheet, transfer material according to any one of claims 1 5, characterized in that the peelable. 画像支持体、画像が記録された色材受容層、および保護シートが、順次積層された記録物であって、
前記色材受容層は水溶性樹脂を含有し、
前記保護シートは、平均重合度が1,500以上5,000以下のポリビニルアルコールを含有し、
前記ポリビニルアルコールの含有量は、0.05質量%以上、2.0質量%以下であることを特徴とする記録物。
An image support, a colorant receiving layer on which an image is recorded, and a protective sheet are sequentially stacked recordings,
The colorant receiving layer contains a water-soluble resin,
The protective sheet contains polyvinyl alcohol having an average degree of polymerization of 1,500 to 5,000 ,
Content of the said polyvinyl alcohol is 0.05 mass% or more and 2.0 mass% or less, The recorded matter characterized by the above-mentioned.
前記ポリビニルアルコールのケン化度は、86 mol%以上であることを特徴とする請求項7に記載の記録物。  The recorded matter according to claim 7, wherein the degree of saponification of the polyvinyl alcohol is 86 mol% or more. 前記保護シートは、アクリル系および/またはウレタン系の樹脂を主成分として形成されることを特徴とする請求項7または8に記載の記録物。  The recorded matter according to claim 7 or 8, wherein the protective sheet is formed mainly of an acrylic and / or urethane resin. 画像支持体、画像が記録された色材受容層、および保護シートが、順次積層された記録物の製造方法であって、
請求項1からのいずれか1項に記載の転写材の色材受容層にインクジェット記録により画像を記録する工程1と、
前記転写材の前記色材受容層を前記画像支持体に加熱圧着する工程2と、
前記転写材から前記基材シートを剥離する工程3と、を含むことを特徴とする記録物の製造方法。
An image support, a colorant receiving layer on which an image is recorded, and a protective sheet are a method for producing a recorded matter in which layers are sequentially laminated,
Step 1 of recording an image by ink jet recording on the colorant receiving layer of the transfer material according to any one of claims 1 to 6 ,
Step 2 of heat-pressing the colorant receiving layer of the transfer material to the image support;
And a step 3 of peeling the base sheet from the transfer material.
JP2018088285A 2018-05-01 2018-05-01 Transfer material, recorded matter, and method for producing recorded matter Active JP6589009B2 (en)