JP5748375B1 - Exterior wall painting method - Google Patents

Exterior wall painting method Download PDF

Info

Publication number
JP5748375B1
JP5748375B1 JP2014068997A JP2014068997A JP5748375B1 JP 5748375 B1 JP5748375 B1 JP 5748375B1 JP 2014068997 A JP2014068997 A JP 2014068997A JP 2014068997 A JP2014068997 A JP 2014068997A JP 5748375 B1 JP5748375 B1 JP 5748375B1
Authority
JP
Japan
Prior art keywords
wall
metal plate
color
plate
metal decorative
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP2014068997A
Other languages
Japanese (ja)
Other versions
JP2015190226A (en
Inventor
清海 濱中
清海 濱中
Original Assignee
株式会社ハマキャスト
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 株式会社ハマキャスト filed Critical 株式会社ハマキャスト
Priority to JP2014068997A priority Critical patent/JP5748375B1/en
Application granted granted Critical
Publication of JP5748375B1 publication Critical patent/JP5748375B1/en
Publication of JP2015190226A publication Critical patent/JP2015190226A/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

【課題】鮮やかな外観や派手な外観を表現でき、長期間美装状態を保ち、かつメンテナンスが不要で長い耐用年数が可能な外壁塗装方法を提供する。【解決手段】本発明の外壁塗装方法は、建築物の外壁塗装方法であって、骨材と合成樹脂を含む塗布材を吹き付け塗装した壁面(17)の一部にカラー金属化粧板(35)を取り付け、カラー金属化粧板(35)の周囲にウレタンプレポリマーを可塑剤として含む湿気硬化性ウレタン組成物をシーリング材(37)として充填し、壁面(17)及びカラー金属化粧板(35)の表面から上塗り材を塗装する。【選択図】図8An outer wall coating method capable of expressing a vivid appearance and a flashy appearance, maintaining a beautiful appearance for a long time, requiring no maintenance, and having a long service life. The exterior wall painting method of the present invention is a exterior wall painting method for a building, in which a color metal decorative plate (35) is applied to a part of a wall surface (17) spray-coated with an application material containing aggregate and synthetic resin. A moisture curable urethane composition containing a urethane prepolymer as a plasticizer is filled around the color metal decorative plate (35) as a sealing material (37), and the wall surface (17) and the color metal decorative plate (35) are filled. Apply topcoat from the surface. [Selection] Figure 8

Description

本発明は、建築物の外壁にカラー金属プレートを取り付けた外壁塗装方法に関する。   The present invention relates to an outer wall coating method in which a color metal plate is attached to an outer wall of a building.

建築物の壁面等の表面は、美観や本体保護上等の観点から、天然石、金属の薄い板、タイル等を貼り付けたり、疑似天然石模様を付けたり、吹き付け塗装を行う等によって施工されている。従来、建築物の壁面等の表面に模様等を付する方法としては、例えば、リシン系(骨材が含まれる配合)及び塗料系の材料をコテ塗り法、ローラー塗装法等によって塗布する方法がある。コテ塗り法は、コテを用いて材料を建築物の表面に移して延ばす方法である。ローラー塗装法は、ローラーやコテを用いて材料を建築物の表面に移し、ローラーによって延ばす方法である。これらは手作業によって行われるため、大きな模様を付することはできるが、厚塗りや大面積の塗装には適していない。   Surfaces such as wall surfaces of buildings are constructed by attaching natural stones, thin metal plates, tiles, etc., quasi-natural stone patterns, spray painting, etc. from the viewpoint of beauty and protection of the main body . Conventionally, as a method of attaching a pattern or the like to the surface of a wall surface or the like of a building, for example, there is a method of applying a lysine-based (compound containing aggregate) and a paint-based material by a trowel coating method, a roller coating method, or the like. is there. The troweling method is a method in which a material is transferred to the surface of a building using a trowel and extended. The roller coating method is a method in which a material is transferred to the surface of a building using a roller or a trowel and extended by a roller. Since these are performed manually, a large pattern can be applied, but they are not suitable for thick coating or large area coating.

このため、圧縮空気を利用し、スプレーガン等から吹き付け材を噴射させることによって塗装する方法が提案されている(特許文献1)。この吹き付け塗装方法は、適度に粉砕した自然石を、合成樹脂中に混入してなる混合材の異なる色のもの複数種を1機のスプレーガン内の別個のタンクにそれぞれ用意し、該複数種の混合材を複数の吹き付け口を有する多頭式スプレーガンの別個の吹き付け口から同時に吹き付けることによって、非混合多色状に塗布する。この塗装面の非汚染仕上げとして、本発明者らはシロキサン架橋型アクリル−珪素重合体を含む上塗り材を使用することにより、40年耐用の塗装方法を下記特許文献2等に提案している。   For this reason, the method of coating by using a compressed air and spraying a spraying material from a spray gun etc. is proposed (patent document 1). In this spray coating method, appropriately pulverized natural stones are mixed in a synthetic resin, and multiple types of mixed materials of different colors are prepared in separate tanks in a single spray gun. The mixed material is sprayed simultaneously from separate spray ports of a multi-head spray gun having a plurality of spray ports, and is applied in an unmixed multicolored state. As the non-contamination finish of the painted surface, the present inventors have proposed a coating method for 40 years in the following Patent Document 2 and the like by using a topcoat material containing a siloxane cross-linked acrylic-silicon polymer.

特公平5−9587号公報Japanese Patent Publication No. 5-9587 特開2009−264011号公報JP 2009-264011 A

しかし、前記従来の技術は、建築物の外壁面に変化が乏しく、鮮やかな外観や派手な外観を表現することは困難であり、長期間美装状態を保ち、かつメンテナンスが不要な外壁塗装方法は困難であった。   However, the conventional technique described above is a method for painting an outer wall, in which a change in the outer wall surface of a building is scarce, it is difficult to express a vivid appearance or a flashy appearance, a beautiful appearance is maintained for a long time, and maintenance is not required. Was difficult.

本発明は、前記従来の問題を解決するため、鮮やかな外観や派手な外観を表現でき、長期間美装状態を保ち、かつメンテナンスが不要で長い耐用年数が可能な外壁塗装方法を提供する。   In order to solve the above-mentioned conventional problems, the present invention provides an outer wall coating method capable of expressing a vivid appearance or a flashy appearance, maintaining a beautiful appearance for a long period of time, and requiring a long service life without requiring maintenance.

本発明の外壁塗装方法は、建築物の外壁塗装方法であって、骨材と合成樹脂を含む塗布材を吹き付け塗装した壁面の一部にカラー金属化粧板を取り付け、前記カラー金属化粧板の周囲にウレタンプレポリマーを可塑剤として含む湿気硬化性ウレタン組成物をシーリング材として充填し、前記壁面及びカラー金属化粧板の表面から上塗り材を塗装することを特徴とする。   The outer wall painting method of the present invention is a method for painting an outer wall of a building, wherein a color metal decorative plate is attached to a part of a wall surface that has been coated by spraying a coating material containing aggregate and synthetic resin. A moisture curable urethane composition containing a urethane prepolymer as a plasticizer is filled as a sealing material, and a top coating material is applied from the surface of the wall surface and the color metal decorative plate.

本発明は、吹き付け塗装した建築物の壁面の一部にカラー金属化粧板を取り付け、カラー金属化粧板の周囲にウレタンプレポリマーを可塑剤として含む湿気硬化性ウレタン組成物をシーリング材として充填し、前記壁面及びカラー金属化粧板の表面から上塗り材を塗装する。これにより、部分的に鮮やかな外観や派手な外観を表現でき、長期間美装状態を保ち、かつメンテナンスが不要で長い耐用年数が可能な外壁塗装方法を提供できる。   The present invention attaches a color metal decorative board to a part of the wall surface of a spray-painted building, and fills the periphery of the color metal decorative board with a moisture curable urethane composition containing a urethane prepolymer as a plasticizer as a sealing material, A top coat material is applied from the wall surface and the surface of the color metal decorative plate. As a result, it is possible to provide a method for painting an outer wall that can express a partially bright appearance or a flashy appearance, maintains a beautiful appearance for a long period of time, requires no maintenance, and has a long service life.

図1Aは本発明の一実施形態におけるカラー金属化粧板の下側金属プレートの模式的平面図、図1Bは同左側面図である。FIG. 1A is a schematic plan view of a lower metal plate of a color metal decorative plate in one embodiment of the present invention, and FIG. 1B is a left side view thereof. 図2Aは同、カラー金属化粧板の上側金属プレートの模式的平面図、図2Bは同右側面図である。2A is a schematic plan view of an upper metal plate of the color metal decorative plate, and FIG. 2B is a right side view thereof. 図3は同、下側金属プレートに上側金属プレートを組み合わせたカラー金属化粧板の側面図である。FIG. 3 is a side view of a color metal decorative plate in which an upper metal plate is combined with a lower metal plate. 図4は、本発明の一実施形態における吹き付け塗装方法で使用する3頭式スプレーガンを示す斜視図である。FIG. 4 is a perspective view showing a three-head spray gun used in the spray coating method according to an embodiment of the present invention. 図5は同、吹き付け塗装方法を示す説明図である。FIG. 5 is an explanatory view showing the spray coating method. 図6Aは同、研磨前の吹き付け塗装層の拡大断面図、図6Bは研磨後の同塗装層の拡大断面図である。FIG. 6A is an enlarged sectional view of the spray coating layer before polishing, and FIG. 6B is an enlarged sectional view of the coating layer after polishing. 図7は同、カラー金属化粧板を建築物の外壁に固定した状態の模式的断面図である。FIG. 7 is a schematic cross-sectional view of the state in which the color metal decorative plate is fixed to the outer wall of the building. 図8は同、上塗り材を塗装している模式的断面図である。FIG. 8 is a schematic cross-sectional view in which a top coat material is applied. 図9は同、正面図である。FIG. 9 is a front view of the same. 図10は本発明の実施例1の紫外線透過試験を示すグラフである。FIG. 10 is a graph showing an ultraviolet transmission test of Example 1 of the present invention. 図11は本発明の別の実施例の仕上げ状態を示す模式的断面図である。FIG. 11 is a schematic cross-sectional view showing a finished state of another embodiment of the present invention.

本発明は、吹き付け塗装した建築物の壁面の一部にカラー金属化粧板を取り付ける。吹き付け塗装の壁面は自然石調あるいは均一色系など様々なものがあり、概して一様であるが、カラー金属化粧板を取り付けることにより、部分的に鮮やかな外観や派手な外観を表現できる。   In the present invention, a color metal decorative plate is attached to a part of a wall surface of a spray-painted building. The wall surface of spray coating has various things such as natural stone tone or uniform color system, and is generally uniform, but by attaching a color metal decorative plate, it is possible to express a partially vivid appearance or flashy appearance.

カラー金属化粧板はステンレス板、アルミ板などを使用するのが好ましい。ステンレス板は耐腐食性が高く、長期間安定であることから好ましい。ステンレス板はプレス加工などにより様々な形状に成形し、蒸着、スパッタリング、イオンプレーティング及びメッキから選ばれるいずれかの手段でカラー装飾する。カラー装飾は、金属の特徴を生かしてゴールド、シルバー等の金属色が好ましい。カラー金属化粧板の金属プレートの厚みは、例えばステンレス鋼SUS304の場合、0.2〜1.2mmが好ましくさらに好ましくは0.3〜1.0mmである。形状は丸、楕円、長円などの円形、三角形、四角形等の多角形、星形、ハート形等のほか、魚、舟、飛行機、野菜、果物、お札、硬貨等様々な形状が可能である。ビルの所有者や企業体のイメージをデザインすることもできる。
表面は平坦形状、凹凸形状、突出形状等であっても良い。このカラー金属化粧板は壁面の任意の箇所に取り付けできる。中でも目地の一部に取り付けると美装効果が大きいため好ましい。
It is preferable to use a stainless steel plate, an aluminum plate or the like as the color metal decorative plate. Stainless steel plates are preferred because they have high corrosion resistance and are stable for a long time. The stainless steel plate is formed into various shapes by press working or the like, and is color-decorated by any means selected from vapor deposition, sputtering, ion plating and plating. The color decoration is preferably a metal color such as gold or silver taking advantage of the characteristics of the metal. For example, in the case of stainless steel SUS304, the thickness of the color metal decorative plate is preferably 0.2 to 1.2 mm, and more preferably 0.3 to 1.0 mm. The shape can be various shapes such as circles, ellipses, ellipses, etc., triangles, quadrilateral polygons, stars, hearts, etc., fish, boats, airplanes, vegetables, fruits, bills, coins, etc. . You can also design the image of the building owner or business entity.
The surface may be a flat shape, an uneven shape, a protruding shape, or the like. This color metal decorative plate can be attached to any part of the wall surface. Above all, it is preferable to attach it to a part of the joint because the beauty effect is large.

カラー金属化粧板は、下側金属プレートと上側金属プレートを含み、上側金属プレートは下側金属プレートに比べて相対的に大きく形成するのが好ましい。これにより下側金属プレートの上に上側金属プレートを取り付けたときに、上側金属プレートが表面に見え、下側金属プレートは上側金属プレートの下に隠れて見えないようにする。上側金属プレートの表面側はカラー装飾した金属プレートとする。   The color metal decorative plate includes a lower metal plate and an upper metal plate, and the upper metal plate is preferably formed relatively larger than the lower metal plate. Thus, when the upper metal plate is mounted on the lower metal plate, the upper metal plate is visible on the surface, and the lower metal plate is hidden under the upper metal plate so that it cannot be seen. The surface side of the upper metal plate is a color-decorated metal plate.

下側金属プレートは壁面又は目地に固定し、下側金属プレートと上側金属プレートは互いに係止する係止部により固定するのが好ましい。一例として、下側金属プレートは中央部分の平坦部と、端には垂直方向に折れ曲がり部分を形成し、前記中央部分には固定ピンを挿入して固定する孔を備え、折れ曲がり部分には上側金属プレートの係止部と互いに係止する係止部を形成する。係止部は一例として係止爪がある。上側金属プレートは中央部分の平坦部と、端には垂直方向に折れ曲がり部分を形成し、折れ曲がり部分には係止部を形成する。外壁の目地に下側金属プレートの固定用孔から固定ピンを打って下側金属プレートを固定し、その上から上側金属プレートの係止部を前記下側金属プレートの係止部に引っ掛けることにより、カラー金属化粧板を固定する。   Preferably, the lower metal plate is fixed to a wall surface or a joint, and the lower metal plate and the upper metal plate are fixed by a locking portion that locks each other. As an example, the lower metal plate is formed with a flat portion at the center portion, a bent portion in the vertical direction at the end, and a hole for inserting and fixing a fixing pin in the central portion, and the upper metal plate at the bent portion. A locking portion that locks with the locking portion of the plate is formed. An example of the locking portion is a locking claw. The upper metal plate has a flat portion at the center portion and a bent portion in the vertical direction at the end, and a locking portion is formed in the bent portion. By fixing the lower metal plate by hitting a fixing pin from the fixing hole of the lower metal plate to the joint of the outer wall, and hooking the locking portion of the upper metal plate on the locking portion of the lower metal plate from above , Fix the color metal decorative board.

本発明の上塗り材は下記A液とB液を含み、
[A液]
(1)フルオロオレフィンとアルキルビニルエーテルの共重合体を含むフッ素樹脂
(2)親水性付与剤として、アルコキシル基の加水分解によるシラノール基を含むシラン系化合物、光触媒酸化チタン、アルカリシリケート系無機塗材、金属アルコキシド系無機材から選ばれる少なくとも一つの物質
(3)紫外線吸収剤
(4)溶剤
[B液]
(1)硬化剤
(2)溶剤
前記A液とB液を混合して上塗り材とし、ローラー塗装する。A液とB液の混合割合は、重量比でA液:B液=70〜95:30〜5が好ましく、さらに好ましくはA液:B液=75〜90:10〜25であり、とくに好ましくはA液:B液=80〜85:20〜15である。
The topcoat material of the present invention contains the following A liquid and B liquid,
[Liquid A]
(1) Fluororesin containing a copolymer of fluoroolefin and alkyl vinyl ether (2) As a hydrophilicity-imparting agent, a silane compound containing a silanol group by hydrolysis of an alkoxyl group, a photocatalytic titanium oxide, an alkali silicate inorganic coating material, At least one substance selected from metal alkoxide-based inorganic materials (3) UV absorber (4) Solvent [Liquid B]
(1) Curing agent (2) Solvent The A liquid and the B liquid are mixed to form a top coat material, and roller coating is performed. The mixing ratio of the A liquid and the B liquid is preferably A liquid: B liquid = 70 to 95:30 to 5, more preferably A liquid: B liquid = 75 to 90:10 to 25, particularly preferably. Is A liquid: B liquid = 80-85: 20-15.

(A)成分のフッ素樹脂のフルオロオレフィンは、テトラフルオロエチレン、クロロトリフルオロエチレンが好適に選ばれるが、併用することも可能である。前記フッ素樹脂の共重合割合は30〜70モル%が好ましい。アルキルビニルエーテル単量体は、CH2 =CRO(CH2n OH(RはHまたはCH3 、nは7〜18の整数)で表わされる水酸基含有長鎖アルキルビニルエーテルが好ましい。前記アルキルビニルエーテル単量体の共重合割合は5〜50モル%が好ましい。上記2成分の他に共重合可能なビニルモノマーが共重合されていても良い。さらに、水酸基と反応する官能基を有する硬化剤(D)を含み、(A)成分と(D)成分の合計に対し、(A)成分が50〜95重量%、(D)成分が5〜50重量%の割合で含有するのが好ましい。 The fluoroolefin of the fluororesin (A) component is preferably selected from tetrafluoroethylene and chlorotrifluoroethylene, but can also be used in combination. The copolymerization ratio of the fluororesin is preferably 30 to 70 mol%. The alkyl vinyl ether monomer is preferably a hydroxyl group-containing long-chain alkyl vinyl ether represented by CH 2 = CRO (CH 2 ) n OH (R is H or CH 3 , n is an integer of 7 to 18). The copolymerization ratio of the alkyl vinyl ether monomer is preferably 5 to 50 mol%. In addition to the two components, a copolymerizable vinyl monomer may be copolymerized. Furthermore, it contains a curing agent (D) having a functional group that reacts with a hydroxyl group, and (A) component is 50 to 95% by weight, and (D) component is 5 to It is preferable to contain in the ratio of 50 weight%.

(D)成分の硬化剤は、被膜の強度と耐久性を高く保持するために加える。この硬化剤は多価イソシアナート類などの常温硬化型のものが好ましい。多価イソシアナートとしては、ヘキサメチレンジイソシアナート、イソホロンジイソシアナート等の無黄変ジイソシアナート類ならびにその付加物が特に有用である。イソシアナート類を用いて常温硬化を行わせる場合には、ジブチルチンジラウレート等の硬化触媒の添加によって硬化を促進させることも可能である。(D)成分の硬化剤により、常温(0〜40℃程度)硬化させることができる。   The (D) component curing agent is added to keep the strength and durability of the coating film high. This curing agent is preferably a room temperature curing type such as polyvalent isocyanates. As the polyvalent isocyanate, non-yellowing diisocyanates such as hexamethylene diisocyanate and isophorone diisocyanate and adducts thereof are particularly useful. When normal temperature curing is performed using isocyanates, curing can be accelerated by adding a curing catalyst such as dibutyltin dilaurate. (D) It can harden at normal temperature (about 0-40 degreeC) with the hardening | curing agent of a component.

(B)成分の親水性付与剤は、上塗り(トップコート)被膜に親水性を与え、雨などの水により汚れ成分を洗い流し、常に美装状態を保つために混合する。この親水性付与剤は、アルコキシル基の加水分解によるシラノール基を含むシラン系化合物、光触媒酸化チタン、アルカリシリケート系無機塗材、金属アルコキシド系無機材から選ばれる少なくとも一つの物質を使用する。このうちアルコキシル基の加水分解によるシラノール基を含むシラン化合物を使用するのかさらに好ましい。シラン化合物としては、1分子中に平均2個以上のアルコキシシリル基、シラノール基およびアシロキシシリル基から選ばれる官能基を有するシラン化合物が好適に採用される。このようなシラン化合物は、シランカップリング剤、シラン系硬化剤、シリコーン系硬化剤、アルコキシシラン、シランアルコキサイドなどの名称で市販されている。親水性付与剤は(A)成分と(D)成分の合計量100重量部に対して5〜50重量部加えるのが好ましい。   The hydrophilicity-imparting agent of component (B) imparts hydrophilicity to the top coat (topcoat) film, and is washed away with water such as rain to mix the components so as to always maintain a beautiful appearance. This hydrophilicity imparting agent uses at least one substance selected from a silane compound containing a silanol group obtained by hydrolysis of an alkoxyl group, a photocatalytic titanium oxide, an alkali silicate inorganic coating material, and a metal alkoxide inorganic material. Of these, it is more preferable to use a silane compound containing a silanol group obtained by hydrolysis of an alkoxyl group. As the silane compound, a silane compound having a functional group selected from an average of two or more alkoxysilyl groups, silanol groups and acyloxysilyl groups in one molecule is suitably employed. Such silane compounds are commercially available under names such as silane coupling agents, silane curing agents, silicone curing agents, alkoxysilanes, and silane alkoxides. The hydrophilicity-imparting agent is preferably added in an amount of 5 to 50 parts by weight based on 100 parts by weight of the total amount of the component (A) and the component (D).

(C)成分の紫外線吸収剤は、紫外線を吸収し被膜の光劣化を防ぐために加える。一例としてベンゾトリアゾール系化合物(BASF(旧チバガイギー)社製、商品名“チヌビン900”)がある。この紫外線吸収剤には光安定剤(同社製、商品名“チヌビン144”)及び/又は表面調整剤(BYKケミー社製、商品名“BYK300”)を併用することもできる。紫外線吸収剤は(A)成分と(D)成分の合計量100重量部に対して0.1〜5重量部加えるのが好ましい。   Component (C), an ultraviolet absorber, is added to absorb ultraviolet rays and prevent photodegradation of the coating. As an example, there is a benzotriazole-based compound (BASF (formerly Ciba Geigy), trade name “Tinuvin 900”). A light stabilizer (manufactured by the company, trade name “TINUVIN 144”) and / or a surface conditioner (manufactured by BYK Chemie, trade name “BYK300”) can also be used in combination with the ultraviolet absorber. The ultraviolet absorber is preferably added in an amount of 0.1 to 5 parts by weight based on 100 parts by weight of the total amount of the component (A) and the component (D).

(E)成分の溶剤は上塗り材塗料の粘度を調整し、ローラー塗装しやすくするために加える。溶剤はトルエン、キシレン、ペンタン、ヘキサン、ヘプタン、ノナン、シクロヘキサン、ソルベッソ#100(エクソン社製)、ソルベッソ#150(エクソン社製)、スワゾール#1000(丸善石油化学社製)、スワゾール#1500(丸善石油化学社製)、スワゾール#1800(丸善石油化学社製)、メタノール、エタノール、プロパノール、ブタノール、イソブタノール、エチレングリコール、プロピレングリコール、ジエチレングリコール、ジプロピレングリコール、ジアセトンアルコール、メチルセロソルブ、セロソルブ、ブチルセロソルブ、セロソルブアセテート、エチルアセテート、ブチルアセテート、イソブチルアセテート、ベンゼン、メチルエチルケトン、メチルイソブチルケトン、イソホロン、シクロヘキサノン、エチルベンゼン、1,3,5-トリメチルベンゼン、高沸点芳香族ナフサなどがある。これらの溶剤は適宜混合して使用しても良い。溶剤は(A)成分と(D)成分の合計量100重量部に対して30〜200重量部加えるのが好ましい。   The solvent of component (E) is added to adjust the viscosity of the top coat and facilitate roller coating. Solvents are toluene, xylene, pentane, hexane, heptane, nonane, cyclohexane, Solvesso # 100 (manufactured by Exxon), Solvesso # 150 (manufactured by Exxon), Swazol # 1000 (manufactured by Maruzen Petrochemical Co., Ltd.), Swazol # 1500 (Maruzen) Petrochemical), Swazol # 1800 (Maruzen Petrochemical), methanol, ethanol, propanol, butanol, isobutanol, ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, diacetone alcohol, methyl cellosolve, cellosolve, butyl cellosolve , Cellosolve acetate, ethyl acetate, butyl acetate, isobutyl acetate, benzene, methyl ethyl ketone, methyl isobutyl ketone, isophorone, cyclohexanone, Ethylbenzene, 1,3,5-trimethylbenzene, and the like high boiling aromatic naphtha. These solvents may be appropriately mixed and used. The solvent is preferably added in an amount of 30 to 200 parts by weight based on 100 parts by weight of the total amount of the components (A) and (D).

上記上塗り材は、トウペ社製、商品名“ニューガーメットDC#500”として市販されている。この塗料を使用してローラー塗装する。ローラー塗装の利点は、外壁表面に凹凸があっても均一膜厚に塗装でき、塗装むらがなく、空気泡も含まず、塗装効率も高いためである。とくに吹き付け塗装による外壁に有効である。塗装後は常温(0〜40℃程度)硬化させる。   The top coating material is commercially available from Toupe under the trade name “New Garmet DC # 500”. This paint is used for roller coating. The advantage of roller coating is that even if there are irregularities on the outer wall surface, it can be applied with a uniform film thickness, there is no coating unevenness, no air bubbles are included, and the coating efficiency is high. It is especially effective for the outer wall by spray painting. After coating, it is cured at room temperature (about 0 to 40 ° C).

本発明の外壁には目地が存在し、前記目地内にはウレタンプレポリマーを可塑剤として含み、ブリードアウト成分を含まない湿気硬化性ウレタン組成物が一成分型シーリング材として充填されており、前記上塗り材を前記目地を含む外壁の上塗り塗装するのが好ましい。これにより、目地も外壁と同様に保護でき、耐用年数を伸ばすことができる。この目地材は、分子内に1〜3個の水酸基を有する(メタ)アクリル化合物またはそのオリゴマー、ポリオールおよび有機ポリイソシアネート化合物を反応させて得られるウレタンプレポリマーを可塑剤とする一成分型シーリング材である。このシーリング材は、オート化学工業社製、商品名“オートン超耐シーラーTF2000”として市販されている。   A joint exists in the outer wall of the present invention, and the joint contains a urethane prepolymer as a plasticizer and is filled with a moisture-curable urethane composition that does not contain a bleed-out component as a one-component sealant, It is preferable to coat the top coat material on the outer wall including the joint. Thereby, a joint can also be protected similarly to an outer wall, and a useful life can be extended. This joint material is a one-component sealing material using a urethane prepolymer obtained by reacting a (meth) acrylic compound having 1 to 3 hydroxyl groups in the molecule or an oligomer thereof, a polyol and an organic polyisocyanate compound as a plasticizer. It is. This sealant is commercially available as a product name “Auton Super Sealer TF2000” manufactured by Auto Chemical Industry Co., Ltd.

従来の一般的なシーリング材は、変性シリコーンなどのベースポリマーに可塑剤としてシリコーンオイルなどのブリードアウトしやすい成分が加えられていた。シーリング材から可塑剤がブリードアウトすると、ブリードアウト成分が外壁を汚す問題が発生したり、目地割れが発生して水漏れの原因になる問題があった。本発明は、数あるシーリング材から特定のものを選択したところに意義がある。このシーリング材はカラー金属化粧板の周囲にも充填する。これにより、カラー金属化粧板の取り付け部に雨水などが入り込まず、長期間安定して壁面もカラー金属化粧板も保持できる。   In a conventional general sealing material, a base polymer such as modified silicone has been added with a component that easily bleeds out such as silicone oil as a plasticizer. When the plasticizer bleeds out from the sealing material, there is a problem that the bleed-out component stains the outer wall, or there is a problem of causing joint leakage and causing water leakage. The present invention is significant when a specific material is selected from a number of sealing materials. This sealing material is also filled around the color metal decorative plate. Accordingly, rainwater or the like does not enter the attachment portion of the color metal decorative plate, and the wall surface and the color metal decorative plate can be held stably for a long period of time.

本発明の壁面は、骨材と合成樹脂を含む塗布材を吹き付け塗装した壁面である。この壁面はリシンガンなど使用した1色吹きの壁面であっても良いし、多色吹きした壁面であっても良い。好ましくは、骨材と合成樹脂を含み、無機粉体を含んでもよい塗布材を非混合多色状に塗装した天然石調壁面である。建築物には一般的にはタイル外壁が多いが、タイル外壁はタイル(陶磁器)とコンクリートとの熱膨張差が大きいことに起因して、タイルが剥離しやすい問題があり、10〜15年ごとにメンテナンス修理が必要であった。これに対して吹き付け壁面は剥離問題が無いことから好ましい。   The wall surface of the present invention is a wall surface that is spray-coated with an application material containing aggregate and synthetic resin. This wall surface may be a one-color blown wall surface using a ricin gun or the like, or a multi-color blown wall surface. Preferably, it is a natural stone-like wall surface that is coated with an unmixed multicolor coating material that includes aggregate and synthetic resin and may include inorganic powder. In general, there are many tile outer walls in buildings, but the tile outer walls have a problem that the tiles are easy to peel off due to the large difference in thermal expansion between the tiles (ceramics) and concrete, every 10 to 15 years Maintenance repair was necessary. On the other hand, the sprayed wall surface is preferable because there is no peeling problem.

本発明においては、好ましくは骨材と合成樹脂を含み、無機粉体を含んでもよい塗布材を使用する。前記において骨材とは、自然石、自然石に顔料を加えて焼き付けた焼付け骨材、セラミック、レンガ、陶磁器、鋼滓等を粉砕し、平均粒子径0.1〜5mm程度に篩分けして整えた粒子をいう。合成樹脂とは、アクリルエマルジョン塗料、ウレタン塗料等の耐光性の高い樹脂であり、塗装面にしたときにマトリックス樹脂になるものをいう。本発明では合成樹脂をマトリックス樹脂に使用するため、塗装面は地震等の震動を受けても破壊することはない。このため、タイル、レンガ、自然石等に比較して、地震の際に落下する危険性はきわめて低い。無機粉体は、例えばシリカ、タルク、クレイなどの自然界に存在する鉱物粉体であり、前記骨材よりは細かい平均粒子に篩分けして調製する。塗布材には、その他増粘剤、pH調整剤、消泡剤、造膜助剤、水及び/又は溶剤を加えてもよい。   In the present invention, a coating material that preferably contains an aggregate and a synthetic resin and may contain an inorganic powder is used. In the above, the aggregate is a natural stone, a baked aggregate obtained by adding a pigment to natural stone, ceramic, bricks, ceramics, steel slag, etc., and sieved to an average particle size of about 0.1 to 5 mm. It refers to arranged particles. Synthetic resins are resins having high light resistance such as acrylic emulsion paints and urethane paints, which become matrix resins when applied to a painted surface. In the present invention, since the synthetic resin is used for the matrix resin, the painted surface is not destroyed even when subjected to vibration such as an earthquake. For this reason, compared with tiles, bricks, natural stones, etc., the risk of falling during an earthquake is extremely low. The inorganic powder is a mineral powder existing in nature such as silica, talc and clay, and is prepared by sieving into finer average particles than the aggregate. Other thickeners, pH adjusters, antifoaming agents, film-forming aids, water and / or solvents may be added to the coating material.

骨材と合成樹脂と水及び/又は溶剤を含み、無機粉体を含んでもよい塗布材は、多頭式スプレーガンを使用して、建築物壁面又は壁面になるパネル等に非混合多色状に塗布する。多頭式スプレーガンは、例えば前記特許文献1又は特公平6−61494号公報に開示されている塗装ガンを使用する。この多頭式スプレーガンは、多色塗材を別々のタンクから別々に圧縮空気と共に弾となって塗布することができ、塗装面は非混合多色状に塗布され、天然石調に形成される。この塗装面の表面は凹凸部を含むので、凸部(突出部)の少なくとも一部は研磨ないしは研削により平面状に形成する。研磨ないしは研削面は、全体の5〜50%とすることが好ましい。このようにすると、自然石のいわゆるバーナー仕上げ面となる。バーナー仕上げとは、大理石や御影石などの自然石の表面に水をまき、火炎バーナーで加熱することにより、石の表面に急激な膨張を起こして破砕させ、表面を荒らして細かい凹凸面とする仕上げ方法である。   The coating material that contains aggregate, synthetic resin, water and / or solvent, and may contain inorganic powder, is made into a non-mixed multicolored form on the building wall or the panel that becomes the wall using a multi-head spray gun. Apply. The multi-head spray gun uses, for example, a coating gun disclosed in Patent Document 1 or Japanese Patent Publication No. 6-61494. This multi-head spray gun can apply a multicolor coating material as a bullet with compressed air separately from different tanks, and the painted surface is applied in a non-mixed multicolored form to form a natural stone tone. Since the surface of the painted surface includes an uneven portion, at least a part of the convex portion (projecting portion) is formed into a flat shape by polishing or grinding. The polished or ground surface is preferably 5 to 50% of the whole. If it does in this way, it will become a so-called burner finish surface of natural stone. Burner finish is a surface of natural stone such as marble or granite that is watered and heated with a flame burner to cause rapid expansion of the surface of the stone and crush it, roughing the surface to a fine uneven surface. Is the method.

本発明において上塗り材は2回塗りするのが好ましい。これにより上塗り材(トップコート)をむらなく塗れ、長期間メンテフリーが達成できる。また、前記上塗り材にはさらに溶剤を添加して粘度35〜55センチポイズ(23℃,BL型,回転数60rpm)に調整して塗装するのが好ましい。これにより均一膜厚に塗装でき、塗装効率もよくなる。   In the present invention, the top coat material is preferably applied twice. As a result, the top coating material (top coat) can be applied evenly, and maintenance-free can be achieved for a long time. Further, it is preferable that the top coating material is further coated with a solvent to adjust the viscosity to 35 to 55 centipoise (23 ° C., BL type, rotation speed 60 rpm). As a result, coating can be performed with a uniform film thickness, and the coating efficiency is improved.

前記上塗り材の塗装量は、乾燥後の固形分で50〜200g/mの範囲が好ましく、80〜150g/mの範囲がさらに好ましい。これにより長期間のメンテフリーが達成できる。 The coating amount of the top coating material is preferably in the range of 50 to 200 g / m 2 and more preferably in the range of 80 to 150 g / m 2 in terms of the solid content after drying. Thereby, long-term maintenance-free can be achieved.

以下実施例を用いて、本発明をさらに具体的に説明する。なお、本発明は下記の実施例に限定されるものではない。下記の図面において、同一符号は同一物を示す。   Hereinafter, the present invention will be described more specifically with reference to examples. In addition, this invention is not limited to the following Example. In the following drawings, the same symbols indicate the same items.

(各特性の測定試験方法)
(1)サンシャインウェザーメーターによる促進耐候性試験
(a)試験機:スガ試験機社製、型番“WE−SUN−HC−DC”
(b)光源:1灯式・セリウム入り有芯カーボンを上下各4本組み合わせ
(c)光線波長:280〜400nm
(d)放射照度:フィルター付き255±45W/m、フィルターなし285±50W/m
(e)光フィルター:耐熱性光学ガラス板使用・8枚1組、255nm以下の短波長成分をカット、3(f)55nmまでの成分を10〜50%透過
(g)放出電力:50V、60A(3000W)
(h)雰囲気温度:63±3℃
(i)シャワー:120分中18分間降雨先降り運転
(j)スプレー水量:2100±100ml/min(pH6.0〜8.0、水温16±5℃)
(k)試料枚数:70×150mm、76枚
(l)運転サイクル:60Hr
(2)光沢
前記サンシャインウェザーメーターによる促進試験後の外壁(目地を含む)とカラー金属化粧板の表面を目視により観察し、次のように評価した。
A:当初と変わらない
B:当初の光沢より劣る
(3)ひび割れ有無
前記サンシャインウェザーメーターによる促進試験後の外壁(目地を含む)とカラー金属化粧板の表面を目視により観察し、次のように評価した。
A:ひび割れなし
B:僅かにひび割れあり、補修必要
C:大きなひび割れあり、補修必要
(4)変色
前記サンシャインウェザーメーターによる促進試験後の外壁(目地を含む)とカラー金属化粧板の表面を目視により観察し、次のように評価した。
A:変色なし
B:変色あるが実用的に問題ない程度で目立たない、補修不要
C:やや目立つ変色、補修必要
D:明らかに変色しており、補修必要
(Measurement test method for each characteristic)
(1) Accelerated weather resistance test with sunshine weather meter
(a) Testing machine: Model number “WE-SUN-HC-DC” manufactured by Suga Test Instruments Co., Ltd.
(b) Light source: 1 lamp type, cerium-filled cored carbon combined with 4 each
(c) Light wavelength: 280-400 nm
(d) Irradiance: 255 ± 45 W / m 2 with filter, 285 ± 50 W / m 2 without filter
(e) Optical filter: Heat-resistant optical glass plate used. 1 set of 8 cuts short wavelength components of 255 nm or less, 3 (f) 10-50% transmission of components up to 55 nm
(g) Emission power: 50V, 60A (3000W)
(h) Atmospheric temperature: 63 ± 3 ° C
(i) Shower: Driving for 18 minutes during 120 minutes
(j) Spray water amount: 2100 ± 100 ml / min (pH 6.0 to 8.0, water temperature 16 ± 5 ° C.)
(k) Number of samples: 70 × 150 mm, 76
(l) Operation cycle: 60 hours
(2) Gloss The outer wall (including joints) and the surface of the color metal decorative plate after the acceleration test by the sunshine weather meter were visually observed and evaluated as follows.
A: No change from the original B: Inferior to the original gloss (3) Presence or absence of cracks The outer wall (including joints) and the surface of the color metal decorative plate after the accelerated test by the sunshine weather meter were visually observed, as follows: evaluated.
A: No crack B: Slightly cracked, repair required C: Large crack, repair required (4) Discoloration Visual observation of the outer wall (including joints) and the surface of the color metal decorative plate after the accelerated test by the sunshine weather meter Observed and evaluated as follows.
A: No discoloration B: Discoloration but inconspicuous to the extent that there is no practical problem, no repair needed C: Some noticeable discoloration, repair required D: Clearly discolored, repair required

(実施例1)
(1)カラー金属化粧板の作成
図1〜3に示すカラー金属化粧板をプレス加工により作成した。図1A−Bに示す下側金属プレート30は、厚み0.5mmのステンレスSUS304プレートとし、縦、横各148.4mm、端部の折り曲げ部の高さ8.5mmとした。中央の平坦部には直径6.8mmの固定ピン取り付け孔31を開け、折り曲げ部には係止部32を8か所設けた。図2A−Bに示す上側金属プレート33は、厚み0.8mmの着色ステンレスSUS304プレートとし、縦、横各150.0mm、端部の折り曲げ部の高さ2.35mmとした。折り曲げ部には係止部34を8か所設けた。上側金属プレート33は蒸着により、ゴールドに着色されている。図3は下側金属プレート30に上側金属プレート33を組み合わせたカラー金属化粧板35の側面図である。係止部32と係止部34が互いに係止し固定される。
Example 1
(1) Creation of a color metal decorative board The color metal decorative board shown in FIGS. 1-3 was produced by press work. The lower metal plate 30 shown in FIGS. 1A and 1B is a stainless steel SUS304 plate having a thickness of 0.5 mm, and has a vertical and horizontal length of 148.4 mm, and a bent portion height of 8.5 mm. A fixed pin mounting hole 31 having a diameter of 6.8 mm was formed in the flat portion at the center, and eight locking portions 32 were provided in the bent portion. The upper metal plate 33 shown in FIGS. 2A and 2B is a colored stainless steel SUS304 plate having a thickness of 0.8 mm, and has a length and width of 150.0 mm each, and a height of the bent portion at the end is 2.35 mm. Eight engaging portions 34 were provided in the bent portion. The upper metal plate 33 is colored gold by vapor deposition. FIG. 3 is a side view of a color metal decorative plate 35 in which the lower metal plate 30 and the upper metal plate 33 are combined. The locking part 32 and the locking part 34 are locked and fixed to each other.

(2)吹き付け塗装
吹き付け材としては、次の成分に調合したものを用いた。
(a)骨材 61.60重量部
(b)アクリルエマルジョン(固形分50%) 25.20重量部
(c)増粘剤(ヒドロキシメチルセルロース) 11.35重量部
(d)pH調整剤(アンモニア水) 0.17重量部
(e)消泡剤(アルコール系) 0.03重量部
(f)造膜助剤(アルコール系) 0.39重量部
(g)水 1.26重量部
作業性や貯蔵の便のために増粘剤、pH調整剤、消泡剤、造膜助剤等が混入されている。ここで、造膜助剤とは、エマルジョンの透明造膜の温度を下げるためのものである。
(2) Spray painting As the spray material, the one prepared in the following components was used.
(A) Aggregate 61.60 parts by weight
(B) Acrylic emulsion (solid content 50%) 25.20 parts by weight
(C) Thickener (hydroxymethylcellulose) 11.35 parts by weight
(D) pH adjuster (ammonia water) 0.17 parts by weight
(E) Defoamer (alcohol) 0.03 parts by weight
(F) Film-forming aid (alcohol) 0.39 parts by weight
(G) Water 1.26 parts by weight Thickeners, pH adjusters, antifoaming agents, film-forming aids and the like are mixed for workability and storage convenience. Here, the film-forming aid is for lowering the temperature of the transparent film-forming of the emulsion.

骨材としては、白色骨材は寒水石等の自然石を粉砕したもの、黒色は黒曜石等の自然石を粉砕したもの、灰色は寒水石を粉砕したものと黒曜石を粉砕したものを混合して使用した。骨材の粒度分布は、建築物用壁装材の模様の表現によって自由に選択することができるが、その強度や美観から、次の表1に示す粒度分布のものを採用した。表1において、メッシュとは1インチ(25.4mm)あたりの篩目の数をいう。なお、骨材の色は目的により様々のものを使用でき、骨材も焼付け骨材、セラミックスなどさまざまなものを使用できる。   As for the aggregate, white aggregate is a mixture of natural stones such as cryolite, black is a mixture of natural stones such as obsidian, and gray is a mixture of cryogenic stones and obsidian. used. The particle size distribution of the aggregate can be freely selected depending on the expression of the pattern of the wall covering material for buildings. From the strength and aesthetic appearance, the particle size distribution shown in the following Table 1 was adopted. In Table 1, mesh means the number of meshes per inch (25.4 mm). Various aggregate colors can be used depending on the purpose, and various aggregates such as baked aggregate and ceramics can be used.

Figure 0005748375
Figure 0005748375

図4は本発明の一実施例における吹き付け塗装方法で使用した3頭式スプレーガンを示す斜視図である。この3頭式スプレーガン12には、3つのタンク1、2、3が設けられており、タンク上部の全体は矩形(直方体形状)である。各タンク1、2、3に色の異なる第1〜第3の吹き付け材7、8、9をそれぞれ別々に収容する。また、タンク1、2、3の下部はテーパー状に細くなっており、一番下の部分にそれぞれ別個に噴射ノズル4、5、6が設けられている。タンク1、2、3内の第1〜第3の吹き付け材7、8、9は、圧縮空気によって噴射ノズル4、5、6からそれぞれ弾(たま)状に噴出させる。噴射ノズル4、5、6の口径はそれぞれ12mm、10mm、6mmであり、第1の吹き付け材(白色)7、第2の吹き付け材(灰色)8、第3の吹き付け材(黒色)9の吐出量比は5:4:1である。この3頭式スプレーガン12には、取っ手10,11がノズルの横に付いており、この取っ手10,11には、圧縮空気を高圧状態(2.0気圧)から低圧状態(1.0気圧)に(及び低圧状態から高圧状態に)切り替えるための切り替えスイッチ(図示せず)が設けられている。   FIG. 4 is a perspective view showing a three-head spray gun used in the spray coating method in one embodiment of the present invention. The three-head spray gun 12 is provided with three tanks 1, 2, and 3, and the entire upper portion of the tank is rectangular (a rectangular parallelepiped shape). The first, second and third spray materials 7, 8 and 9 having different colors are accommodated in the tanks 1, 2 and 3, respectively. Further, the lower portions of the tanks 1, 2, and 3 are tapered, and spray nozzles 4, 5, and 6 are separately provided at the lowermost portions. The first to third spray materials 7, 8, 9 in the tanks 1, 2, 3 are ejected from the spray nozzles 4, 5, 6 in a bullet shape by compressed air. The nozzles 4, 5, and 6 have a diameter of 12 mm, 10 mm, and 6 mm, respectively, and discharge of the first spray material (white) 7, the second spray material (gray) 8, and the third spray material (black) 9. The quantitative ratio is 5: 4: 1. The three-head spray gun 12 has handles 10 and 11 attached to the side of the nozzle. The handles 10 and 11 are supplied with compressed air from a high pressure state (2.0 atm) to a low pressure state (1.0 atm). ) (And a switching switch (not shown) for switching from a low pressure state to a high pressure state).

図5は本発明の一実施例における吹き付け塗装方法を示す説明図である。建築物用パネル13は、縦150mm、横70mm、厚さ3mmの繊維補強樹脂板を使用した。建築物用パネル13の表面には目地となる部分に目地ダミー材24(ポリエチレン発泡シートの表面に粘着剤を一体化したもの)を貼り付けておいた。噴射ノズル4、5、6からそれぞれ弾状に噴出させた噴射物14,15,16を建築物外壁用パネル13に塗装し、乾燥することにより基材層17を得た。この基材層のままでも塗布材は非混合多色状に塗布されており、天然石調壁面であった。   FIG. 5 is an explanatory view showing a spray coating method in one embodiment of the present invention. As the building panel 13, a fiber reinforced resin plate having a length of 150 mm, a width of 70 mm, and a thickness of 3 mm was used. On the surface of the building panel 13, a joint dummy material 24 (one obtained by integrating a pressure-sensitive adhesive on the surface of a polyethylene foam sheet) was attached to a joint portion. The jets 14, 15, and 16 ejected in a bullet shape from the jet nozzles 4, 5, and 6, respectively, were applied to the building outer wall panel 13 and dried to obtain a base material layer 17. Even with this base material layer, the coating material was applied in an unmixed multicolored form, and was a natural stone-like wall surface.

図6Aは得られた基材層17の拡大断面図である。建築物外壁13に塗装された基材層は、全体が大きな凹凸表面となっており、研磨線矢印19に沿って凸部18をプレートサンダーにより研磨した。図6Bは研磨した後の基材層17の拡大断面図である。基材層17は、研磨により平面部分20と凹部21となり、平面部分20があることにより、天然石のバーナー仕上げに近い表面形態となった。基材層17の厚さは約2mmであった。   FIG. 6A is an enlarged cross-sectional view of the obtained base material layer 17. The base material layer painted on the building outer wall 13 has a large uneven surface as a whole, and the protrusion 18 was polished by a plate sander along the polishing line arrow 19. FIG. 6B is an enlarged cross-sectional view of the base material layer 17 after polishing. The base material layer 17 became a flat surface portion 20 and a concave portion 21 by polishing, and due to the presence of the flat surface portion 20, the surface shape was close to the burner finish of natural stone. The thickness of the base material layer 17 was about 2 mm.

図6Bに示すように、目地ダミー材24を剥離し、溝となった部分にシーリング材25を充填した。このシーリング材は一成分型である市販のオート化学工業社製、商品名“オートン超耐シーラーTF2000”(以下「ウレタン組成物」とも言う)を用いた。   As shown in FIG. 6B, the joint dummy material 24 was peeled off, and the sealing material 25 was filled in the groove portion. As the sealing material, a one-component commercial product manufactured by Auto Chemical Industry Co., Ltd., trade name “Auton Super Sealer TF2000” (hereinafter also referred to as “urethane composition”) was used.

得られた壁面にカラー金属化粧板35を取り付けた。図7に示すように下側金属プレートの固定ピン取り付け孔に固定ピン36をねじ込み、まず下側金属プレートを固定し、次に下側金属プレートの上に上側金属プレートを乗せて押し込み、互いの係止部を係止させることにより固定した。次いで前記シーリング材37をカラー金属化粧板35の周囲に充填した。   A color metal decorative plate 35 was attached to the obtained wall surface. As shown in FIG. 7, the fixing pin 36 is screwed into the fixing pin mounting hole of the lower metal plate, the lower metal plate is first fixed, and then the upper metal plate is put on the lower metal plate and pushed into each other. It was fixed by locking the locking part. Next, the sealing material 37 was filled around the color metal decorative plate 35.

その後、基材層17とシーリング材25,37とカラー金属化粧板35の表面に、ローラー塗装具26を用いて上塗り塗装を2回実施した。1回目の上塗り塗装は常温(25℃)で24時間硬化させた。図8は研磨後の基材層の表面に上塗り塗装の2回目を実施している断面説明図である。上塗り材は市販のトウペ社製、商品名“ニューガーメットDC#500”を用い、A液とB液を重量比でA液:B液=83:17の割合で混合し、この混合物100重量部に対してエチルベンゼン24重量部、1,3,5-トリメチルベンゼン5重量部、トルエン38重量部、キシレン24重量部、高沸点芳香族ナフサ9重量部の混合溶剤を15重量部加えて粘度50センチポイズ(23℃,BL型,回転数60rpm)に調整し、上塗り材の塗装量は、乾燥後の固形分で100g/mとした。得られた天然石調塗装物27は、サンシャインウェザーメーターによる促進試験で10000時間(50年に相当)までは、ひび割れやクラックはなく、耐久性のあることが確認できた。シーリング材からのブリードアウト汚れもなかった。結果はまとめて表2に示す。また紫外線透過試験において、図10に示すように320〜380nmの紫外線を99%カットし、透過部分は1%であった。 Thereafter, top coating was performed twice on the surface of the base material layer 17, the sealing materials 25 and 37, and the color metal decorative plate 35 using the roller coating tool 26. The first overcoating was cured at room temperature (25 ° C.) for 24 hours. FIG. 8 is a cross-sectional explanatory view in which the second overcoating is performed on the surface of the substrate layer after polishing. The top coat material is a product name “New Garmet DC # 500” manufactured by Toupe Co., Ltd., and A liquid and B liquid are mixed at a weight ratio of A liquid: B liquid = 83: 17. 15 parts by weight of a mixed solvent of 24 parts by weight of ethylbenzene, 5 parts by weight of 1,3,5-trimethylbenzene, 38 parts by weight of toluene, 24 parts by weight of xylene, and 9 parts by weight of high-boiling aromatic naphtha are added to a total of 50 parts by weight. It was adjusted to centipoise (23 ° C., BL type, rotation speed 60 rpm), and the coating amount of the top coating material was 100 g / m 2 in terms of solid content after drying. The obtained natural stone-like coated product 27 was confirmed to be durable without cracks or cracks up to 10,000 hours (equivalent to 50 years) in an accelerated test using a sunshine weather meter. There was no bleed-out stain from the sealing material. The results are summarized in Table 2. Moreover, in the ultraviolet-ray transmission test, as shown in FIG. 10, 99% of 320-380 nm ultraviolet rays were cut, and the transmission part was 1%.

(実施例2)
上塗り材を1回塗りとした以外は実施例1と同様に実験した。得られた塗装物は、サンシャインウェザーメーターによる促進試験で9000時間(45年に相当)までは、ひび割れやクラックはなく、耐久性のあることが確認できた。シーリング材からのブリードアウト汚れもなかった。結果はまとめて表2に示す。
(Example 2)
An experiment was conducted in the same manner as in Example 1 except that the top coating material was applied once. The obtained coated product was confirmed to be durable with no cracks or cracks until 9000 hours (equivalent to 45 years) in an accelerated test using a sunshine weather meter. There was no bleed-out stain from the sealing material. The results are summarized in Table 2.

Figure 0005748375
Figure 0005748375

図9は建築物の外壁にカラー金属化粧板35を取り付けて上塗り塗装をした後の仕上げ状態を示す外面図である。基材層27は御影石などの天然石調の模様を有し、目地25を備え、目地25の交差した位置にカラー金属化粧板35が取り付けられている。カラー金属化粧板35の色調はゴールドであった。カラー金属化粧板35は他の外壁部から突出した外観を有し、凹凸感があり、立体模様や立体形状が強調され、美観の高い外壁塗装方法であることが確認できた。   FIG. 9 is an external view showing a finished state after the color metal decorative plate 35 is attached to the outer wall of the building and the top coat is applied. The base material layer 27 has a natural stone-like pattern such as granite, has a joint 25, and a color metal decorative plate 35 is attached at a position where the joint 25 intersects. The color tone of the color metal decorative plate 35 was gold. It was confirmed that the color metal decorative plate 35 had an appearance protruding from other outer wall portions, had an unevenness, emphasized a three-dimensional pattern and a three-dimensional shape, and was a highly beautiful outer wall coating method.

(実施例3)
図11は本発明の別の実施例の仕上げ状態を示す模式的断面図である。カラー金属化粧板の下側金属プレート39をビス36で壁面13に固定し、その上に上側金属プレート40を被せて固定ツメ41で固定し、周囲にシーリング材37を充填し、上塗り材38を塗装した以外は実施例1と同様に実施した。このカラー金属化粧板も他の外壁部から突出した外観を有し、凹凸感があり、立体模様や立体形状が強調され、美観の高く、耐久性も高いことが確認できた。
(Example 3)
FIG. 11 is a schematic cross-sectional view showing a finished state of another embodiment of the present invention. The lower metal plate 39 of the color metal decorative plate is fixed to the wall surface 13 with screws 36, and the upper metal plate 40 is placed thereon and fixed with the fixing claws 41, the sealing material 37 is filled around, and the top coating material 38 is applied. The same procedure as in Example 1 was performed except that the coating was performed. It was confirmed that this color metal decorative board also had an appearance protruding from the other outer wall part, had a feeling of unevenness, emphasized a three-dimensional pattern and a three-dimensional shape, high aesthetics and high durability.

本発明は一般の建築物、ビル、マンション、工場、事務所などの外壁に好適である。とくに集合住宅(マンション)などで通常行われている10〜15年ごとの大規模修繕工事を大幅に延長することができ、修繕管理コストを大幅に低下することができる。   The present invention is suitable for outer walls of general buildings, buildings, condominiums, factories, offices and the like. Particularly, large-scale repair work every 10 to 15 years that is normally performed in an apartment house (apartment) can be greatly extended, and the repair management cost can be greatly reduced.

1,2,3 タンク
4,5,6 噴射ノズル
7,8,9 吹き付け材
10,11 取っ手
12 3頭式スプレーガン
13 建築物用パネル
14,15,16 噴射物
17 基材層
18 凸部
19 研磨線
20 平面部分
21 凹部
22 上塗り第1層
23 上塗り第2層
24 目地ダミー材
25 目地シーリング材
26 ローラー塗装具
27 天然石調塗装物
30,39 下側金属プレート
31 固定ピン取り付け孔
32,34 係止部
33,40 上側金属プレート
35 カラー金属化粧板
36 固定ピン
37 カラー金属化粧板用シーリング材
38 上塗り材
41 固定ツメ
1, 2, 3 Tank 4, 5, 6 Spray nozzle 7, 8, 9 Spraying material 10, 11 Handle 12 Three-head spray gun 13 Building panel 14, 15, 16 Spray 17 Base material layer 18 Projection 19 Polishing line 20 Plane portion 21 Recess 22 Top coat first layer 23 Top coat second layer 24 Joint dummy material 25 Joint sealant 26 Roller coating tool 27 Natural stone-like paint 30, 39 Lower metal plate 31 Fixing pin attachment holes 32, 34 Stop portions 33, 40 Upper metal plate 35 Color metal decorative plate 36 Fixing pin 37 Sealing material 38 for color metal decorative plate Top coating material 41 Fixed claw

Claims (9)

建築物の外壁塗装方法であって、
骨材と合成樹脂を含む塗布材を吹き付け塗装した壁面の一部にカラー金属化粧板を取り付け、前記カラー金属化粧板の周囲にウレタンプレポリマーを可塑剤として含む湿気硬化性ウレタン組成物をシーリング材として充填し、
前記壁面及びカラー金属化粧板の表面から上塗り材を塗装することを特徴とする外壁塗装方法。
A method for painting an outer wall of a building,
A color metal decorative plate is attached to a part of the wall surface, which is coated by spraying a coating material containing aggregate and synthetic resin, and a moisture curable urethane composition containing a urethane prepolymer as a plasticizer is sealed around the color metal decorative plate. As filling and
An outer wall coating method, wherein a top coating material is applied from the surfaces of the wall surface and the color metal decorative plate.
前記カラー金属化粧板は、下側金属プレートと上側金属プレートを含み、前記上側金属プレートは前記下側金属プレートに比べて相対的に大きく、
前記上側金属プレートの表面側はカラー装飾した金属プレートであり、
前記下側金属プレートは前記壁面又は目地に固定し、
前記下側金属プレートと前記上側金属プレートは互いに係止する係止部により固定する請求項1に記載の外壁塗装方法。
The color metal decorative plate includes a lower metal plate and an upper metal plate, and the upper metal plate is relatively larger than the lower metal plate,
The surface side of the upper metal plate is a color-decorated metal plate,
The lower metal plate is fixed to the wall surface or joint,
The outer wall coating method according to claim 1, wherein the lower metal plate and the upper metal plate are fixed by a locking portion that locks each other.
前記カラー金属化粧板はステンレス製であり、上側金属プレートの表面側は蒸着、スパッタリング、イオンプレーティング及びメッキから選ばれるいずれかの手段でカラー装飾されている請求項1又は2に記載の外壁塗装方法。   3. The exterior wall coating according to claim 1, wherein the color metal decorative plate is made of stainless steel, and the surface side of the upper metal plate is color-decorated by any means selected from vapor deposition, sputtering, ion plating, and plating. Method. 前記カラー金属化粧板は、前記目地の一部に取り付ける請求項1〜3のいずれかに記載の外壁塗装方法。   The said color metal decorative board is an outer wall coating method in any one of Claims 1-3 attached to a part of said joint. 前記壁面は、骨材と合成樹脂を含み、無機粉体を含んでもよい塗布材を非混合多色状に吹き付け塗装した天然石調壁面である請求項1〜4のいずれかに記載の外壁塗装方法。   The outer wall coating method according to any one of claims 1 to 4, wherein the wall surface is a natural stone-like wall surface that includes an aggregate and a synthetic resin and is spray-coated with an unmixed multicolor coating material that may include an inorganic powder. . 前記上塗り材は下記A液とB液を含み、
[A液]
(1)フルオロオレフィンとアルキルビニルエーテルの共重合体を含むフッ素樹脂
(2)親水性付与剤として、アルコキシル基の加水分解によるシラノール基を含むシラン系化合物、光触媒酸化チタン、アルカリシリケート系無機塗材、金属アルコキシド系無機材から選ばれる少なくとも一つの物質
(3)紫外線吸収剤
(4)溶剤
[B液]
(1)硬化剤
(2)溶剤
前記A液とB液を混合して上塗り材とする請求項1〜5のいずれかに記載の外壁塗装方法。
The top coating material includes the following A liquid and B liquid,
[Liquid A]
(1) Fluororesin containing a copolymer of fluoroolefin and alkyl vinyl ether (2) As a hydrophilicity-imparting agent, a silane compound containing a silanol group by hydrolysis of an alkoxyl group, a photocatalytic titanium oxide, an alkali silicate inorganic coating material, At least one substance selected from metal alkoxide-based inorganic materials (3) UV absorber (4) Solvent [Liquid B]
(1) Curing agent (2) Solvent The outer wall coating method according to any one of claims 1 to 5, wherein the liquid A and the liquid B are mixed to obtain a top coating material.
前記上塗り材は2回塗りする請求項1〜6のいずれか1項に記載の外壁塗装方法。   The outer wall coating method according to claim 1, wherein the top coat material is applied twice. 前記上塗り材にはさらに溶剤を添加して粘度35〜55センチポイズ(23℃,BL型,回転数60rpm)に調整して塗装する請求項1〜7のいずれか1項に記載の外壁塗装方法。   The exterior coating method according to any one of claims 1 to 7, wherein a solvent is further added to the top coating material to adjust the viscosity to 35 to 55 centipoise (23 ° C, BL type, rotation speed 60 rpm). 前記上塗り材の塗装量は、乾燥後の固形分で50〜200g/mの範囲である請求項1〜8のいずれか1項に記載の外壁塗装方法。 The outer wall coating method according to any one of claims 1 to 8, wherein a coating amount of the top coating material is in a range of 50 to 200 g / m 2 in terms of solid content after drying.
JP2014068997A 2014-03-28 2014-03-28 Exterior wall painting method Expired - Fee Related JP5748375B1 (en)