JP5594835B2 - Alignment film material and liquid crystal display device - Google Patents

Alignment film material and liquid crystal display device Download PDF

Info

Publication number
JP5594835B2
JP5594835B2 JP2010233973A JP2010233973A JP5594835B2 JP 5594835 B2 JP5594835 B2 JP 5594835B2 JP 2010233973 A JP2010233973 A JP 2010233973A JP 2010233973 A JP2010233973 A JP 2010233973A JP 5594835 B2 JP5594835 B2 JP 5594835B2
Authority
JP
Japan
Prior art keywords
compound
liquid crystal
group
alignment
atom
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2010233973A
Other languages
Japanese (ja)
Other versions
JP2011022612A (en
Inventor
正樹 松森
冨岡  安
茂 松山
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Panasonic Liquid Crystal Display Co Ltd
Japan Display Inc
Original Assignee
Panasonic Liquid Crystal Display Co Ltd
Japan Display Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Panasonic Liquid Crystal Display Co Ltd, Japan Display Inc filed Critical Panasonic Liquid Crystal Display Co Ltd
Priority to JP2010233973A priority Critical patent/JP5594835B2/en
Publication of JP2011022612A publication Critical patent/JP2011022612A/en
Application granted granted Critical
Publication of JP5594835B2 publication Critical patent/JP5594835B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は、光配向法を適用する配向膜材料とこの配向膜材料を用いて形成した配向膜を備えた液晶表示装置に関する。   The present invention relates to an alignment film material to which a photo-alignment method is applied and a liquid crystal display device including an alignment film formed using the alignment film material.

通常、液晶表示装置の表示は、一対の基板間に挟まれた液晶層の液晶分子に電界を印加することにより液晶分子の配向方向を変化させ、それにより生じた液晶層の光学特性の変化により行われる。   Normally, the display of a liquid crystal display device changes the alignment direction of the liquid crystal molecules by applying an electric field to the liquid crystal molecules of the liquid crystal layer sandwiched between a pair of substrates, and the resulting change in the optical characteristics of the liquid crystal layer. Done.

従来、画素毎に薄膜トランジスタ等のスイッチング素子を備えた、所謂アクティブ駆動型液晶表示装置は、液晶層を挟持する一対の基板のそれぞれに電極を設け、液晶層に印加する電界の方向が基板界面に対してほぼ垂直になるように設定され、液晶層を構成する液晶分子の光旋光性を利用して表示を行うツイステッドネマチック(Twisted Nematic:TN)表示方式に代表される。このTN方式の液晶表示装置においては視野角が狭いことが最大の課題とされている。   Conventionally, a so-called active drive type liquid crystal display device having a switching element such as a thin film transistor for each pixel is provided with electrodes on each of a pair of substrates sandwiching the liquid crystal layer, and the direction of the electric field applied to the liquid crystal layer is at the substrate interface. The display is represented by a twisted nematic (TN) display method which is set so as to be substantially perpendicular to the liquid crystal and performs display using the optical rotation of liquid crystal molecules constituting the liquid crystal layer. In this TN type liquid crystal display device, a narrow viewing angle is the biggest problem.

一方、一対の基板の一方に形成した櫛歯電極を用いて発生する電界が当該基板面にほぼ平行な成分を有するようにして液晶層を構成する液晶分子をほぼ基板と平行な面内で回転動作させ、液晶層の複屈折性を用いて表示を行うIPS方式が、下記特許文献1、特許文献2等に開示されている。このIPS方式は液晶分子の面内スイッチングに起因して従来のTN方式に比べて視野角が広く、低負荷容量である、などの利点があり、TN方式に代わる新たな液晶表示装置として有望視され近年急速に進歩している。   On the other hand, the liquid crystal molecules constituting the liquid crystal layer are rotated in a plane substantially parallel to the substrate so that the electric field generated using the comb electrode formed on one of the pair of substrates has a component substantially parallel to the substrate surface. An IPS system that operates and performs display using the birefringence of a liquid crystal layer is disclosed in the following Patent Document 1, Patent Document 2, and the like. This IPS system has advantages such as a wider viewing angle and lower load capacity than the conventional TN system due to in-plane switching of liquid crystal molecules, and it is promising as a new liquid crystal display device replacing the TN system. In recent years, it has made rapid progress.

なお、下記特許文献1には、スペーサビーズと液晶層との間に、偏光照射により液晶配向能を付与する材料を用いて配向膜を形成することによって、コントラストを320とした液晶表示装置が記載され、また、下記特許文献2には、直線偏光を高分子膜に照射する配向方法によりコントラストを250とした液晶表示装置が記載されている。   Patent Document 1 listed below describes a liquid crystal display device having a contrast of 320 by forming an alignment film between a spacer bead and a liquid crystal layer using a material that imparts liquid crystal alignment ability by irradiation of polarized light. Patent Document 2 listed below describes a liquid crystal display device having a contrast of 250 by an alignment method in which linearly polarized light is irradiated onto a polymer film.

このような視角特性(輝度コントラスト比、階調・色調反転)に優れ、表示の明るいIPS方式の液晶表示装置(以下「IPS−TFT−LCD」という。)は、表示領域が大きなモニターやテレビなどへ向けた有力な技術である。   An IPS liquid crystal display device (hereinafter referred to as “IPS-TFT-LCD”) having excellent viewing angle characteristics (brightness contrast ratio, gradation / tone inversion) and bright display (hereinafter referred to as “IPS-TFT-LCD”) has a large display area, such as a monitor or a television It is a powerful technology for

液晶表示装置では、液晶層を挟持する一対の基板の当該液晶層との界面には液晶配向制御能を付与した配向制御膜が形成される。しかし、今後20型以上のより大きな画面に対応したIPS−TFT−LCDを実用化するには、サイズの大きい表示装置(大型パネル)用の新しい構造やプロセスの開発が必要である。   In the liquid crystal display device, an alignment control film having a liquid crystal alignment control ability is formed on the interface between the pair of substrates sandwiching the liquid crystal layer and the liquid crystal layer. However, in order to put IPS-TFT-LCDs compatible with larger screens of 20-inch or larger into the future, it is necessary to develop new structures and processes for large-sized display devices (large panels).

特に、液晶層に対面する表面に段差構造が多いIPS−TFT−LCDにおいては、配向制御膜に大画面にわたって均一な配向処理を施すことは困難である。配向制御膜に配向処理を施す際のマージンは、従来型のTN方式、とりわけ現在主流のノーマリオープン型TN方式(低電圧で明表示、高電圧で暗表示)に比べて著しく狭い。マージンが狭い理由は以下の(1)(2)(3)に説明する3点である。   In particular, in an IPS-TFT-LCD having many step structures on the surface facing the liquid crystal layer, it is difficult to perform uniform alignment treatment over the large screen on the alignment control film. The margin for performing the alignment treatment on the alignment control film is significantly narrower than that of the conventional TN system, particularly the currently mainstream normally open TN system (light display at low voltage, dark display at high voltage). The reason why the margin is narrow is three points described in (1), (2) and (3) below.

(1)段差構造
IPS−TFT−LCDにおいては、原理上数μm程度の幅を持つ細長い電極(櫛歯電極(Inter digital electrode )と称する場合もある)を多数配設する必要がある。そのため、微細な段差構造が形成される。
(1) In a step structure IPS-TFT-LCD, it is necessary to dispose a large number of elongated electrodes (sometimes referred to as interdigital electrodes) having a width of about several μm in principle. Therefore, a fine step structure is formed.

段差の大きさは、電極の厚みやその上に形成される各種の膜の形状により決まるが、通常10nm以上である。高透過率画素構造では、無機絶縁膜が厚く形成されており、無機絶縁膜以下の段差凹凸はある程度平坦化されている。   The size of the step is determined by the thickness of the electrode and the shape of various films formed thereon, but is usually 10 nm or more. In the high transmittance pixel structure, the inorganic insulating film is formed thick, and the unevenness below the inorganic insulating film is flattened to some extent.

したがって、高透過率画素構造の配向制御膜の段差は、主に有機絶縁膜上の電極に起因している。これらの膜の最上層にポリイミド等の高分子膜からなる配向制御膜(配向膜とも称する)が形成される。   Therefore, the step of the alignment control film having a high transmittance pixel structure is mainly caused by the electrode on the organic insulating film. An alignment control film (also referred to as an alignment film) made of a polymer film such as polyimide is formed on the uppermost layer of these films.

従来の量産技術においては、この配向制御膜上をラビング処理し、液晶配向能(初期配向)を付与する。一方で、ラビング用の布は、太さが10〜30μm程度の細い繊維を束ねて構成されており、実質的にはこの細い繊維一本一本が、配向膜の局所的な部分に一定方向の剪断力を与えることで液晶配向能を付与する処理がなされる。   In the conventional mass production technique, the alignment control film is rubbed to give liquid crystal alignment ability (initial alignment). On the other hand, the rubbing cloth is formed by bundling thin fibers having a thickness of about 10 to 30 μm, and each of these thin fibers substantially has a certain direction in a local portion of the alignment film. A treatment for imparting liquid crystal alignment ability is performed by applying a shearing force of.

繊維としては、数ミクロン程度の極細繊維も存在するが、ラビング用としてはある程度の摩擦力を付与するための剛性が要求されることから、このような極細繊維を用いたものは実用化されていない。   As fibers, there are microfibers of several microns, but for rubbing, rigidity is required to give a certain amount of friction, so those using such ultrafine fibers have been put to practical use. Absent.

IPS方式での電極間隔も上記繊維の径と同程度の10〜30μm程度であるため、段差近傍のラビングは十分になされず、配向が乱れやすい。この配向の乱れは黒レベルの上昇、ならびにそれによるコントラスト比の低下や、輝度の不均一性といった画質の低下を引き起こす。   Since the electrode spacing in the IPS system is about 10 to 30 μm, which is the same as the diameter of the fiber, rubbing in the vicinity of the step is not sufficient, and the orientation tends to be disturbed. This disturbance in orientation causes an increase in black level and a decrease in image quality such as a decrease in contrast ratio and nonuniform luminance.

(2)配向角
IPS−TFT−LCDにおいては、初期配向方向は原理上電極が伸びた方向、或いはそれと垂直な方向からある一定以上の角度をもってずらして設定する必要がある。ここで電極とは、信号配線電極、画素内の共通電極、画素電極を指す。
(2) Orientation angle In the IPS-TFT-LCD, the initial orientation direction must be set by shifting the initial orientation direction by a certain angle or more from the direction in which the electrode extends in principle or the direction perpendicular thereto. Here, the electrode refers to a signal wiring electrode, a common electrode in a pixel, and a pixel electrode.

初期配向の方向をラビングで規定するには、前述のように10〜30μm程度の繊維で所定角度方向に擦る必要があるが、信号配線電極、画素内の共通電極、画素電極といった一定方向に伸びた配線とその端部の段差により、設定の角度から段差方向に繊維が引きずられてしまい配向が乱れ、それによる黒レベルの上昇などの画質低下を引き起こす。   In order to define the direction of initial orientation by rubbing, it is necessary to rub in a predetermined angle direction with fibers of about 10 to 30 μm as described above, but it extends in a certain direction such as a signal wiring electrode, a common electrode in a pixel, and a pixel electrode. Due to the wiring and the step at the end thereof, the fibers are dragged in the step direction from the set angle, and the orientation is disturbed, thereby causing a reduction in image quality such as an increase in black level.

(3)暗レベルの沈み込み
IPS−TFT−LCDの特徴の一つとして、暗レベル(黒表示)の沈み込みが良好である点が挙げられる。そのため、他の方式に比較して配向の乱れが目立ちやすい。
(3) Dark level sinking One feature of the IPS-TFT-LCD is that the dark level (black display) sinking is good. Therefore, the disorder of orientation is more conspicuous than other methods.

従来のノーマリオープン型TN方式では、暗レベルが高電圧を印加した状態で得られる。この場合、高電圧では、液晶分子のほとんどが基板面に垂直な一方向である電界方向に揃っており、その液晶分子配列と偏光板の配置との関係で、暗レベルが得られている。したがって、暗レベルの均一性は原理上低電圧時の初期配向状態にはあまり依存しない。   In the conventional normally open type TN system, the dark level is obtained with a high voltage applied. In this case, at a high voltage, most of the liquid crystal molecules are aligned in the electric field direction which is one direction perpendicular to the substrate surface, and a dark level is obtained due to the relationship between the liquid crystal molecule arrangement and the arrangement of the polarizing plates. Therefore, the uniformity of the dark level does not depend much on the initial alignment state at low voltage in principle.

さらに、人間の目は、輝度のムラを輝度の相対的な比率として認識し、かつ対数スケールに近い反応をするため、暗レベルの変動には敏感である。この観点からも高電圧で、強制的に一方向に液晶分子を配列させる従来のノーマリオープン型TN方式では、初期配向状熊に鈍感になり有利である。   Furthermore, the human eye recognizes uneven luminance as a relative ratio of luminance, and reacts close to a logarithmic scale, so it is sensitive to changes in the dark level. From this point of view, the conventional normally open type TN method in which liquid crystal molecules are forcibly arranged in one direction at a high voltage is insensitive to the initial alignment bear.

一方、IPS方式では、低電圧或いは電圧ゼロにおいて暗レベルの表示をするため、初期配向状態の乱れには敏感である。特に、液晶分子配向方向を上下基板上で互いに平行とするホモジニアス配列とし、かつ一方の偏光板の光透過軸をその液晶分子配向方向に平行、他方の偏光板を直交とした配置(複屈折モードと呼ばれる)では、液晶層に入射した偏光光は、直線偏光をほとんど乱されずに伝搬する。このことは暗レベルを沈み込ませるのに有効である。複屈折モードの透過率Tは、一般に、次の式で表せる。   On the other hand, since the IPS system displays a dark level at a low voltage or zero voltage, it is sensitive to disturbance of the initial alignment state. In particular, an arrangement in which the liquid crystal molecular alignment directions are homogeneously aligned on the upper and lower substrates, the light transmission axis of one polarizing plate is parallel to the liquid crystal molecular alignment direction, and the other polarizing plate is orthogonal (birefringence mode). In other words, the polarized light incident on the liquid crystal layer propagates the linearly polarized light with little disturbance. This is useful for sinking dark levels. The transmittance T in the birefringence mode can be generally expressed by the following formula.

T=T0・sin2{2θ(E)}・sin2{(π・deff・Δn)/λ}   T = T0 · sin2 {2θ (E)} · sin2 {(π · deff · Δn) / λ}

ここで、T0は係数で、主として液晶パネルに使用される偏光板の透過率で決まる数値、θ(E)は液晶分子の配向方向(液晶層の実効的な光軸)と偏光透過軸のなす角度、Eは印加電界強度、deffは液晶層の実効的な厚さ、Δnは液晶の屈折率異方性、λは光の波長を表す。   Here, T0 is a coefficient, which is a numerical value mainly determined by the transmittance of the polarizing plate used in the liquid crystal panel, and θ (E) is formed by the alignment direction of liquid crystal molecules (effective optical axis of the liquid crystal layer) and the polarization transmission axis. Angle, E is the applied electric field strength, deff is the effective thickness of the liquid crystal layer, Δn is the refractive index anisotropy of the liquid crystal, and λ is the wavelength of light.

また、ここで、液晶層の実効的な厚さdeff 液晶の屈折率異方性Δnの積、すなわちdeff・Δnをリタデーションという。なお、ここでの液晶層の厚さdeffは液晶層全体の厚さではなく、電圧が印加されたとき、実際に配向方向を変える液晶層の厚さに相当する。   Further, here, the effective thickness deff of the liquid crystal layer deff The product of the refractive index anisotropy Δn of the liquid crystal, that is, deff · Δn is referred to as retardation. Note that the thickness deff of the liquid crystal layer here is not the thickness of the entire liquid crystal layer, but corresponds to the thickness of the liquid crystal layer that actually changes the alignment direction when a voltage is applied.

何故なら、液晶層の界面近傍の液晶分子は、界面でのアンカリングの影響により、電圧が印加されてもその配向方向を変えないためである。したがって、基板によって挟持された液晶層全体の厚さをdLCとすると、この厚さdLCとdeffの間には、常にdeff<dLCの関係があり、その差は液晶パネルに用いる液晶材料と、液晶層と接する界面、例えば、配向膜材料の種類によって異なるが、概ね20nm〜40nm程度と見積もることができる。   This is because the liquid crystal molecules in the vicinity of the interface of the liquid crystal layer do not change the orientation direction even when a voltage is applied due to the influence of anchoring at the interface. Therefore, if the thickness of the entire liquid crystal layer sandwiched between the substrates is dLC, there is always a relationship of def <dLC between the thickness dLC and diff, and the difference is between the liquid crystal material used for the liquid crystal panel and the liquid crystal Although it differs depending on the interface in contact with the layer, for example, the type of alignment film material, it can be estimated to be approximately 20 nm to 40 nm.

上記の式から明らかなように、電界強度に依存するのはsin2{2θ(E)}の項であり、角度θを電界強度Eに応じて変えることで輝度が調整できる。 As apparent from the above equation, the term sin 2 {2θ (E)} depends on the electric field strength, and the luminance can be adjusted by changing the angle θ according to the electric field strength E.

ノーマリークローズ型にするには、電圧無印加時にθ=0度となるよう偏光板を設定するため、初期配向方向の乱れに敏感になるように作用する。   In order to obtain a normally closed type, the polarizing plate is set so that θ = 0 ° when no voltage is applied, so that it acts so as to be sensitive to disturbance in the initial alignment direction.

このようにIPS方式では、配向均一性が非常に重要な要素であり、現在用いられているラビング法の問題が明らかになってきている。 As described above, in the IPS system, alignment uniformity is a very important factor, and the problem of the rubbing method currently used is becoming clear.

一般的に、ラビング配向処理には摩擦により発生する静電気によるTFT破損やラビング布の毛先の乱れや塵による配向乱れによる表示不良、さらにはラビング布の交換頻度が多いなどラビング処理法に関わる問題が多い。   Generally, in rubbing alignment treatment, problems related to the rubbing treatment method, such as TFT damage due to static electricity generated by friction, rubbing of the tip of the rubbing cloth, orientation failure due to dust, and frequent replacement of the rubbing cloth There are many.

これらのラビング配向処理の問題を解決する目的で、ラビングなしで液晶の配向させるいわゆる「ラビングレス」配向法が検討され、様々な方法が提案されている。そのなかでも、偏光した紫外線等を高分子膜の表面に照射し、ラビング処理をすることなく液晶分子を配向させる光配向法が提案されている。   In order to solve these problems of rubbing alignment treatment, a so-called “rubbing-less” alignment method in which liquid crystals are aligned without rubbing has been studied, and various methods have been proposed. Among them, a photo-alignment method has been proposed in which the surface of a polymer film is irradiated with polarized ultraviolet rays or the like and liquid crystal molecules are aligned without rubbing treatment.

その例として、下記非特許文献1に開示された方法は、従来のラビング処理を必要とせず、偏光した光照射により一定方向に液晶を配向させることが特徴である。   As an example, the method disclosed in Non-Patent Document 1 below is characterized in that the liquid crystal is aligned in a certain direction by irradiation with polarized light without requiring a conventional rubbing treatment.

この光配向法によれば、ラビング法による膜表面の傷や静電気等の問題がなく、また工業的な生産を考慮した際の製造プロセスとしてより簡便であることが利点であり、今後のラビング処理を用いない新たな液晶配向処理方法として注目されている。   According to this photo-alignment method, there are no problems such as scratches on the film surface or static electricity due to the rubbing method, and it is advantageous that it is simpler as a manufacturing process when considering industrial production. Attention has been focused on as a new liquid crystal alignment treatment method that does not use.

これまでの報告で使用されている液晶配向膜材料として、偏光した光に対する光化学的感度を得る必要性から、高分子の側鎖に光反応性基を導入した高分子化合物を用いることが提案されている。   As a liquid crystal alignment film material used in previous reports, it was proposed to use a polymer compound in which a photoreactive group was introduced into the side chain of the polymer because of the need to obtain photochemical sensitivity to polarized light. ing.

その代表的な例として、ポリビニルシンナメートが挙げられるが、この場合光照射による側鎖部分での二量化により高分子膜中に異方性を発現し液晶を配向させるものと考えられている。   A typical example is polyvinyl cinnamate. In this case, it is considered that the liquid crystal is oriented by developing anisotropy in the polymer film by dimerization at the side chain portion by light irradiation.

また、その他として、高分子材料中に低分子の二色性アゾ色素を分散し、この膜表面に対して偏光した光を照射することで一定の方向に液晶分子を配向させうることが提案されている。   In addition, it has been proposed that low molecular dichroic azo dyes can be dispersed in a polymer material and liquid crystal molecules can be aligned in a certain direction by irradiating polarized light onto the film surface. ing.

またさらには、特定のポリイミド膜に偏光した紫外線等を照射することによって液晶分子が配向することが報告されている。この場合光照射により、一定方向のポリイミド主鎖が分解することにより液晶配向を発現しているものと考えられる。   Furthermore, it has been reported that liquid crystal molecules are aligned by irradiating a specific polyimide film with polarized ultraviolet rays or the like. In this case, it is considered that the liquid crystal alignment is expressed by decomposing the polyimide main chain in a certain direction by light irradiation.

特許第3303766号明細書Japanese Patent No. 3303766 特開平11-218765号公報JP 11-218765 A

ギボンズら、「ネイチャー」351巻、49ページ(1991年)(W.M. Gibbons et al., Nature, 351, 49(1991) )Gibbons et al., “Nature”, 351, 49 (1991) (W.M. Gibbons et al., Nature, 351, 49 (1991))

このようにラビング配向法の問題点を解決するラビングレス配向法として光照射による光配向法が提案、検討されているが、実用上以下のような問題点を抱えている。   As described above, a photo-alignment method by light irradiation has been proposed and studied as a rubbing-less alignment method for solving the problems of the rubbing alignment method, but has the following problems in practice.

ポリビニルシンナメート等に代表される高分子側鎖に光反応性基を導入した高分子材料系では、配向の熱安定性が十分ではなく実用性の面ではまだ十分な信頼性が得られてはいない。   In the polymer material system in which a photoreactive group is introduced into a polymer side chain represented by polyvinyl cinnamate, the thermal stability of orientation is not sufficient, and sufficient reliability is still obtained in terms of practicality. Not in.

またこの場合、液晶の配向を発現させる構造部位が高分子の側鎖部分であると考えられることから、液晶分子をより均一に配向させ、かつより強い配向を得る上では必ずしも好ましいとは言えない。   In this case, it is considered that the structural part that develops the alignment of the liquid crystal is the side chain portion of the polymer, and therefore it is not necessarily preferable for aligning the liquid crystal molecules more uniformly and obtaining a stronger alignment. .

また、低分子の二色性色素を高分子中に分散した場合には、液晶を配向させる色素自体が低分子であり、実用的な観点からみて熱的、あるいは光に対する信頼性の面で課題が残されている。   In addition, when a low-molecular dichroic dye is dispersed in a polymer, the dye itself that orients the liquid crystal is a low-molecular substance, which is a problem in terms of thermal or light reliability from a practical viewpoint. Is left behind.

さらに、特定のポリイミドに偏光した紫外線を照射する方法においては、ポリイミド自体としては、耐熱性等の信頼性は高いものの、その配向機構が光による分解に起因していると考えられることから、実用面において十分な信頼性を確保するのが困難である。   Furthermore, in the method of irradiating a specific polyimide with polarized ultraviolet rays, although the polyimide itself has high reliability such as heat resistance, it is considered that its orientation mechanism is caused by decomposition by light. It is difficult to ensure sufficient reliability in terms of surface.

すなわち、今後この偏光照射を用いた液晶配向を実際に応用する場合には、液晶を単に初期的に配向させるだけでなく、信頼性の観点から、より安定な配向を発現させることが必要とされる。   In other words, in the future, when applying this liquid crystal alignment using polarized light irradiation, it is necessary not only to align the liquid crystal initially but also to develop a more stable alignment from the viewpoint of reliability. The

また、実際の工業的な応用を考えた場合、熱的にも安定な高分子構造を選択することが望まれている。これらの点で、従来光照射による液晶配向に対して提案されている高分子材料は、配向力及びその安定性の面で必ずしも十分ではなく、光照射によるラビングレス配向を実現する大きな課題となっているのが実情である。   In consideration of actual industrial application, it is desired to select a thermally stable polymer structure. In these respects, the polymer materials conventionally proposed for liquid crystal alignment by light irradiation are not necessarily sufficient in terms of alignment force and stability, which is a big problem for realizing rubbing-less alignment by light irradiation. It is the actual situation.

したがって、本発明の目的は、以上のようなIPS−TFT−LCDの固有の問題である配向処理の製造マージンが狭いという問題を解決し、初期配向方向の変動による表示不良の発生を低減し、かつ安定な液晶配向を実現し、コントラスト比を高めた高品位な画質を有する特に大型の液晶表示装置を提供することにある。   Therefore, an object of the present invention is to solve the problem that the manufacturing margin of the alignment process, which is an inherent problem of the IPS-TFT-LCD, is narrow, and to reduce the occurrence of display defects due to fluctuations in the initial alignment direction. Another object of the present invention is to provide a particularly large liquid crystal display device that realizes stable liquid crystal alignment and has high image quality with an increased contrast ratio.

また、本発明の他の目的は、量産性に優れた高画質・高精細度の液晶表示装置を提供することにある。   Another object of the present invention is to provide a liquid crystal display device with high image quality and high definition that is excellent in mass productivity.

上記目的を達成するため、本発明は、少なくとも一方が透明な一対の基板と、前記一対の基板間に配置された液晶層と、前記一対の基板の一方の基板に形成され、前記液晶層に印加するための電極群及びこれらの電極に接続された複数のアクティブ素子と、前記液晶層と前記一対の基板の少なくともどちらか一方の基板の間に配置された配向制御膜と、前記一対の基板の少なくともどちらか一方の基板に形成され前記液晶層の分子配向状態に応じて光学特性を変える偏光手段とを有し、前記配向制御膜の少なくとも一方が、光反応性のポリイミド及び/又はポリアミック酸からなり、ほぼ直線に偏光した光を照射して配向制御膜を形成することを特徴とする。   To achieve the above object, the present invention is formed on a pair of substrates, at least one of which is transparent, a liquid crystal layer disposed between the pair of substrates, and one of the pair of substrates, An electrode group for applying, a plurality of active elements connected to these electrodes, an alignment control film disposed between at least one of the liquid crystal layer and the pair of substrates, and the pair of substrates A polarizing means which is formed on at least one of the substrates and changes the optical characteristics according to the molecular alignment state of the liquid crystal layer, and at least one of the alignment control films is a photoreactive polyimide and / or polyamic acid. The alignment control film is formed by irradiating light polarized in a substantially straight line.

また、本発明は、前記液晶層に印加される電界が、前記電極群の形成された基板面に対してほぼ平行であることを特徴とする。   Further, the invention is characterized in that an electric field applied to the liquid crystal layer is substantially parallel to a substrate surface on which the electrode group is formed.

また、本発明は、配向制御膜上の液晶層中の液晶分子の長軸方向が、光照射したほぼ直線に偏光した偏光軸と平行又は直交(垂直)していることを特徴とする。特に、光反応性の配向制御膜が、酸無水物として少なくともシクロブタンテトラカルボン酸二無水物、ジアミンとして少なくとも芳香族ジアミン化合物から構成されるポリアミック酸又はポリイミドであることが望ましい。   Further, the present invention is characterized in that the major axis direction of the liquid crystal molecules in the liquid crystal layer on the alignment control film is parallel or orthogonal (perpendicular) to the polarization axis polarized in a substantially straight line irradiated with light. In particular, the photoreactive alignment control film is desirably a polyamic acid or polyimide composed of at least a cyclobutanetetracarboxylic dianhydride as an acid anhydride and at least an aromatic diamine compound as a diamine.

また、前記シクロブタンテトラカルボン酸二無水物及びその誘導体が、下記一般式〔化合物1〕〜〔化合物3〕で示される化合物であることを特徴とする。

Figure 0005594835
Figure 0005594835
Figure 0005594835
(但し、R1,R2,R3,R4はそれぞれ独立に水素原子、フッ素原子、塩素原子、臭素原子、フェニル基又は炭素数1〜6のアルキル基、アルコキシ基又はビニル基[−(CH2)m−CH=CH2,m=0,1,2]、又はアセチル基[−(CH2)m−CH≡CH2,m=0,1,2]) The cyclobutanetetracarboxylic dianhydride and derivatives thereof are compounds represented by the following general formulas [Compound 1] to [Compound 3].
Figure 0005594835
Figure 0005594835
Figure 0005594835
(However, R1, R2, R3, and R4 are each independently a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, a phenyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group, or a vinyl group [— (CH2) m— CH = CH2, m = 0, 1, 2] or acetyl group [-(CH2) m-CH≡CH2, m = 0, 1, 2])

また、前記芳香族ジアミン化合物が、下記一般式〔化合物4〕〜〔化合物22〕からなる化合物群から選択される化合物の少なくとも1種を含有することを特徴とする。

Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
(但し、化合物4から化合物19のR1〜R8及び化合物20のR1、R2はそれぞれ独立に水素原子、フッ素原子、塩素原子、又は炭素数1〜6のアルキル基、アルコキシ基、又はビニル基[−(CH2)m−CH=CH2,m=0,1,2]、又はアセチル基[−(CH2)m−CH≡CH2,m=0,1,2]を示す。また、化合物10〜12においてXは−CH2−,−NH−,−CO−,−O−,−S−の結合基を示す。また、化合物20のR3、R4及び化合物21、22のR1はそれぞれ独立に炭素数1〜6のアルキル基を示す。) Further, the aromatic diamine compound contains at least one compound selected from the group consisting of the following general formulas [compound 4] to [compound 22].
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
(However, R1 to R8 of Compound 4 to Compound 19 and R1 and R2 of Compound 20 are each independently a hydrogen atom, a fluorine atom, a chlorine atom, or an alkyl group having 1 to 6 carbon atoms, an alkoxy group, or a vinyl group [- (CH2) m-CH = CH2, m = 0,1,2] or an acetyl group [-(CH2) m-CH≡CH2, m = 0,1,2]. X represents a bonding group of —CH 2 —, —NH—, —CO—, —O—, —S—, wherein R 3 and R 4 of Compound 20 and R 1 of Compounds 21 and 22 each independently represent 1 to 6 represents an alkyl group.)

また、配向制御膜の膜厚を1nmから100nmのように薄膜にすることにより、光の透過性が向上すること、さらに偏光照射による光反応の効率が向上し効果的である。また、液晶表示装置を作製した場合にも、液晶を駆動する電圧を有効に液晶層に印加するのに効果的である。   Further, by making the orientation control film as thin as 1 nm to 100 nm, it is effective to improve the light transmittance and to improve the efficiency of the photoreaction by irradiation of polarized light. Further, when a liquid crystal display device is manufactured, it is effective to apply a voltage for driving the liquid crystal to the liquid crystal layer effectively.

さらに、電極上の配向制御膜の膜厚が1nm〜50nm、さらに1nm〜30nmと薄膜化することにより液晶表示装置の各画素内の電極/配向制御膜/液晶層/配向制御膜/電極の間に残留する直流電圧成分(いわゆる残留DC電圧)を低減することが可能となり、ひいては残像、焼き付き特性が向上するなど効果的である。   Further, the film thickness of the alignment control film on the electrode is reduced to 1 nm to 50 nm, and further to 1 nm to 30 nm, so that between each electrode / alignment control film / liquid crystal layer / alignment control film / electrode in each pixel of the liquid crystal display device. It is possible to reduce the direct current voltage component (so-called residual DC voltage) remaining in the image, which is effective in improving afterimage and image sticking characteristics.

また、本発明は、液晶表示装置の液晶層のプレチルト角が1度以下であることに特徴がある。また、従来のラビング配向法では、電極段差端部がラビング布の繊維のガイドとして作用し、段差部が伸びた方向に繊維が引き込まれたり、段差のコーナー部に繊維が届かず配向処理ができず配向不良が生じたりする。   Further, the present invention is characterized in that the pretilt angle of the liquid crystal layer of the liquid crystal display device is 1 degree or less. Also, with the conventional rubbing alignment method, the electrode step edge acts as a fiber guide for the rubbing cloth, and the fiber is drawn in the direction in which the step extends, or the fiber does not reach the corner of the step and the alignment process can be performed. Orientation failure may occur.

特に、画素電極、又は共通電極、又は共通電極配線の少なくとも一方が透明な電極で構成されている場合には、電極段差近傍の配向状態が目立つため、本発明が有効である。   In particular, when at least one of the pixel electrode, the common electrode, or the common electrode wiring is formed of a transparent electrode, the alignment state in the vicinity of the electrode step is conspicuous, and the present invention is effective.

特に、透明電極がイオンドープ酸化チタン膜、又はイオンドープ酸化亜鉛膜(ZnO)で構成されている場合には、本発明が有効に作用する。   In particular, when the transparent electrode is composed of an ion-doped titanium oxide film or an ion-doped zinc oxide film (ZnO), the present invention works effectively.

また、一方で画素電極及びそれと対向する共通電極が、お互いに平行に配置されジグザグな屈曲構造からなる場合には、液晶配向膜が下地の有機絶縁膜との密着性に劣る場合があり、従来のラビング配向処理を施すと、配向膜の剥がれなどの表示不良を引き起こす場合がある。このような場合には本発明は有効である。   On the other hand, when the pixel electrode and the common electrode facing it are arranged in parallel to each other and have a zigzag bent structure, the liquid crystal alignment film may be inferior in adhesion to the underlying organic insulating film. When the rubbing alignment treatment is performed, display defects such as peeling of the alignment film may occur. In such a case, the present invention is effective.

また、本発明は、共通電極及び/又は画素電極が、有機絶縁膜上に形成され、その有機絶縁膜及び電極上に液晶配向膜が形成されている場合に、特に有効である。   The present invention is particularly effective when the common electrode and / or the pixel electrode is formed on the organic insulating film and the liquid crystal alignment film is formed on the organic insulating film and the electrode.

また、本発明は、液晶層と前記一対の基板上に形成されている配向制御膜との二つの界面における液晶分子の配向制御方向がほぼ同一方向であることに特徴を有する。   In addition, the present invention is characterized in that the alignment control directions of the liquid crystal molecules at the two interfaces between the liquid crystal layer and the alignment control film formed on the pair of substrates are substantially the same direction.

そして、本発明は、液晶配向膜に偏光照射することにより液晶配向処理を付与することを特徴とする。   And this invention is characterized by providing a liquid crystal aligning process by irradiating polarized light to a liquid crystal aligning film.

本発明によれば、配向処理に用いる偏光の光波長が200から400nmの範囲であることを特徴とする。さらに、本発明は、配向処理に用いるほぼ直線に偏光した第一の波長の光と、第二の波長の光の少なくとも2種類の波長の偏光を用いる場合にさらに有効である。   According to the present invention, the light wavelength of polarized light used for the alignment treatment is in the range of 200 to 400 nm. Furthermore, the present invention is more effective when using polarized light having at least two types of wavelengths, that is, light having the first wavelength and light having the second wavelength, which are polarized substantially linearly, used for the alignment treatment.

また、本発明は、液晶配向制御膜のガラス転移温度が250℃以上であることを特徴とする。   In addition, the present invention is characterized in that the liquid crystal alignment control film has a glass transition temperature of 250 ° C. or higher.

さらに、本発明は、液晶配向膜に偏光照射により液晶配向能を付与する場合に、加熱、赤外線照射、遠赤外線照射、電子線照射、放射線照射のうち少なくとも一つの処理を加えることにより、さらに有効に作用する。配向制御膜に偏光照射することにより液晶配向能を付与する際に、加熱、赤外線照射、遠赤外線照射、電子線照射、放射線照射を加えることにより、偏光照射による液晶配向能付与を加速、さらには架橋反応などを誘起することにより、液晶配向能を促進、安定化するのに効果的である。   Furthermore, the present invention is more effective by adding at least one of heating, infrared irradiation, far-infrared irradiation, electron beam irradiation, and radiation irradiation when imparting liquid crystal alignment ability to the liquid crystal alignment film by polarized light irradiation. Act on. When imparting liquid crystal alignment ability by irradiating the alignment control film with polarized light, by applying heating, infrared irradiation, far-infrared irradiation, electron beam irradiation, and radiation irradiation, liquid crystal alignment ability provision by polarized irradiation is accelerated. Inducing a cross-linking reaction or the like is effective in promoting and stabilizing the liquid crystal alignment ability.

特に、加熱、赤外線照射、遠赤外線照射、電子線照射、放射線照射のうち少なくとも一つの処理を偏光照射処理と時間的な重なりをもって行うことにより、本発明はさらに有効に作用する。   In particular, the present invention operates more effectively by performing at least one of heating, infrared irradiation, far-infrared irradiation, electron beam irradiation, and radiation irradiation with the time of overlapping with the polarized irradiation treatment.

また、配向制御膜のイミド化焼成処理と偏光照射処理を時間的な重なりをもって行うことによっても、本発明は有効に作用する。特に、液晶配向膜に偏光照射に加え、加熱、赤外線照射、遠赤外線照射、電子線照射、放射線照射のうち少なくとも一つの処理を行う場合に、配向制御膜の温度が100°C〜400°Cの範囲であること、さらには150°C〜300°Cの範囲であることが望ましい。   The present invention also works effectively by performing the imidization baking treatment of the alignment control film and the polarization irradiation treatment with time overlap. In particular, when the liquid crystal alignment film is subjected to at least one of heating, infrared irradiation, far-infrared irradiation, electron beam irradiation, and radiation irradiation in addition to polarized light irradiation, the temperature of the alignment control film is 100 ° C to 400 ° C. It is desirable that the temperature be in the range of 150 ° C to 300 ° C.

また、加熱、赤外線照射、遠赤外線照射の処理は、配向制御膜のイミド化焼成処理と兼用することも可能であり有効である。   Also, the heating, infrared irradiation, and far infrared irradiation treatments can be combined with the imidization baking treatment of the orientation control film, and are effective.

また、本発明において、目標とするコントラストは、500:1以上であり、目標とする残像が解消される時間は、5分以内であることとする。なお、残像の解消される時間は下記の実施形態において定義される方法にて決定される。なお、本発明は、目標とするコントラストが500:1以上の高コントラストにより高画質化されているために、従来の目標とするコントラストが約200:1の低コントラストの残像評価に比べて残像の消失の判断基準が厳しく、目標とする残像が解消される時間を5分以内とした。   In the present invention, the target contrast is 500: 1 or more, and the time for eliminating the target afterimage is 5 minutes or less. In addition, the time for eliminating the afterimage is determined by a method defined in the following embodiment. In the present invention, since the target contrast is improved by the high contrast of 500: 1 or higher, the afterimage of the afterimage is lower than the conventional low contrast afterimage evaluation of about 200: 1. The criterion for disappearance was strict, and the time required for eliminating the target afterimage was set within 5 minutes.

以上説明したように、本発明によれば、IPS方式の液晶表示装置において、配向処理の製造マージンが狭いという固有の問題を解決し、初期配向方向の変動による表示不良の発生を低減し、かつ安定な液晶配向を実現し、量産性に優れ、かつコントラスト比を高めた高品位な画質を有する液晶表示装置を提供することができる。   As described above, according to the present invention, in the IPS liquid crystal display device, the inherent problem that the manufacturing margin of the alignment process is narrow is solved, the occurrence of display defects due to the change in the initial alignment direction is reduced, and It is possible to provide a liquid crystal display device that realizes stable liquid crystal alignment, is excellent in mass productivity, and has high quality image quality with an increased contrast ratio.

以上説明したように、本発明によれば、IPS方式の液晶表示装置において、配向処理の製造マージンが狭いという固有の問題を解決し、初期配向方向の変動による表示不良の発生を低減し、かつ安定な液晶配向を実現し、量産性に優れ、かつコントラスト比を高めた高品位な画質を有する液晶表示装置を提供することができる。   As described above, according to the present invention, in the IPS liquid crystal display device, the inherent problem that the manufacturing margin of the alignment process is narrow is solved, the occurrence of display defects due to the change in the initial alignment direction is reduced, and It is possible to provide a liquid crystal display device that realizes stable liquid crystal alignment, is excellent in mass productivity, and has high quality image quality with an increased contrast ratio.

本発明による液晶表示装置の第1の実施の形態の画素構成を説明する画素部分の断面図。1 is a cross-sectional view of a pixel portion illustrating a pixel configuration of a first embodiment of a liquid crystal display device according to the present invention. 本発明による液晶表示装置の第1の実施の形態の画素構成を説明する画素部分の平面図及び断面図。2A and 2B are a plan view and a cross-sectional view of a pixel portion illustrating a pixel configuration of a liquid crystal display device according to a first embodiment of the invention. 本発明による液晶表示装置の第2の実施の形態の画素構成を説明する画素部分の断面図。Sectional drawing of the pixel part explaining the pixel structure of 2nd Embodiment of the liquid crystal display device by this invention. 本発明による液晶表示装置の第2の実施の形態である液晶表示装置の画素構成を説明する画素部分の平面図及び断面図。The top view and sectional drawing of the pixel part explaining the pixel structure of the liquid crystal display device which is 2nd Embodiment of the liquid crystal display device by this invention. 本発明による液晶表示装置の第3の実施の形態の画素構成を説明する画素部分の断面図。Sectional drawing of the pixel part explaining the pixel structure of 3rd Embodiment of the liquid crystal display device by this invention. 本発明による液晶表示装置の第4の実施の形態の画素構成を説明する画素部分の断面図。Sectional drawing of the pixel part explaining the pixel structure of 4th Embodiment of the liquid crystal display device by this invention. 本発明による液晶表示装置の第5の実施の形態である液晶表示装置の画素構成を説明する画素部分の断面図。Sectional drawing of the pixel part explaining the pixel structure of the liquid crystal display device which is 5th Embodiment of the liquid crystal display device by this invention. 本発明による液晶表示装置の第5の実施の形態である液晶表示装置の画素構成を説明する画素部分の平面図。The top view of the pixel part explaining the pixel structure of the liquid crystal display device which is 5th Embodiment of the liquid crystal display device by this invention.

以下、本発明の実施の形態について、図面を参照して詳細に説明する。なお、以下では薄膜トランジスタ等のアクティブ素子を形成した基板をアクティブマトリクス基板という。また、その対向基板にカラーフィルタを有する場合は、これをカラーフィルタ基板ともいう。   Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. Hereinafter, a substrate on which an active element such as a thin film transistor is formed is referred to as an active matrix substrate. In addition, when the counter substrate has a color filter, this is also referred to as a color filter substrate.

また、本発明において、目標として望ましいコントラストは、500:1以上であり、目標とする残像が解消される時間は、5分以内が望ましい。なお、残像の解消される時間は下記の実施の形態において定義される方法にて決定される。なお、本発明は、目標とするコントラストが500:1以上の高コントラストにより高画質化されているために、従来の目標とするコントラストが約200:1の低コントラストの残像評価に比べて残像の消失の判断基準が厳しく、目標とする残像が解消される時間を5分以内とした。   In the present invention, the desired contrast as a target is 500: 1 or more, and the time for eliminating the target afterimage is preferably within 5 minutes. Note that the time for eliminating the afterimage is determined by a method defined in the following embodiment. In the present invention, since the target contrast is improved by the high contrast of 500: 1 or higher, the afterimage of the afterimage is lower than the conventional low contrast afterimage evaluation of about 200: 1. The criterion for disappearance was strict, and the time required for eliminating the target afterimage was set within 5 minutes.

図1は、本発明による液晶表示装置の第1の実施の形態を説明する一画素付近の模式断面図である。   FIG. 1 is a schematic cross-sectional view of the vicinity of one pixel for explaining a first embodiment of a liquid crystal display device according to the present invention.

また、図2は本発明による液晶表示装置の第1の実施の形態を説明する一画素付近の構成を説明するアクティブマトリクス基板の模式図であり、図2(a)は平面図、図2(b)は図2(a)のA−A'線に沿った断面図、図2(c)は図2(a)のB−B'線に沿った断面図を示す。   FIG. 2 is a schematic view of an active matrix substrate for explaining a configuration in the vicinity of one pixel for explaining the first embodiment of the liquid crystal display device according to the present invention. FIG. 2 (a) is a plan view, and FIG. 2B is a cross-sectional view taken along line AA ′ in FIG. 2A, and FIG. 2C is a cross-sectional view taken along line BB ′ in FIG.

また、図1は図2(a)のA−A'線に沿った断面の一部に対応する。なお、図2(b)と図2(c)の断面図は、要部構成を強調して模式的に示すもので、図2(a)のA−A'線、B−B'線の切断部に一対一で対応しない。例えば、図2(b)では図1に示す半導体膜116は図示せず、図2(c)では対向電極とコモン配線120を接続するスルーホールは一箇所のみを代表して示してある。   FIG. 1 corresponds to a part of a cross section taken along line AA ′ in FIG. Note that the cross-sectional views of FIGS. 2 (b) and 2 (c) schematically show the configuration of the main part and schematically show the AA ′ line and BB ′ line in FIG. 2 (a). There is no one-to-one correspondence with the cutting part. For example, in FIG. 2B, the semiconductor film 116 shown in FIG. 1 is not shown, and in FIG. 2C, only one through hole connecting the counter electrode and the common wiring 120 is shown as a representative.

本実施の形態の液晶表示装置では、アクティブマトリクス基板としてガラス基板101上には、Cr(クロム)からなるゲート電極(走査信号電極)104及びコモン配線(共通電極配線)120(図2)が配置され、このゲート電極104及び共通電極配線120を覆うように窒化シリコンからなるゲート絶縁膜107が形成されている。   In the liquid crystal display device of the present embodiment, a gate electrode (scanning signal electrode) 104 and a common wiring (common electrode wiring) 120 (FIG. 2) made of Cr (chromium) are arranged on a glass substrate 101 as an active matrix substrate. A gate insulating film 107 made of silicon nitride is formed so as to cover the gate electrode 104 and the common electrode wiring 120.

また、ゲート電極104上には、ゲート絶縁膜107を介してアモルファスシリコン又はポリシリコンからなる半導体膜116が配置され、アクティブ素子として薄膜トランジスタ(TFT)の能動層として機能するようにされている。   A semiconductor film 116 made of amorphous silicon or polysilicon is disposed on the gate electrode 104 with a gate insulating film 107 interposed therebetween, and functions as an active layer of a thin film transistor (TFT) as an active element.

また、半導体膜116のパターンの一部に重畳するようにCr・Mo(クロム/モリブデン)よりなるドレイン電極(映像信号配線)106とソース電極(画素電極)105が配置され、これら全てを被覆するように窒化シリコンよりなる保護絶縁膜108が形成されている。   In addition, a drain electrode (video signal wiring) 106 and a source electrode (pixel electrode) 105 made of Cr · Mo (chromium / molybdenum) are arranged so as to overlap a part of the pattern of the semiconductor film 116 and cover all of them. Thus, a protective insulating film 108 made of silicon nitride is formed.

また、図2(c)に模式的に示したように、ゲート絶縁膜107と保護絶縁膜108を貫通して形成されたスルーホール118を介して共通電極配線120に接続するコモン電極(共通電極)103がオーバーコート層(有機保護膜)112上に配置されている。   Further, as schematically shown in FIG. 2C, a common electrode (common electrode) connected to the common electrode wiring 120 through a through hole 118 formed through the gate insulating film 107 and the protective insulating film 108. ) 103 is disposed on the overcoat layer (organic protective film) 112.

また、図2(a)から分かるように、平面的には一画素の領域においてその画素電極105に対向するように、共通電極配線120よりスルーホール118を介して引き出されている共通電極103が形成されている。   Further, as can be seen from FIG. 2A, the common electrode 103 led out from the common electrode wiring 120 through the through hole 118 is opposed to the pixel electrode 105 in a region of one pixel in plan view. Is formed.

したがって、本発明の第1の実施の形態においては、画素電極105は有機保護膜112の下層の保護絶縁膜108のさらに下層に配置され、有機保護膜112上に共通電極103が配置された構成となっている。これらの複数の画素電極105と共通電極103とに挟まれた領域で、一画素が構成される構造となっている。   Therefore, in the first embodiment of the present invention, the pixel electrode 105 is disposed further below the protective insulating film 108 below the organic protective film 112, and the common electrode 103 is disposed on the organic protective film 112. It has become. One pixel is configured in a region sandwiched between the plurality of pixel electrodes 105 and the common electrode 103.

また、以上のように構成した単位画素をマトリクス状に配置したアクティブマトリクス基板の表面、すなわち、共通電極103が形成された有機保護膜112上には配向制御膜109が形成されている。   An alignment control film 109 is formed on the surface of the active matrix substrate in which the unit pixels configured as described above are arranged in a matrix, that is, on the organic protective film 112 on which the common electrode 103 is formed.

一方、図1に示されたように、対向基板を構成するガラス基板102には、カラーフィルタ層111が、遮光部(ブラックマトリクス)113で画素毎に区切られて配置され、また、カラーフィルタ層111及び遮光部113上は、透明な絶縁性材料からなる有機保護膜112で覆われている。さらに、その有機保護膜112上にも配向制御膜109が形成されてカラーフィルタ基板を構成している。   On the other hand, as shown in FIG. 1, the color filter layer 111 is arranged on the glass substrate 102 constituting the counter substrate so as to be divided for each pixel by a light shielding portion (black matrix) 113, and the color filter layer 111 and the light shielding part 113 are covered with an organic protective film 112 made of a transparent insulating material. Further, an alignment control film 109 is also formed on the organic protective film 112 to constitute a color filter substrate.

これらの配向制御膜109は、高圧水銀ランプを光源とし、石英板を積層したパイル偏光子を用いて取り出される紫外線の直線偏光照射により液晶配向能が付与されている。   These alignment control films 109 are provided with liquid crystal alignment capability by irradiation with ultraviolet linearly polarized light extracted using a pile polarizer with a quartz plate laminated using a high-pressure mercury lamp as a light source.

アクティブマトリクス基板を構成するガラス基板101と対向電極を構成するガラス基板102が、配向制御膜109の面で対向配置され、これらの間に液晶分子110で構成される液晶層(液晶組成物層)110'が配置されているように構成されている。   A glass substrate 101 constituting an active matrix substrate and a glass substrate 102 constituting a counter electrode are arranged opposite to each other on the surface of the alignment control film 109, and a liquid crystal layer (liquid crystal composition layer) composed of liquid crystal molecules 110 therebetween. 110 'is arranged.

また、アクティブマトリクス基板を構成するガラス基板101及び対向電極を構成するガラス基板102の外側の面のそれぞれには、偏光板114が形成されている。   A polarizing plate 114 is formed on each of the outer surfaces of the glass substrate 101 constituting the active matrix substrate and the glass substrate 102 constituting the counter electrode.

以上のようにして薄膜トランジスタを用いたアクティブマトリクス型液晶表示装置(すなわち、TFT液晶表示装置)が構成される。   As described above, an active matrix liquid crystal display device using thin film transistors (that is, a TFT liquid crystal display device) is configured.

このTFT液晶表示装置では、液晶組成物層110'を構成する液晶分子110は、電界無印加時には、対向配置されている基板101,102面にほぼ平行に配向された状態となり、光配向処理で規定された初期配向方向に向いた状態でホモジニアス配向している。   In this TFT liquid crystal display device, the liquid crystal molecules 110 constituting the liquid crystal composition layer 110 ′ are aligned substantially parallel to the opposing surfaces of the substrates 101 and 102 when no electric field is applied. Homogeneous alignment is performed in a state in which the initial alignment direction is specified.

ここで、ゲート電極104に電圧を印加して薄膜トランジスタ(TFT)をオンにすると、画素電極105と共通電極103の間の電位差により液晶組成物層に電界117が印加され、液晶組成物が持つ誘電異方性と電界との相互作用により液晶組成物層を構成する液晶分子110は電界方向にその向きを変える。このとき液晶組成物層の屈折異方性と偏光板114の作用により本液晶表示装置の光透過率を変化させ表示を行うことができる。   Here, when a voltage is applied to the gate electrode 104 to turn on the thin film transistor (TFT), an electric field 117 is applied to the liquid crystal composition layer due to a potential difference between the pixel electrode 105 and the common electrode 103, and thus the dielectric property of the liquid crystal composition. The liquid crystal molecules 110 constituting the liquid crystal composition layer change the direction in the electric field direction by the interaction between the anisotropy and the electric field. At this time, display can be performed by changing the light transmittance of the present liquid crystal display device by the refractive anisotropy of the liquid crystal composition layer and the action of the polarizing plate 114.

また、有機保護膜112は、絶縁性、透明性に優れるアクリル系樹脂、エポキシアクリル系樹脂、又はポリイミド系樹脂などの熱硬化性樹脂を用いればよい。また、有機保護膜112として、光硬化性の透明な樹脂を用いてもよいし、ポリシロキサン系の樹脂など無機系の材料を用いてもよい。さらには、有機保護膜112が配向制御膜109を兼ねるものであってもよい。   The organic protective film 112 may be formed using a thermosetting resin such as an acrylic resin, an epoxy acrylic resin, or a polyimide resin that is excellent in insulation and transparency. Further, as the organic protective film 112, a photocurable transparent resin may be used, or an inorganic material such as a polysiloxane resin may be used. Furthermore, the organic protective film 112 may also serve as the alignment control film 109.

以上のように、第1の実施の形態によれば、配向制御膜109の液晶配向制御能をバフ布で直接摩擦するラビング配向処理ではなく、非接触の光配向法を用いることにより、電極近傍に局所的な配向の乱れがなく、表示領域全面に渡り均一な配向を付与することが可能となる。   As described above, according to the first embodiment, the non-contact photo-alignment method is used instead of the rubbing alignment process in which the liquid crystal alignment control ability of the alignment control film 109 is directly rubbed with a buff cloth. Thus, there is no local disturbance of orientation, and uniform orientation can be provided over the entire display region.

次に、本発明による液晶表示装置の第2の実施の形態を説明する。図3は、本発明による液晶表示装置の第2の実施の形態を説明する一画素付近の模式断面図である。   Next, a second embodiment of the liquid crystal display device according to the present invention will be described. FIG. 3 is a schematic sectional view of the vicinity of one pixel for explaining a second embodiment of the liquid crystal display device according to the present invention.

また、図4は、本発明による液晶表示装置の第2の実施の形態を説明する一画素付近の構成を説明するアクティブマトリクス基板の模式図であり、図4(a)は平面図、図4(b)は図4(a)のA−A'線に沿った断面図、図4(c)は図4(a)のB−B'線に沿った断面図を示す。   FIG. 4 is a schematic view of an active matrix substrate for explaining a configuration in the vicinity of one pixel for explaining a second embodiment of the liquid crystal display device according to the present invention. FIG. 4 (a) is a plan view, and FIG. 4B is a cross-sectional view taken along line AA ′ in FIG. 4A, and FIG. 4C is a cross-sectional view taken along line BB ′ in FIG.

また、図3は図4(a)のA−A'線に沿った断面の一部を示している。なお、図4(b)と図4(c)の断面図は、要部構成を強調して模式的に示すもので、図4(a)のA−A'線、B−B'線の切断部に一対一で対応しない。例えば、図4(b)では図3に示す半導体膜116は図示していない。   FIG. 3 shows a part of a cross section taken along the line AA ′ in FIG. Note that the cross-sectional views of FIG. 4B and FIG. 4C schematically show the configuration of the main part, and are schematically shown by the lines AA ′ and BB ′ in FIG. There is no one-to-one correspondence with the cutting part. For example, FIG. 4B does not show the semiconductor film 116 shown in FIG.

本発明の第2の実施の形態の液晶表示装置では、アクティブマトリクス基板を構成するガラス基板101上には、Crよりなるゲート電極104及び共通電極配線120が配置され、ゲート電極104と共通電極配線120を覆うように窒化シリコンからなるゲート絶縁膜107が形成されている。   In the liquid crystal display device according to the second embodiment of the present invention, the gate electrode 104 and the common electrode wiring 120 made of Cr are arranged on the glass substrate 101 constituting the active matrix substrate, and the gate electrode 104 and the common electrode wiring are arranged. A gate insulating film 107 made of silicon nitride is formed so as to cover 120.

また、ゲート電極104上には、ゲート絶縁膜107を介してアモルファスシリコン或いはポリシリコンからなる半導体膜116が配置され、アクティブ素子である薄膜トランジスタ(TFT)の能動層として機能するようにされている。   A semiconductor film 116 made of amorphous silicon or polysilicon is disposed on the gate electrode 104 through a gate insulating film 107 so as to function as an active layer of a thin film transistor (TFT) as an active element.

また、半導体膜116のパターンの一部に重畳するようにクロム・モリブデンよりなるドレイン電極106,ソース電極(画素電極)105が配置され、これら全てを被覆するように窒化シリコンよりなる保護絶縁膜108が形成されている。   Further, a drain electrode 106 and a source electrode (pixel electrode) 105 made of chromium / molybdenum are arranged so as to overlap a part of the pattern of the semiconductor film 116, and a protective insulating film 108 made of silicon nitride is formed so as to cover all of them. Is formed.

この保護絶縁膜108上には、有機保護膜112が配置されている。この有機保護膜112は、例えばアクリル樹脂などの透明な材料から構成する。   An organic protective film 112 is disposed on the protective insulating film 108. The organic protective film 112 is made of a transparent material such as acrylic resin.

また、画素電極105はITO(In2O3:Sn)などの透明電極から構成されている。   The pixel electrode 105 is composed of a transparent electrode such as ITO (In2O3: Sn).

共通電極103は、ゲート絶縁膜107、保護絶縁膜108、有機保護膜112を貫通するスルーホール118を介し、共通電極配線120に接続している。   The common electrode 103 is connected to the common electrode wiring 120 through a through hole 118 that penetrates the gate insulating film 107, the protective insulating film 108, and the organic protective film 112.

液晶を駆動する電界を与える場合に、画素電極105と対をなす共通電極103は、平面的に一画素の領域を囲うように形成されている。   When an electric field for driving the liquid crystal is applied, the common electrode 103 that forms a pair with the pixel electrode 105 is formed so as to surround a region of one pixel in a plane.

また、この共通電極103は、有機保護膜(オーバーコート層)112の上に配置されている。そして、この共通電極103は、上部から見たときに下層に配置しているドレイン電極106、走査信号配線104及び能動素子である薄膜トランジスタ(TFT)を隠すように配置され、半導体膜116を遮光する遮光層を兼ねている。   The common electrode 103 is disposed on the organic protective film (overcoat layer) 112. The common electrode 103 is arranged so as to hide the drain electrode 106, the scanning signal wiring 104, and the thin film transistor (TFT) which is an active element when viewed from above, and shields the semiconductor film 116. Also serves as a light shielding layer.

なお、以上のように構成した単位画素(一画素)をマトリクス状に配置したアクティブマトリクス基板を構成するガラス基板101の表面、すなわち、有機保護膜112上及びその上に形成された共通電極103の上には、配向制御膜109が形成されている。   The surface of the glass substrate 101 constituting the active matrix substrate in which the unit pixels (one pixel) configured as described above are arranged in a matrix, that is, on the organic protective film 112 and the common electrode 103 formed thereon. An alignment control film 109 is formed thereon.

一方、対向基板を構成するガラス102にも、カラーフィルタ層111及びその上に形成される有機保護膜112、配向制御膜109が形成されている。   On the other hand, the color filter layer 111, the organic protective film 112 formed thereon, and the orientation control film 109 are also formed on the glass 102 constituting the counter substrate.

また、第1の実施の形態と同様に、高圧水銀ランプを光源とし、石英板を積層したパイル偏光子を用いて取り出される紫外線の直線偏光照射により、これらの配向制御膜109に液晶配向能が付与されている。   Similarly to the first embodiment, these alignment control films 109 have a liquid crystal alignment ability by irradiation with ultraviolet linearly polarized light extracted using a pile polarizer with a quartz plate laminated using a high-pressure mercury lamp as a light source. Has been granted.

そして、ガラス基板101と対向基板102が、配向制御膜109の形成面で対向配置され、これらの間に液晶分子110で構成された液晶組成物層110'が配置されているように構成されている。また、ガラス基板101及び対向基板102の外側の面のそれぞれには偏光板114が形成されている。   The glass substrate 101 and the counter substrate 102 are arranged so as to face each other on the formation surface of the alignment control film 109, and the liquid crystal composition layer 110 ′ composed of the liquid crystal molecules 110 is arranged therebetween. Yes. A polarizing plate 114 is formed on each of the outer surfaces of the glass substrate 101 and the counter substrate 102.

このように、本発明の第2の実施の形態においても、先に述べた第1の実施の形態と同様に、画素電極105は有機保護膜112及び保護絶縁膜108の下層に配置され、画素電極105と有機保護膜112との上に共通電極103が配置された構成となっている。   As described above, also in the second embodiment of the present invention, the pixel electrode 105 is disposed below the organic protective film 112 and the protective insulating film 108 as in the first embodiment described above. The common electrode 103 is disposed on the electrode 105 and the organic protective film 112.

また、共通電極103の電気抵抗が十分低い場合には、当該共通電極103は最下層に形成されている共通電極配線120も兼ねることができる。その際には、最下層に配置している共通電極配線120の形成及びそれに伴うスルーホールの加工を省くことができる。   Further, when the electric resistance of the common electrode 103 is sufficiently low, the common electrode 103 can also serve as the common electrode wiring 120 formed in the lowermost layer. In that case, the formation of the common electrode wiring 120 arranged in the lowermost layer and the processing of the through hole associated therewith can be omitted.

この第2の実施の形態では、図4(a)に示すように格子状に形成された共通電極103に囲まれた領域で一画素が構成され、画素電極105とあわせて一画素を4つの領域に分割するように配置されている。   In the second embodiment, as shown in FIG. 4A, one pixel is formed in a region surrounded by the common electrode 103 formed in a lattice shape, and four pixels are combined with the pixel electrode 105. It is arranged so as to be divided into areas.

また、画素電極105及びそれと対向する共通電極103がお互いに平行に配置されたジグザグな屈曲構造からなり、一画素が2つ以上の複数の副画素を形成している。これにより面内での色調変化を相殺する構造となっている。   In addition, the pixel electrode 105 and the common electrode 103 facing the pixel electrode 105 have a zigzag bent structure in which the pixel electrode 105 and the common electrode 103 are arranged in parallel to each other, and one pixel forms two or more subpixels. As a result, the color tone change in the plane is offset.

また、図5は、本発明による液晶表示装置の第3の実施の形態を説明する一画素付近の模式断面図である。図中、前記した各実施例の図面と同一符号は同一機能部分に対応する。   FIG. 5 is a schematic cross-sectional view of the vicinity of one pixel for explaining a third embodiment of the liquid crystal display device according to the present invention. In the drawing, the same reference numerals as those in the drawings of the respective embodiments described above correspond to the same functional parts.

図5に示すように、本実施の形態では、保護絶縁膜108の下層に配置した画素電極105を、スルーホール118を介して有機保護膜112上に引き上げて共通電極103と同層に配置した。この構成とした場合には、液晶を駆動する電圧をさらに低減することが可能である。   As shown in FIG. 5, in this embodiment mode, the pixel electrode 105 disposed under the protective insulating film 108 is pulled up on the organic protective film 112 through the through hole 118 and disposed in the same layer as the common electrode 103. . In this configuration, the voltage for driving the liquid crystal can be further reduced.

以上のように構成されたTFT液晶表示装置では、電界無印加時には、液晶組成物層110'を構成する液晶分子110は、対向配置されているガラス基板101と102の面にほぼ平行な状態となり、光配向処理で規定された初期配向方向に向いた状態でホモジニアス配向している。   In the TFT liquid crystal display device configured as described above, when no electric field is applied, the liquid crystal molecules 110 constituting the liquid crystal composition layer 110 ′ are in a state substantially parallel to the surfaces of the glass substrates 101 and 102 disposed opposite to each other. Homogeneous alignment is performed in the initial alignment direction defined by the photo-alignment treatment.

ここで、ゲート電極104に電圧を印加して薄膜トランジスタ(TFT)をオンにすると、画素電極105と共通電極103の間の電位差により液晶組成物層110'に電界117が印加され、液晶組成物が持つ誘電異方性と電界との相互作用により液晶分子110は電界方向にその向きを変える。このとき液晶組成物層110'の屈折異方性と偏光板114の作用により液晶表示装置の光透過率を変化させ表示を行うことができる。   Here, when a voltage is applied to the gate electrode 104 to turn on the thin film transistor (TFT), an electric field 117 is applied to the liquid crystal composition layer 110 ′ due to a potential difference between the pixel electrode 105 and the common electrode 103, and the liquid crystal composition is Due to the interaction between the dielectric anisotropy and the electric field, the liquid crystal molecules 110 change the direction in the electric field direction. At this time, display can be performed by changing the light transmittance of the liquid crystal display device by the refractive anisotropy of the liquid crystal composition layer 110 ′ and the action of the polarizing plate 114.

また、上記した本発明の各実施の形態においては、1つの画素における共通電極と画素電極から構成される表示領域は、複数組設けることが可能である。このように複数組設けることによって、1つの画素が大きい場合でも、画素電極と共通電極との間の距離を短くできるので、液晶を駆動させるために印加する電圧を小さくできる。   In each of the embodiments of the present invention described above, a plurality of display areas each including a common electrode and a pixel electrode in one pixel can be provided. By providing a plurality of sets in this manner, even when one pixel is large, the distance between the pixel electrode and the common electrode can be shortened, so that the voltage applied to drive the liquid crystal can be reduced.

また、上記した本発明の各実施の形態においては、画素電極と共通電極の少なくとも一方を構成する透明導電膜の材料としては、特に制限はないが、加工の容易さ、信頼性の高さ等を考慮して、インジウム−チン−オキサイド(ITO)のようなチタン酸化物にイオンドープされた透明導電膜又はイオンドープされた亜鉛酸化物を用いるのが望ましい。   In each of the embodiments of the present invention described above, the material of the transparent conductive film constituting at least one of the pixel electrode and the common electrode is not particularly limited, but is easy to process, high in reliability, etc. Therefore, it is desirable to use a transparent conductive film ion-doped with titanium oxide such as indium-tin-oxide (ITO) or ion-doped zinc oxide.

一般的に、IPS方式においては、従来のTN方式に代表される縦電界方式と異なり基板面との界面チルトが原理的に必要なく、界面チルト角が小さいほど視角特性がよいことが知られており、光反応性の配向制御膜においても小さい界面チルト角が望ましく、特に1度以下が効果的である。   In general, in the IPS system, it is known that the interface tilt with the substrate surface is not necessary in principle, unlike the vertical electric field system typified by the conventional TN system, and the viewing angle characteristics are better as the interface tilt angle is smaller. Even in the photo-reactive alignment control film, a small interface tilt angle is desirable, and an angle of 1 degree or less is particularly effective.

次に、本発明による液晶表示装置における液晶配向制御膜のラビングレス配向法を用いた配向制御膜の形成について説明する。本発明による配向制御膜の形成工程のフローは以下の(1)〜(4)のようになる。   Next, formation of the alignment control film using the rubbing-less alignment method of the liquid crystal alignment control film in the liquid crystal display device according to the present invention will be described. The flow of the alignment control film forming process according to the present invention is as follows (1) to (4).

(1)配向制御膜の塗膜・形成(表示領域全面にわたり均一な塗膜を形成する)。   (1) Coating / formation of orientation control film (forms a uniform coating over the entire display area).

(2)配向制御膜のイミド化焼成(ワニス溶剤の除去と耐熱性の高いポリイミド化を促進する)。   (2) Imidization firing of the orientation control film (removal of varnish solvent and promotion of polyimide with high heat resistance are promoted).

(3)偏光照射による液晶配向能付与(表示領域に均一な配向能を付与する)。   (3) Giving liquid crystal alignment ability by applying polarized light (giving uniform alignment ability to the display area).

(4)(加熱、赤外線照射、遠赤外線照射、電子線照射、放射線照射) による配向能の促進・安定化。   (4) Promotion / stabilization of alignment ability by (heating, infrared irradiation, far infrared irradiation, electron beam irradiation, radiation irradiation).

以上の4段階のプロセスを介して配向制御膜を形成するが、上記(1)〜(4)のプロセスの順番に限定されるものではなく、以下(I)(II)のような場合には、さらなる効果が期待される。   The alignment control film is formed through the above four-stage process, but is not limited to the order of the above processes (1) to (4). In the following cases (I) and (II) Further effects are expected.

(I)上記(3)、(4)を時間的に重なるように処理することにより液晶配向能付与を加速し架橋反応などを誘起することで、さらに効果的に配向制御膜を形成することが可能となる。   (I) By processing the above (3) and (4) so as to overlap in time, the alignment control film can be formed more effectively by accelerating the provision of liquid crystal alignment ability and inducing a crosslinking reaction or the like. It becomes possible.

(II)上記(4)の加熱、赤外線照射、遠赤外線照射などを用いる場合には、上記(2)、(3)、(4)を時間的にオーバーラップさせることにより、上記(4)のプロセスが上記(2)のイミド化プロセスを兼ねることも可能となり、短時間に配向制御膜の形成が可能となる。   (II) When using the heating, infrared irradiation, far-infrared irradiation, etc. of the above (4), the above (2), (3), (4) are overlapped in time, The process can also serve as the imidization process (2), and the alignment control film can be formed in a short time.

次に、本発明による液晶表示装置の製造方法の具体的な実施例について説明する。   Next, specific examples of the manufacturing method of the liquid crystal display device according to the present invention will be described.

第1実施例は、前記した本発明の第1の実施形態で説明した液晶表示装置に対応する。以下、本発明の第1実施例について、図1及び図2を参照して詳細に説明する。   The first example corresponds to the liquid crystal display device described in the first embodiment of the present invention. Hereinafter, a first embodiment of the present invention will be described in detail with reference to FIGS.

本発明の第1実施例である液晶表示装置を製造する場合において、アクティブマトリクス基板を構成するガラス基板101及び対向基板(カラーフィルタ基板)を構成するガラス基板102として、厚みが0.7mmで表面を研磨したガラス基板を用いる。   When manufacturing the liquid crystal display device according to the first embodiment of the present invention, the glass substrate 101 constituting the active matrix substrate and the glass substrate 102 constituting the counter substrate (color filter substrate) have a thickness of 0.7 mm and the surface. A glass substrate polished is used.

ガラス基板101に形成する薄膜トランジスタはソース電極(画素電極)105、ドレイン電極(信号電極)106、ゲート電極(走査電極)104及び半導体膜(アモルファスシリコン)116から構成される。   A thin film transistor formed on the glass substrate 101 includes a source electrode (pixel electrode) 105, a drain electrode (signal electrode) 106, a gate electrode (scanning electrode) 104, and a semiconductor film (amorphous silicon) 116.

走査電極104、共通電極配線120及び信号電極106、画素電極105は、全てクロム膜をパターニングして形成し、画素電極105と共通電極103との間隔は7μmとした。   The scanning electrode 104, the common electrode wiring 120, the signal electrode 106, and the pixel electrode 105 were all formed by patterning a chromium film, and the distance between the pixel electrode 105 and the common electrode 103 was 7 μm.

なお、共通電極103と画素電極105については、低抵抗でパターニングの容易なクロム膜を使用したが、ITO膜を使用し透明電極を構成して、より高い輝度特性の達成することも可能である。   For the common electrode 103 and the pixel electrode 105, a chromium film having low resistance and easy patterning is used. However, a transparent electrode can be formed using an ITO film to achieve higher luminance characteristics. .

ゲート絶縁膜107と保護絶縁膜108は窒化珪素からなり、膜厚はそれぞれ0.3μmとした。その上にはアクリル系樹脂を塗布し、220°C、1時間の加熱処理により透明で絶縁性のある有機保護膜112を形成した。   The gate insulating film 107 and the protective insulating film 108 were made of silicon nitride, and the film thicknesses were each 0.3 μm. An acrylic resin was applied thereon, and a transparent and insulating organic protective film 112 was formed by heat treatment at 220 ° C. for 1 hour.

次に、フォトリソグラフィ、エッチング処理により、図2(c)に示すように共通電極配線120までスルーホールを形成し、共通電極配線120と接続する共通電極103をパターニングして形成した。   Next, through holes were formed up to the common electrode wiring 120 by photolithography and etching, and the common electrode 103 connected to the common electrode wiring 120 was formed by patterning as shown in FIG.

その結果、単位画素(一画素)内では、図2(a)に示すように、画素電極105が3本の共通電極103の間に配置されている構成となり、画素数は1024×3(R、G、Bに対応)本の信号電極106と768本の走査電極104とから構成される1024×3×768個とするアクティブマトリクス基板を形成した。   As a result, in the unit pixel (one pixel), as shown in FIG. 2A, the pixel electrode 105 is arranged between the three common electrodes 103, and the number of pixels is 1024 × 3 (R , G, and B), an active matrix substrate having 1024 × 3 × 768 composed of signal electrodes 106 and 768 scanning electrodes 104 was formed.

次に、配向制御膜として、下記一般式〔化合物23〕に示す1,4−ジアミノピリジンと下記一般式〔化合物24〕に示す1−メチル−1,2,3,4−シクロブタンテトラカルボン酸二無水物からなるポリアミック酸ワニスを、樹脂分濃度5重量%、NMP60重量%、γブチルラクトン20重量%、ブチルセロソルブ15重量%に調整し、上記アクティブマトリクス基板の上に印刷形成して220°Cで30分の熱処理によりイミド化し、約70nmの緻密なポリイミド配向制御膜109を形成する。

Figure 0005594835
Figure 0005594835
Next, as the alignment control film, 1,4-diaminopyridine represented by the following general formula [Compound 23] and 1-methyl-1,2,3,4-cyclobutanetetracarboxylic acid diester represented by the following general formula [Compound 24] are used. A polyamic acid varnish composed of an anhydride was adjusted to a resin concentration of 5% by weight, NMP 60% by weight, γ-butyllactone 20% by weight, butyl cellosolve 15% by weight, printed on the active matrix substrate at 220 ° C. Imidization is performed by heat treatment for 30 minutes to form a dense polyimide orientation control film 109 having a thickness of about 70 nm.
Figure 0005594835
Figure 0005594835

同様に、ITOを成膜した、もう一方のガラス基板102の表面にも同様のポリアミック酸ワニスを印刷形成し、220°Cで30分の熱処理を行い、約70nmの緻密なポリイミド膜からなる配向制御膜109を形成した。   Similarly, the same polyamic acid varnish is printed on the surface of the other glass substrate 102 on which ITO has been formed, heat-treated at 220 ° C. for 30 minutes, and an orientation composed of a dense polyimide film of about 70 nm. A control film 109 was formed.

その表面に液晶配向能を付与するために、偏光UV(紫外線)光をポリイミド配向制御膜109に照射した。光源には高圧水銀ランプを用い、干渉フィルタを介して、240nm〜380nmの範囲のUV光を取り出し、石英基板を積層したパイル偏光子を用いて偏光比約10:1の直線偏光とし、約5J/cm2の照射エネルギーで照射した。 In order to give the liquid crystal alignment ability to the surface, the polyimide alignment control film 109 was irradiated with polarized UV (ultraviolet) light. A high pressure mercury lamp is used as a light source, UV light in the range of 240 nm to 380 nm is taken out through an interference filter, and is converted into linearly polarized light with a polarization ratio of about 10: 1 using a pile polarizer laminated with a quartz substrate. Irradiation was performed with an irradiation energy of / cm 2 .

その結果、配向制御膜表面の液晶分子の配向方向は、照射した偏光UVの偏光方向に対し、直交方向であることがわかった。   As a result, it was found that the alignment direction of the liquid crystal molecules on the surface of the alignment control film was orthogonal to the polarization direction of the irradiated polarized UV light.

次に、これらの2枚のガラス基板101、102を、それぞれの液晶配向能を有する配向制御膜109を有する表面を相対向させて、分散させた球形のポリマビ−ズからなるスペ−サを介在させ、周辺部にシ−ル剤を塗布し、液晶表示装置となる液晶表示パネル(セルとも称する)を組み立てた。2枚のガラス基板の液晶配向方向は、互いにほぼ並行で、かつ印加電界方向とのなす角度を75゜とした。   Next, these two glass substrates 101 and 102 are interspersed with spacers made of spherical polymer beads dispersed with their surfaces having alignment control films 109 having liquid crystal alignment ability facing each other. Then, a sealant was applied to the peripheral portion, and a liquid crystal display panel (also referred to as a cell) to be a liquid crystal display device was assembled. The liquid crystal alignment directions of the two glass substrates were substantially parallel to each other, and the angle formed with the applied electric field direction was 75 °.

このセルに誘電異方性Δεが正で、その値が10.2(1kHz、20°C)であり、屈折率異方性Δnが0.075(波長590nm、20°C)、ねじれ弾性定数K2が7.0pN、ネマティック−等方相転移温度T(N−I)が約76°Cのネマティック液晶組成物Aを真空で注入し、紫外線硬化型樹脂からなる封止材で封止した。液晶層の厚み(ギャップ)は4.2μmの液晶パネルを製作した。   This cell has a positive dielectric anisotropy Δε, a value of 10.2 (1 kHz, 20 ° C.), a refractive index anisotropy Δn of 0.075 (wavelength 590 nm, 20 ° C.), and a torsional elastic constant. A nematic liquid crystal composition A having a K2 of 7.0 pN and a nematic-isotropic phase transition temperature T (NI) of about 76 ° C. was injected in a vacuum and sealed with a sealing material made of an ultraviolet curable resin. A liquid crystal panel having a liquid crystal layer thickness (gap) of 4.2 μm was produced.

この液晶表示パネルのリタデーション(Δnd)は、約0.31μmとなる。また、このパネルに用いた配向制御膜と液晶組成物と同等のものを用いてホモジニアス配向の液晶表示パネルを作製し、クリスタルローテーション法を用いて液晶のプレチルト角を測定したところ約0.2度を示した。   The retardation (Δnd) of this liquid crystal display panel is about 0.31 μm. Also, a homogeneous alignment liquid crystal display panel was prepared using the alignment control film and the liquid crystal composition used in this panel, and the pretilt angle of the liquid crystal was measured using the crystal rotation method. showed that.

この液晶表示パネルを2枚の偏光板114で挾み、一方の偏光板の偏光透過軸を上記の液晶配向方向とほぼ平行とし、他方をそれに直交するように配置した。   This liquid crystal display panel was sandwiched between two polarizing plates 114, and the polarizing transmission axis of one polarizing plate was set substantially parallel to the liquid crystal alignment direction, and the other was arranged so as to be orthogonal thereto.

その後、駆動回路、バックライトなどを接続してモジュール化し、アクティブマトリクス型の液晶表示装置を得た。本実施例では低電圧で暗表示、高電圧で明表示となるノーマリークローズ特性とした。   Thereafter, a drive circuit, a backlight, and the like were connected to form a module, and an active matrix liquid crystal display device was obtained. In this embodiment, a normally closed characteristic is obtained in which dark display is performed at a low voltage and bright display is performed at a high voltage.

次に、本発明の第1実施例である上記の液晶表示装置の表示品位を評価したところ、コントラスト比600対1の高品位の表示が確認されるとともに、中間調表示時における広視野角が確認された。   Next, when the display quality of the liquid crystal display device according to the first embodiment of the present invention was evaluated, a high quality display with a contrast ratio of 600: 1 was confirmed, and a wide viewing angle at the time of halftone display was obtained. confirmed.

また次に、本発明の第1実施例である液晶表示装置の画像の焼き付け、残像を定量的に測定するため、ホトダイオードを組合せたオシロスコープを用いて評価した。   Next, in order to quantitatively measure image printing and afterimage of the liquid crystal display device according to the first embodiment of the present invention, evaluation was performed using an oscilloscope combined with a photodiode.

まず、画面上に最大輝度でウインドウパターンを30分間表示し、その後、残像が最も目立つ中間調表示、ここでは輝度が最大輝度の10%となるように全面を切り換え、ウインドウパターンのエッジ部のパターンが消えるまでの時間を残像緩和時間として評価した。ただし、ここで許容される残像緩和時間は5分以下である。   First, the window pattern is displayed on the screen at the maximum brightness for 30 minutes, and then the halftone display in which the afterimage is most noticeable. Here, the entire surface is switched so that the brightness is 10% of the maximum brightness, and the pattern of the edge portion of the window pattern. The time until disappearance was evaluated as the afterimage relaxation time. However, the afterimage relaxation time allowed here is 5 minutes or less.

その結果、使用温度範囲(0°C〜50°C)において、残像の緩和時間は1分以下であり、目視による画質残像検査においても、画像の焼き付け、残像による表示むらも一切見られず、高い表示特性が得られた。   As a result, in the operating temperature range (0 ° C. to 50 ° C.), the afterimage relaxation time is 1 minute or less, and even in visual image quality afterimage inspection, image burning and display unevenness due to afterimage are not seen at all. High display characteristics were obtained.

従来、光配向では液晶の配向性を付与することはできるが、アンカリングエネルギー、すなわち、配向した液晶分子を配向膜表面に束縛するエネルギーが、一般のラビング配向に比べ弱いといわれている。   Conventionally, although alignment of liquid crystals can be imparted by photo-alignment, it is said that anchoring energy, that is, energy for constraining aligned liquid crystal molecules to the alignment film surface is weaker than that of general rubbing alignment.

このアンカリングエネルギーが弱いと液晶表示装置の製品としての信頼性が不足するとも言われている。特に、ホモジニアス配向の場合には、極角方向のアンカリングエネルギーよりも方位角方向のアンカリングエネルギーが重要といわれている。   If the anchoring energy is weak, it is said that the reliability of the liquid crystal display device is insufficient. In particular, in the case of homogeneous orientation, anchoring energy in the azimuth direction is more important than anchoring energy in the polar angle direction.

そこで、この様にして得た液晶表示装置と同一の配向膜材料を用い、同一プロセスでガラス基板上に配向膜を形成、配向処理し、同一の液晶組成物を封入して液晶セルを作製し、トルクバランス法(長谷川ほか、液晶学会討論会講演予行集3B12(2001)p.251)により、界面における液晶分子と配向膜表面とのねじれ結合の強さ、方位角方位アンカリングエネルギーA2を測定すると、7.0×10‐4N/mであった。以下で示す比較例1では、このA2は8.6×10‐5N/mである。 Therefore, using the same alignment film material as the liquid crystal display device thus obtained, an alignment film is formed on the glass substrate by the same process, the alignment treatment is performed, and the same liquid crystal composition is sealed to produce a liquid crystal cell. Measure the strength of torsional coupling between the liquid crystal molecules and the alignment film surface at the interface and the azimuthal anchoring energy A2 by the torque balance method (Hasegawa et al., Liquid Crystal Society Annual Meeting Lecture Collection 3B12 (2001) p.251) Then, was 7.0 × 10- 4 N / m. In Comparative Example 1 shown below, the A2 is 8.6 × 10- 5 N / m.

第2実施例で用いた配向制御膜以外は第1実施例と同様にして、酸二無水物として、下記一般式〔化合物25〕に示したテトラカルボン酸二無水物と、下記一般式〔化合物26〕に示したジアミン化合物として3,4−ジアミノチオフェンからなるポリアミック酸を基板表面に印刷形成して、220°Cで30分の焼成でイミド化を行い、膜厚約40nmに成膜した。その後、その表面にKrFエキシマレーザの波長248nmと窒素レーザの337nmの偏光UVを用いた光照射による光配向処理を行った。

Figure 0005594835
Figure 0005594835
The tetracarboxylic dianhydride shown in the following general formula [Compound 25] and the following general formula [Compound] as the acid dianhydride are the same as in the first example except for the orientation control film used in the second example. 26], a polyamic acid composed of 3,4-diaminothiophene was printed on the surface of the substrate, imidized by baking at 220 ° C. for 30 minutes, and a film thickness of about 40 nm was formed. Thereafter, the surface was subjected to photo-alignment treatment by light irradiation using polarized UV light having a wavelength of 248 nm of KrF excimer laser and 337 nm of nitrogen laser.
Figure 0005594835
Figure 0005594835

その後、第1実施例と同様にネマティック液晶組成物Aを封入後、100°Cで10分のアニーリングを施し、上記の照射偏光方向に対してほぼ垂直方向に良好な液晶配向を得た。   Then, after encapsulating the nematic liquid crystal composition A in the same manner as in the first example, annealing was performed at 100 ° C. for 10 minutes, and good liquid crystal alignment was obtained in a direction substantially perpendicular to the irradiation polarization direction.

このようにして、液晶層の厚みdが4.0μmの液晶表示パネルを得た。また、この液晶表示パネルに用いた配向制御膜と液晶組成物と同等のものを用いて、ホモジニアス配向の液晶表示パネルを作製し、クリスタルローテーション法を用いて液晶のプレチルト角を測定したところ約0.5度を示した。   Thus, a liquid crystal display panel having a liquid crystal layer thickness d of 4.0 μm was obtained. Further, a homogeneous alignment liquid crystal display panel was prepared using the alignment control film and the liquid crystal composition used in this liquid crystal display panel, and the pretilt angle of the liquid crystal was measured by the crystal rotation method. .5 degrees.

次に、第1実施例同様の方法で、液晶表示装置の表示品位を評価したところ、第1実施例の液晶表示装置とほぼ同等のコントラスト比が、全面に渡り500:1を越える高品位の表示が確認されるとともに、中間調表示時における広い視野角も確認された。   Next, when the display quality of the liquid crystal display device was evaluated in the same manner as in the first example, the contrast ratio almost equivalent to that of the liquid crystal display device of the first example was high quality exceeding 500: 1 over the entire surface. The display was confirmed, and a wide viewing angle during halftone display was also confirmed.

また、第1実施例と同様にして、この液晶表示装置の画像の焼き付け、残像の緩和時間を定量評価したところ、0°C〜50°Cの使用温度範囲において、残像の緩和時間は約1分であり、目視による画質残像検査においても、画像の焼き付け、残像による表示むらも一切見られず、実施例1同等の高い表示特性が得られた。   Similarly to the first embodiment, the image printing and afterimage relaxation time of this liquid crystal display device were quantitatively evaluated. As a result, the afterimage relaxation time was about 1 in the operating temperature range of 0 ° C. to 50 ° C. Even in visual image quality afterimage inspection, no image burning or display unevenness due to afterimage was observed, and high display characteristics equivalent to Example 1 were obtained.

〔比較例1〕
本実施例の効果を説明するための比較例として、配向制御膜以外は第1実施例の場合と同様にして、酸二無水物として、下記一般式〔化合物27〕に示したピロメリット酸二無水物と、ジアミン化合物として、下記一般式〔化合物28〕に示したm−フェニレンジアミンからなるポリアミック酸ワニスを用いて液晶表示パネルを構成した。

Figure 0005594835
Figure 0005594835
[Comparative Example 1]
As a comparative example for explaining the effect of the present example, pyromellitic acid dibenzoate represented by the following general formula [Compound 27] was used as an acid dianhydride in the same manner as in the first example except for the orientation control film. A liquid crystal display panel was constructed using a polyamic acid varnish composed of m-phenylenediamine represented by the following general formula [Compound 28] as an anhydride and a diamine compound.
Figure 0005594835
Figure 0005594835

これを第1実施例と同様の方法で表示品位を評価したところ、第1実施例の液晶表示装置とほぼ同等の広い視野角が確認されたものの、コントラスト比が、全面に渡り100:1を下回る表示であることが確認された。   When the display quality was evaluated in the same manner as in the first example, a wide viewing angle almost the same as that of the liquid crystal display device in the first example was confirmed, but the contrast ratio was 100: 1 over the entire surface. It was confirmed that the display was lower.

また、第1実施例と同様にして、この液晶表示装置の画像の焼き付け、残像の緩和時間を定量評価したところ、0°C〜50°Cの使用温度範囲において残像の緩和時間が、約20分と、目視による画質残像検査においても残像の緩和時間が遅く、実施例1同等の高い表示特性は得られなかった。なお、方位角方位アンカリングエネルギーA2の値は約8.6×10‐5N/mであった。 Further, in the same manner as in the first embodiment, when the image printing and afterimage relaxation time of this liquid crystal display device were quantitatively evaluated, the afterimage relaxation time was about 20 in the operating temperature range of 0 ° C to 50 ° C. Even in visual image quality afterimage inspection, the afterimage relaxation time was slow, and high display characteristics equivalent to Example 1 were not obtained. The value of the azimuthal orientation anchoring energy A2 was about 8.6 × 10- 5 N / m.

第3実施例で用いた配向制御膜以外は第1実施例と同様にして、酸二無水物として、下記一般式〔化合物29〕に示す1,3−ジメチル−1,2,3,4−シクロブタンテトラカルボン酸二無水物と、下記一般式〔化合物30〕に示すピロメリット酸二無水物をモル比にして7:3とし、ジアミン化合物として、下記一般式〔化合物31〕に示すp−フェニレンジアミンを用いて、ポリアミック酸ワニスを調整し液晶表示パネルを作製した。その際、配向制御膜の膜厚は約50nmとした。

Figure 0005594835
Figure 0005594835
Figure 0005594835
Except for the orientation control film used in the third example, the acid dianhydride was used as an acid dianhydride as shown in the following general formula [Compound 29] 1,3-dimethyl-1,2,3,4- Cyclobutanetetracarboxylic dianhydride and pyromellitic dianhydride represented by the following general formula [Compound 30] in a molar ratio of 7: 3, and a diamine compound, p-phenylene represented by the following general formula [Compound 31] A polyamic acid varnish was prepared using diamine to prepare a liquid crystal display panel. At that time, the film thickness of the orientation control film was about 50 nm.
Figure 0005594835
Figure 0005594835
Figure 0005594835

次に、第1実施例と同様の方法で、液晶表示装置の表示品位を評価したところ、第1実施例の液晶表示装置とほぼ同等のコントラスト比が、全面に渡り550:1を越える高品位の表示が確認されるとともに、中間調表示時における広い視野角も確認された。   Next, when the display quality of the liquid crystal display device was evaluated in the same manner as in the first example, the contrast ratio almost the same as that of the liquid crystal display device of the first example was higher than 550: 1 over the entire surface. And a wide viewing angle during halftone display were also confirmed.

また、本発明の第1実施例と同様にして、この液晶表示装置の画像の焼き付け、残像の緩和時間を定量評価したところ、0°C〜50°Cの使用温度範囲において残像の緩和時間は、約1分であり、目視による画質残像検査においても、画像の焼き付け、残像による表示むらも一切見られず、実施例1同等の高い表示特性が得られた。   Similarly to the first embodiment of the present invention, when the image printing and afterimage relaxation time of this liquid crystal display device were quantitatively evaluated, the afterimage relaxation time was 0 ° C to 50 ° C in the operating temperature range. In the visual image afterimage inspection, no image printing or display unevenness due to the afterimage was observed at all, and the same high display characteristics as in Example 1 were obtained.

さらに、配向制御膜に用いたポリアミック酸ワニスの上記2種類の酸無水物1,3−ジメチル−1,2,3,4−シクロブタンテトラカルボン酸二無水物とピロメリット酸二無水物の組成比を1:1と3:7した2種類のポリアミック酸ワニスを調整し、それぞれを用いて2種類の液晶表示パネルを作製した。この液晶表示パネルを用いた液晶表示装置のコントラスト比は、それぞれ約450:1、180:1の結果を得た。   Furthermore, the composition ratio of the above two types of acid anhydrides 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride and pyromellitic dianhydride of the polyamic acid varnish used for the orientation control film Two types of polyamic acid varnishes having a ratio of 1: 1 and 3: 7 were prepared, and two types of liquid crystal display panels were produced using each. The contrast ratio of the liquid crystal display device using this liquid crystal display panel was about 450: 1 and 180: 1, respectively.

また、残像の緩和時間は、それぞれ約3分と8分という結果が得られ、酸無水物1,3−ジメチル−1,2,3,4−シクロブタンテトラカルボン酸二無水物とピロメリット酸二無水物の組成比3:7の場合にはその他の場合に比べ表示特性が著しく低下した。   The afterimage relaxation times were about 3 minutes and 8 minutes, respectively, and the acid anhydride 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride and pyromellitic acid 2 were obtained. When the composition ratio of the anhydride was 3: 7, the display characteristics were remarkably reduced as compared with the other cases.

次に、本発明の第2の実施形態である液晶表示装置の具体的構成として、第4実施例を図3及び図4を用いて説明する。本発明の第4実施例である液晶表示装置を製造する場合において、ガラス基板101及び102としては、厚みが0.7mmで表面を研磨したガラス基板を用いる。   Next, as a specific configuration of the liquid crystal display device according to the second embodiment of the present invention, a fourth example will be described with reference to FIGS. In the case of manufacturing the liquid crystal display device according to the fourth embodiment of the present invention, as the glass substrates 101 and 102, glass substrates having a thickness of 0.7 mm and polished surfaces are used.

薄膜トランジスタはソース電極(画素電極)105、ドレイン電極(信号電極)106、ゲート電極(走査電極)104及び半導体膜(アモルファスシリコン)116から構成される。走査電極104は、アルミニウム膜をパターニングし、共通電極配線120及び信号電極106は、クロム膜をパターニングし、画素電極105は、ITO膜をパターニングし、図4(a)に示すように、走査電極104以外はジグザグに屈曲した電極配線パターンに形成した。その際屈曲の角度は10度に設定した。ゲート絶縁膜107と保護絶縁膜108は窒化珪素からなり、膜厚はそれぞれ0.3μmとした。   The thin film transistor includes a source electrode (pixel electrode) 105, a drain electrode (signal electrode) 106, a gate electrode (scanning electrode) 104, and a semiconductor film (amorphous silicon) 116. The scan electrode 104 is formed by patterning an aluminum film, the common electrode wiring 120 and the signal electrode 106 are formed by patterning a chromium film, and the pixel electrode 105 is formed by patterning an ITO film. As shown in FIG. The electrode wiring patterns other than 104 were formed in a zigzag bent electrode wiring pattern. At that time, the angle of bending was set to 10 degrees. The gate insulating film 107 and the protective insulating film 108 were made of silicon nitride, and the film thicknesses were each 0.3 μm.

次に、フォトリソグラフィ法とエッチング処理により、図4(c)に示すように、共通電極配線120まで約10μm径の円筒状にスルーホール118を形成し、その上にはアクリル系樹脂を塗布し、220°C、で1時間の加熱処理により透明で絶縁性のある誘電率約4の層間絶縁膜112を約1μm厚に形成した。この層間絶縁膜112により表示領域の画素電極105の段差起因の凹凸ならびに隣接する画素間のカラーフィルタ層111の境界部分の段差凹凸を平坦化した。   Next, as shown in FIG. 4C, through holes 118 are formed in a cylindrical shape having a diameter of about 10 μm to the common electrode wiring 120 by photolithography and etching, and an acrylic resin is applied thereon. An interlayer insulating film 112 having a dielectric constant of about 4 having a dielectric constant of about 4 μm was formed by heat treatment at 220 ° C. for 1 hour to a thickness of about 1 μm. By this interlayer insulating film 112, the unevenness due to the step of the pixel electrode 105 in the display area and the step unevenness of the boundary portion of the color filter layer 111 between adjacent pixels are flattened.

その後、約7μm径にスルーホール118を再度エッチング処理し、その上から共通電極配線120と接続する共通電極103をITO膜をパターニングして形成した。その際、画素電極105と共通電極103との間隔は7μmとした。さらに、この共通電極103は、映像信号配線106、走査信号配線104及び薄膜トランジスタの上部を覆い画素を囲むように格子状に形成し、遮光層を兼ねるようにした。   Thereafter, the through hole 118 was etched again to a diameter of about 7 μm, and the common electrode 103 connected to the common electrode wiring 120 was formed by patterning the ITO film thereon. At that time, the distance between the pixel electrode 105 and the common electrode 103 was set to 7 μm. Further, the common electrode 103 is formed in a lattice shape so as to cover the upper part of the video signal wiring 106, the scanning signal wiring 104, and the thin film transistor so as to surround the pixel, and also serves as a light shielding layer.

その結果、単位画素内では図4(a)に示すように、画素電極105が3本の共通電極103の間に配置されている構成となり、画素数は1024×3(R、G、Bに対応)本の信号電極106と768本の走査電極104とから構成される1024×3×768個とするアクティブマトリクス基板が得られた。   As a result, in the unit pixel, as shown in FIG. 4A, the pixel electrode 105 is arranged between the three common electrodes 103, and the number of pixels is 1024 × 3 (R, G, B). Correspondence) A 1024 × 3 × 768 active matrix substrate composed of signal electrodes 106 and 768 scanning electrodes 104 was obtained.

次に、配向制御膜109として、下記一般式〔化合物32〕に示す1,2,3,4−テトラメチル−1,2,3,4−シクロブタンテトラカルボン酸二無水物と、下記一般式〔化合物33〕に示すm−フェニレンジアミンからなるポリアミック酸ワニスを用い、膜厚約60nmの配向制御膜を作製し、その配向処理方法は、実施例1と同様の偏光UVを約3Jcm-2の照射エネルギーで照射した。ただし、偏光UV照射中に、配向制御膜の形成してある基板をホットプレート上で約150℃に加熱処理も同時に実施した。

Figure 0005594835
Figure 0005594835
Next, as the orientation control film 109, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride represented by the following general formula [Compound 32] and the following general formula [ Using a polyamic acid varnish composed of m-phenylenediamine shown in Compound 33], an alignment control film having a film thickness of about 60 nm was prepared, and the alignment treatment method was the same as in Example 1 with irradiation of polarized UV of about 3 Jcm-2. Irradiated with energy. However, during the polarized UV irradiation, the substrate on which the alignment control film was formed was also subjected to a heat treatment at about 150 ° C. on a hot plate.
Figure 0005594835
Figure 0005594835

次に、これらの2枚のガラス基板を、それぞれの液晶配向膜を有する表面を相対向させて、分散させた球形のポリマービーズからなるスペーサを介在させて、周辺部にシール剤を塗布し、液晶表示パネルを組み立てた。2枚のガラス基板の液晶配向方向は、互いにほぼ並行で、かつ印加電界方向とのなす角度を75゜とした。   Next, with these two glass substrates, the surfaces having the respective liquid crystal alignment films are opposed to each other, a spacer made of dispersed spherical polymer beads is interposed, and a sealant is applied to the peripheral portion, A liquid crystal display panel was assembled. The liquid crystal alignment directions of the two glass substrates were substantially parallel to each other, and the angle formed with the applied electric field direction was 75 °.

この液晶表示パネルに誘電異方性Δεが正で、その値が10.2(1kHz、20°C)であり、屈折率異方性Δnが0.075(波長590nm、20°C)、ねじれ弾性定数K2が7.0pN、ネマティック−等方相転移温度T(N−I)が約76°Cのネマティック液晶組成物Aを真空で注入し、紫外線硬化型樹脂からなる封止材で封止した。液晶層の厚み(ギャップ)は4.2μmの液晶パネルを製作した。このパネルのリタデーション(Δnd)は、約0.31μmとなる。   This liquid crystal display panel has a positive dielectric anisotropy Δε, a value of 10.2 (1 kHz, 20 ° C.), a refractive index anisotropy Δn of 0.075 (wavelength 590 nm, 20 ° C.), and a twist. A nematic liquid crystal composition A having an elastic constant K2 of 7.0 pN and a nematic-isotropic phase transition temperature T (NI) of about 76 ° C. is injected in a vacuum and sealed with a sealing material made of an ultraviolet curable resin. did. A liquid crystal panel having a liquid crystal layer thickness (gap) of 4.2 μm was produced. The retardation (Δnd) of this panel is about 0.31 μm.

また、この液晶表示パネルに用いた配向制御膜と液晶組成物と同等のものを用いてホモジニアス配向の液晶表示パネルを作製し、クリスタルローテーション法を用いて液晶のプレチルト角を測定したところ約0.2度を示した。   Further, a homogeneous alignment liquid crystal display panel was prepared using the alignment control film and the liquid crystal composition equivalent to the liquid crystal display panel, and the pretilt angle of the liquid crystal was measured by the crystal rotation method. Showed twice.

このパネルを2枚の偏光板114で挾み、一方の偏光板の偏光透過軸を上記の液晶配向方向とほぼ平行とし、他方をそれに直交するように配置した。その後、駆動回路、バックライトなどを接続してモジュール化し、アクティブマトリクス型の液晶表示装置を得た。本実施例では低電圧で暗表示、高電圧で明表示となるノーマリークローズ特性とした。   This panel was sandwiched between two polarizing plates 114, and the polarizing transmission axis of one polarizing plate was made substantially parallel to the liquid crystal alignment direction, and the other was arranged so as to be orthogonal thereto. Thereafter, a drive circuit, a backlight, and the like were connected to form a module, and an active matrix liquid crystal display device was obtained. In this embodiment, a normally closed characteristic is obtained in which dark display is performed at a low voltage and bright display is performed at a high voltage.

次に、本発明の第4実施例である液晶表示装置の表示品位を評価したところ、第1の実施例の液晶表示装置に比べて開口率が高く、コントラスト比600:1の高品位の表示が確認されるとともに、中間調表示時における広視野角も確認された。   Next, when the display quality of the liquid crystal display device according to the fourth embodiment of the present invention was evaluated, the aperture ratio was higher than that of the liquid crystal display device according to the first embodiment, and a high quality display with a contrast ratio of 600: 1. As well as a wide viewing angle during halftone display.

また、本発明の第1実施例と同様にして、この液晶表示装置の画像の焼き付け、残像の緩和時間を定量評価したところ、0°C〜50°Cの使用温度範囲において残像の緩和時間は、約1分であり、目視による画質残像検査においても、画像の焼き付け、残像による表示むらも一切見られず、実施例1同等の高い表示特性が得られた。   Similarly to the first embodiment of the present invention, when the image printing and afterimage relaxation time of this liquid crystal display device were quantitatively evaluated, the afterimage relaxation time was 0 ° C to 50 ° C in the operating temperature range. In the visual image afterimage inspection, no image printing or display unevenness due to the afterimage was observed at all, and the same high display characteristics as in Example 1 were obtained.

また、本実施例と同様の方法でガラス基板上に作製した配向制御膜を削り取り、示差走査熱量計(DSC;Differential Scanning Calorimetry )を用いて、配向制御膜のガラス転移温度を評価したところ、50°C〜300°Cまでの温度範囲では明確なガラス転移点を確認することができなかった。したがって、本実施例の配向制御膜のガラス転移温度は測定温度上限の300°C以上と考えられる。   Moreover, when the orientation control film produced on the glass substrate by the method similar to a present Example was scraped off and the glass transition temperature of the orientation control film was evaluated using the differential scanning calorimeter (DSC), 50 was measured. A clear glass transition point could not be confirmed in the temperature range from ° C to 300 ° C. Therefore, the glass transition temperature of the alignment control film of this example is considered to be 300 ° C. or more, which is the upper limit of the measurement temperature.

配向制御膜として、下記一般式〔化合物34〕に示す1,2,3,4−シクロブタンテトラカルボン酸二無水物と、下記一般式〔化合物35〕に示す2,7−ジアミノカルバゾールからなるポリアミック酸ワニスを用い、膜厚約100nmの配向制御膜を作製し、その配向処理方法は、第1実施例と同様の高圧水銀ランプからの光を干渉フィルタと石英のパイル偏光子を用いて、240nm〜380nmの波長範囲で10:1の偏光比の偏光UVとし、照射エネルギーは約5J/cm2 で照射した。それ以外は第4実施例と同様にして第5実施例の液晶表示パネルを作製した。

Figure 0005594835
Figure 0005594835
As an orientation control film, a polyamic acid comprising 1,2,3,4-cyclobutanetetracarboxylic dianhydride represented by the following general formula [Compound 34] and 2,7-diaminocarbazole represented by the following general formula [Compound 35] An alignment control film having a film thickness of about 100 nm is prepared using a varnish, and the alignment treatment method uses light from a high-pressure mercury lamp similar to that of the first embodiment using an interference filter and a quartz pile polarizer. Irradiation was performed with a polarized UV of 10: 1 in the wavelength range of 380 nm and an irradiation energy of about 5 J / cm2. Other than that was carried out similarly to 4th Example, and produced the liquid crystal display panel of 5th Example.
Figure 0005594835
Figure 0005594835

この液晶表示パネルを用いて得た液晶表示装置の表示品位を評価したところ、第4実施例の液晶表示装置と同等の高品位の表示が確認された。また中間調表示時における広視野角も確認された。   When the display quality of the liquid crystal display device obtained using this liquid crystal display panel was evaluated, a high quality display equivalent to that of the liquid crystal display device of the fourth example was confirmed. Also, a wide viewing angle during halftone display was confirmed.

また、本発明の第1実施例と同様にして、この第5実施例の液晶表示装置の画像の焼き付け、残像の緩和時間を定量評価したところ、0°C〜45°Cの使用温度範囲において、残像の緩和時間は、第4実施例4同様に1分以下であり、目視による画質残像検査においても、画像の焼き付け、残像による表示むらも一切見られず、高い表示特性が得られた。   Similarly to the first embodiment of the present invention, when the image printing and afterimage relaxation times of the liquid crystal display device of the fifth embodiment were quantitatively evaluated, the operating temperature range of 0 ° C. to 45 ° C. was used. The afterimage relaxation time was 1 minute or less as in the fourth embodiment, and even in visual image quality afterimage inspection, no image burn-in and display unevenness due to afterimage were observed, and high display characteristics were obtained.

また、第4実施例と同様の方法でガラス基板上に作製した配向制御膜を削り取り、示差走査熱量計(DSC;Differential Scanning Calorimetry )を用いて、配向制御膜のガラス転移温度を評価したところ、50°C〜300°Cまでの温度範囲では明確なガラス転移点を確認することができなかった。したがって、本実施例の配向制御膜のガラス転移温度は測定温度上限の300°C以上と考えられる。   Moreover, when the orientation control film | membrane produced on the glass substrate by the method similar to 4th Example was shaved off and the glass transition temperature of the orientation control film was evaluated using the differential scanning calorimeter (DSC; Differential Scanning Calorimetry), A clear glass transition point could not be confirmed in the temperature range from 50 ° C to 300 ° C. Therefore, the glass transition temperature of the alignment control film of this example is considered to be 300 ° C. or more, which is the upper limit of the measurement temperature.

また、酸無水物として1,3−ジメチル−1,2,3,4−シクロブタンテトラカルボン酸二無水物を用い、照射エネルギーを約3J/cm2として本実施例と同様に液晶表示装置を作製、評価したところ、本実施例と同等の表示特性を持つ液晶表示装置が得られた。   Further, 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride was used as the acid anhydride, and the liquid crystal display device was produced in the same manner as in this example, with the irradiation energy set to about 3 J / cm 2. As a result of evaluation, a liquid crystal display device having display characteristics equivalent to those of this example was obtained.

また、酸無水物として1,2,3,4−テトラメチル−1,2,3,4−シクロブタンテトラカルボン酸二無水物を用い、照射エネルギーを約2J/cm2として本実施例と同様に液晶表示装置を作製したところ、本実施例と同等の表示特性を持つ液晶表示装置が得られた。   Also, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride is used as the acid anhydride, and the irradiation energy is about 2 J / cm @ 2 as in the present embodiment. When a display device was produced, a liquid crystal display device having display characteristics equivalent to those of this example was obtained.

液晶表示装置のセルギャップ制御に用いているポリマービーズからなるスペーサの代わりに、予めアクティブマトリクス基板の配向制御膜を形成する前にネガ型の感光性のアクリル系樹脂を塗布・露光・現像処理により、約10μm径の柱状にパターニングして、各画素のTFT部分の近傍で走査配線104の上層の遮光層である共通電極103上に形成し、その後に配向制御膜として、ジアミン化合物として、下記一般式〔化合物36〕に示した1−アミノ−2−(4’−アミノフェニル)−エテンと、下記一般式〔化合物37〕に示した3,6−ジアミノインダセンをモル比1:2の割合とし、酸無水物として、下記一般式〔化合物38〕に示した1,3−ジクロロ−1,2,3,4−シクロブタンテトラカルボン酸二無水物を用いてポリアミック酸ワニスを調整し、膜厚約40nmに製膜した。

Figure 0005594835
Figure 0005594835
Figure 0005594835
Instead of the spacers made of polymer beads used to control the cell gap of the liquid crystal display device, a negative photosensitive acrylic resin is applied, exposed and developed before forming the alignment control film on the active matrix substrate in advance. Then, patterning is performed in a column shape with a diameter of about 10 μm, and is formed on the common electrode 103 that is the upper light shielding layer of the scanning wiring 104 in the vicinity of the TFT portion of each pixel, and then as a diamine compound as an alignment control film, 1-amino-2- (4′-aminophenyl) -ethene represented by the formula [Compound 36] and 3,6-diaminoindacene represented by the following general formula [Compound 37] in a molar ratio of 1: 2. And 1,3-dichloro-1,2,3,4-cyclobutanetetracarboxylic dianhydride represented by the following general formula [Compound 38] Adjust the mix acid varnish was formed to a thickness of about 40 nm.
Figure 0005594835
Figure 0005594835
Figure 0005594835

また、その配向処理方法は実施例5と同様の高圧水銀ランプからの光を干渉フィルタと石英のパイル偏光子を用いて240nm〜310nmの波長範囲で10:1の偏光比の偏光UVとし、照射エネルギーは約3J/cm2 で照射した。また同時に軟X線発生装置を用い軟X線を近距離から照射した。   In addition, the alignment treatment method is to irradiate light from a high-pressure mercury lamp similar to that in Example 5 with polarized light UV having a polarization ratio of 10: 1 in a wavelength range of 240 nm to 310 nm using an interference filter and a quartz pile polarizer. The energy was irradiated at about 3 J / cm2. At the same time, soft X-rays were irradiated from a short distance using a soft X-ray generator.

以上の工程以外は第5実施例と同様にして第6の実施例となる液晶表示装置を作し、本発明の第6実施例である液晶表示装置の表示品位を評価したところ、第5実施例の液晶表示装置に比べて高いコントラスト比を示す高品位の表示が確認された。   Except for the above steps, the liquid crystal display device according to the sixth embodiment was made in the same manner as in the fifth embodiment, and the display quality of the liquid crystal display device according to the sixth embodiment of the present invention was evaluated. A high-quality display showing a high contrast ratio as compared with the liquid crystal display device of the example was confirmed.

また、中間調表示時における広視野角も確認された。これは第5実施例の液晶表示装置に見られる画素内にランダムに分布するスペーサビーズ周りの液晶の配向の乱れに起因した光漏れが完全に除去されたためと考えられる。   Also, a wide viewing angle during halftone display was confirmed. This is considered to be because light leakage due to the disorder of the alignment of the liquid crystal around the spacer beads randomly distributed in the pixels found in the liquid crystal display device of the fifth embodiment is completely removed.

また、本発明の第1実施例と同様にして、この第6実施例の液晶表示装置の画像の焼き付け、残像の緩和時間を定量評価したところ、残像の緩和時間は実施例5と同様に1分以下であり、目視による画質残像検査においても、画像の焼き付け、残像による表示むらも一切見られず、高い表示特性が得られた。   Similarly to the first embodiment of the present invention, when the image printing and afterimage relaxation time of the liquid crystal display device of the sixth embodiment were quantitatively evaluated, the afterimage relaxation time was 1 as in the fifth embodiment. Even in visual image quality afterimage inspection, no image burn-in and display unevenness due to afterimage were observed, and high display characteristics were obtained.

第7実施例で用いた配向制御膜及びその配向処理条件以外は第4実施例4同様にして、下記一般式〔化合物39〕に示したジアミン化合物として2,7−ジアミノジベンゾチオフェンと、下記一般式〔化合物40〕に示した酸二無水物として1,2,3−トリメチル−1、2、3、4−シクロブタンテトラカルボン酸二無水物からなるポリアミック酸を基板表面に印刷形成して、230°Cで30分の焼成してイミド化を行い、膜厚約30nmに成膜した。

Figure 0005594835
Figure 0005594835
Except for the alignment control film used in the seventh example and the alignment treatment conditions, 2,7-diaminodibenzothiophene as the diamine compound represented by the following general formula [Compound 39] and A polyamic acid composed of 1,2,3-trimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride as the acid dianhydride represented by the formula [Compound 40] is printed on the surface of the substrate. The film was baked at ° C for 30 minutes for imidization to form a film having a thickness of about 30 nm.
Figure 0005594835
Figure 0005594835

その後、その表面に遠赤外線を照射しながら、窒素レーザの337nmの偏光UVを照射エネルギー約4J/cm2で照射することにより光配向処理を行った。そのときの配向制御膜の温度は約200°Cであった。 Then, photoirradiation processing was performed by irradiating the surface with far-infrared rays and irradiating polarized UV of 337 nm of a nitrogen laser with an irradiation energy of about 4 J / cm 2 . The temperature of the orientation control film at that time was about 200 ° C.

その後、第4実施例と同様にネマティック液晶組成物Aを封入後、100°Cで10分のアニーリングを施し、上記の照射偏光方向に対してほぼ垂直方向に良好な液晶配向を得た。   Then, after encapsulating the nematic liquid crystal composition A in the same manner as in the fourth example, annealing was performed at 100 ° C. for 10 minutes, and good liquid crystal alignment was obtained in a direction substantially perpendicular to the irradiation polarization direction.

このようにして、液晶層の厚みdが4.0μmの液晶表示装置を得た。また、このパネルに用いた配向制御膜と液晶組成物と同等のものを用いてホモジニアス配向のセルを作製し、クリスタルローテーション法を用いて液晶のプレチルト角を測定したところ約0.3度を示した。   Thus, a liquid crystal display device having a liquid crystal layer thickness d of 4.0 μm was obtained. In addition, a homogeneous alignment cell was prepared using the alignment control film and the liquid crystal composition used for this panel, and the pretilt angle of the liquid crystal was measured using the crystal rotation method. It was.

次に、第1実施例と同様の方法で、本発明の第7実施例である液晶表示装置の表示品位を評価したところ、第1の実施例の液晶表示装置とほぼ同等のコントラスト比が全面に渡り600:1を越える高品位の表示が確認されるとともに、中間調表示時における広い視野角も確認された。   Next, when the display quality of the liquid crystal display device according to the seventh embodiment of the present invention was evaluated in the same manner as in the first embodiment, the contrast ratio almost the same as that of the liquid crystal display device of the first embodiment was obtained. In addition, high-quality display exceeding 600: 1 was confirmed, and a wide viewing angle during halftone display was also confirmed.

また、本発明の第1実施例と同様にして、この第7実施例の液晶表示装置の画像の焼き付け、残像の緩和時間を定量評価したところ、残像の緩和時間は1分以下であり、目視による画質残像検査においても、画像の焼き付け、残像による表示むらも一切見られず、高い表示特性が得られた。   Similarly to the first embodiment of the present invention, when the image printing and afterimage relaxation time of the liquid crystal display device of the seventh embodiment were quantitatively evaluated, the afterimage relaxation time was 1 minute or less and Even in the image quality afterimage inspection, no image burning or display unevenness due to the afterimage was observed, and high display characteristics were obtained.

第8実施例で用いた配向制御膜及びその配向処理条件以外は第4実施例と同様にして、ジアミン化合物として、下記一般式〔化合物41〕に示した2,7−ジアミノフェナジンと、酸二無水物として、下記一般式〔化合物42〕に示した1−メチル−1、2、3、4−シクロブタンテトラカルボン酸二無水物からなるポリアミック酸を基板表面に印刷形成して、230°C、30分の焼成、イミド化を行い、膜厚約20nmに製膜した。

Figure 0005594835
Figure 0005594835
Except for the alignment control film used in the eighth example and the alignment treatment conditions, in the same manner as in the fourth example, 2,7-diaminophenazine represented by the following general formula [Compound 41], and diacid As an anhydride, a polyamic acid composed of 1-methyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride represented by the following general formula [Compound 42] was printed on a substrate surface, and 230 ° C., Baking for 30 minutes and imidization were performed to form a film having a thickness of about 20 nm.
Figure 0005594835
Figure 0005594835

その後、その表面に遠赤外線を照射しながら、窒素レーザの337nmの偏光UVを用いた光照射による光配向処理を行った。そのときの配向制御膜の温度は約200°Cであった。その後、第4実施例と同様にネマティック液晶組成物Aを封入後、100°Cで10分のアニーリングを施し、上記の照射偏光方向に対してほぼ垂直方向に良好な液晶配向を得た。   Thereafter, a photo-alignment treatment was performed by irradiating the surface with far-infrared rays using light irradiation using polarized UV light of 337 nm of a nitrogen laser. The temperature of the orientation control film at that time was about 200 ° C. Then, after encapsulating the nematic liquid crystal composition A in the same manner as in the fourth example, annealing was performed at 100 ° C. for 10 minutes, and good liquid crystal alignment was obtained in a direction substantially perpendicular to the irradiation polarization direction.

このようにして、液晶層の厚みdが4.0μmの液晶表示装置を得た。また、このパネルに用いた配向制御膜と液晶組成物と同等のものを用いてホモジニアス配向のセルを作製し、クリスタルローテーション法を用いて液晶のプレチルト角を測定したところ約0.3度を示した。   Thus, a liquid crystal display device having a liquid crystal layer thickness d of 4.0 μm was obtained. In addition, a homogeneous alignment cell was prepared using the alignment control film and the liquid crystal composition used for this panel, and the pretilt angle of the liquid crystal was measured using the crystal rotation method. It was.

次に、第1実施例と同様の方法で、本発明の第8実施例である液晶表示装置の表示品位を評価したところ、第4実施例の液晶表示装置とほぼ同等のコントラスト比が全面に渡り600:1を越える高品位の表示が確認されるとともに、中間調表示時における広い視野角も確認された。   Next, when the display quality of the liquid crystal display device according to the eighth embodiment of the present invention was evaluated in the same manner as in the first embodiment, the contrast ratio almost the same as that of the liquid crystal display device of the fourth embodiment was observed on the entire surface. A high-quality display exceeding 600: 1 was confirmed, and a wide viewing angle during halftone display was also confirmed.

また、本発明の第1実施例と同様にして、この第8実施例の液晶表示装置の画像の焼き付け、残像の緩和時間を定量評価したところ、残像の緩和時間は2分以下であり、目視による画質残像検査においても、画像の焼き付け、残像による表示むらも一切見られず、高い表示特性が得られた。   Similarly to the first embodiment of the present invention, when the image printing and afterimage relaxation time of the liquid crystal display device of the eighth embodiment were quantitatively evaluated, the afterimage relaxation time was 2 minutes or less and Even in the image quality afterimage inspection, no image burning or display unevenness due to the afterimage was observed, and high display characteristics were obtained.

また、本実施例で用いた配向制御膜は、遠赤外線照射及び窒素レーザの偏光UV照射の組み合わせ以外にも、例えば高圧水銀ランプからの光を干渉フィルタ、石英のパイル偏光子を介して300nm〜380nmの波長範囲の偏光UVを照射エネルギー約3J/cm2で照射した場合にも、上記のような高い表示特性が得られることが分かった。 In addition to the combination of far infrared irradiation and polarized UV irradiation of a nitrogen laser, the alignment control film used in this example is not limited to 300 nm to light from an high pressure mercury lamp, for example, via an interference filter and a quartz pile polarizer. It has been found that the above high display characteristics can be obtained even when polarized UV light having a wavelength range of 380 nm is irradiated at an irradiation energy of about 3 J / cm 2 .

さらに、10.5μmの炭酸ガスレーザーを200mJ照射しながら上記300〜380nmの偏光UVを照射した場合にも上記同様の高い表示特性が得られることが分かった。   Furthermore, it was found that the same high display characteristics as above were obtained when the polarized UV of 300 to 380 nm was irradiated while irradiating the carbon dioxide laser of 10.5 μm with 200 mJ.

以下、本発明の第9実施例について、図5を用いて説明する。本発明の第9実施例である液晶表示装置を製造する場合において、基板101、102としては、厚みが0.7mmで表面を研磨したガラス基板を用いる。   The ninth embodiment of the present invention will be described below with reference to FIG. In manufacturing the liquid crystal display device according to the ninth embodiment of the present invention, glass substrates whose thickness is 0.7 mm and whose surface is polished are used as the substrates 101 and 102.

薄膜トランジスタはソース電極(画素電極)105、ドレイン電極(信号電極)106、ゲート電極(走査電極)104及び半導体膜(アモルファスシリコン)116から構成される。走査電極104はアルミニウム膜をパターニングし、共通電極配線120、信号電極106及び画素電極105はクロム膜をパターニングして形成した。   The thin film transistor includes a source electrode (pixel electrode) 105, a drain electrode (signal electrode) 106, a gate electrode (scanning electrode) 104, and a semiconductor film (amorphous silicon) 116. The scanning electrode 104 was formed by patterning an aluminum film, and the common electrode wiring 120, the signal electrode 106, and the pixel electrode 105 were formed by patterning a chromium film.

ゲート絶縁膜107と保護絶縁膜108は窒化珪素からなり、膜厚はそれぞれ0.3μmとした。その上にアクリル系樹脂を塗布し、220°C、1時間の加熱処理により透明で絶縁性のある誘電率約4の有機保護膜112を約1.0μm厚に形成した。この有機保護膜112により表示領域の画素電極105の段差起因の凹凸ならびに隣接する画素間の段差凹凸を平坦化した。   The gate insulating film 107 and the protective insulating film 108 were made of silicon nitride, and the film thicknesses were each 0.3 μm. An acrylic resin was applied thereon, and a transparent and insulating organic protective film 112 having a dielectric constant of about 4 was formed to a thickness of about 1.0 μm by heat treatment at 220 ° C. for 1 hour. With this organic protective film 112, the unevenness due to the step of the pixel electrode 105 in the display region and the unevenness between the adjacent pixels are flattened.

次に、フォトリソグラフィ法とエッチング処理により、図5に示すように画素電極105まで約10μm径の円筒状にスルーホール118を形成し、その上からソース電極105と接続する画素電極105をITO膜をパターニングして形成した。   Next, through holes 118 are formed in a cylindrical shape with a diameter of about 10 μm up to the pixel electrode 105 by photolithography and etching, as shown in FIG. 5, and the pixel electrode 105 connected to the source electrode 105 is formed thereon from the ITO film. Was formed by patterning.

また、共通電極配線120についても約10μm径の円筒状にスルーホール118を形成し、その上からITO膜をパターニングして共通電極103を形成した。その際、画素電極105と共通電極103との間隔は7μmとし、走査電極104以外はジグザグに屈曲した電極配線パターンに形成した。その際、屈曲の角度は10度に設定した。   The common electrode wiring 120 was also formed with a through hole 118 in a cylindrical shape having a diameter of about 10 μm, and the ITO film was patterned thereon to form the common electrode 103. At that time, the distance between the pixel electrode 105 and the common electrode 103 was 7 μm, and the electrode wiring pattern other than the scanning electrode 104 was formed in a zigzag bent electrode wiring pattern. At that time, the angle of bending was set to 10 degrees.

さらに、この共通電極103は映像信号配線106、走査信号配線104及び薄膜トランジスタの上部を覆い画素を囲むように格子状に形成し、遮光層を兼ねるようにした。   Further, the common electrode 103 is formed in a lattice shape so as to cover the upper part of the video signal wiring 106, the scanning signal wiring 104, and the thin film transistor so as to surround the pixel, and also serves as a light shielding layer.

その結果、単位画素内に2種類のスルーホール118が形成されている以外は実施例4とほぼ同様に、画素電極105が3本の共通電極103の間に配置されている構成となり、画素数は1024×3(R、G、Bに対応)本の信号電極106と768本の走査電極104とから構成される1024×3×768個とするアクティブマトリクス基板を形成した。   As a result, the pixel electrode 105 is arranged between the three common electrodes 103 in substantially the same manner as in Example 4 except that two types of through-holes 118 are formed in the unit pixel. Formed 1024 × 3 × 768 active matrix substrates composed of 1024 × 3 (corresponding to R, G, and B) signal electrodes 106 and 768 scanning electrodes 104.

以上のように画素構造、用いる配向制御膜以外は第4実施例と同様として、図5に示すように第9実施例の液晶表示装置を作製した。   As described above, the liquid crystal display device of the ninth example was manufactured as shown in FIG. 5 in the same manner as in the fourth example except for the pixel structure and the alignment control film to be used.

本実施例で用いた配向制御膜はジアミンとして、下記一般式〔化合物43〕に示した1,4−ジアミノ−2―ビニルベンゼンと、下記一般式〔化合物44〕に示した4,4’ジアミノジフェニルアミンをモル比2:1の割合とし、酸二無水物として、下記一般式〔化合物45〕に示した1、2、3、4−シクロブタンテトラカルボン酸二無水物と、下記一般式〔化合物46〕に示した1−アミノ−1,2,3,4−シクロブタンテトラカルボン酸ニ無水物をモル比1:2の割合として合成したポリアミック酸ワニスを用い、膜厚約30nmの配向制御膜を作製した。

Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
The alignment control film used in this example is diamine, 1,4-diamino-2-vinylbenzene represented by the following general formula [Compound 43], and 4,4 ′ diamino represented by the following general formula [Compound 44]. Diphenylamine was used in a molar ratio of 2: 1, and as the acid dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride represented by the following general formula [Compound 45] and the following general formula [Compound 46 An alignment control film having a film thickness of about 30 nm is produced using a polyamic acid varnish obtained by synthesizing 1-amino-1,2,3,4-cyclobutanetetracarboxylic dianhydride shown in the above formula at a molar ratio of 1: 2. did.
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835

次に、本実施例の液晶表示装置の表示品位を評価したところ、第1実施例の液晶表示装置と同等の高品位の表示が確認されるとともに、中間調表示時における広視野角も確認された。   Next, when the display quality of the liquid crystal display device of this example was evaluated, a high-quality display equivalent to that of the liquid crystal display device of the first example was confirmed, and a wide viewing angle during halftone display was also confirmed. It was.

次に、本発明の第1実施例と同様にして、本実施例の液晶表示装置の画像の焼き付け、残像の緩和時間を定量評価したところ、残像の緩和時間は1分以下であり、目視による画質残像検査においても、画像の焼き付け、残像による表示むらも一切見られず、高い表示特性が得られた。   Next, in the same manner as in the first embodiment of the present invention, when the image printing and afterimage relaxation time of the liquid crystal display device of this embodiment were quantitatively evaluated, the afterimage relaxation time was 1 minute or less, which was visually observed. Even in the image quality afterimage inspection, no image burning or display unevenness due to the afterimage was observed, and high display characteristics were obtained.

図5に示すように、TFTに直接接続されている画素電極が基板最表面に形成され、その上には薄い配向制御膜が形成される場合には、通常のラビング配向処理を行うと摩擦による帯電が発生し、場合によっては表面近傍の画素電極を介してTFT素子がダメージを受けることがある。このような場合は、本実施例のようなラビングレスの光配向処理が非常に有効である。   As shown in FIG. 5, when a pixel electrode directly connected to the TFT is formed on the outermost surface of the substrate and a thin alignment control film is formed thereon, a normal rubbing alignment process causes friction. Charging occurs, and in some cases, the TFT element may be damaged through the pixel electrode near the surface. In such a case, the rubbing-less photo-alignment treatment as in this embodiment is very effective.

図6は、本発明による液晶表示装置の第4の実施の形態を説明する一画素付近の模式断面図である。本実施例の液晶表示装置を製造する場合において、ガラス基板101と102としては、厚みが0.7mmで表面を研磨したガラス基板を用いる。   FIG. 6 is a schematic sectional view of the vicinity of one pixel for explaining a fourth embodiment of the liquid crystal display device according to the present invention. In the case of manufacturing the liquid crystal display device of this embodiment, glass substrates 101 and 102 are glass substrates whose thickness is 0.7 mm and whose surface is polished.

薄膜トランジスタはソース電極(画素電極)105、ドレイン電極(信号電極)106、ゲート電極(走査電極)104及び半導体膜(アモルファスシリコン)116から構成される。走査電極104、共通電極配線120及び信号電極106、画素電極105及び共通電極103は、全てクロム膜をパターニングして形成し、画素電極105と共通電極103との間隔は7μmとした。   The thin film transistor includes a source electrode (pixel electrode) 105, a drain electrode (signal electrode) 106, a gate electrode (scanning electrode) 104, and a semiconductor film (amorphous silicon) 116. The scanning electrode 104, the common electrode wiring 120 and the signal electrode 106, the pixel electrode 105, and the common electrode 103 were all formed by patterning a chromium film, and the distance between the pixel electrode 105 and the common electrode 103 was 7 μm.

ゲート絶縁膜107と保護絶縁膜108は窒化珪素からなり、膜厚はそれぞれ0.3μmとした。その上には配向制御膜としてジアミン化合物に、下記一般式〔化合物47〕に示した2,5−ジアミノピロールと、酸二無水物として、下記一般式〔化合物48〕に示した1,2,3,4−シクロブタンテトラカルボン酸二無水物からなるポリアミック酸ワニスを基板表面に印刷形成して、230°C、30分の焼成、イミド化を行い、膜厚約50nmに成膜した。

Figure 0005594835
Figure 0005594835
The gate insulating film 107 and the protective insulating film 108 were made of silicon nitride, and the film thicknesses were each 0.3 μm. On top of that, a diamine compound as an alignment control film, 2,5-diaminopyrrole represented by the following general formula [Compound 47], and 1,2,2 represented by the following general formula [Compound 48] as an acid dianhydride. A polyamic acid varnish composed of 3,4-cyclobutanetetracarboxylic dianhydride was printed on the substrate surface, and baked and imidized at 230 ° C. for 30 minutes to form a film having a thickness of about 50 nm.
Figure 0005594835
Figure 0005594835

その後、真空中でその表面に5eV、約0.5μC/cm2の電子線を照射しながら、高圧水銀ランプからの光を干渉フィルタ、石英のパイル偏光子を介して220nm〜380nmの波長範囲の偏光UVを照射エネルギー約3J/cm2で照射し光配向処理を施した。 Then, while irradiating the surface with an electron beam of 5 eV and about 0.5 μC / cm 2 in a vacuum, the light from the high-pressure mercury lamp passes through an interference filter and a quartz pile polarizer in the wavelength range of 220 nm to 380 nm. Polarization UV was irradiated at an irradiation energy of about 3 J / cm 2 to perform photo-alignment treatment.

その結果、画素数は1024×3(R、G、Bに対応)本の信号電極106と768本の走査電極104とから構成される1024×3×768個とするアクティブマトリクス基板を形成した。   As a result, an active matrix substrate having 1024 × 3 × 768 pixels composed of 1024 × 3 (corresponding to R, G, B) signal electrodes 106 and 768 scan electrodes 104 was formed.

以上のように画素構造以外は実施例1と同様として図6に示すような本実施例の液晶表示装置を作製した。   As described above, a liquid crystal display device of this example as shown in FIG. 6 was manufactured in the same manner as Example 1 except for the pixel structure.

本実施例の液晶表示装置の表示品位を評価したところ、第1実施例の液晶表示装置と同等の高品位の表示が確認されるとともに、中間調表示時における広視野角も確認された。   When the display quality of the liquid crystal display device of this example was evaluated, high-quality display equivalent to that of the liquid crystal display device of the first example was confirmed, and a wide viewing angle during halftone display was also confirmed.

次に、本発明の第1実施例と同様にして、この本実施例の液晶表示装置の画像の焼き付け、残像の緩和時間を定量評価したところ、残像の緩和時間は2分以下であり、目視による画質残像検査においても、画像の焼き付け、残像による表示不良は認められなかった。   Next, in the same manner as in the first embodiment of the present invention, when the image printing and afterimage relaxation time of the liquid crystal display device of this embodiment were quantitatively evaluated, the afterimage relaxation time was 2 minutes or less and In the image quality afterimage inspection by, no image burn-in or display failure due to afterimage was found.

また、本実施例で用いたジアミン化合物の誘導体である下記一般式〔化合物49〕に示した2,5−ジアミノ−3−ビニルピロールをモル比で50%導入し合成したポリアミック酸ワニスを用いた場合には、偏光UVの照射エネルギーが約2J/cm2において同等の高い表示特性が得られた。

Figure 0005594835
Further, a polyamic acid varnish synthesized by introducing 50% by mole of 2,5-diamino-3-vinylpyrrole represented by the following general formula [Compound 49], which is a derivative of the diamine compound used in this example, was used. In this case, the same high display characteristics were obtained when the irradiation energy of polarized UV was about 2 J / cm 2.
Figure 0005594835

第11実施例で用いた配向制御膜の組成ならびに配向制御膜形成、配向処理方法以外は第10実施例と同様にし、本実施例の配向制御膜のジアミン化合物として、下記一般式〔化合物50〕に示したチミン誘導体と、酸二無水物として、下記一般式〔化合物51〕に示す1,2,3,4−テトラメチル−1、2、3、4−シクロブタンテトラカルボン酸二無水物からなるポリアミック酸ワニスを基板表面に印刷形成して、90°C、2分の熱処理によるレベリングを行い、膜厚約35nmに成膜した。

Figure 0005594835
Figure 0005594835
Except for the composition of the alignment control film used in the eleventh example, the formation of the alignment control film, and the alignment treatment method, the same process as in the tenth example was carried out. As the diamine compound of the alignment control film of this example, And a 1,2,3,4-tetramethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride represented by the following general formula [Compound 51] as an acid dianhydride A polyamic acid varnish was printed on the substrate surface and leveled by heat treatment at 90 ° C. for 2 minutes to form a film with a thickness of about 35 nm.
Figure 0005594835
Figure 0005594835

その後、その表面に遠赤外線を照射し、膜表面を約230°Cに保持しながら、高圧水銀ランプからの光を干渉フィルタ、石英のパイル偏光子を介して220〜380nmの波長範囲の偏光UVを照射エネルギー約5J/cm2で照射し光配向処理を施した。処理後の配向制御膜の膜厚は約25nmであった。 Thereafter, the surface is irradiated with far-infrared rays, and the light from the high-pressure mercury lamp is polarized in the wavelength range of 220 to 380 nm through an interference filter and a quartz pile polarizer while maintaining the film surface at about 230 ° C. Was irradiated at an irradiation energy of about 5 J / cm 2 to give a photo-alignment treatment. The film thickness of the orientation control film after the treatment was about 25 nm.

その後、第10実施例と同様に図6に示すような本実施例の液晶表示装置を作製し、ネマティック液晶組成物Aを封入後、100°C、10分のアニーリングを施し、上記の照射偏光方向に対してほぼ垂直方向に良好な液晶配向を得た。このようにして、液晶層の厚みdが4.0μmの液晶表示装置を得た。   Thereafter, a liquid crystal display device of this example as shown in FIG. 6 was prepared in the same manner as the tenth example, and after nematic liquid crystal composition A was sealed, annealing was performed at 100 ° C. for 10 minutes, and the above-mentioned irradiation polarized light was applied. Good liquid crystal alignment was obtained in a direction substantially perpendicular to the direction. Thus, a liquid crystal display device having a liquid crystal layer thickness d of 4.0 μm was obtained.

また、このパネルに用いた配向制御膜と液晶組成物と同等のものを用いてホモジニアス配向のセルを作製し、クリスタルローテーション法を用いて液晶のプレチルト角を測定したところ約0.1度を示した。   In addition, a homogeneous alignment cell was prepared using the alignment control film and the liquid crystal composition used in this panel, and the pretilt angle of the liquid crystal was measured using the crystal rotation method. It was.

次に、第1実施例と同様の方法で、本実施例の液晶表示装置の表示品位を評価したところ、一般にラビング配向処理で見られる電極段差近傍の配向不良による光漏れがなく、第1の実施例の液晶表示装置とほぼ同等のコントラスト比が、全面に渡り600:1を越える高品位の表示が確認されるとともに、中間調表示時における広い視野角も確認された。   Next, when the display quality of the liquid crystal display device of this example was evaluated in the same manner as in the first example, there was no light leakage due to misalignment in the vicinity of the electrode step generally seen in the rubbing alignment process. A high-quality display with a contrast ratio almost equal to that of the liquid crystal display device of the example exceeding 600: 1 over the entire surface was confirmed, and a wide viewing angle during halftone display was also confirmed.

また、本発明の第1実施例と同様にして、この第11実施例の液晶表示装置の画像の焼き付け、残像の緩和時間を定量評価したところ、残像の緩和時間は1分以下であり、目視による画質残像検査においても、画像の焼き付け、残像による表示むらも一切見られず、高い表示特性が得られた。   Further, in the same manner as in the first embodiment of the present invention, when the image printing and afterimage relaxation time of the liquid crystal display device of the eleventh embodiment were quantitatively evaluated, the afterimage relaxation time was 1 minute or less. Even in the image quality afterimage inspection, no image burning or display unevenness due to the afterimage was observed, and high display characteristics were obtained.

また、波長範囲220〜260nmの偏光紫外線を3J/cm2照射し、別光源から260〜400nmの無偏光の紫外線を5J/cm2照射した以外は本実施例と同様にして液晶表示装置を作製、評価したところ、上記本実施例と同等の表示特性を持つ液晶表示装置が得られた。 Further, a liquid crystal display device was produced in the same manner as in this example, except that polarized ultraviolet rays having a wavelength range of 220 to 260 nm were irradiated with 3 J / cm 2 and unpolarized ultraviolet rays having a wavelength of 260 to 400 nm were irradiated with 5 J / cm 2 from another light source. As a result of evaluation, a liquid crystal display device having display characteristics equivalent to those of the present example was obtained.

第12実施例用いた配向制御膜の組成ならびに配向制御膜形成、配向処理方法以外は実施例9と同様にして、本実施例の配向制御膜のジアミン化合物として、下記一般式〔化合物52〕に示したケイ皮酸エステル誘導体と、酸二無水物として、下記一般式〔化合物53〕に示した1、2、3、4−シクロブタンテトラカルボン酸二無水物からなるポリアミック酸ワニスを基板表面に印刷形成して90°C、2分の熱処理によるレベリングを行い、膜厚約40nmに製膜した。

Figure 0005594835
Figure 0005594835
Except for the composition of the alignment control film and the alignment control film formation and alignment treatment method used in the twelfth example, the diamine compound of the alignment control film of this example is represented by the following general formula [Compound 52] as in Example 9. A polyamic acid varnish comprising 1,2,3,4-cyclobutanetetracarboxylic dianhydride represented by the following general formula [Compound 53] is printed on the substrate surface as the cinnamate derivative shown and acid dianhydride. After forming, leveling by heat treatment at 90 ° C. for 2 minutes was performed to form a film having a thickness of about 40 nm.
Figure 0005594835
Figure 0005594835

その後、その表面に遠赤外線を照射し、膜表面を約250°Cに保持しながら、高圧水銀ランプからの光を干渉フィルタ、石英のパイル偏光子を介して220〜280nmの波長範囲の偏光UVを照射エネルギー約3J/cm2で照射し、イミド化焼成処理ならびに光配向処理を施した。処理後の配向制御膜の膜厚は約25nmであった。 Thereafter, the surface is irradiated with far-infrared rays, and the light from the high-pressure mercury lamp is polarized UV in the wavelength range of 220 to 280 nm through an interference filter and a quartz pile polarizer while maintaining the film surface at about 250 ° C. Was irradiated at an irradiation energy of about 3 J / cm 2 to perform imidization baking treatment and photo-alignment treatment. The film thickness of the orientation control film after the treatment was about 25 nm.

その後、実施例9と同様に図5に示すような本実施例12の液晶表示装置を作製し、ネマティック液晶組成物Aを封入後、100°C、10分のアニーリングを施し、上記の照射偏光方向に対してほぼ平行な方向に良好な液晶配向を得た。このようにして、液晶層の厚みdが4.0μmの液晶表示装置を得た。   Thereafter, a liquid crystal display device of Example 12 as shown in FIG. 5 was prepared in the same manner as Example 9, and after nematic liquid crystal composition A was sealed, it was annealed at 100 ° C. for 10 minutes, and the above-mentioned irradiation polarized light was applied. Good liquid crystal alignment was obtained in a direction substantially parallel to the direction. Thus, a liquid crystal display device having a liquid crystal layer thickness d of 4.0 μm was obtained.

また、このパネルに用いた配向制御膜と液晶組成物と同等のものを用いてホモジニアス配向のセルを作製し、クリスタルローテーション法を用いて液晶のプレチルト角を測定したところ約0.1度を示した。   In addition, a homogeneous alignment cell was prepared using the alignment control film and the liquid crystal composition used in this panel, and the pretilt angle of the liquid crystal was measured using the crystal rotation method. It was.

次に、第1実施例と同様の方法で、本発明の第7実施例である液晶表示装置の表示品位を評価したところ、一般にラビング配向処理で見られる電極段差近傍の配向不良による光漏れがなく、第1実施例の液晶表示装置とほぼ同等のコントラスト比が、全面に渡り600:1を越える高品位の表示が確認されるとともに、中間調表示時における広い視野角も確認された。 Next, when the display quality of the liquid crystal display device according to the seventh embodiment of the present invention was evaluated in the same manner as in the first embodiment, light leakage due to misalignment in the vicinity of the electrode step generally observed in the rubbing alignment treatment was observed. In addition, a high-quality display having a contrast ratio almost equal to that of the liquid crystal display device of the first embodiment exceeding 600: 1 over the entire surface was confirmed, and a wide viewing angle during halftone display was also confirmed.

また、本発明の第1実施例と同様にして、この第12実施例の液晶表示装置の画像の焼き付け、残像の緩和時間を定量評価したところ、0°C〜50°Cの使用温度範囲において残像の緩和時間は1分以下であり、目視による画質残像検査においても、画像の焼き付け、残像による表示むらも一切見られず、高い表示特性が得られた。   Similarly to the first embodiment of the present invention, when the image printing and afterimage relaxation times of the liquid crystal display device of the twelfth embodiment were quantitatively evaluated, the operating temperature range of 0 ° C. to 50 ° C. was used. The afterimage relaxation time was 1 minute or less, and even in visual image quality afterimage inspection, no image burn-in and display unevenness due to afterimage were observed, and high display characteristics were obtained.

次に、本発明の第5の実施形態である液晶表示装置の具体的構成として第13実施例を図7及び図8を用いて説明する。本発明の第13実施例である液晶表示装置を製造する場合において、基板101としては、厚みが0.7mmで表面を研磨したガラス基板を用いる。   Next, a thirteenth example will be described with reference to FIGS. 7 and 8 as a specific configuration of the liquid crystal display device according to the fifth embodiment of the present invention. In manufacturing the liquid crystal display device according to the thirteenth embodiment of the present invention, a glass substrate having a thickness of 0.7 mm and a polished surface is used as the substrate 101.

図7は、図8のA−A'線に沿った断面図であって、基板101上には電極103,105,106,104の短絡を防止するための絶縁膜107,薄膜トランジスタ及び電極105,106を保護する保護絶縁膜108を形成してTFT基板とする。   FIG. 7 is a cross-sectional view taken along the line AA ′ of FIG. 8. On the substrate 101, an insulating film 107, a thin film transistor and an electrode 105 for preventing a short circuit of the electrodes 103, 105, 106, 104 are provided. A protective insulating film 108 for protecting 106 is formed to form a TFT substrate.

図8は、薄膜トランジスタ及び電極103,105,106の構造を示す。薄膜トランジスタはソース電極(画素電極)105,ドレイン電極(信号電極)106,ゲート電極(走査電極)104及び半導体膜(アモルファスシリコン)116から構成される。   FIG. 8 shows the structure of the thin film transistor and the electrodes 103, 105, and 106. The thin film transistor includes a source electrode (pixel electrode) 105, a drain electrode (signal electrode) 106, a gate electrode (scanning electrode) 104, and a semiconductor film (amorphous silicon) 116.

走査電極104はアルミニウム膜をパターニングし、信号電極106はクロム膜をパターニングし、そして共通電極103と画素電極105とはITOをパターニングして形成する。   The scan electrode 104 is formed by patterning an aluminum film, the signal electrode 106 is formed by patterning a chromium film, and the common electrode 103 and the pixel electrode 105 are formed by patterning ITO.

絶縁膜107と保護絶縁膜108は窒化珪素からなり、膜厚はそれぞれ0.2μmと0.3μmとした。容量素子は画素電極105と共通電極103で絶縁膜107,108を挟む構造として形成する。   The insulating film 107 and the protective insulating film 108 were made of silicon nitride, and the film thicknesses were set to 0.2 μm and 0.3 μm, respectively. The capacitor is formed to have a structure in which the insulating films 107 and 108 are sandwiched between the pixel electrode 105 and the common electrode 103.

画素電極105は、ベタ形状の共通電極103の上層に重畳する形で配置されている。画素数は1024×3(R,G,Bに対応)本の信号電極106と768本の走査電極104とから構成される1024×3×768個とする。   The pixel electrode 105 is arranged so as to overlap the upper layer of the solid-shaped common electrode 103. The number of pixels is 1024 × 3 × 768 including 1024 × 3 (corresponding to R, G, and B) signal electrodes 106 and 768 scanning electrodes 104.

基板102上には、本発明の第1実施例である液晶表示装置と同様の構成のブラックマトリクス113付きカラーフィルタ111を形成し、対向カラーフィルタ基板とした。 On the substrate 102, a color filter 111 with a black matrix 113 having the same configuration as that of the liquid crystal display device according to the first embodiment of the present invention was formed to form a counter color filter substrate.

次に、配向制御膜として、ジアミン化合物に下記一般式〔化合物54〕に示す2,5−ジアミノピリミジンと、下記一般式〔化合物55〕に示す1,2−ジアミノエテンをモル比3:1の割合とし、酸無水物として、下記一般式〔化合物56〕に示す1,2,3,4−シクロブタンテトラカルボン酸二無水物と、下記一般式〔化合物57〕に示す1,2,3,4−テトラメチル−1,2,3,4−シクロブタンテトラカルボン酸二無水物のモル比2:1からなるポリアミック酸ワニスを、樹脂分濃度5重量%、NMP60重量%、γブチルラクトン20重量%、ブチルセロソルブ15重量%に調整し、上記アクティブマトリクス基板の上に印刷形成して220°Cで30分の熱処理によりイミド化し、約110nmの緻密なポリイミド配向制御膜109を形成する。

Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Next, as an alignment control film, 2,5-diaminopyrimidine represented by the following general formula [Compound 54] and 1,2-diaminoethene represented by the following general formula [Compound 55] are mixed in a diamine compound in a molar ratio of 3: 1. As an acid anhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride represented by the following general formula [Compound 56] and 1,2,3,4- represented by the following general formula [Compound 57] A polyamic acid varnish having a molar ratio of tetramethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride of 2: 1, a resin concentration of 5% by weight, NMP 60% by weight, γ-butyllactone 20% by weight, butyl cellosolve Adjusted to 15% by weight, printed on the active matrix substrate, imidized by heat treatment at 220 ° C for 30 minutes, and dense polyimide orientation control of about 110 nm A film 109 is formed.
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835

同様に、ITOを成膜した、もう一方のガラス基板102の表面にも同様のポリアミック酸ワニスを印刷形成し、220°Cで30分の熱処理を行い、約110nmの緻密なポリイミド膜からなる配向制御膜109を形成した。   Similarly, the same polyamic acid varnish is printed on the surface of the other glass substrate 102 on which ITO has been formed, heat-treated at 220 ° C. for 30 minutes, and an orientation composed of a dense polyimide film of about 110 nm. A control film 109 was formed.

その表面に液晶配向能を付与するために、遠赤外線を照射しながら、偏光UV(紫外線)光をポリイミド配向制御膜109に照射した。光源には高圧水銀ランプを用い、干渉フィルタを介して、240nm〜380nmの範囲のUV光を取り出し、石英基板を積層したパイル偏光子を用いて偏光比約10:1の直線偏光とし、約2J/cm2の照射エネルギーで照射した。そのときの配向制御膜の温度は約120°Cであった。 In order to impart the liquid crystal alignment ability to the surface, the polyimide alignment control film 109 was irradiated with polarized UV (ultraviolet) light while irradiating far infrared rays. A high pressure mercury lamp is used as a light source, UV light in the range of 240 nm to 380 nm is taken out through an interference filter, and is made into linearly polarized light having a polarization ratio of about 10: 1 using a pile polarizer laminated with a quartz substrate. Irradiation was performed with an irradiation energy of / cm 2 . The temperature of the orientation control film at that time was about 120 ° C.

その結果、配向制御膜表面の液晶分子の配向方向は、照射した偏光UVの偏光方向に対し、直交方向であることがわかった。   As a result, it was found that the alignment direction of the liquid crystal molecules on the surface of the alignment control film was orthogonal to the polarization direction of the irradiated polarized UV light.

TFT基板及びカラーフィルタ基板における配向制御膜109の配向方向は互いにほぼ平行とし、かつ印加電界117の方向とのなす角度を15度とした。これらの基板間に平均粒径が4μmの高分子ビーズをスペーサとして分散し、TFT基板とカラーフィルタ基板との間に液晶110を挟み込んだ。液晶110は、第1実施例と同じ液晶組成物Aを用いた。   The alignment directions of the alignment control film 109 on the TFT substrate and the color filter substrate were substantially parallel to each other, and the angle formed with the direction of the applied electric field 117 was 15 degrees. Polymer beads having an average particle diameter of 4 μm were dispersed as spacers between these substrates, and the liquid crystal 110 was sandwiched between the TFT substrate and the color filter substrate. As the liquid crystal 110, the same liquid crystal composition A as in the first example was used.

TFT基板とカラーフィルタ基板とを挟む2枚の偏光板114はクロスニコルに配置した。そして、低電圧で暗状態,高電圧で明状態をとるノーマリークローズ特性を採用した。   The two polarizing plates 114 sandwiching the TFT substrate and the color filter substrate were arranged in crossed Nicols. A normally closed characteristic that takes a dark state at a low voltage and a bright state at a high voltage is adopted.

そして、本発明の第13実施例である液晶表示装置を駆動するシステムの構成は第1実施例と同様であるので、構成の詳細は省略する。   Since the configuration of the system for driving the liquid crystal display device according to the thirteenth embodiment of the present invention is the same as that of the first embodiment, the details of the configuration are omitted.

次に、本発明の第13実施例である液晶表示装置の表示品位を評価したところ、第1実施例の液晶表示装置に比べて開口率が高く、コントラスト比650:1の高品位の表示が確認されるとともに、中間調表示時における広視野角も確認された。   Next, when the display quality of the liquid crystal display device according to the thirteenth embodiment of the present invention was evaluated, the aperture ratio was higher than that of the liquid crystal display device of the first embodiment, and a high quality display with a contrast ratio of 650: 1 was obtained. As well as being confirmed, a wide viewing angle during halftone display was also confirmed.

また、本発明の第1実施例と同様にして、この液晶表示装置の画像の焼き付け、残像の緩和時間を定量評価したところ、0°C〜50°Cの使用温度範囲において残像の緩和時間は約1分であり、目視による画質残像検査においても、画像の焼き付け、残像による表示むらも一切見られず、実施例1同等の高い表示特性が得られた。   Similarly to the first embodiment of the present invention, when the image printing and afterimage relaxation time of this liquid crystal display device were quantitatively evaluated, the afterimage relaxation time was 0 ° C to 50 ° C in the operating temperature range. It was about 1 minute, and even in visual image quality afterimage inspection, no image burn-in and display unevenness due to afterimage were observed, and high display characteristics equivalent to Example 1 were obtained.

また、第1実施例と同様の方法で液晶配向膜界面の方位角方向アンカリングエネルギーA2を評価したところ、約1.0x10-3N/m以上の値が得られた。   Further, when the azimuthal anchoring energy A2 at the liquid crystal alignment film interface was evaluated by the same method as in the first example, a value of about 1.0 × 10 −3 N / m or more was obtained.

101,102…ガラス基板、103…共通電極(コモン電極)、104…走査電極(ゲ−ト電極)、105…画素電極(ソ−ス電極)、106…信号電極(ドレイン電極)、107…ゲート絶縁膜、108…保護絶縁膜、109…配向制御膜、110…液晶分子、110'…液晶層(液晶組成物層)、111…カラーフィルタ、112…有機保護膜(層間絶縁膜)、113…遮光膜(ブラックマトリクス)、114…偏光板、116…半導体膜、117…電界方向、118…スルーホール、120…共通電極配線。   DESCRIPTION OF SYMBOLS 101,102 ... Glass substrate, 103 ... Common electrode (common electrode), 104 ... Scanning electrode (gate electrode), 105 ... Pixel electrode (source electrode), 106 ... Signal electrode (drain electrode), 107 ... Gate Insulating film 108 ... Protective insulating film 109 ... Orientation control film 110 ... Liquid crystal molecule 110 '... Liquid crystal layer (liquid crystal composition layer) 111 ... Color filter 112 ... Organic protective film (interlayer insulating film) 113 ... Light shielding film (black matrix), 114... Polarizing plate, 116... Semiconductor film, 117... Electric field direction, 118.

Claims (8)

光反応性の配向制御膜に用いられる配向膜材料であって、
前記配向膜材料が、シクロブタンテトラカルボン酸二無水物及びその誘導体とジアミン化合物からなるポリアミック酸またはポリイミドとからなり、
前記シクロブタンテトラカルボン酸二無水物及びその誘導体が、下記一般式で示される化合物1から化合物3(但し、R1,R2,R3,R4はそれぞれ独立に水素原子、フッ素原子、塩素原子、臭素原子、フェニル基又は炭素数1〜6のアルキル基、アルコキシ基又はビニル基[−(CH2)m−CH=CH2,m=0,1,2]、又はアルキニル基[−(CH2)m−CH≡CH,m=0,1,2])からなる化合物群から選択される化合物の少なくとも1種を含有し、
前記ジアミン化合物が、下記一般式で示される化合物5から化合物18、化合物21、または化合物22(但し、化合物5から化合物18のR1〜R8はそれぞれ独立に水素原子、フッ素原子、塩素原子、または炭素数1〜6のアルキル基、アルコキシ基、又はビニル基[−(CH2)m−CH=CH2,m=0,1,2]、またはアルキニル基[−(CH2)m−CH≡CH,m=0,1,2]を示す。また、化合物10〜12においてXは−CH2−,−NH−,−CO−,−O−,または−S−の結合基を示す。また、化合物21、22のR1はそれぞれ独立に炭素数1〜6のアルキル基を示す。)からなる化合物群から選択される化合物の少なくとも1種を含有する配向膜材料。
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
An alignment film material used for a photo-reactive alignment control film,
The alignment film material is composed of polyamic acid or polyimide composed of cyclobutanetetracarboxylic dianhydride and its derivative and a diamine compound,
The cyclobutanetetracarboxylic dianhydride and derivatives thereof are represented by the following general formulas 1 to 3 (wherein R1, R2, R3, and R4 are independently a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, A phenyl group or an alkyl group having 1 to 6 carbon atoms, an alkoxy group or a vinyl group [— (CH 2 ) m —CH═CH 2 , m = 0, 1, 2], or an alkynyl group [— (CH 2 ) m — At least one compound selected from the group consisting of CH≡CH, m = 0, 1, 2]),
The diamine compound is compound 5 to compound 18, compound 21, or compound 22 represented by the following general formula (wherein R1 to R8 of compound 5 to compound 18 are each independently a hydrogen atom, a fluorine atom, a chlorine atom, or a carbon atom) An alkyl group, an alkoxy group, or a vinyl group [— (CH 2 ) m—CH═CH 2 , m = 0,1,2] or an alkynyl group [— (CH 2 ) m—CH≡CH , M = 0, 1, 2] In compounds 10 to 12, X represents a —CH 2 —, —NH—, —CO—, —O—, or —S— bonding group. R1 of compounds 21 and 22 each independently represents an alkyl group having 1 to 6 carbon atoms.) An alignment film material containing at least one compound selected from the group consisting of compounds.
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
前記ジアミン化合物が、さらに、下記一般式で示される化合物19または化合物20(化合物19及び化合物20のR1、R2はそれぞれ独立に水素原子、フッ素原子、塩素原子、または炭素数1〜6のアルキル基、アルコキシ基、またはビニル基[−(CH2)m−CH=CH2,m=0,1,2]、またはアルキニル基[−(CH2)m−CH≡CH,m=0,1,2]を示す。また、化合物20のR3、R4はそれぞれ独立に炭素数1〜6のアルキル基を示す。)からなる化合物群から選択される化合物の少なくとも1種を含有する請求項1に記載の配向膜材料。
Figure 0005594835
Figure 0005594835
The diamine compound may further be compound 19 or compound 20 represented by the following general formula (R1 and R2 of compound 19 and compound 20 are each independently a hydrogen atom, a fluorine atom, a chlorine atom, or an alkyl group having 1 to 6 carbon atoms. , An alkoxy group, or a vinyl group [— (CH 2 ) m—CH═CH 2 , m = 0,1,2,], or an alkynyl group [— (CH 2 ) m—CH≡CH, m = 0,1, 2) In addition, R3 and R4 of Compound 20 each independently represents an alkyl group having 1 to 6 carbon atoms.) The compound 20 comprises at least one compound selected from the group consisting of compounds. Alignment film material.
Figure 0005594835
Figure 0005594835
光反応性の配向制御膜に用いられる配向膜材料であって、
前記配向膜材料が、シクロブタンテトラカルボン酸二無水物及びその誘導体とジアミン化合物からなるポリアミック酸またはポリイミドとからなり、
前記シクロブタンテトラカルボン酸二無水物及びその誘導体が、下記一般式で示される化合物1(但し、R1,R2,R3,R4はそれぞれ独立に水素原子、フッ素原子、塩素原子、臭素原子、フェニル基又は炭素数1〜6のアルキル基、アルコキシ基又はビニル基[−(CH2)m−CH=CH2,m=0,1,2]、又はアルキニル基[−(CH2)m−CH≡CH,m=0,1,2])を含有し、
前記ジアミン化合物が、下記一般式で示される化合物7(但し、化合物7のR1〜R2はそれぞれ独立に水素原子、フッ素原子、塩素原子、または炭素数1〜6のアルキル基、アルコキシ基、又はビニル基[−(CH2)m−CH=CH2,m=0,1,2]、またはアルキニル基[−(CH2)m−CH≡CH,m=0,1,2]を示す。)および化合物19(化合物19のR1、R2はそれぞれ独立に水素原子、フッ素原子、塩素原子、または炭素数1〜6のアルキル基、アルコキシ基、またはビニル基[−(CH2)m−CH=CH2、m=0,1,2]、またはアルキニル基[−(CH2)m−CH≡CH,m=0,1,2]を示す。)を含有する配向膜材料。
Figure 0005594835
Figure 0005594835
Figure 0005594835
An alignment film material used for a photo-reactive alignment control film,
The alignment film material is composed of polyamic acid or polyimide composed of cyclobutanetetracarboxylic dianhydride and its derivative and a diamine compound,
The cyclobutanetetracarboxylic dianhydride and derivatives thereof are compounds 1 represented by the following general formula (where R1, R2, R3 and R4 are each independently a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, a phenyl group or An alkyl group having 1 to 6 carbon atoms, an alkoxy group or a vinyl group [— (CH 2 ) m—CH═CH 2 , m = 0, 1, 2], or an alkynyl group [— (CH 2 ) m—CH≡CH , M = 0, 1, 2]),
The diamine compound is a compound 7 represented by the following general formula (wherein R1 to R2 of the compound 7 are each independently a hydrogen atom, a fluorine atom, a chlorine atom, or an alkyl group having 1 to 6 carbon atoms, an alkoxy group, or vinyl) A group [— (CH 2 ) m—CH═CH 2 , m = 0,1,2] or an alkynyl group [— (CH 2 ) m—CH≡CH, m = 0,1,2]. And Compound 19 (R1 and R2 of Compound 19 are each independently a hydrogen atom, a fluorine atom, a chlorine atom, or an alkyl group, alkoxy group, or vinyl group having 1 to 6 carbon atoms [— (CH 2 ) m—CH═CH 2 , m = 0,1,2], or an alignment film material containing an alkynyl group [— (CH 2 ) m—CH≡CH, m = 0,1,2].
Figure 0005594835
Figure 0005594835
Figure 0005594835
前記シクロブタンテトラカルボン酸二無水物及びその誘導体が、さらに、下記一般式で示される化合物1(但し、R1,R2,R3,R4はそれぞれ独立に水素原子、フッ素原子、塩素原子、臭素原子、フェニル基または炭素数1〜6のアルキル基、アルコキシ基又はビニル基[−(CH2)m−CH=CH2,m=0,1,2]、またはアルキニル基[−(CH2)m−CH≡CH,m=0,1,2])からなる化合物群から選択される化合物の1種を含有する請求項1に記載の配向膜材料。
Figure 0005594835
The cyclobutanetetracarboxylic dianhydride and derivatives thereof are further compound 1 represented by the following general formula (where R1, R2, R3 and R4 are independently a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, phenyl Group or an alkyl group having 1 to 6 carbon atoms, an alkoxy group or a vinyl group [— (CH 2 ) m—CH═CH 2 , m = 0, 1, 2], or an alkynyl group [— (CH 2 ) m—CH 2. The alignment film material according to claim 1, comprising one compound selected from the group consisting of ≡CH, m = 0, 1, 2]).
Figure 0005594835
光反応性の配向制御膜に用いられる配向膜材料であって、
前記配向膜材料が、シクロブタンテトラカルボン酸二無水物及びその誘導体とジアミン化合物からなるポリアミック酸またはポリイミドとからなり、
前記シクロブタンテトラカルボン酸二無水物及びその誘導体が、下記一般式で示される化合物1(但し、R1,R2,R3,R4はそれぞれ独立に水素原子、フッ素原子、塩素原子、臭素原子、フェニル基又は炭素数1〜6のアルキル基、アルコキシ基又はビニル基[−(CH2)m−CH=CH2、m=0,1,2]、又はアルキニル基[−(CH2)m−CH≡CH、m=0,1,2])を含み、
前記ジアミン化合物が、下記一般式で示される化合物4および化合物44、または、化合物16および化合物18(但し、化合物4、16、18のR1〜R6はそれぞれ独立に水素原子、フッ素原子、塩素原子、または炭素数1〜6のアルキル基、アルコキシ基、又はビニル基[−(CH2)m−CH=CH2、 m=0,1,2]、またはアルキニル基[−(CH2)m−CH≡CH,m=0,1,2]を示す。)を含有する配向膜材料(但し、R1〜R4がすべて水素原子である化合物1を含む場合、及び1,3−ジメチル−1,2,3,4−シクロブタンテトラカルボン酸二無水物を含む場合を除く)。
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
An alignment film material used for a photo-reactive alignment control film,
The alignment film material is composed of polyamic acid or polyimide composed of cyclobutanetetracarboxylic dianhydride and its derivative and a diamine compound,
The cyclobutanetetracarboxylic dianhydride and derivatives thereof are compounds 1 represented by the following general formula (where R1, R2, R3 and R4 are each independently a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, a phenyl group or An alkyl group having 1 to 6 carbon atoms, an alkoxy group or a vinyl group [— (CH 2 ) m—CH═CH 2 , m = 0, 1, 2], or an alkynyl group [— (CH 2 ) m—CH≡CH M = 0, 1, 2]),
The diamine compound is a compound 4 and a compound 44 represented by the following general formula, or a compound 16 and a compound 18 (provided that R1 to R6 of the compounds 4, 16, and 18 are each independently a hydrogen atom, a fluorine atom, a chlorine atom, Alternatively, an alkyl group having 1 to 6 carbon atoms, an alkoxy group, or a vinyl group [— (CH 2 ) m—CH═CH 2 , m = 0, 1, 2], or an alkynyl group [— (CH 2 ) m—CH ≡CH, m = 0, 1, 2]) (provided that compound 1 in which R1 to R4 are all hydrogen atoms includes compound 1, and 1,3-dimethyl-1,2, Except when it contains 3,4-cyclobutanetetracarboxylic dianhydride ).
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
光反応性の配向制御膜に用いられる配向膜材料であって、
前記光反応性の配向制御膜が、シクロブタンテトラカルボン酸二無水物及びその誘導体とジアミン化合物からなるポリアミック酸またはポリイミドとからなり、
前記シクロブタンテトラカルボン酸二無水物及びその誘導体が、下記一般式で示される化合物2または3(但し、R1,R2,R3,R4はそれぞれ独立に水素原子、フッ素原子、塩素原子、臭素原子、フェニル基または炭素数1〜6のアルキル基、アルコキシ基またはビニル基[−(CH2)m−CH=CH2、m=0,1,2]、またはアルキニル基[−(CH2)m−CH≡CH、m=0,1,2])からなる化合物群から選択される化合物の少なくとも一種を含有し、
前記ジアミン化合物が、下記一般式で示される化合物4から化合物22(但し、化合物5から化合物18のRl〜R8はそれぞれ独立に水素原子、フッ素原子、塩素原子、または炭素数1〜6のアルキル基、アルコキシ基、またはビニル基[−(CH2)m−CH=CH2、m=0,1,2]、またはアルキニル基[−(CH2)m−CH≡CH、m=0、1、2]を示す。また、化合物10〜12においてXは−CH2−,−NH−,−CO−,−O−,−S−の結合基を示す。また、化合物21、22のR1はそれぞれ独立に炭素数1〜6のアルキル基を示す。また、化合物4、化合物19及び化合物20のR1、R2はそれぞれ独立に水素原子、フッ素原子、塩素原子、又は炭素数1〜6のアルキル基、アルコキシ基、又はビニル基[−(CH2)m−CH−CH2、m=0,1,2]、又はアルキニル基[−(CH2)m−CH≡CH、m=0,1,2]を示す。また、化合物20のR3、R4はそれぞれ独立に炭素数1〜6のアルキル基を示す。)からなる化合物群から選択される化合物の少なくとも1種を含有することを特徴とする配向膜材料。
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
An alignment film material used for a photo-reactive alignment control film,
The photoreactive alignment control film is composed of polyamic acid or polyimide composed of cyclobutanetetracarboxylic dianhydride and its derivative and a diamine compound,
The cyclobutanetetracarboxylic dianhydride and derivatives thereof are compounds 2 or 3 represented by the following general formula (where R1, R2, R3, and R4 are independently a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, phenyl Group or an alkyl group having 1 to 6 carbon atoms, an alkoxy group or a vinyl group [— (CH 2 ) m—CH═CH 2 , m = 0,1,2,2], or an alkynyl group [— (CH 2 ) m—CH At least one compound selected from the group consisting of ≡CH, m = 0, 1, 2]),
The diamine compound is compound 4 to compound 22 represented by the following general formula (wherein R1 to R8 of compound 5 to compound 18 are each independently a hydrogen atom, a fluorine atom, a chlorine atom, or an alkyl group having 1 to 6 carbon atoms) , an alkoxy group or a vinyl group, [- (CH 2) m -CH = CH 2, m = 0,1,2], or an alkynyl group [- (CH 2) m- CH≡CH, m = 0,1, In the compounds 10 to 12, X represents a bonding group of —CH 2 —, —NH—, —CO—, —O—, —S—, and R 1 of the compounds 21 and 22 represents Each independently represents an alkyl group having 1 to 6 carbon atoms, and R 1 and R 2 of compound 4, compound 19 and compound 20 are each independently a hydrogen atom, a fluorine atom, a chlorine atom, or an alkyl group having 1 to 6 carbon atoms, Alkoxy group or vinyl group [ (CH 2) m-CH- CH 2, m = 0,1,2], or alkynyl group [-. Shows a (CH 2) m-CH≡CH, m = 0,1,2] Furthermore, compound 20 R3 and R4 each independently represents an alkyl group having 1 to 6 carbon atoms.) An alignment film material comprising at least one compound selected from the group consisting of compounds consisting of:
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
Figure 0005594835
前記光反応性の配向制御膜が、シクロブタンテトラカルボン酸二無水物及びその誘導体とジアミン化合物からなるポリアミック酸又はポリイミドの繰り返し構造を少なくとも50%以上含んでいることを特徴とする請求項1乃至のいずれか1項に記載の配向膜材料。 The photoreactive alignment control film, according to claim 1 to 6, characterized in that it includes a repeating structure of a polyamic acid or a polyimide consisting cyclobutane tetracarboxylic dianhydride and its derivative and a diamine compound in which at least 50% or more The alignment film material according to any one of the above. 前記配向膜材料として、さらに、NMP、γブチルラクトンまたはブチルセロソルブを含む請求項1乃至のいずれか1項に記載の配向膜材料。
Examples alignment film material, further, NMP, alignment film material according to any one of claims 1 to 7 including the γ-butyrolactone or butyl cellosolve.
JP2010233973A 2010-10-18 2010-10-18 Alignment film material and liquid crystal display device Active JP5594835B2 (en)