JP3517341B2 - PSA composition for surface protective PSA sheet - Google Patents
PSA composition for surface protective PSA sheetInfo
- Publication number
- JP3517341B2 JP3517341B2 JP30008197A JP30008197A JP3517341B2 JP 3517341 B2 JP3517341 B2 JP 3517341B2 JP 30008197 A JP30008197 A JP 30008197A JP 30008197 A JP30008197 A JP 30008197A JP 3517341 B2 JP3517341 B2 JP 3517341B2
- Authority
- JP
- Japan
- Prior art keywords
- sensitive adhesive
- peeling
- pressure
- weight
- speed
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Fee Related
Description
【0001】[0001]
【発明の属する技術分野】本発明は、塗膜の低温接着性
及び高速剥離性に優れた表面保護粘着シート用の粘着剤
組成物に関するものである。TECHNICAL FIELD The present invention relates to a pressure-sensitive adhesive composition for a surface-protective pressure-sensitive adhesive sheet, which has excellent low-temperature adhesiveness and high-speed peelability of a coating film.
【0002】[0002]
【従来の技術】従来、塗装完成車の車体表面の上塗り塗
装面を保護する方法としては、塗膜面にパラフィンワッ
クスを薄く塗布する方法がある。しかしながら、この方
法は保護機能が十分でなく、かつパラフィンワックスの
除去に手間がかかったり、除去時に生じる廃液が環境汚
染につながる等の問題を有している。2. Description of the Related Art Conventionally, as a method of protecting the top coating surface of the vehicle body of a finished coating vehicle, there is a method of applying paraffin wax thinly on the coating surface. However, this method has problems that the protective function is not sufficient, that it takes time to remove the paraffin wax, and that the waste liquid generated during the removal leads to environmental pollution.
【0003】また、特開平6−73352、特開平9−
3420等に示された塗装面に直接、表面保護粘着シー
トを貼り付ける方法も知られているが、これらの粘着シ
ートは、撥水性、耐汚染性に優れた難接着性塗膜に対
し、特に低温時の接着性が悪く、冬期車両輸送時に剥が
れてしまう問題を抱えている。In addition, JP-A-6-73352 and JP-A-9-
A method of directly attaching a surface protective pressure-sensitive adhesive sheet to the coated surface shown in 3420 etc. is also known, but these pressure-sensitive adhesive sheets are particularly useful for difficult-to-adhere coating films excellent in water repellency and stain resistance. Adhesion at low temperature is poor, and it has a problem that it peels off during transportation in winter.
【0004】これに対して、低温特性の良好な塗膜保護
粘着シートとして、スチレンとジエン系炭化水素のラン
ダム共重合体の水素添加物を主成分とする粘着層をもつ
表面保護粘着シートが提案されている(特開平8−12
956)。また、ポリイソブチレン、ブチルゴム及びポ
リブテンの1種以上を主成分とする粘着剤を支持体に塗
布した塗膜の表面保護フィルムが提案されている(特開
平8−143829)。しかしながら、これは車両輸送
時に剥がれることはないものの、輸送後に保護シートを
剥がす場合、高速剥離時の剥離力が重くなるため、剥離
作業性が悪かったり、粘着付与樹脂の影響で塗膜表面に
貼り跡が残るという問題がある。On the other hand, a surface protective pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer containing a hydrogenated product of a random copolymer of styrene and a diene-based hydrocarbon as a main component is proposed as a coating-film protective pressure-sensitive adhesive sheet having good low-temperature properties. (Japanese Patent Laid-Open No. 8-12
956). Further, there has been proposed a surface protective film of a coating film obtained by coating a support with an adhesive containing at least one of polyisobutylene, butyl rubber and polybutene as a main component (JP-A-8-143829). However, although it does not peel off during transportation of the vehicle, when peeling off the protective sheet after transportation, the peeling force during high-speed peeling becomes heavy, so the peeling workability is poor, and it sticks to the coating film surface due to the effect of the tackifying resin. There is a problem that traces remain.
【0005】[0005]
【発明が解決しようとする課題】本発明は、撥水性、耐
汚染性に優れた難接着性塗膜に対する接着性、特に低温
時の接着性に優れ、かつ剥離したときに被着面に汚れや
貼り跡を残さずに容易に高速剥離可能な低温用表面保護
粘着シート用の粘着剤を提供することを目的とする。DISCLOSURE OF THE INVENTION The present invention has excellent water repellency, stain resistance, and adhesion to a coating having poor adhesion, particularly at low temperature, and when peeled, stains the adherend surface. An object of the present invention is to provide a pressure-sensitive adhesive for a low-temperature surface-protective pressure-sensitive adhesive sheet that can be easily peeled off at high speed without leaving a sticking mark.
【0006】[0006]
【課題を解決するための手段】本発明は、ポリイソブチ
レン及び/又はブチルゴム50〜100重量%並びにポ
リブテン50〜0重量%からなるブレンド物100重量
部に対し、ロジン系粘着付与樹脂として、水素添加され
たロジンエステル樹脂5〜30重量部を添加したことを
特徴とする車体表面の塗膜保護粘着シート用の粘着剤組
成物を提供するものである。According to the present invention, 100 parts by weight of a blend comprising 50 to 100% by weight of polyisobutylene and / or butyl rubber and 50 to 0% by weight of polybutene is hydrogenated as a rosin-based tackifying resin. The present invention provides a pressure-sensitive adhesive composition for a coating film-protecting pressure-sensitive adhesive sheet on a vehicle body surface, characterized in that 5 to 30 parts by weight of the rosin ester resin is added.
【0007】[0007]
【発明の実施の形態】本発明の表面保護粘着シート用の
粘着剤組成物においては、ポリイソブチレン及び/又は
ブチルゴム50〜100重量%並びにポリブテン50〜
0重量%からなるブレンド物100重量部に対し、ロジ
ン系粘着付与樹脂5〜30重量部を添加することによっ
て、上記課題を改善することができた。BEST MODE FOR CARRYING OUT THE INVENTION In a pressure-sensitive adhesive composition for a surface-protective pressure-sensitive adhesive sheet of the present invention, polyisobutylene and / or butyl rubber 50 to 100% by weight and polybutene 50 to 50% by weight are used.
The above problems could be improved by adding 5 to 30 parts by weight of a rosin-based tackifying resin to 100 parts by weight of a blend consisting of 0% by weight.
【0008】本発明の粘着剤組成物において、ポリイソ
ブチレン及び/又はブチルゴム並びにポリブテンからな
るブレンド物中のポリブテン含量が50重量%を超える
場合には、高速剥離時の剥離力が重くなって剥離作業性
が悪くなったり、耐候性が悪くなったりする。In the pressure-sensitive adhesive composition of the present invention, when the polybutene content of the blend consisting of polyisobutylene and / or butyl rubber and polybutene exceeds 50% by weight, the peeling force at the time of high-speed peeling becomes heavy and the peeling work is performed. The performance may be poor, or the weather resistance may be poor.
【0009】本発明に使用するポリイソブチレン及び/
又はブチルゴムは、粘度平均分子量が40万〜150万
であるものが好ましい。粘度平均分子量が40万未満の
場合には高速剥離時の剥離力が重くなり、剥離作業性が
悪くなる。150万を超える場合には難接着塗膜に対す
る低温接着性が悪くなる。Polyisobutylene and / or used in the present invention
Alternatively, the butyl rubber preferably has a viscosity average molecular weight of 400,000 to 1,500,000. When the viscosity average molecular weight is less than 400,000, the peeling force during high-speed peeling becomes heavy and the peeling workability deteriorates. If it exceeds 1.5 million, the low-temperature adhesiveness to the difficult-to-adhere coating film becomes poor.
【0010】本発明に使用するポリブデンは、数平均分
子量が400〜3,000であるものが好ましい。数平
均分子量が400未満の場合には高速剥離時の剥離力が
重くなり、剥離作業性が悪くなる。3,000を超える
場合には難接着性塗膜に対する低温接着性が悪くなる。The polybutene used in the present invention preferably has a number average molecular weight of 400 to 3,000. When the number average molecular weight is less than 400, the peeling force during high-speed peeling becomes heavy and the peeling workability deteriorates. When it exceeds 3,000, the low-temperature adhesiveness to the coating film having poor adhesion becomes poor.
【0011】本発明の粘着剤組成物において、ポリイソ
ブチレン及び/又はブチルゴム並びにポリブテンからな
るブレンド物100重量部に対するロジン系粘着付与樹
脂の添加が5重量部未満の場合には、難接着性塗膜に対
する低温接着性が悪くなる。ロジン系粘着付与樹脂の添
加が30重量部を超える場合には、低温接着性や耐候性
が悪くなり、被着面を汚染したりする。In the pressure-sensitive adhesive composition of the present invention, when the amount of the rosin-based tackifying resin added to 100 parts by weight of the blend of polyisobutylene and / or butyl rubber and polybutene is less than 5 parts by weight, a film having poor adhesiveness is formed. Low temperature adhesiveness to. When the amount of the rosin-based tackifying resin added exceeds 30 parts by weight, the low temperature adhesiveness and weather resistance are deteriorated and the adherend surface is contaminated.
【0012】本発明に使用するロジン系粘着付与樹脂
は、ロジンエステル系樹脂が好ましく、更に耐候性の点
からも水素添加されたロジンエステル樹脂がより好まし
い。The rosin-based tackifying resin used in the present invention is preferably a rosin ester-based resin, and more preferably a hydrogenated rosin ester-based resin from the viewpoint of weather resistance.
【0013】本発明の粘着剤組成物を用いた表面保護粘
着シートは、ぬれ性(JIS K6760に準拠)が3
0dyn/cm未満の難接着性塗膜に対して、−20℃雰囲気
での接着力(180°ピール力、剥離速度0.3m/
分、JIS Z0237に準拠)が0.4N /10mm以
上、23℃雰囲気での高速剥離力(180°ピール力、
前処理70℃×24時間、剥離速度40m/分、JIS
Z0237に準拠)が2N /10mm未満であることを
特徴とする。−20℃雰囲気での接着力が0.4N /1
0mm未満の場合には、低温接着性が悪くなり低温輸送時
に剥がれ易くなる。23℃雰囲気での高速剥離力が2N
/10mm以上の場合には剥離作業性が悪くなる。The surface protective pressure-sensitive adhesive sheet using the pressure-sensitive adhesive composition of the present invention has a wettability (based on JIS K6760) of 3
Adhesive strength (180 ° peeling force, peeling speed 0.3 m /
Min., JIS Z0237) 0.4N / 10mm or more, high-speed peeling force (180 ° peeling force, 23 ° C atmosphere)
Pretreatment 70 ° C x 24 hours, peeling speed 40m / min, JIS
(Based on Z0237) is less than 2N / 10 mm. Adhesive strength at -20 ℃ is 0.4N / 1
When the thickness is less than 0 mm, the low temperature adhesiveness is deteriorated and peeling easily occurs at low temperature transportation. High-speed peeling force of 2N at 23 ℃
When it is / 10 mm or more, the peeling workability becomes poor.
【0014】本発明の粘着剤組成物は、本発明の目的を
損なわない範囲で必要に応じて、それぞれ各種添加剤を
配合することができる。すなわち、オイル、パラフィン
ワックス、エポキシ系可塑剤、ポリエステル系可塑剤等
の軟化剤;酸化チタン等の顔料;タルク、炭酸カルシウ
ム等の充填剤;ステアリン酸、ステアリン酸アミド、ス
テアリン酸カルシウム、ステアリン酸バリウム、ステア
リン酸亜鉛等の滑剤;フェノール系、ホスファイト系、
チオエーテル系等の酸化防止剤;ベンゾトリアゾール
系、ヒンダードアミン系、ベンゾエート系等の紫外線吸
収剤;ガラスバルーン、シリカバルーン等の無機系中空
粒子;アクリル系、高分子量ポリオレフィン系パウダー
等の高分子微小球;シリコーン系、長鎖アルキル系等の
剥離性付与剤等を適宜添加することができる。The pressure-sensitive adhesive composition of the present invention may contain various additives, if necessary, within a range not impairing the object of the present invention. That is, oils, paraffin wax, softeners such as epoxy plasticizers and polyester plasticizers; pigments such as titanium oxide; fillers such as talc and calcium carbonate; stearic acid, stearamide, calcium stearate, barium stearate, Lubricants such as zinc stearate; phenol-based, phosphite-based,
Antioxidants such as thioethers; UV absorbers such as benzotriazoles, hindered amines and benzoates; inorganic hollow particles such as glass balloons and silica balloons; polymer microspheres such as acrylic and high molecular weight polyolefin powders; A silicone-based or long-chain alkyl-based releasability-imparting agent or the like can be appropriately added.
【0015】本発明の粘着剤組成物を使用する塗膜保護
シートの基材層の厚さは6〜1,000μm のフィルム
が好ましく、基材の組成としては、ポリエステル、ナイ
ロン、ポリ塩化ビニル、ポリエチレン、ポリプロピレ
ン、エチレンとプロピレンの共重合体、エチレンとプロ
ピレンとジエンの共重合体、エチレンとブテン−1の共
重合体、エチレンとα−オレフィンの共重合体、エチレ
ンと酢酸ビニルの共重合体、エチレンと(メタ)アクリ
ル酸の共重合体、エチレンとメチル(メタ)アクリレー
トの共重合体、エチレンとエチル(メタ)アクリレート
の共重合体、エチレンを主成分とするポリマー間に金属
イオン結合を有するアイオノマー樹脂、オレフィン結晶
・ジエン系炭化水素・オレフィン結晶ブロック共重合体
(水素添加物も含む)、スチレン・ジエン系炭化水素・
オレフィン結晶ブロック共重合体(水素添加物も含
む)、スチレン・ジエン系炭化水素ランダム共重合体
(水素添加物も含む)等の樹脂1種又は2種以上のブレ
ンド、あるいはアロイ、更にこれに、酸化チタン等の顔
料;タルク、炭酸カルシウム等の充填剤;ステアリン
酸、ステアリン酸アミド、ステアリン酸カルシウム、ス
テアリン酸バリウム、ステアリン酸亜鉛等の滑剤;フェ
ノール系、ホスファイト系、チオエーテル系等の酸化防
止剤;ベンゾトリアゾール系、ヒンダードアミン系、ベ
ンゾエート系等の紫外線吸収剤;ガラスバルーン、シリ
カバルーン等の無機系中空粒子;高分子量ポリオレフィ
ン系パウダー等の高分子量微小球;シリコーン系、長鎖
アルキル系等の剥離性付与剤等を適宜添加したものを使
用することができる。The base material layer of the coating film protective sheet using the pressure-sensitive adhesive composition of the present invention is preferably a film having a thickness of 6 to 1,000 μm. The base material composition is polyester, nylon, polyvinyl chloride, Polyethylene, polypropylene, copolymer of ethylene and propylene, copolymer of ethylene, propylene and diene, copolymer of ethylene and butene-1, copolymer of ethylene and α-olefin, copolymer of ethylene and vinyl acetate A copolymer of ethylene and (meth) acrylic acid, a copolymer of ethylene and methyl (meth) acrylate, a copolymer of ethylene and ethyl (meth) acrylate, and a metal ion bond between ethylene-based polymers. Ionomer resin, olefin crystal / diene hydrocarbon / olefin crystal block copolymer (including hydrogenated products) Styrene-diene hydrocarbon-
One or more resins such as olefin crystal block copolymers (including hydrogenated products) and styrene / diene hydrocarbon random copolymers (including hydrogenated products), blends, or alloys; Pigments such as titanium oxide; fillers such as talc and calcium carbonate; lubricants such as stearic acid, stearamide, calcium stearate, barium stearate and zinc stearate; antioxidants such as phenols, phosphites, thioethers, etc. UV absorbers such as benzotriazole-based, hindered amine-based, benzoate-based; inorganic hollow particles such as glass balloons and silica balloons; high-molecular weight microspheres such as high-molecular-weight polyolefin powder; silicone-based, long-chain alkyl-based release It is possible to use a material to which a property-imparting agent or the like is appropriately added.
【0016】本発明の粘着剤組成物は、1〜200μm
、好ましくは5〜50μm の厚さになるように、支持
基材に溶展塗工、熱溶融押出塗工、又は基材層樹脂と共
に共押出する等の公知の方法によって使用することがで
きる。The pressure-sensitive adhesive composition of the present invention has a content of 1 to 200 μm.
It can be used by a known method such as spread coating, hot melt extrusion coating, or co-extrusion with a base layer resin on a supporting substrate so that the thickness is preferably 5 to 50 μm.
【0017】[0017]
【実施例】以下、本発明の実施例を挙げて具体的に説明
するが、本発明はこれらの実施例に限定されるものでは
ない。EXAMPLES Hereinafter, the present invention will be specifically described with reference to examples, but the present invention is not limited to these examples.
【0018】使用した成分は、次のとおりである。The components used are as follows.
【0019】(1)ポリイソブチレン(以下「PIB」
と略称する)
PIB−1:ビスタネックスMML80(エクソン社製
ポリイソブチレン、粘度平均分子量99万)
(2)ブチルゴム(以下「IIR」と略称する)
IIR−1:JSRブチル268(日本合成ゴム社製ブ
チルゴム、粘度平均分子量45万)
(3)ポリブテン(以下「PB」と略称する)
PB−1:出光ポリブテン300R(出光石油化学社製
ポリブテン、数平均分子量1,500)
(4)粘着付与樹脂(以下「AR」と略称する)
AR−1:パインクリスタルKE−311(荒川化学工
業社製水素添加ロジンエステル系樹脂)
AR−2:クリアロンP−85(ヤスハラケミカル社製
水素添加テルペン系樹脂)
AR−3:アルコンP−100(荒川化学工業社製脂環
族飽和炭化水素系樹脂)
AR−4:YSポリスターT115(ヤスハラケミカル
社製テルペンフェノール系樹脂)
(5)添加剤(以下「AD」と略称する)
AD−1:チヌビン622LD(チバガイギー社製ヒン
ダードアミン系紫外線安定剤)
AD−2:イルガノックス565(チバガイギー社製ヒ
ンダードフェノール系酸化防止剤)(1) Polyisobutylene (hereinafter "PIB")
PIB-1: Vistanex MML80 (polyisobutylene manufactured by Exxon Co., viscosity average molecular weight 990,000) (2) Butyl rubber (hereinafter abbreviated as “IIR”) IIR-1: JSR butyl 268 (manufactured by Japan Synthetic Rubber Co., Ltd.) Butyl rubber, viscosity average molecular weight 450,000) (3) Polybutene (abbreviated as "PB" hereinafter) PB-1: Idemitsu Polybutene 300R (Polybutene by Idemitsu Petrochemical Co., Ltd., number average molecular weight 1,500) (4) Tackifying resin ( AR-1: Pine Crystal KE-311 (hydrogenated rosin ester resin manufactured by Arakawa Chemical Industry Co., Ltd.) AR-2: Clearon P-85 (hydrogenated terpene resin manufactured by Yasuhara Chemical Co., Ltd.) AR- 3: Alcon P-100 (Arakawa Chemical Industry's alicyclic saturated hydrocarbon resin) AR-4: YS Polystar T1 15 (Terpene phenolic resin manufactured by Yasuhara Chemical Co., Ltd.) (5) Additive (abbreviated as "AD" hereinafter) AD-1: Tinuvin 622LD (Hindered amine UV stabilizer manufactured by Ciba Geigy) AD-2: Irganox 565 (Ciba Geigy) (Made by hindered phenolic antioxidant)
【0020】実施例1〜6及び比較例1〜8
厚さ60μm の白色ポリエチレンフィルムの片面に、表
1に示した組成の粘着剤組成物をトルエン溶媒に溶解し
た後、各々10μm の厚さに溶展塗工した。Examples 1 to 6 and Comparative Examples 1 to 8 A pressure-sensitive adhesive composition having the composition shown in Table 1 was dissolved in a toluene solvent on one side of a white polyethylene film having a thickness of 60 μm. It was spread coating.
【0021】[0021]
【表1】 [Table 1]
【0022】実施例1〜6及び比較例1〜8において得
られた表面保護粘着シートをアクリル系難接着性塗膜に
貼付し、同被着体への低温接着性、高速剥離性、耐候性
について試験した。なお、耐候性はウェザオメーターに
てカーボンアーク照射後の再剥離性、剥離後の被着面の
汚染、貼り跡の有無を評価した。The surface protective pressure-sensitive adhesive sheets obtained in Examples 1 to 6 and Comparative Examples 1 to 8 were attached to an acrylic hard-to-adhere coating film, and the low-temperature adhesiveness to the adherend, high-speed peelability and weather resistance were obtained. Was tested. The weather resistance was evaluated by a weatherometer for removability after carbon arc irradiation, contamination of the adhered surface after peeling, and presence or absence of sticking marks.
【0023】難接着性塗膜:ぬれ性(JIS K676
0に準拠)30dyn/cm未満の難接着性アクリル系塗膜
(シリコーン含有)
カーボンアーク照射:サンシャインウェザオメーターに
よるカーボンアーク300時間照射(降雨60時間)
低温接着性:−20℃雰囲気での180°ピール力(被
着体;難接着性アクリル系塗膜、剥離速度;0.3m/
分、JIS Z0237に準拠)を測定、評価結果;良
好 0.4N /10mm以上、悪い 0.4N /10mm未
満(難接着性アクリル系塗料を塗装した完成車に表面保
護粘着シートサンプルを貼付、−20℃雰囲気で時速1
00kmの速度で走行テストを行い、剥がれの有無を評価
した結果から設定)
高速剥離性:23℃雰囲気での180°ピール力(被着
体;難粘着性アクリル系塗膜、剥離速度;40m/分、
JIS Z0237に準拠)を測定、評価結果;良好
2N /10mm未満、悪い 2N /10mm以上(難接着性
アクリル系塗料を塗装した完成車に表面保護粘着シート
サンプルを貼付、剥離作業性を評価した結果から設定)
再剥離性:カーボンアーク照射後に23℃雰囲気で手で
剥離、評価結果;良好 簡単に剥離可能、悪い 剥離困
難
被着面の汚染・貼り跡:高速剥離性評価後、再剥離評価
後の被着体について目視評価Difficult-to-adhesive coating film: wettability (JIS K676
0) Difficult-to-adhesive acrylic coating less than 30 dyn / cm (containing silicone) Carbon arc irradiation: Carbon arc 300 hours irradiation by sunshine weatherometer (60 hours rainfall) Low temperature adhesion: 180 in -20 ° C atmosphere ° Peeling force (adherent; hardly adhesive acrylic coating, peeling speed; 0.3m /
Min., According to JIS Z0237), evaluation result; good 0.4N / 10mm or more, bad 0.4N / 10mm or less (paste the surface protective adhesive sheet sample on a completed car coated with a non-adhesive acrylic paint,- 1 hour / hour in 20 ° C atmosphere
Run test at a speed of 00 km and set based on the result of evaluation of the presence or absence of peeling) High speed peelability: 180 ° peeling force in an atmosphere of 23 ° C (adherend: difficult-to-adhesive acrylic coating, peeling speed: 40 m / Minutes,
(Based on JIS Z0237) was measured and evaluated;
Less than 2N / 10mm, bad 2N / 10mm or more (set based on the result of pasting the surface protection adhesive sheet sample on the completed car coated with the non-adhesive acrylic paint and evaluating the peeling workability) Removability: 23 after carbon arc irradiation Peeling by hand in ℃ atmosphere, evaluation result; Good Easy peeling, bad Difficulty peeling Contamination / sticking mark on adherend: Visual evaluation of adherend after high-speed peelability evaluation and re-peeling evaluation
【0024】試験結果を表2に示す。The test results are shown in Table 2.
【0025】[0025]
【表2】 [Table 2]
【0026】表2の実施例1〜6の結果から明らかなよ
うに、本発明の粘着剤組成物を用いた低温用表面保護粘
着シートは、難接着性塗膜に対する低温接着性が良好
で、高速剥離力が軽い。またカーボンアーク照射後の剥
離も容易で、被着面を汚染したり、貼り跡を残したりし
なかった。As is clear from the results of Examples 1 to 6 in Table 2, the low-temperature surface-protective pressure-sensitive adhesive sheet using the pressure-sensitive adhesive composition of the present invention has good low-temperature adhesiveness to a difficult-to-adhere coating film, High speed peeling force is light. Further, peeling after the carbon arc irradiation was easy, and the adherend surface was not contaminated and no trace of sticking was left.
【0027】他方、比較例1のように、粘着剤配合中に
ポリイソブチレン単独で、粘着付与樹脂を含まない場合
には、難接着性塗膜に対する低温接着性が悪くなる。On the other hand, as in Comparative Example 1, when polyisobutylene alone is contained in the pressure-sensitive adhesive formulation and no tackifying resin is contained, the low-temperature adhesiveness to the poorly-adhesive coating film becomes poor.
【0028】比較例2のように、粘着剤配合中にポリイ
ソブチレンとポリブテンのブレンドのみで粘着付与樹脂
を含まない場合にも、難接着性塗膜に対する低温接着性
が悪くなる。Even in the case where only the blend of polyisobutylene and polybutene is contained in the pressure-sensitive adhesive composition and no tackifying resin is contained as in Comparative Example 2, the low-temperature adhesiveness to the poorly-adhesive coating film is deteriorated.
【0029】比較例3のように、粘着剤配合中にポリイ
ソブチレンとポリブテンからなるブレンド物100重量
部に対するロジン系粘着付与樹脂が30重量部を超える
場合には、低温接着性、高速剥離性、耐候性が悪くなっ
たり、被着面を汚染したりする。As in Comparative Example 3, when the rosin-based tackifying resin was more than 30 parts by weight with respect to 100 parts by weight of the blend of polyisobutylene and polybutene during the formulation of the adhesive, low temperature adhesiveness, high speed peelability, The weather resistance will deteriorate and the adherend will be contaminated.
【0030】比較例4のように、粘着剤配合中のブレン
ド物に占めるポリブテンの比率が50重量%を超える場
合には、高速剥離性や耐候性が悪くなる。As in Comparative Example 4, when the proportion of polybutene in the blended product in the composition of the pressure-sensitive adhesive exceeds 50% by weight, the high speed peelability and the weather resistance are deteriorated.
【0031】比較例5のように、粘着剤配合中にポリイ
ソブチレンを含まず、ポリブテンに粘着付与樹脂を添加
しただけの場合には、高速剥離性や耐候性が悪くなった
り、被着面を汚染したりする。As in Comparative Example 5, when polyisobutylene was not included in the pressure-sensitive adhesive composition and only the tackifying resin was added to polybutene, the high-speed peelability and weather resistance were deteriorated, and the adherend surface was To pollute.
【0032】比較例6のように、粘着剤配合中の粘着付
与樹脂にロジン系樹脂を用いず、テルペン系樹脂を用い
た場合には、難接着性塗膜に対する低温接着性が悪くな
る。As in Comparative Example 6, when a terpene resin is used instead of a rosin resin as the tackifying resin in the pressure-sensitive adhesive composition, the low-temperature adhesiveness to the coating film having poor adhesion deteriorates.
【0033】比較例7のように、粘着剤配合中の粘着付
与樹脂にロジン系樹脂を用いず、石油系樹脂を用いた場
合には、難接着性塗膜に対する低温接着性が悪くなる。As in Comparative Example 7, when a petroleum resin is used instead of a rosin resin as the tackifying resin in the pressure-sensitive adhesive formulation, the low-temperature adhesiveness to the poorly-adhesive coating film deteriorates.
【0034】比較例8のように、粘着剤配合中の粘着付
与樹脂にロジン系樹脂を用いず、テルペンフェノール系
樹脂を用いた場合には、耐候性が悪くなったり、被着面
を汚染したりする。As in Comparative Example 8, when a terpene phenol resin was used instead of a rosin resin as the tackifying resin in the adhesive formulation, the weather resistance was poor and the adherend surface was contaminated. Or
【0035】[0035]
【発明の効果】本発明の粘着剤組成物は、高速剥離時の
剥離力は軽いが、難接着性塗膜に対する接着性に乏しい
ポリイソブチレン及び/又はブチルゴムに対し、一定範
囲の量のポリブテン及びロジン系粘着付与樹脂を加える
ことにより、高速剥離力が軽く、難接着性塗膜に対する
低温接着性を改善した表面保護粘着シートを提供する。EFFECT OF THE INVENTION The pressure-sensitive adhesive composition of the present invention has a low peeling force at high-speed peeling, but has a certain range of polybutene and polybutylene and / or butyl rubber having poor adhesion to a difficult-to-adhere coating film. Provided is a surface-protective pressure-sensitive adhesive sheet having a high-speed peeling force which is light by adding a rosin-based tackifying resin and which has improved low-temperature adhesiveness to a difficult-to-adhere coating film.
───────────────────────────────────────────────────── フロントページの続き (72)発明者 比野 欣之輔 東京都文京区関口二丁目3番3号 ニチ バン株式会社内 (56)参考文献 特開 昭54−96539(JP,A) 特開 昭60−123574(JP,A) 特開 平8−143829(JP,A) (58)調査した分野(Int.Cl.7,DB名) C09J 1/00 - 201/10 ─────────────────────────────────────────────────── ─── Continuation of front page (72) Inventor Kinnosuke Hino 2-3-3 Sekiguchi, Bunkyo-ku, Tokyo Nichiban Co., Ltd. (56) Reference JP-A-54-96539 (JP, A) Special features Kai 60-123574 (JP, A) JP-A-8-143829 (JP, A) (58) Fields investigated (Int.Cl. 7 , DB name) C09J 1/00-201/10
Claims (2)
50〜100重量%並びにポリブテン50〜0重量%か
らなるブレンド物100重量部に対し、ロジン系粘着付
与樹脂として、水素添加されたロジンエステル樹脂5〜
30重量部を添加したことを特徴とする車体表面の塗膜
保護粘着シート用の粘着剤組成物。1. A hydrogenated rosin ester resin 5 as a rosin-based tackifying resin is added to 100 parts by weight of a blend comprising 50 to 100% by weight of polyisobutylene and / or butyl rubber and 50 to 0% by weight of polybutene.
A pressure-sensitive adhesive composition for a coating film-protecting pressure-sensitive adhesive sheet on a vehicle body surface, comprising 30 parts by weight.
に対して、−20℃雰囲気での接着力(180°ピール
力、剥離速度0.3m/分)が0.4N/10mm以上、2
3℃雰囲気での高速剥離力(180°ピール力、前処理
70℃×24時間、剥離速度40m/分)が2N/10mm
未満である、請求項1記載の組成物。2. Adhesive strength (180 ° peel force, peeling speed 0.3 m / min) in an atmosphere of −20 ° C. is 0.4 N / 10 mm with respect to a coating having poor wettability of less than 30 dyn / cm. Above 2
High speed peeling force (180 ° peeling force, pretreatment 70 ° C x 24 hours, peeling speed 40m / min) in 2 ℃ / 10mm in 3 ℃ atmosphere
The composition of claim 1, which is less than.