JP2873886B2 - Silver halide photographic material and processing method thereof - Google Patents

Silver halide photographic material and processing method thereof

Info

Publication number
JP2873886B2
JP2873886B2 JP3116611A JP11661191A JP2873886B2 JP 2873886 B2 JP2873886 B2 JP 2873886B2 JP 3116611 A JP3116611 A JP 3116611A JP 11661191 A JP11661191 A JP 11661191A JP 2873886 B2 JP2873886 B2 JP 2873886B2
Authority
JP
Japan
Prior art keywords
group
silver halide
mol
compound
present
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP3116611A
Other languages
Japanese (ja)
Other versions
JPH04330433A (en
Inventor
勉 荒井
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Fujifilm Holdings Corp
Original Assignee
Fuji Photo Film Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Fuji Photo Film Co Ltd filed Critical Fuji Photo Film Co Ltd
Priority to JP3116611A priority Critical patent/JP2873886B2/en
Priority to DE69230387T priority patent/DE69230387T2/en
Priority to EP92106853A priority patent/EP0514675B1/en
Publication of JPH04330433A publication Critical patent/JPH04330433A/en
Priority to US08/480,946 priority patent/US5942384A/en
Application granted granted Critical
Publication of JP2873886B2 publication Critical patent/JP2873886B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【産業上の利用分野】本発明は、ハロゲン化銀写真感光
材料に関するものであり、特に高照度短時間露光におい
て、高感度かつ迅速処理適性に優れたハロゲン化銀写真
感光材料およびその現像処理方法に関するものである。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a silver halide photographic light-sensitive material, and more particularly, to a silver halide photographic light-sensitive material excellent in high sensitivity and rapid processing suitability in high-illuminance short-time exposure, and a developing method thereof. It is about.

【0002】[0002]

【従来の技術】写真感光材料の露光方法の一つに、原図
を走査し、その画像信号に基づいてハロゲン化銀写真感
光材料上に露光を行い、原図の画像に対応するネガ画像
もしくはポジ画像を形成する所謂スキャナー方式による
画像形成方法が知られている。スキャナー方式による画
像形成方法を実用した記録装置は種々あるが、網点発生
器を用いる所謂ドットジェネレーター方式が現在では数
多く用いられている。これらのスキャナー方式記録装置
の記録用光源としては、従来グローランプ、キセノンラ
ンプ、水銀ランプ、タングステンランプ、発光ダイオー
ドなどが用いられてきた。しかしこれらの光源はいずれ
も出力が弱く寿命が短いという実用上の欠点を有してい
た。これらの欠点を補うものとして、He−Neレー
ザ、アルゴンレーザ、He−Cdレーザ、半導体レーザ
などのコヒーレントなレーザ光源をスキャナー方式の光
源として用いるスキャナーがある。これらのキスャナー
に使用される感光材料には種々の特性が要求されるが、
特に10-3〜10-8秒という短時間露光で露光されるた
め、このような条件下でも、高感度かつ高コントラスト
であることが必須条件となる。また、レーザー管の寿命
を長く保つために出力を絞るには、高感度な感光材料の
方が有利である。また良好な網点を得るためにはレーザ
ービームをスリットなどを用いて整形することも必要で
あり、それにより低下するレーザ出力に対応するために
は高感度な感光材料が必要となる。
2. Description of the Related Art One of the methods for exposing a photographic light-sensitive material is to scan an original drawing and to expose the silver halide photographic light-sensitive material on the basis of an image signal thereof, thereby obtaining a negative image or a positive image corresponding to the image of the original drawing. There is known an image forming method using a so-called scanner method for forming an image. There are various types of recording apparatuses that use the image forming method based on the scanner system, but a so-called dot generator system using a halftone generator has been widely used at present. Glow lamps, xenon lamps, mercury lamps, tungsten lamps, light-emitting diodes, and the like have been used as recording light sources for these scanner recording apparatuses. However, each of these light sources has a practical disadvantage that the output is weak and the life is short. To compensate for these drawbacks, there is a scanner that uses a coherent laser light source such as a He-Ne laser, an argon laser, a He-Cd laser, or a semiconductor laser as a light source of a scanner system. Various characteristics are required for the photosensitive material used for these kisana,
In particular, since exposure is performed with a short exposure time of 10 −3 to 10 −8 seconds, high sensitivity and high contrast are essential conditions even under such conditions. In addition, a high-sensitivity photosensitive material is more advantageous for reducing the output in order to keep the life of the laser tube long. Further, in order to obtain a good halftone dot, it is necessary to shape the laser beam using a slit or the like, and a high-sensitivity photosensitive material is required in order to cope with the reduced laser output.

【0003】更に近年は、印刷業界においても作業の効
率化、スピードアップは強く望まれており、スキャニン
グの高速化及び感光材料の処理時間の短縮化に対する広
範囲なニーズが存在している。これら印刷分野のニーズ
に応えるために、露光機(スキャナー、プロッター)に
おいてはスキャニングの高速化、および高画質化のため
の線数増加やビームのしぼり込みが望まれており、ハロ
ゲン化銀写真感光材料においては、高感度で処理安定性
に優れ、かつ迅速に現像処理することができることが望
まれている。ここでいう迅速現像処理とはフィルムの先
端を自動現像機に挿入してから、現像槽、渡り部分、水
洗槽、乾燥部分を通過してフィルムの先端が乾燥部から
出て来た時間が15〜60秒である処理を言う。
[0003] In recent years, there has been a strong demand in the printing industry for work efficiency and speed-up, and there is a wide range of needs for faster scanning and shorter processing time for photosensitive materials. In order to respond to the needs in the printing field, exposure machines (scanners, plotters) are required to have a higher scanning speed and an increased number of lines and a narrower beam for higher image quality. It is desired that the material has high sensitivity, excellent processing stability, and can be rapidly developed. The rapid development process referred to here means that after inserting the leading end of the film into the automatic processor, it takes 15 minutes for the leading end of the film to come out of the drying section after passing through the developing tank, the transfer section, the washing tank, and the drying section.処理 60 seconds.

【0004】本発明者は、これらの目的のために塩化銀
が30モル%以上のハロゲン化銀粒子にイリジウム化合
物と鉄、レニウム、ルテニウム、オスミウム化合物を併
用すると効果があることを発見したが、この方法は、若
干高感化するものの、現像進行速度が遅く、現像時間の
短い迅速処理の場合に低感軟調化して、画質を損なうこ
とが問題であった。また特公昭57−22090号に記
載の方法のように水溶性イリジウム化合物を含んだハロ
ゲン化銀をセレン増感剤で増感する方法ではまだ低感度
であった。
The present inventor has found that it is effective to use an iridium compound and an iron, rhenium, ruthenium or osmium compound in combination with silver halide grains containing 30 mol% or more of silver chloride for these purposes. Although this method slightly increases the sensitivity, it has a problem in that the development progress speed is slow, and in the case of rapid processing in which the development time is short, the sensitivity is low and the image quality is impaired. In the method of sensitizing a silver halide containing a water-soluble iridium compound with a selenium sensitizer as in the method described in JP-B-57-22090, the sensitivity was still low.

【0005】[0005]

【発明が解決しようとする課題】本発明の目的は、高照
度露光時に高感なハロゲン化銀写真感光材料を提供する
ことにある。本発明の更に別の目的は、迅速処理を行っ
ても高感度でかつ良好な画質を与えるハロゲン化銀写真
感光材料及びその現像処理方法を提供することにある。
本発明の更に別の目的は現像液、定着液の補充量を下げ
ても高感でかつ良好な画質を与えるハロゲン化銀写真感
光材料及びその現像処理方法を提供することにある。
SUMMARY OF THE INVENTION An object of the present invention is to provide a silver halide photographic light-sensitive material which is highly sensitive to high illuminance exposure. Still another object of the present invention is to provide a silver halide photographic light-sensitive material which can provide high sensitivity and good image quality even when subjected to rapid processing, and a method for developing the same.
Still another object of the present invention is to provide a silver halide photographic light-sensitive material capable of providing a high-sensitivity and good image quality even when the replenishing amounts of a developing solution and a fixing solution are reduced, and a development processing method thereof.

【0006】[0006]

【課題を解決するための手段】上記本発明の目的は、塩
化銀が30モル%以上のハロゲン化銀からなり、かつ銀
に対して10-6モル以下のイリジウム化合物と、10-3
モル以下の鉄、レニウム、ルテニウム、オスミウム化合
物の少なくとも1種を含有し、かつ該感光性乳剤層がセ
レン増感剤で増感されたハロゲン化銀写真感光材料を用
いることにより達成された。
An object of the present invention is to provide an iridium compound in which silver chloride is composed of silver halide of 30 mol% or more and 10 -6 mol or less based on silver, and 10 -3 mol or less.
This was achieved by using a silver halide photographic light-sensitive material containing at least one compound of at most one mole of iron, rhenium, ruthenium and osmium compounds, and wherein the light-sensitive emulsion layer was sensitized with a selenium sensitizer.

【0007】本発明の具体的構成について詳細に説明す
る。本発明に係わるハロゲン化銀写真乳剤はハロゲン化
銀として、塩化銀、塩臭化銀もしくは塩沃臭化銀を含有
する。この時塩化銀は30モル%以上、より好ましくは
60モル%以上含有する。また沃化銀含有率は5モル%
以下、さらに好ましくは2モル%以下が良い。ハロゲン
化銀粒子の形状は、立方体、十四面体、八面体、不定
型、板状いずれでも良いが立方体もしくは板状が好まし
い。ハロゲン化銀粒子の平均粒径は0.01μm〜1μ
mが好ましいが、より好ましくは0.4μm以下であ
り、{(粒径の標準変差)/(平均粒径)}×100で
表わされる変動係数が15%以下、より好ましくは10
%以下の粒径分布の狭いものが好ましい。ハロゲン化銀
粒子は内部と表層が均一な相から成っていても、異なる
相からなっていてもよい。本発明に用いられる写真乳剤
は、P.Glafkides 著 Chimie et Physique Photographiq
ue(Paul Montel社刊、1967年)、G. F. Duffin著 P
hotographic Emulsion Chemistry(The Focal Press刊、
1966年)、V. L. Zelikman etal著 Making and Coa
ting Photographic Emulsion(The Focal Press 刊、1
964年)などに記載された方法を用いて調製すること
ができる。即ち、酸性法、中性法、アンモニア法等のい
ずれでもよく、又可溶性銀塩と可溶性ハロゲン塩を反応
させる形成としては、片側混合法、同時混合法、それら
の組合せなどのいずれを用いてもよい。粒子を銀イオン
過剰の下において形成させる方法(いわゆる逆混合法)
を用いることもできる。同時混合法の一つの形式として
ハロゲン化銀の生成される液相中のpAgを一定に保つ
方法、即ち、いわゆるコントロールド・ダブルジェット
法を用いることもできる。この方法によると、結晶形が
規則的で粒子サイズが均一に近いハロゲン化銀乳剤が得
られる。また、粒子サイズを均一にするためには、英国
特許1,535,016号、特公昭48−36890、
同52−16364号に記載されているように、硝酸銀
やハロゲン化アルカリの添加速度を粒子成長速度に応じ
て変化させる方法や、英国特許4,242,445号、
特開昭55−158124号に記載されているように水
溶液の濃度を変化させる方法を用いて、臨界飽和度を越
えない範囲において早く成長させることが好ましい。本
発明のハロゲン化銀乳剤の粒子形成は、四置換チオ尿
素、有機チオエーテル化合物の如きハロゲン化銀溶剤の
存在下で行うことが好ましい。本発明で用いられる好ま
しい四置換チオ尿素ハロゲン化銀溶剤は、特開昭53−
82408、同55−77737などに記載された次の
一般式(I)で表わされる化合物である。一般式(I)
The specific configuration of the present invention will be described in detail. The silver halide photographic emulsion according to the present invention contains silver chloride, silver chlorobromide or silver chloroiodobromide as silver halide. At this time, silver chloride is contained in an amount of 30 mol% or more, more preferably 60 mol% or more. The silver iodide content is 5 mol%
The content is more preferably 2 mol% or less. The shape of the silver halide grains may be any of cubic, tetradecahedral, octahedral, irregular, and tabular, but is preferably cubic or tabular. The average grain size of the silver halide grains is 0.01 μm to 1 μm.
m is preferred, and more preferably 0.4 μm or less, and the coefficient of variation represented by {(standard variation of particle size) / (average particle size)} × 100 is 15% or less, more preferably 10% or less.
% Or less having a narrow particle size distribution. In the silver halide grains, the inside and the surface layer may be composed of a uniform phase or may be composed of different phases. The photographic emulsion used in the present invention is Chimie et Physique Photographiq by P. Glafkides.
ue (Paul Montel, 1967), GF Duffin P
hotographic Emulsion Chemistry (The Focal Press,
1966), Making and Coa by VL Zelikman et al.
ting Photographic Emulsion (The Focal Press, 1
964). That is, any of an acidic method, a neutral method, an ammonia method and the like may be used, and a method of reacting a soluble silver salt with a soluble halide may be any one of a one-sided mixing method, a double-sided mixing method, and a combination thereof. Good. Method of forming grains in excess of silver ions (so-called reverse mixing method)
Can also be used. As one type of the double jet method, a method in which pAg in a liquid phase in which silver halide is formed is kept constant, that is, a so-called controlled double jet method can be used. According to this method, a silver halide emulsion having a regular crystal form and a nearly uniform grain size can be obtained. In order to make the particle size uniform, British Patent 1,535,016, JP-B-48-36890,
As described in JP-B-52-16364, a method of changing the addition rate of silver nitrate or alkali halide in accordance with the grain growth rate, a method disclosed in British Patent No. 4,242,445,
It is preferable to use a method of changing the concentration of the aqueous solution as described in JP-A-55-158124 to grow the solution quickly within a range not exceeding the critical saturation. The grain formation of the silver halide emulsion of the present invention is preferably carried out in the presence of a silver halide solvent such as a tetrasubstituted thiourea or an organic thioether compound. The preferred tetrasubstituted thiourea silver halide solvent used in the present invention is disclosed in
Compounds represented by the following general formula (I) described in, for example, 82408 and 55-77737. General formula (I)

【0008】[0008]

【化1】 Embedded image

【0009】一般式(I)について説明する。式中、R
1 、R2 、R3 及びR4 は、置換または未置換のアルキ
ル基、アルケニル基(アリル基など)、あるいは、置換
または未置換のアリールを表わし、これらは互いに同じ
でも異なってもよく、R1 〜R4 の炭素数の合計は30
以下が好ましい。また、R1 とR2 、R2 とR3 、ある
いはR3 とR4 で結合して5ないし6員の複素環イミダ
ゾリジンチオン、ピペリジン、モルホリンなどを作るこ
ともできる。上記アルキル基は直鎖又は分岐のものの両
方が用いられる。アルキル基の置換基としては、例えば
ヒドロキシ基(−OH)、カルボキシ基、スルホン酸
基、アミノ基、アルキル残基が1〜5個の炭素原子を有
するアルコキシ基(o−アルキル)、フェニル基または
5ないし6員の複素環(フランなど)である。アリール
基の置換基としては、ヒドロキシ基、カルボキシ基また
はスルホン酸基である。ここで、特に好ましくは、R1
〜R4 のうち、アルキル基が3つ以上で、各アルキル基
の炭素数は1〜5、アリール基はフェニル基、さらにR
1 〜R4 の炭素数の合計は20以下である。本発明に用
いることのできる化合物の例として次のものを挙げるこ
とができる。
The general formula (I) will be described. Where R
1 , R 2 , R 3 and R 4 represent a substituted or unsubstituted alkyl group, an alkenyl group (such as an allyl group), or a substituted or unsubstituted aryl, which may be the same or different, The total number of carbon atoms of 1 to R 4 is 30
The following is preferred. R 1 and R 2 , R 2 and R 3 , or R 3 and R 4 can be combined to form a 5- or 6-membered heterocyclic imidazolidinethione, piperidine, morpholine, or the like. Both linear and branched alkyl groups are used. Examples of the substituent of the alkyl group include a hydroxy group (—OH), a carboxy group, a sulfonic acid group, an amino group, an alkoxy group (o-alkyl) in which the alkyl residue has 1 to 5 carbon atoms, a phenyl group, It is a 5- or 6-membered heterocyclic ring (such as furan). The substituent of the aryl group is a hydroxy group, a carboxy group or a sulfonic group. Here, particularly preferably, R 1
To R 4 , there are three or more alkyl groups, each alkyl group has 1 to 5 carbon atoms, the aryl group is a phenyl group,
The total number of carbon atoms of 1 to R 4 is 20 or less. Examples of the compounds that can be used in the present invention include the following.

【0010】[0010]

【化2】 Embedded image

【0011】[0011]

【化3】 Embedded image

【0012】[0012]

【化4】 Embedded image

【0013】[0013]

【化5】 Embedded image

【0014】本発明に好ましく用いられる有機チオエー
テルハロゲン化銀溶剤は例えば特公昭47−11386
号(米国特許3,574,628号)等に記載された酸
素原子と硫黄原子がエチレンによりへだてられている基
(例えば−O−CH2 CH2 −S−)を少なくとも1つ
含む化合物、特開昭54−155828号(米国特許
4,276,374号)に記載された両端にアルキル基
(このアルキル基は各々ヒドロキシ、アミノ、カルボキ
シ、アミド又はスルホンの中から選ばれる少なくとも2
個の置換基を有する)を持つ鎖状のチオエーテル化合物
である。具体的には次のような例を挙げることができ
る。
The organic thioether silver halide solvent preferably used in the present invention is, for example, JP-B-47-11386.
No. (U.S. Patent No. 3,574,628) comprising at least one compound group wherein oxygen atom and a sulfur atom are separated by an ethylene (e.g. -O-CH 2 CH 2 -S-) in the like, especially An alkyl group at both ends described in Japanese Unexamined Patent Publication No. 54-155828 (U.S. Pat. No. 4,276,374) wherein each alkyl group is at least two groups selected from hydroxy, amino, carboxy, amide or sulfone
Thioether compound having two substituents). Specifically, the following examples can be given.

【0015】[0015]

【化6】 Embedded image

【0016】ハロゲン化銀溶剤の添加量は、用いる化合
物の種類および目的とする粒子サイズ、ハロゲン組成な
どにより異なるが、ハロゲン化銀1モルあたり10-5
10-2モルが好ましい。ハロゲン化銀溶剤の使用により
目的以上の粒子サイズになる場合は粒子形成時の温度、
銀塩溶液、ハロゲン塩溶液の添加時間などを変えること
により所望の粒子サイズにすることができる。
The amount of the silver halide solvent to be added varies depending on the kind of the compound used, the intended grain size, the halogen composition, and the like, but it is 10 -5 to 1 mol per mol of the silver halide.
10 -2 mol is preferred. If the grain size exceeds the target by using a silver halide solvent, the temperature during grain formation,
A desired particle size can be obtained by changing the addition time of the silver salt solution or the halogen salt solution.

【0017】本発明に用いられるイリジウム化合物とし
て、水溶性イリジウム化合物を用いることができる。例
えば、ハロゲン化イリジウム(III)化合物、またハロゲ
ン化イリジウム(IV) 化合物、またイリジウム錯塩で配
位子としてハロゲン、アミン類、オキザラト等を持つも
の、例えばヘキサクロロイリジウム(III)あるいは(I
V)錯塩、ヘキサアンミンイリジウム(III)あるいは(I
V)錯塩、トリオキザラトイリジウム(III)あるいは(I
V)錯塩などが挙げられる。本発明においては、これら
の化合物の中からIII 価のものとIV価のものを任意に組
合せて用いることができる。これらのイリジウム化合物
は水あるいは適当な溶媒に溶解して用いられるが、イリ
ジウム化合物の溶液を安定化させるために一般によく行
われる方法、即ちハロゲン化水素水溶液(例えば塩酸、
臭酸、フッ酸等)、あるいはハロゲン化アルカリ(例え
ばKCl、NaCl、KBr、NaBr等)を添加する
方法を用いることができる。水溶性イリジウムを用いる
代わりに、ハロゲン化銀粒子調製時にあらかじめイリジ
ウムをドープしてある別のハロゲン化銀粒子を添加して
溶解させることも可能である。本発明に係わるイリジウ
ム化合物の全添加量は、最終的に形成されるハロゲン化
銀1モル当たり1×10-8〜1×10-6モルが適当であ
り、好ましくは5×10-8〜1×10-6モルである。こ
れらの化合物の添加は、ハロゲン化銀乳剤の製造時及
び、乳剤を塗布する前の各段階において適宜行なうこと
ができるが、特に、粒子形成時に添加し、ハロゲン化銀
粒子中に組み込まれることが好ましい。具体的化合物と
しては、塩化第1イリジウム(III)、臭化第1イリジウ
ム(III)、塩化第2イリジウム(IV)、ヘキサクロロイ
リジウム(III)酸ナトリウム、ヘキサクロロイリジウム
(III)塩、ヘキサアミンイリジウム(IV)塩、トリオキ
ザラトイリジウム(III)塩、トリオキザラトイリジウム
(IV)塩、などのハロゲンアミン類、オキザラト錯塩類
が好ましい。
As the iridium compound used in the present invention, a water-soluble iridium compound can be used. For example, an iridium (III) halide compound, an iridium (IV) halide compound, or an iridium complex salt having a ligand such as hexachloroiridium (III) or (I)
V) Complex salts, hexaammineiridium (III) or (I
V) Complex salts, trioxalatoiridium (III) or (I
V) Complex salts and the like. In the present invention, these compounds may be used in any combination of III-valent and IV-valent compounds. These iridium compounds are used after being dissolved in water or a suitable solvent. However, a method generally used for stabilizing the solution of the iridium compound, that is, an aqueous hydrogen halide solution (for example, hydrochloric acid,
For example, a method of adding bromic acid, hydrofluoric acid, or the like, or an alkali halide (eg, KCl, NaCl, KBr, NaBr, or the like) can be used. Instead of using water-soluble iridium, it is also possible to add and dissolve another silver halide grain doped with iridium in advance during the preparation of the silver halide grain. The total amount of the iridium compound according to the present invention is suitably from 1 × 10 -8 to 1 × 10 -6 mol, preferably from 5 × 10 -8 to 1 mol, per mol of the finally formed silver halide. × 10 -6 mol. These compounds can be appropriately added during the production of a silver halide emulsion and at each stage before coating the emulsion. In particular, it is possible to add these compounds during grain formation and to incorporate them into silver halide grains. preferable. Specific compounds include iridium (III) chloride, iridium (III) bromide, iridium (IV) chloride, sodium hexachloroiridium (III), hexachloroiridium (III) salt, hexaamine iridium ( IV) Salts, trioxalatoiridium (III) salts, trioxalatoiridium (IV) salts, and other halogen amines, and oxalato complex salts are preferred.

【0018】本発明に用いられる鉄化合物は2価または
3価の鉄イオン含有化合物で、好ましくは本発明で用い
られる濃度範囲で水溶性をもつ鉄塩や鉄錯塩である。具
体的には ヒ酸第一鉄 臭化第一鉄 炭酸第一鉄 塩化第一鉄 クエン酸第一鉄 フッ化第一鉄 ぎ酸第一鉄 グルコン酸第一鉄 水酸化第一鉄 よう化第一鉄 乳酸第一鉄 しゅう酸第一鉄 リン酸第一鉄 こはく酸第一鉄 硫酸第一鉄 チオシアン酸第一鉄 硝酸第一鉄 硝酸第一鉄アンモニウム 塩基性酢酸第二鉄 アルブミン酸第二鉄 酢酸第二鉄アンモニウム 臭化第二鉄 塩化第二鉄 クロル酸第二鉄 クエン酸第二鉄 フッ化第二鉄 ぎ酸第二鉄 グリセロ・リン酸第二鉄 水酸化第二鉄 酸性リン酸第二鉄 硝酸第二鉄 リン酸第二鉄 ピロリン酸第二鉄 ピロリン酸第二鉄ナトリウム チオシアン化第二鉄 硫酸第二鉄 硫酸第二鉄アンモニウム 硫酸第二鉄グアニジン クエン酸第二鉄アンモニウム ヘキサンシアノ鉄(II)酸カリウム ベンタシアノアンミン第一鉄カリウム エチレンジニトリロ四酢酸第二鉄ナトリウム ヘキサシアノ鉄(III)酸カリウム 塩化トリス(ジピリジル)第二鉄 ベンタシアノニトロシル第二鉄カリウム 塩化ヘキサレア第二鉄 特にヘキサシアノ鉄(II)酸塩、ヘキサシアノ鉄(III)
酸塩、チオシアン酸第一鉄塩やチオシアン酸第二鉄塩が
顕著な効果を表す。
The iron compound used in the present invention is a divalent or trivalent iron ion-containing compound, and is preferably a water-soluble iron salt or iron complex in the concentration range used in the present invention. Specifically, ferrous arsenate, ferrous bromide, ferrous carbonate, ferrous chloride, ferrous citrate, ferrous fluoride, ferrous formate, ferrous gluconate, and ferrous hydroxide iodide Ferrous ferrous ferrous ferrous ferrous oxalate ferrous phosphate ferrous succinate ferrous thiocyanate ferrous nitrate ammonium ferrous nitrate basic ferric acetate ferric albumate Ferric ammonium acetate Ferric bromide Ferric chloride Ferric chloride Ferric citrate Ferric fluoride Ferric formate Glyceroferric phosphate Ferric hydroxide Acidic phosphoric acid Ferric ferric nitrate Ferric phosphate Ferric pyrophosphate Sodium ferric pyrophosphate Ferric thiocyanate Ferric sulfate Ammonium ferric sulfate Ferric guanidine sulfate Ferric ammonium citrate Hexanocyanoiron Potassium (II) acid potassium pentacyanoammine Chirenjinitoriro tetraacetate sodium ferric potassium hexacyanoferrate (III) chloride tris (dipyridyl) ferric preventor cyano nitrosyl ferric potassium chloride Hekisarea ferric particularly hexacyanoferrate (II), hexacyanoferrate (III)
Acid salts, ferrous thiocyanate and ferric thiocyanate exhibit remarkable effects.

【0019】本発明に用いられる、レニウム、ルテニウ
ム、オスミウム化合物はヨーロッパ公開特許(EP)0
336689A号、同0336427A1号、同033
6425A1号、同0336426A1号に記載された
六座配位錯体が好ましく、特にシアニド配位子を少なく
とも4個以上含むものが好ましい。好ましい態様におい
てはこれらの化合物は次のような式によって表わすこと
ができる。 〔M(Cn)6−yy n ここに、Mはレニウム、ルテニウム、オスミウムであ
り、Lは架橋配位子であり、yは整数0、1、又は2で
あり、そしてnは−2、−3又は−4である。具体例と
しては 〔Re(CN)5-4 〔Ru(CN)5-4 〔Os(CN)5-4 〔ReF(CN)5-4 〔RuF(CN)5-4 〔OsF(CN)5-4 〔ReCl(CN)5-4 〔RuCl(CN)5-4 〔OsCl(CN)5-4 〔ReBr(CN)5-4 〔RuBr(CN)5-4 〔OsBr(CN)5-4 〔ReI(CN)5-4 〔RuI(CN)5-4 〔OsI(CN)5-4 〔ReF2 (CN)4-4 〔RuF2 (CN)5-4 〔OsF2 (CN)5-4 〔ReCl2 (CN)4-4 〔RuCl2 (CN)4-4 〔OsCl2 (CN)4-4 〔RuBr2 (CN)4-4 〔OsBr2 (CN)4-4 〔ReBr2 (CN)4-4 〔RuI2 (CN)4-4 〔OsI2 (CN)5-4 〔Ru(CN)5(OCN)〕-4 〔Os(CN)5(OCN)〕-4 〔Ru(CN)5(SCN)〕-4 〔Os(CN)5(SCN)〕-4 〔Ru(CN)5(N3)〕-4 〔Os(CN)5(N3)〕-4 〔Ru(CN)5(H2 O)〕-3 〔Os(CN)5(H2 O)〕-3 が挙げられる。
The rhenium, ruthenium, and osmium compounds used in the present invention are disclosed in European Patent Application (EP) 0
No. 336689A, No. 0336427A1, No. 033
The hexadentate coordination complexes described in Nos. 6425A1 and 0336426A1 are preferable, and those containing at least four or more cyanide ligands are particularly preferable. In a preferred embodiment, these compounds can be represented by the formula: [M (Cn) 6 -yL y ] n where M is rhenium, ruthenium, osmium, L is a bridging ligand, y is an integer 0, 1, or 2, and n is- 2, -3 or -4. As a specific example, [Re (CN) 5 ] -4 [Ru (CN) 5 ] -4 [Os (CN) 5 ] -4 [ReF (CN) 5 ] -4 [RuF (CN) 5 ] -4 [ OsF (CN) 5 ] -4 [ReCl (CN) 5 ] -4 [RuCl (CN) 5 ] -4 [OsCl (CN) 5 ] -4 [ReBr (CN) 5 ] -4 [RuBr (CN) 5 ] -4 [OsBr (CN) 5] -4 [ReI (CN) 5] -4 [RuI (CN) 5] -4 [OSI (CN) 5] -4 [ReF 2 (CN) 4] -4 [ RuF 2 (CN) 5 ] -4 [OsF 2 (CN) 5 ] -4 [ReCl 2 (CN) 4 ] -4 [RuCl 2 (CN) 4 ] -4 [OsCl 2 (CN) 4 ] -4 [ RuBr 2 (CN) 4 ] -4 [OsBr 2 (CN) 4 ] -4 [ReBr 2 (CN) 4 ] -4 [RuI 2 (CN) 4 ] -4 [OsI 2 (CN) 5 ] -4 [ Ru (CN) 5 (OCN)] -4 [Os (CN) 5 (OCN)] - 4 [Ru (CN) 5 (SCN)] -4 [Os (CN) 5 (SCN)] -4 [Ru (CN) 5 (N 3 )] -4 [Os (CN) 5 (N 3 )] - 4 [Ru (CN) 5 (H 2 O)] -3 [Os (CN) 5 (H 2 O)] -3 .

【0020】上記の鉄、レニウム、ルテニウム、オスミ
ウム化合物は、ハロゲン化銀粒子形成中に添加すること
が好ましい。添加位置としては、粒子中に均一に分布さ
せても、また粒子形成の初期、中期、後期に局在化させ
ても良いが、粒子形成の後期、すなわち最終粒子径の5
0%、より好ましくは80%が形成された後に添加する
ことが好ましい。添加量は銀1モルに対し10-3モル以
下であるが、好ましくは10-6〜10-4モルである。本
発明においては第VIII族に含まれる他の金属、すなわち
コバルト、ニッケル、ロジウム、パラジウム、白金など
を併用しても良い。特に塩化ロジウム、ヘキサクロロジ
ウム(III)酸アンモニウムのごときロジウム塩との併用
は硬調な乳剤が得られ有利である。
The above iron, rhenium, ruthenium and osmium compounds are preferably added during the formation of silver halide grains. The addition position may be uniformly distributed in the particles, or may be localized in the initial, middle and late stages of the particle formation.
It is preferred to add after 0%, more preferably 80%, has been formed. The addition amount is 10 -3 mol or less, preferably 10 -6 to 10 -4 mol, per 1 mol of silver. In the present invention, other metals contained in Group VIII, that is, cobalt, nickel, rhodium, palladium, platinum and the like may be used in combination. In particular, when used in combination with a rhodium salt such as rhodium chloride or ammonium hexachlorodimate (III), a hard emulsion can be advantageously obtained.

【0021】本発明で用いられるセレン増感剤として
は、従来公知の特許に開示されているセレン化合物を用
いることができる。すなわち通常、不安定型セレン化合
物および/または非不安定型セレン化合物を添加して、
高温、好ましくは40℃以上で乳剤を一定時間攪拌する
ことにより用いられる。不安定型セレン化合物としては
特公昭44−15748号、特公昭43−13489
号、特願平2−130976号、特願平2−22930
0号などに記載の化合物を用いることが好ましい。具体
的な不安定セレン増感剤としては、イソセレノシアネー
ト類(例えばアリルイソセレノシアネートの如き脂肪族
イソセレノシアネート類)、セレノ尿素類、セレノケト
ン類、セレノアミド類、セレノカルボン酸類(例えば、
2−セレノプロピオン酸、2−セレノ酪酸)、セレノエ
ステル類、ジアシルセレニド類(例えば、ビス(3−ク
ロロ−2,6−ジメトキシベンゾイル)セレニド)、セ
レノホスフェート類、ホスフィンセレニド類、コロイド
状金属セレンなどがあげられる。不安定型セレン化合物
の好ましい類型を上に述べたがこれらは限定的なもので
はない。当業技術者には写真乳剤の増感剤としての不安
定型セレン化合物といえば、セレンが不安定である限り
に於いて該化合物の構造はさして重要なものではなく、
セレン増感剤分子の有機部分はセレンを担持し、それを
不安定な形で乳剤中に存在せしめる以外何らの役割をも
たないことが一般に理解されている。本発明において
は、かかる広範な概念の不安定セレン化合物が有利に用
いられる。本発明で用いられる非不安定型セレン化合物
としては特公昭46−4553号、特公昭52−344
92号および特公昭52−34491号に記載の化合物
が用いられる。非不安定型セレン化合物としては例えば
亜セレン酸、セレノシアン化カリウム、セレナゾール
類、セレナゾール類の四級塩、ジアリールセレニド、ジ
アリールジセレニド、ジアルキルセレニド、ジアルキル
ジセレニド、2−セレナゾリジンジオン、2−セレノオ
キサゾリジンチオンおよびこれらの誘導体等があげられ
る。これらのセレン化合物のうち、好ましくは以下の一
般式(III) 及び(IV)があげられる。一般式(III)
As the selenium sensitizer used in the present invention, selenium compounds disclosed in conventionally known patents can be used. That is, usually, an unstable selenium compound and / or a non-unstable selenium compound is added,
It is used by stirring the emulsion at a high temperature, preferably at 40 ° C. or higher for a certain period of time. Unstable selenium compounds include JP-B-44-15748 and JP-B-43-13489.
No., Japanese Patent Application No. 2-130976, Japanese Patent Application No. 2-2930
It is preferable to use the compounds described in No. 0 or the like. Specific examples of unstable selenium sensitizers include isoselenocyanates (eg, aliphatic isoselenocyanates such as allyl isoselenocyanate), selenoureas, selenoketones, selenoamides, and selenocarboxylic acids (for example,
2-selenopropionic acid, 2-selenobutyric acid), selenoesters, diacylselenides (eg, bis (3-chloro-2,6-dimethoxybenzoyl) selenide), selenophosphates, phosphine selenides, colloidal metal selenium And so on. Although the preferred types of unstable selenium compounds have been described above, they are not intended to be limiting. Skilled artisans say that an unstable selenium compound as a sensitizer for photographic emulsions is not so important as long as selenium is unstable,
It is generally understood that the organic portion of the selenium sensitizer molecule carries selenium and has no role other than to make it present in the emulsion in an unstable form. In the present invention, an unstable selenium compound having such a broad concept is advantageously used. Non-labile selenium compounds used in the present invention include JP-B-46-4553 and JP-B-52-344.
No. 92 and Japanese Patent Publication No. 52-34491 are used. Non-labile selenium compounds include, for example, selenous acid, potassium selenocyanide, selenazoles, quaternary salts of selenazoles, diaryl selenides, diaryl diselenides, dialkyl selenides, dialkyl diselenides, 2-selenazolidinediones, 2-selenooxazolidinethione and derivatives thereof. Of these selenium compounds, the following general formulas (III) and (IV) are preferred. General formula (III)

【0022】[0022]

【化7】 Embedded image

【0023】式中、Z1 およびZ2 はそれぞれ同じでも
異なっていてもよく、アルキル基(例えば、メチル基、
エチル基、t−ブチル基、アダマンチル基、t−オクチ
ル基)、アルケニル基(例えば、ビニル基、プロペニル
基)、アラルキル基(例えば、ベンジル基、フェネチル
基)、アリール基(例えば、フェニル基、ペンタフルオ
ロフェニル基、4−クロロフェニル基、3−ニトロフェ
ニル基、4−オクチルスルファモイルフェニル基、α−
ナフチル基)、複素環基(例えば、ピリジル基、チェニ
ル基、フリル基、イミダゾリル基)、−NR
1 (R2 )、−OR3 または−SR4 を表す。R1 、R
2 、R3 およびR4 はそれぞれ同じでも異なっていても
よく、アルキル基、アラルキル基、アリール基または複
素環基を表す。アルキル基、アラルキル基、アリール基
または複素環基としてはZ1 と同様な例があげられる。
ただし、R1 およびR2 は水素原子またはアシル基(例
えば、アセチル基、プロパノイル基、ベンゾイル基、ヘ
プタフルオロブタノイル基、ジフルオロアセチル基、4
−ニトロベンゾイル基、α−ナフトイル基、4−トリフ
ルオロメチルベンゾイル基)であってもよい。一般式(I
II) 中、好ましくはZ1 はアルキル基、アリール基また
は−NR1 (R2 )を表し、Z2 は−NR5 (R6 )を
表す。R1 、R2 、R5 およびR6 はそれぞれ同じでも
異なっていてもよく、水素原子、アルキル基、アリール
基、またはアシル基を表す。一般式(III) 中、より好ま
しくはN,N−ジアルキルセレノ尿素、N,N,N’−
トリアルキル−N’−アシルセレノ尿素、テトラアルキ
ルセレノ尿素、N,N−ジアルキル−アリールセレノア
ミド、N−アルキル−N−アリール−アリールセレノア
ミドを表す。一般式(IV)
In the formula, Z 1 and Z 2 may be the same or different and each represents an alkyl group (eg, a methyl group,
Ethyl group, t-butyl group, adamantyl group, t-octyl group), alkenyl group (eg, vinyl group, propenyl group), aralkyl group (eg, benzyl group, phenethyl group), aryl group (eg, phenyl group, pentane group) Fluorophenyl group, 4-chlorophenyl group, 3-nitrophenyl group, 4-octylsulfamoylphenyl group, α-
A naphthyl group), a heterocyclic group (e.g., a pyridyl group, a cyenyl group, a furyl group, an imidazolyl group), -NR
1 (R 2), - represents the OR 3 or -SR 4. R 1 , R
2 , R 3 and R 4 may be the same or different and each represents an alkyl group, an aralkyl group, an aryl group or a heterocyclic group. Alkyl group, an aralkyl group, the same examples as Z 1 is exemplified as an aryl group or a heterocyclic group.
Here, R 1 and R 2 represent a hydrogen atom or an acyl group (for example, acetyl group, propanoyl group, benzoyl group, heptafluorobutanoyl group, difluoroacetyl group,
-Nitrobenzoyl group, α-naphthoyl group, 4-trifluoromethylbenzoyl group). General formula (I
In II), preferably, Z 1 represents an alkyl group, an aryl group or —NR 1 (R 2 ), and Z 2 represents —NR 5 (R 6 ). R 1 , R 2 , R 5 and R 6 may be the same or different and each represents a hydrogen atom, an alkyl group, an aryl group, or an acyl group. In formula (III), more preferably N, N-dialkylselenourea, N, N, N'-
Represents trialkyl-N′-acylselenourea, tetraalkylselenourea, N, N-dialkyl-arylselenoamide, N-alkyl-N-aryl-arylselenoamide. General formula (IV)

【0024】[0024]

【化8】 Embedded image

【0025】式中、Z3 、Z4 およびZ5 はそれぞれ同
じでも異なっていてもよく、脂肪族基、芳香族基、複素
環基、−OR7 、−NR8 (R9 )、−SR10、−Se
11、X、水素原子を表す。R7 、R10およびR11は脂
肪族基、芳香族基、複素環基、水素原子またはカチオン
を表し、R8 およびR9 は脂肪族基、芳香族基、複素環
基または水素原子を表し、Xはハロゲン原子を表す。一
般式(IV)において、Z3 、Z4 、Z5 、R7 、R8 、R
9 、R10およびR11で表される脂肪族基は直鎖、分岐ま
たは環状のアルキル基、アルケニル基、アルキニル基、
アラルキル基(例えば、メチル基、エチル基、n−プロ
ピル基、イソプロピル基、t−ブチル基、n−ブチル
基、n−オクチル基、n−デシル基、n−ヘキサデシル
基、シクロペンチル基、シクロヘキシル基、アリル基、
2−ブテニル基、3−ペンテニル基、プロパルギル基、
3−ペンチニル基、ベンジル基、フェネチル基)を表
す。一般式(IV)において、Z3 、Z4 、Z5 、R7 、R
8 、R9 、R10およびR11で表される芳香族基は単環ま
たは縮環のアリール基(例えば、フェニル基、ペンタフ
ルオロフェニル基、4−クロロフェニル基、3−スルホ
フェニル基、α−ナフチル基、4−メチルフェニル基)
を表す。一般式(IV)において、Z3 、Z4 、Z5
7 、R8 、R9 、R10およびR11で表される複素環基
は窒素原子、酸素原子または硫黄原子のうち少なくとも
一つを含む3〜10員環の飽和もしくは不飽和の複素環
基(例えば、ピリジル基、チェニル基、フリル基、チア
ゾリル基、イミダゾリル基、ベンズイミダゾリル基)を
表す。一般式(IV)において、R7 、R10およびR11で表
されるカチオンはアルカリ金属原子またはアンモニウム
を表し、Xで表されるハロゲン原子は、例えばフッ素原
子、塩素原子、臭素原子または沃素原子を表す。一般式
(IV)中、好ましくはZ3 、Z4 またはZ5 は脂肪族基、
芳香族基または−OR7を表し、R7 は脂肪族基または
芳香族基を表す。一般式(IV)中、より好ましくはトリア
ルキルホスフィンセレニド、トリアリールホスフィンセ
レニド、トリアルキルセレノホスフェートまたはトリア
リールセレノホスフェートを表す。以下に一般式(III)
および(IV)で表される化合物の具体例を示すが、本発明
はこれに限定されるものではない。
In the formula, Z 3 , Z 4 and Z 5 may be the same or different, and may be an aliphatic group, an aromatic group, a heterocyclic group, —OR 7 , —NR 8 (R 9 ), —SR 10 , -Se
R 11 , X represents a hydrogen atom. R 7 , R 10 and R 11 represent an aliphatic group, an aromatic group, a heterocyclic group, a hydrogen atom or a cation, and R 8 and R 9 represent an aliphatic group, an aromatic group, a heterocyclic group or a hydrogen atom , X represents a halogen atom. In the general formula (IV), Z 3 , Z 4 , Z 5 , R 7 , R 8 , R
The aliphatic group represented by 9 , R 10 and R 11 is a linear, branched or cyclic alkyl group, alkenyl group, alkynyl group,
Aralkyl groups (e.g., methyl, ethyl, n-propyl, isopropyl, t-butyl, n-butyl, n-octyl, n-decyl, n-hexadecyl, cyclopentyl, cyclohexyl, Allyl group,
2-butenyl group, 3-pentenyl group, propargyl group,
3-pentynyl group, benzyl group, phenethyl group). In the general formula (IV), Z 3 , Z 4 , Z 5 , R 7 , R
The aromatic group represented by 8 , R 9 , R 10 and R 11 is a monocyclic or condensed aryl group (for example, phenyl, pentafluorophenyl, 4-chlorophenyl, 3-sulfophenyl, α- Naphthyl group, 4-methylphenyl group)
Represents In the general formula (IV), Z 3 , Z 4 , Z 5 ,
The heterocyclic group represented by R 7 , R 8 , R 9 , R 10 and R 11 is a 3- to 10-membered saturated or unsaturated heterocyclic ring containing at least one of a nitrogen atom, an oxygen atom and a sulfur atom. Represents a group (for example, a pyridyl group, a cyenyl group, a furyl group, a thiazolyl group, an imidazolyl group, a benzimidazolyl group). In the general formula (IV), the cation represented by R 7 , R 10 and R 11 represents an alkali metal atom or ammonium, and the halogen atom represented by X is, for example, a fluorine atom, a chlorine atom, a bromine atom or an iodine atom. Represents General formula
In (IV), preferably, Z 3 , Z 4 or Z 5 is an aliphatic group,
Represents an aromatic group or —OR 7 , and R 7 represents an aliphatic group or an aromatic group. In the general formula (IV), more preferably, it represents a trialkylphosphine selenide, a triarylphosphine selenide, a trialkylselenophosphate or a triarylselenophosphate. The general formula (III) below
Specific examples of the compounds represented by (IV) and (IV) are shown below, but the present invention is not limited thereto.

【0026】[0026]

【化9】 Embedded image

【0027】[0027]

【化10】 Embedded image

【0028】[0028]

【化11】 Embedded image

【0029】[0029]

【化12】 Embedded image

【0030】[0030]

【化13】 Embedded image

【0031】[0031]

【化14】 Embedded image

【0032】[0032]

【化15】 Embedded image

【0033】[0033]

【化16】 Embedded image

【0034】セレン増感法に関しては、米国特許第15
74944号、同第1602592号、同第16234
99号、同第3297446号、3297447号、同
第3320069号、同第3408196号、同第34
08197号、同第3442653号、同第34206
70号、同第3591385号、フランス特許第269
3038号、同第2093209号、特公昭52−34
491号、同52−34492号、同53−295号、
同57−22090号、特開昭59−180536号、
同59−185330号、同59−181337号、同
59−187338号、同59−192241号、同6
0−150046号、同60−151637号、同61
−246738号、特開平3−4221号、特願平1−
287380号、同1−250950号、同1−254
441号、同2−34090号、同2−110558
号、同2−130976号、同2−139183号、同
2−229300号更に、英国特許第255846号、
同第861984号及び、H.E. Spencer ら著、Journal
of Photographic Science 誌、31巻、158〜16
9ページ(1983年)等に開示されている。
Regarding the selenium sensitization method, US Pat.
No. 74944, No. 1602592, No. 16234
No. 99, No. 3297446, No. 3297449, No. 3320069, No. 3408196, No. 34
08197, 3434453, 34206
No. 70, No. 3591385, French Patent No. 269
No. 3038, No. 2093209, Japanese Patent Publication No. 52-34
No. 491, No. 52-34492, No. 53-295,
No. 57-22090, JP-A-59-180536,
59-185330, 59-181337, 59-187338, 59-192241, 6
No. 0-150046, No. 60-151637, No. 61
Japanese Patent Application No. Hei.
287380, 1-250950, 1-254
No. 441, No. 2-34090, No. 2-110558
Nos. 2-130976, 2-139183, 2-229300, and further, British Patent No. 255846,
No. 861984 and HE Spencer et al., Journal
of Photographic Science, Volume 31, 158-16
9 (1983).

【0035】これらのセレン増感剤は水またはメタノー
ル、エタノールなどの有機溶媒の単独または混合溶媒に
溶解しまたは、特願平2−264447号、同2−26
4448号に記載の形態にて化学増感時に添加される。
好ましくは化学増感開始前に添加される。使用されるセ
レン増感剤は1種に限られず上記セレン増感剤の2種以
上を併用して用いることができる。不安定セレン化合物
と非不安定セレン化合物を併用してもよい。本発明に使
用されるセレン増感剤の添加量は、用いるセレン増感剤
の活性度、ハロゲン化銀の種類や大きさ、熟成の温度お
よび時間などにより異なるが、好ましくは、ハロゲン化
銀1モル当り1×10-8モル以上である。より好ましく
は1×10-7モル以上1×10-5モル以下である。セレ
ン増感剤を用いた場合の化学熟成の温度は好ましくは4
5℃以上である。より好ましくは50℃以上、80℃以
下である。pAgおよびpHは任意である。例えばpH
は4から9までの広い範囲で本発明の効果は得られる。
セレン増感は、ハロゲン化銀溶剤の存在下で行うことに
は、より効果的である。
These selenium sensitizers are dissolved in water or an organic solvent such as methanol or ethanol, alone or in a mixed solvent, or disclosed in Japanese Patent Application Nos. 2-26447 and 2-2647.
No. 4448, added during chemical sensitization.
Preferably, it is added before the start of chemical sensitization. The selenium sensitizer used is not limited to one, and two or more of the above-described selenium sensitizers can be used in combination. An unstable selenium compound and a non-unstable selenium compound may be used in combination. The addition amount of the selenium sensitizer used in the present invention varies depending on the activity of the selenium sensitizer used, the type and size of silver halide, the ripening temperature and time, and the like. It is at least 1 × 10 -8 mol per mol. More preferably, it is 1 × 10 −7 mol or more and 1 × 10 −5 mol or less. The temperature of chemical ripening when using a selenium sensitizer is preferably 4
5 ° C. or higher. More preferably, it is 50 ° C. or more and 80 ° C. or less. pAg and pH are arbitrary. For example, pH
The effect of the present invention can be obtained in a wide range from 4 to 9.
Selenium sensitization is more effective when performed in the presence of a silver halide solvent.

【0036】本発明で用いることができるハロゲン化銀
溶剤としては、米国特許第3,271,157号、同第
3,531,289号、同第3,574,628号、特
開昭54−1019号、同54−158917号等に記
載された(a)有機チオエーテル類、特開昭53−82
408号、同55−77737号、同55−2982号
等に記載された(b)チオ尿素誘導体、特開昭53−1
44319号に記載された(c)酸素または硫黄原子と
窒素原子とにはさまれたチオカルボニル基を有するハロ
ゲン化銀溶剤、特開昭54−100717号に記載され
た(d)イミダゾール類、(e)亜硫酸塩、(f)チオ
シアネート等が挙げられる。特に好ましい溶剤として
は、チオシアネートおよびテトラメチルチオ尿素があ
る。また用いられる溶剤の量は種類によっても異なる
が、例えばチオシアネートの場合、好ましい量はハロゲ
ン化銀1モル当り1×10-4モル以上、1×10-2モル
以下である。
Examples of the silver halide solvent which can be used in the present invention include US Pat. Nos. 3,271,157, 3,531,289, 3,574,628, and JP-A-54-628. (A) Organic thioethers described in JP-A Nos. 1019 and 54-158917;
(B) thiourea derivatives described in JP-A Nos. 408, 55-77737 and 55-2982;
(C) a silver halide solvent having a thiocarbonyl group sandwiched between an oxygen or sulfur atom and a nitrogen atom, (d) imidazoles described in JP-A-54-100717, e) sulfites, and (f) thiocyanate. Particularly preferred solvents include thiocyanate and tetramethylthiourea. The amount of the solvent used varies depending on the kind. For example, in the case of thiocyanate, the preferred amount is 1 × 10 −4 mol or more and 1 × 10 −2 mol or less per mol of silver halide.

【0037】本発明のハロゲン化銀写真乳剤は、化学増
感においてイオウ増感及び/又は金増感を併用すること
によりさらに高感度、低かぶりを達成することができ
る。イオウ増感は、通常、イオウ増感剤を添加して、高
温、好ましくは40℃以上で乳剤を一定時間攪拌するこ
とにより行われる。また、金増感は、通常、金増感剤を
添加して、高温、好ましくは40℃以上で乳剤を一定時
間攪拌することにより行われる。上記のイオウ増感には
硫黄増感剤として公知のものを用いることができる。例
えばチオ硫酸塩、チオ尿素類、アリルイソチアシアネー
ト、シスチン、p−トルエンチオスルホン酸塩、ローダ
ニンなどが挙げられる。その他米国特許第1,574,
944号、同第2,410,689号、同第2,27
8,947号、同第2,728,668号、同第3,5
01,313号、同第3,656,955号各明細書、
ドイツ特許1,422,869号、特公昭56−249
37号、特開昭55−45016号公報等に記載されて
いる硫黄増感剤も用いることができる。硫黄増感剤の添
加量は、乳剤の感度を効果的に増大させるのに十分な量
でよい。この量は、pH、温度、ハロゲン化銀粒子の大
きさなどの種々の条件の下で相当の範囲にわたって変化
するが、ハロゲン化銀1モル当り1×10-7モル以上、
5×10-4モル以下が好ましい。
The silver halide photographic emulsion of the present invention can achieve higher sensitivity and lower fog by using sulfur sensitization and / or gold sensitization in chemical sensitization. Sulfur sensitization is usually carried out by adding a sulfur sensitizer and stirring the emulsion at a high temperature, preferably at 40 ° C. or higher for a certain period of time. Further, gold sensitization is usually performed by adding a gold sensitizer and stirring the emulsion at a high temperature, preferably at 40 ° C. or higher for a certain period of time. Known sulfur sensitizers can be used for the sulfur sensitization. For example, thiosulfates, thioureas, allylisothiocyanate, cystine, p-toluenethiosulfonate, rhodanine and the like can be mentioned. Other US Patent No. 1,574
No. 944, No. 2,410,689, No. 2,27
No. 8,947, No. 2,728,668, No. 3,5
Nos. 01,313 and 3,656,955,
German Patent 1,422,869, JP-B-56-249
No. 37, JP-A-55-45016 and the like can also be used. The addition amount of the sulfur sensitizer may be an amount sufficient to effectively increase the sensitivity of the emulsion. This amount varies over a considerable range under various conditions such as pH, temperature, silver halide grain size, etc., but is not less than 1 × 10 −7 mol per mol of silver halide.
It is preferably at most 5 × 10 -4 mol.

【0038】上記の金増感の金増感剤としては金の酸化
数が+1価でも+3価でもよく、金増感剤として通常用
いられる金化合物を用いることができる。代表的な例と
しては塩化金酸塩、カリウムクロロオーレート、オーリ
ックトリクロライド、カリウムオーリックチオシアネー
ト、カリウムヨードオーレート、テトラシアノオーリッ
クアシド、アンモニウムオーロチオシアネート、ピリジ
ルトリクロロゴールドなどが挙げられる。金増感剤の添
加量は種々の条件により異なるが、目安としてはハロゲ
ン化銀1モル当り1×10-7モル以上5×10-4モル以
下が好ましい。化学熟成に際して、ハロゲン化銀溶剤お
よびセレン増感剤またはセレン増感剤と併用することが
できるイオウ増感剤および/または金増感剤等の添加の
時期および順位については特に制限を設ける必要はな
く、例えば化学熟成の初期(好ましくは)または化学熟
成進行中に上記化合物を同時に、あるいは添加時点を異
にして添加することができる。また添加に際しては、上
記の化合物を水または水と混合し得る有機溶剤、例えば
メタノール、エタノール、アセトン等の単液あるいは混
合液に溶解せしめて添加させればよい。
As the gold sensitizer for the gold sensitization, the oxidation number of gold may be +1 or +3, and gold compounds usually used as gold sensitizers can be used. Representative examples include chloroaurate, potassium chloroaurate, auric trichloride, potassium auric thiocyanate, potassium iodooleate, tetracyano auric acidide, ammonium aurothiocyanate, pyridyl trichlorogold, and the like. Although the amount of the gold sensitizer to be added varies depending on various conditions, the standard is preferably 1 × 10 −7 mol to 5 × 10 −4 mol per mol of silver halide. During chemical ripening, there is no particular limitation on the timing and order of addition of a sulfur sensitizer and / or a gold sensitizer which can be used in combination with a silver halide solvent and a selenium sensitizer or a selenium sensitizer. For example, the above compounds can be added at the same time or at a different point in time, for example, at the beginning (preferably) of chemical ripening or during the progress of chemical ripening. In addition, the compound may be added by dissolving the above compound in water or an organic solvent miscible with water, for example, a single solution or a mixed solution of methanol, ethanol, acetone or the like.

【0039】本発明の感光材料には、感光材料の製造工
程、保存中あるいは写真処理中のカブリを防止しあるい
は写真性能を安定化させる目的で、種々の化合物を含有
させることができる。すなわちアゾール類たとえばベン
ゾチアゾリウム塩、ニトロインダゾール類、クロロベン
ズイミダゾール類、ブロモベンズイミダゾール類、メル
カプトチアゾール類、メルカプトベンゾチアゾール類、
メルカプトチアジアゾール類、アミノトリアゾール類、
ベンゾチアゾール類、ニトロベンゾトリアゾール類、な
ど;メルカプトピリミジン類;メルカプトトリアジン
類;たとえばオキサゾリンチオンのようなチオケト化合
物;アザインデン類、たとえばトリアザインデン類、テ
トラアザインデン類(特に4−ヒドロキシ置換(1,
3,3a,7)テトラザインデン類)、ペンタアザイン
デン類など;ベンゼンチオスルフォン酸、ベンゼンスル
フィン酸、ベンゼンスルフォン酸アミド等のようなカブ
リ防止剤または安定剤として知られた多くの化合物を加
えることができる。特にポリヒドロキシベンゼン化合物
は、感度は損うことなく耐圧力性を向上させる点で好ま
しい。ポリヒドロキシベンゼン化合物は下記のいずれか
の構造を持つ化合物であることが好ましい。一般式
(V)
The light-sensitive material of the present invention can contain various compounds for the purpose of preventing fog during the production process, storage or photographic processing of the light-sensitive material, or stabilizing photographic performance. That is, azoles such as benzothiazolium salts, nitroindazoles, chlorobenzimidazoles, bromobenzimidazoles, mercaptothiazoles, mercaptobenzothiazoles,
Mercaptothiadiazoles, aminotriazoles,
Benzothiazoles, nitrobenzotriazoles, etc .; mercaptopyrimidines; mercaptotriazines; thioketo compounds such as oxazolinethione; azaindenes such as triazaindenes, tetraazaindenes (especially 4-hydroxy-substituted (1,
3,3a, 7) tetrazaindenes), pentaazaindenes and the like; many compounds known as antifoggants or stabilizers such as benzenethiosulfonic acid, benzenesulfinic acid, benzenesulfonamide and the like are added. be able to. Particularly, a polyhydroxybenzene compound is preferable in that the pressure resistance is improved without impairing the sensitivity. The polyhydroxybenzene compound is preferably a compound having any one of the following structures. General formula (V)

【0040】[0040]

【化17】 Embedded image

【0041】次に一般式(V)について説明する。Xと
Yはそれぞれ−H、−OH、ハロゲン原子、−OM(M
はアルカリ金属イオン)、−アルキル基、フェニル基、
アミノ基、カルボニル基、スルホン基、スルホン化フェ
ニル基、スルホン化アルキル基、スルホン化アミノ基、
スルホン化カルボニル基、カルボキシフェニル基、カル
ボキシアルキル基、カルボキシアミノ基、ヒドロキシフ
ェニル基、ヒドロキシアルキル基、アルキルエーテル
基、アルキルフェニル基、アルキルチオエーテル基、又
はフェニルチオエーテル基である。以下に一般式(V)
の化合物の具体例を示す。
Next, the general formula (V) will be described. X and Y are each -H, -OH, a halogen atom, -OM (M
Is an alkali metal ion), -alkyl group, phenyl group,
Amino group, carbonyl group, sulfone group, sulfonated phenyl group, sulfonated alkyl group, sulfonated amino group,
A sulfonated carbonyl group, a carboxyphenyl group, a carboxyalkyl group, a carboxyamino group, a hydroxyphenyl group, a hydroxyalkyl group, an alkyl ether group, an alkylphenyl group, an alkylthioether group, or a phenylthioether group. The general formula (V) below
Specific examples of the compound are shown below.

【0042】[0042]

【化18】 Embedded image

【0043】[0043]

【化19】 Embedded image

【0044】[0044]

【化20】 Embedded image

【0045】ポリヒドロキシベンゼン化合物は、感材中
の乳剤層に添加しても、乳剤層以外の層中に添加しても
良い。添加量は1モルに対して10-5〜1モルの範囲が
有効であり、10-3モル〜10-1モルの範囲が特に有効
である。本発明を用いて作られた感光材料には、親水性
コロイド層にフィルター染料として、あるいはイラジェ
ーション防止その他種々の目的で水溶性染料を含有して
もよい。このような染料には、オキソノール染料、ヘミ
オキソノール染料、スチリル染料、メロシアニン染料、
シアニン染料及びアゾ染料が包含される。なかでもオキ
ソノール染料;ヘミオキソノール染料及びメロシアニン
染料が有用である。
The polyhydroxybenzene compound may be added to the emulsion layer in the light-sensitive material or may be added to layers other than the emulsion layer. The amount added is preferably in the range of 10 -5 to 1 mol per mol, and particularly preferably in the range of 10 -3 to 10 -1 mol. The light-sensitive material prepared by using the present invention may contain a water-soluble dye in the hydrophilic colloid layer as a filter dye or for various purposes such as prevention of irradiation. Such dyes include oxonol dyes, hemioxonol dyes, styryl dyes, merocyanine dyes,
Cyanine dyes and azo dyes are included. Among them, oxonol dyes; hemioxonol dyes and merocyanine dyes are useful.

【0046】本発明の感光性ハロゲン化銀乳剤は、増感
色素によって比較的長波長の青色光、緑色光、赤色光ま
たは赤外光に分光増感されてもよい。増感色素として
は、シアニン色素、メロシアニン色素、コンプレックス
シアニン色素、コンプレックスメロシアニン色素、ホロ
ホーラーシアニン色素、スチリル色素、ヘミシアニン色
素、オキソノール色素、ヘミオキソノール色素等を用い
ることができる。本発明に使用される有用な増感色素は
例えばRESEARCH DISCLOSURE Item 17643 IV −A
項(1978年12月p.23)、同 Item 1831X項
(1979年8月p.437)に記載もしくは引用された
文献に記載されている。特に各種スキャナー光源の分光
特性に適した分光感度を有する増感色素を有利に選択す
ることができる。 例えば A)アルゴンレーザー光源に対しては、特開昭60−1
62247号、特開平2−48653号、米国特許2,
161,331号、西独特許936,071号記載のシ
ンプルメロシアニン類、B)ヘリウム−ネオンレザー光
源に対しては、特開昭50−62425号、同54−1
8726号、同59−102229号に示された三核シ
アニン色素類、C)LED光源に対しては特公昭48−
42172号、同51−9609号、同55−3981
8号、特開昭62−284343号に記載されたチアカ
ルボシアニン類、D)半導体レーザー光源に対しては特
開昭59−191032号、特開昭60−80841号
に記載されたトリカルボシアニン類、特開昭59−19
2242号に記載された4−キノリン核を含有するジカ
ルボシアニン類などが有利に選択される。以下にそれら
の増感色素の代表的化合物を示す。 A)の具体的化合物例
The photosensitive silver halide emulsion of the present invention may be spectrally sensitized to blue light, green light, red light or infrared light having a relatively long wavelength by a sensitizing dye. As the sensitizing dye, a cyanine dye, a merocyanine dye, a complex cyanine dye, a complex merocyanine dye, a holo-holerocyanine dye, a styryl dye, a hemicyanine dye, an oxonol dye, a hemioxonol dye, and the like can be used. Useful sensitizing dyes for use in the present invention are, for example, RESEARCH DISCLOSURE Item 17643 IV-A
(Dec. 1978, p. 23) and Item 1831X (August 1979, p. 437). In particular, a sensitizing dye having a spectral sensitivity suitable for the spectral characteristics of various scanner light sources can be advantageously selected. For example, A) For an argon laser light source,
No. 62247, JP-A-2-48653, U.S. Pat.
Nos. 161 and 331 and simple merocyanines described in West German Patent 936,071; and B) helium-neon leather light sources.
No. 8726, 59-102229, and C) LED light sources.
No. 42172, No. 51-9609, No. 55-3981
8, thiacarbocyanines described in JP-A-62-284343, and D) tricarbocyanines described in JP-A-59-19032 and JP-A-60-80841 for semiconductor laser light sources. Kind, JP-A-59-19
Dicarbocyanines containing a 4-quinoline nucleus described in No. 2242 are advantageously selected. The representative compounds of these sensitizing dyes are shown below. Specific compound examples of A)

【0047】[0047]

【化21】 Embedded image

【0048】B)の具体的化合物例Specific examples of compound B)

【0049】[0049]

【化22】 Embedded image

【0050】C)の具体的化合物例Specific examples of compound C)

【0051】[0051]

【化23】 Embedded image

【0052】[0052]

【化24】 Embedded image

【0053】D)の具体的化合物例Specific compound examples of D)

【0054】[0054]

【化25】 Embedded image

【0055】これらの増感色素は単独に用いてもよい
が、それらの組合せを用いてもよく、増感色素の組合せ
は特に、強色増感の目的でしばしば用いられる。増感色
素とともに、それ自身分光増感作用をもたない色素ある
いは可視光を実質的に吸収しない物質であって、強色増
感を示す物質を乳剤中に含んでもよい。有用な増感色
素、強色増感を示す色素の組合せ及び強色増感を示す物
質はリサーチ・ディスクロージャー(Research Disclos
ure)176巻17643(1978年12月発行)第2
3頁IVのJ項に記載されている。本発明の増感色素の含
有量はハロゲン化銀乳剤の粒子径、ハロゲン組成、化学
増感の方法と程度、該化合物を含有させる層とハロゲン
化銀乳剤の関係、カブリ防止化合物の種類などに応じて
最適の量を選択することが望ましく、その選択のための
試験の方法は当業者のよく知るところである。通常は好
ましくはハロゲン化銀1モル当り10-7モルないし1×
10-2モル、特に10-6モルないし5×10-3モルの範
囲で用いられる。
These sensitizing dyes may be used alone or in combination, and the combination of sensitizing dyes is often used particularly for supersensitization. Along with the sensitizing dye, the emulsion may contain a dye which does not itself have a spectral sensitizing effect or a substance which does not substantially absorb visible light and exhibits supersensitization. Useful sensitizing dyes, combinations of dyes exhibiting supersensitization and substances exhibiting supersensitization are described in Research Disclos.
ure) 176, 17643 (issued December 1978) No. 2
It is described in section J on page 3, IV. The content of the sensitizing dye of the present invention depends on the grain size of the silver halide emulsion, the halogen composition, the method and degree of chemical sensitization, the relationship between the layer containing the compound and the silver halide emulsion, the type of antifoggant compound, and the like. It is desirable to select the optimal amount accordingly, and the methods of testing for that selection are well known to those skilled in the art. Usually, it is preferably from 10 -7 mol to 1 × per mol of silver halide.
It is used in an amount of 10 −2 mol, particularly 10 −6 mol to 5 × 10 −3 mol.

【0056】本発明の写真感光材料の写真乳剤層には感
度上昇、コントラスト上昇、または現像促進の目的で、
たとえばポリアルキレンオキシドまたはそのエーテル、
エステル、アミンなどの誘導体、チオエーテル化合物、
チオモルフォリン類、四級アンモニウム塩化合物、ウレ
タン誘導体、尿素誘導体、イミダゾール誘導体、3−ピ
ラゾリドン類アミノフェノール類等の現像主薬を含んで
も良い。なかでも3−ピラゾリドン類(1−フェニル−
3−ピラゾリドン、1−フェニル−4−メチル−4−ヒ
ドロキシメチル−3−ピラゾリドンなど)が好ましく、
通常5g/m2以下で用いられ、0.01〜0.2g/m2
がより好ましい。本発明の写真乳剤及び非感光性の親水
性コロイドには無機または有機の硬膜剤を含有してよ
い。例えば活性ビニル化合物(1,3,5−トリアクリ
ロイル−ヘキサヒドロ−s−トリアジン、ビス(ビニル
スルホニル)メチルエーテル、N,N−メチレンビス−
〔β−(ビニルスルホニル)プロピオンアミド〕な
ど)、活性ハロゲン化物(2,4−ジクロル−6−ヒド
ロキシ−s−トリアジンなど)、ムコハロゲン酸類(ム
コクロル酸など)、N−カルバモイルピリジニウム塩類
(1−モルホリ)カルボニル−3−ピリジニオ)メタン
スルホナートなど)、ハロアミジニウム塩類(1−(1
−クロロ−1−ピリジノメチレン)ピロリジニウム、2
−ナフタレンスルホナートなど)を単独または組み合わ
せて用いることができる。なかでも、特開昭53−41
220号、同53−57257号、同59−16254
6号、同60−80846号に記載の活性ビニル化合物
および米国特許3,325,287号に記載の活性ハロ
ゲン化物が好ましい。本発明を用いて作られる感光材料
の写真乳剤層または他の親水性コロイド層には塗布助
剤、帯電防止、スベリ性改良、乳化分散、接着防止及び
写真特性改良(例えば、現像促進、硬調化、増感)等種
々の目的で、種々の界面活性剤を含んでもよい。例えば
サポニン(ステロイド系)、アルキレンオキサイド誘導
体(例えばポリエチレングリコール、ポリエチレングリ
コール/ポリプロピレングリコール縮合物、ポリエチレ
ングリコールアルキルエーテル類又はポリエチレングリ
コールアルキルアリールエーテル類、ポリエチレングリ
コールエステル類、ポリエチレングリコールソルビタン
エステル類、ポリアルキレングリコールアルキルアミン
又はアミド類、シリコーンのポリエチレンオキサイド付
加物類)、グリシドール誘導体(例えばアルケニルコハ
ク酸ポリグリセリド、アルキルフェノールポリグリセリ
ド)、多価アルコールの脂肪酸エステル類、糖のアルキ
ルエステル類などの非イオン性界面活性剤;アルキルカ
ルボン酸塩、アルキルスルフォン酸塩、アルキルベンゼ
ンスルフォン酸塩、アルキルナフタレンスルフォン酸
塩、アルキル硫酸エステル類、アルキルリン酸エステル
類、N−アシル−N−アルキルタウリン類、スルホコハ
ク酸エステル類、スルホアルキルポリオキシエチレンア
ルキルフェニルエーテル類、ポリオキシエチレンアルキ
ルリン酸エステル類などのような、カルボキシ基、スル
ホ基、ホスホ基、硫酸エステル基、リン酸エステル基等
の酸性基を含むアニオン界面活性剤;アミノ酸塩、アミ
ノアルキルスルホン酸類、アミノアルキル硫酸又はリン
酸エステル類、アルキルベタイン類、アミンオキシド類
などの両性界面活性剤;アルキルアミン塩類、脂肪族あ
るいは芳香族第4級アンモニウム塩類、ピリジニウム、
イミダゾリウムなどの複素環第4級アンモニウム塩類、
及び脂肪族又は複素環を含むホスホニウム又はスルホニ
ウム塩類などのカチオン界面活性剤を用いることができ
る。また、帯電防止のためには特開昭60−80849
号などに記載された含フッ素系界面活性剤を用いること
が好ましい。
In the photographic emulsion layer of the photographic light-sensitive material of the present invention, for the purpose of increasing sensitivity, increasing contrast, or promoting development,
For example, polyalkylene oxide or its ether,
Derivatives such as esters and amines, thioether compounds,
Developing agents such as thiomorpholines, quaternary ammonium salt compounds, urethane derivatives, urea derivatives, imidazole derivatives, 3-pyrazolidones and aminophenols may be contained. Among them, 3-pyrazolidones (1-phenyl-
3-pyrazolidone, 1-phenyl-4-methyl-4-hydroxymethyl-3-pyrazolidone) are preferred,
Usually used at 5 g / m 2 or less, 0.01 to 0.2 g / m 2
Is more preferred. The photographic emulsion and the non-photosensitive hydrophilic colloid of the present invention may contain an inorganic or organic hardener. For example, active vinyl compounds (1,3,5-triacryloyl-hexahydro-s-triazine, bis (vinylsulfonyl) methyl ether, N, N-methylenebis-
[Β- (vinylsulfonyl) propionamide]), active halides (eg, 2,4-dichloro-6-hydroxy-s-triazine), mucohalic acids (eg, mucochloric acid), N-carbamoylpyridinium salts (1- Morpholi) carbonyl-3-pyridinio) methanesulfonate, etc.), haloamidinium salts (1- (1
-Chloro-1-pyridinomethylene) pyrrolidinium, 2
-Naphthalene sulfonate) can be used alone or in combination. Above all, JP-A-53-41
No. 220, No. 53-57257, No. 59-16254
No. 6, No. 60-80846 and active halides described in U.S. Pat. No. 3,325,287 are preferred. The photographic emulsion layer or other hydrophilic colloid layer of the light-sensitive material prepared by using the present invention may have coating aids, antistatic, slipperiness improvement, emulsification / dispersion, adhesion prevention and photographic property improvement (eg, development acceleration, high contrast For various purposes such as sensitization), various surfactants may be contained. For example, saponins (steroids), alkylene oxide derivatives (eg, polyethylene glycol, polyethylene glycol / polypropylene glycol condensate, polyethylene glycol alkyl ethers or polyethylene glycol alkyl aryl ethers, polyethylene glycol esters, polyethylene glycol sorbitan esters, polyalkylene glycol) Nonionic surfactants such as alkylamines or amides, polyethylene oxide adducts of silicone, glycidol derivatives (eg, alkenyl succinic acid polyglycerides, alkylphenol polyglycerides), fatty acid esters of polyhydric alcohols, and alkyl esters of sugars. Agent: alkyl carboxylate, alkyl sulfonate, alkyl benzene sulfo Acid salts, alkyl naphthalene sulfonates, alkyl sulfates, alkyl phosphates, N-acyl-N-alkyl taurines, sulfosuccinates, sulfoalkyl polyoxyethylene alkyl phenyl ethers, polyoxyethylene alkyl phosphorus Anionic surfactants containing an acidic group such as a carboxy group, a sulfo group, a phospho group, a sulfate group or a phosphate group, such as acid esters; amino acid salts, aminoalkyl sulfonic acids, aminoalkyl sulfate or phosphoric acid Amphoteric surfactants such as esters, alkyl betaines and amine oxides; alkylamine salts, aliphatic or aromatic quaternary ammonium salts, pyridinium,
Heterocyclic quaternary ammonium salts such as imidazolium,
And cationic surfactants such as phosphonium or sulfonium salts containing aliphatic or heterocyclic rings. In order to prevent charging, Japanese Patent Application Laid-Open No. Sho 60-80849
It is preferable to use the fluorinated surfactant described in the above item.

【0057】本発明の写真感光材料には写真乳剤層その
他の親水性コロイド層に接着防止の目的でシリカ、酸化
マグネシウム、ポリメチルメタクリレート等のマット剤
を含むことができる。本発明で用いられる感光材料には
寸度安定性の目的で水不溶または難溶性合成ポリマーの
分散物を含むことができる。たとえばアルキル(メタ)
アクリレート、アルコキシアクリル(メタ)アクリレー
ト、グリシジル(メタ)アクリレート、などの単独もし
くは組合わせ、またはこれらとアクリル酸、メタアクリ
ル酸、などの組合せを単量体成分とするポリマーを用い
ることができる。写真乳剤の縮合剤または保護コロイド
としては、ゼラチンを用いるのが有利であるが、それ以
外の親水性コロイドも用いることができる。たとえばゼ
ラチン誘導体、ゼラチンと他の高分子とのグラフトポリ
マー、アルブミン、カゼイン等の蛋白質;ヒドロキシエ
チルセルロース、カルボキシメチルセルロース、セルロ
ース硫酸エステル類等の如きセルロース誘導体、アルギ
ン酸ソーダ、澱粉誘導体などの糖誘導体、ポリビニルア
ルコール、ポリビニルアルコール部分アセタール、ポリ
−N−ビニルピロリドン、ポリアクリル酸、ポリメタク
リル酸、ポリアクリルアミド、ポリビニルイミダゾー
ル、ポリビニルピラゾール等の単一あるいは共重合体の
如き多種の合成親水性高分子物質を用いることができ
る。ゼラチンとしては石灰処理ゼラチンのほか、酸処理
ゼラチンを用いてもよく、ゼラチン加水分解物、ゼラチ
ン酵素分解物も用いることができる。本発明で用いられ
るハロゲン化銀乳剤層には、アルキルアクリレートの如
きポリマーラテックスを含有せしめることができる。本
発明の感光材料の支持体としてはセルローストリアセテ
ート、セルロースジアセテート、ニトロセルロース、ポ
リスチレン、ポリエチレンテレフタレート紙、バライタ
塗覆紙、ポリオレフィン被覆紙などを用いることができ
る。
The photographic light-sensitive material of the present invention may contain a matting agent such as silica, magnesium oxide or polymethyl methacrylate for the purpose of preventing adhesion to the photographic emulsion layer or other hydrophilic colloid layers. The light-sensitive material used in the present invention may contain a dispersion of a water-insoluble or hardly soluble synthetic polymer for the purpose of dimensional stability. For example, alkyl (meth)
A polymer having a monomer component of acrylate, alkoxyacryl (meth) acrylate, glycidyl (meth) acrylate, or the like alone or in combination, or a combination thereof with acrylic acid, methacrylic acid, or the like can be used. Gelatin is advantageously used as a condensing agent or protective colloid of the photographic emulsion, but other hydrophilic colloids can also be used. For example, gelatin derivatives, graft polymers of gelatin and other macromolecules, proteins such as albumin and casein; cellulose derivatives such as hydroxyethylcellulose, carboxymethylcellulose and cellulose sulfates; sugar derivatives such as sodium alginate and starch derivatives; polyvinyl alcohol Use of various kinds of synthetic hydrophilic high-molecular substances such as mono- or copolymers such as polyvinyl alcohol partial acetal, poly-N-vinylpyrrolidone, polyacrylic acid, polymethacrylic acid, polyacrylamide, polyvinylimidazole and polyvinylpyrazole Can be. As gelatin, in addition to lime-processed gelatin, acid-processed gelatin may be used, and gelatin hydrolyzate and gelatin enzyme hydrolyzate can also be used. The silver halide emulsion layer used in the present invention may contain a polymer latex such as an alkyl acrylate. As a support of the light-sensitive material of the present invention, cellulose triacetate, cellulose diacetate, nitrocellulose, polystyrene, polyethylene terephthalate paper, baryta-coated paper, polyolefin-coated paper and the like can be used.

【0058】本発明に使用する現像液に用いる現像主薬
には特別な制限はないが、良好な網点品質を得やすい点
で、ジヒドロキシベンゼン類を含むことが好ましく、ジ
ヒドロキシベンゼン類と1−フェニル−3−ピラゾリド
ン類の組合せまたはジヒドロキシベンゼン類とp−アミ
ノフェノール類の組合せを用いる場合もある。本発明に
用いるジヒドロキシベンゼン現像主薬としてはハイドロ
キノン、クロロハイドロキノン、ブロムハイドロキノ
ン、イソプロピルハイドロキノン、メチルハイドロキノ
ン、2,3−ジクロロハイドロキノン、2,5−ジクロ
ロハイドロキノン、2,3−ジブロムハイドロキノン、
2,5−ジメチルハイドロキノンなどがあるが特にハイ
ドロキノンが好ましい。本発明に用いる1−フェニル−
3−ピラゾリドン又はその誘導体の現像主薬としては1
−フェニル−3−ピラゾリドン、1−フェニル−4,4
−ジメチル−3−ピラゾリドン、1−フェニル−4−メ
チル−4−ヒドロキシメチル−3−ピラゾリドン、1−
フェニル−4,4−ジヒドロキシメチル−3−ピラゾリ
ドン、1−フェニル−5−メチル−3−ピラゾリドン、
1−p−アミノフェニル−4,4−ジメチル−3−ピラ
ゾリドン、1−p−トリル−4,4−ジメチル−3−ピ
ラゾリドン、1−p−トリル−4−メチル−4−ヒドロ
キシメチル−3−ピラゾリドンなどがある。本発明に用
いるp−アミノフェノール系現像主薬としてはN−メチ
ル−p−アミノフェノール、p−アミノフェノール、N
−(β−ヒドロキシエチル)−p−アミノフェノール、
N−(4−ヒドロキシフェニル)グリシン、2−メチル
−p−アミノフェノール、p−ベンジルアミノフェノー
ル等があるが、なかでもN−メチル−p−アミノフェノ
ールが好ましい。現像主薬は通常0.05モル/リット
ル〜0.8モル/リットルの量で用いられるのが好まし
い。またジヒドロキシベンゼン類と1−フェニル−3−
ピラゾリドン類又はp・アミノ・フェノール類との組合
せを用いる場合には前者を0.05モル/リットル−
0.5モル/リットル、後者を0.06モル/リットル
以下の量で用いるのが好ましい。本発明に用いる亜硫酸
塩の保恒剤としては亜硫酸ナトリウム、亜硫酸カリウ
ム、亜硫酸リチウム、亜硫酸アンモニウム、重亜硫酸ナ
トリウム、メタ重亜硫酸カリウム、ホルムアルデヒド重
亜硫酸ナトリウムなどがある。亜硫酸塩は0.3モル/
リットル以上、特に0.4モル/リットル以上が好まし
い。また上限は2.5モル/リットルまで、特に、1.
2までとするのが好ましい。pHの設定のために用いる
アルカリ剤には水酸化ナトリウム、水酸化カリウム、炭
酸ナトリウム、炭酸カリウム、第三リン酸ナトリウム、
第三リン酸カリウム、ケイ酸ナトリウム、ケイ酸カリウ
ムの如きpH調節剤や緩衝剤を含む。上記成分以外に用
いられる添加剤としてはホウ酸、ホウ砂などの化合物、
臭化ナトリム、臭化カリウム、沃化カリウムの如き現像
抑制剤:エチレングリコール、ジエチレングリコール、
トリエチレングリコール、ジメチルホルムアミド、メチ
ルセロソルブ、ヘキシレングリコール、エタノール、メ
タノールの如き有機溶剤:1−フェニル−5−メルカプ
トテトラゾール、2−メルカプトベンツイミダゾール−
5−スルホン酸ナトリウム塩等のメルカプト系化合物、
5−ニトロインダゾール等のインダゾール系化合物、5
−メチルベンツトリアゾール等のベンツトリアゾール系
化合物などのカブリ防止剤を含んでもよく、更に必要に
応じて色調剤、界面活性剤、消泡剤、硬水軟化剤、硬膜
剤、などを含んでもよい。特に特開昭56−10624
4号に記載のアミノ化合物、特公昭48−35493号
に記載のイミダゾール化合物が現像促進あるいは感度上
昇という点で好ましい。本発明に用いられる現像液に
は、銀汚れ防止剤として特開昭56−24347号に記
載の化合物、現像ムラ防止剤として(特開昭62−21
2,651号)に記載の化合物、溶解助剤として特開昭
61−267759号に記載の化合物を用いることがで
きる。
The developing agent used in the developer used in the present invention is not particularly limited, but preferably contains dihydroxybenzenes in that good halftone dot quality can be easily obtained. A combination of -3-pyrazolidones or a combination of dihydroxybenzenes and p-aminophenols may be used. As the dihydroxybenzene developing agent used in the present invention, hydroquinone, chlorohydroquinone, bromohydroquinone, isopropylhydroquinone, methylhydroquinone, 2,3-dichlorohydroquinone, 2,5-dichlorohydroquinone, 2,3-dibromohydroquinone,
There are 2,5-dimethylhydroquinone and the like, but hydroquinone is particularly preferred. 1-phenyl- used in the present invention
The developing agent for 3-pyrazolidone or a derivative thereof is 1
-Phenyl-3-pyrazolidone, 1-phenyl-4,4
-Dimethyl-3-pyrazolidone, 1-phenyl-4-methyl-4-hydroxymethyl-3-pyrazolidone, 1-
Phenyl-4,4-dihydroxymethyl-3-pyrazolidone, 1-phenyl-5-methyl-3-pyrazolidone,
1-p-aminophenyl-4,4-dimethyl-3-pyrazolidone, 1-p-tolyl-4,4-dimethyl-3-pyrazolidone, 1-p-tolyl-4-methyl-4-hydroxymethyl-3- And pyrazolidone. Examples of the p-aminophenol-based developing agent used in the present invention include N-methyl-p-aminophenol, p-aminophenol and N-methylphenol.
-(Β-hydroxyethyl) -p-aminophenol,
There are N- (4-hydroxyphenyl) glycine, 2-methyl-p-aminophenol, p-benzylaminophenol and the like, among which N-methyl-p-aminophenol is preferable. The developing agent is preferably used in an amount of usually 0.05 mol / l to 0.8 mol / l. Also, dihydroxybenzenes and 1-phenyl-3-
When a combination with pyrazolidones or p-amino-phenols is used, the former is used in an amount of 0.05 mol / liter.
It is preferred to use 0.5 mol / l and the latter in an amount of 0.06 mol / l or less. Examples of the sulfite preservative used in the present invention include sodium sulfite, potassium sulfite, lithium sulfite, ammonium sulfite, sodium bisulfite, potassium metabisulfite, and formaldehyde sodium bisulfite. 0.3 mol of sulfite /
It is preferably at least liter, especially at least 0.4 mol / liter. The upper limit is up to 2.5 mol / l, especially 1.
It is preferably up to 2. Alkali agents used for setting the pH include sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate tribasic,
PH adjusters and buffers such as potassium tertiary phosphate, sodium silicate and potassium silicate are included. Compounds such as boric acid and borax as additives used in addition to the above components,
Development inhibitors such as sodium bromide, potassium bromide and potassium iodide: ethylene glycol, diethylene glycol,
Organic solvents such as triethylene glycol, dimethylformamide, methyl cellosolve, hexylene glycol, ethanol and methanol: 1-phenyl-5-mercaptotetrazole, 2-mercaptobenzimidazole-
Mercapto compounds such as 5-sulfonic acid sodium salt,
Indazole compounds such as 5-nitroindazole, 5
-It may contain an antifoggant such as a benztriazole-based compound such as methylbenztriazole, and may further contain, if necessary, a color tone agent, a surfactant, an antifoaming agent, a water softener, and a hardening agent. In particular, JP-A-56-10624
The amino compound described in No. 4 and the imidazole compound described in JP-B-48-35493 are preferred in terms of accelerating development or increasing sensitivity. The developer used in the present invention includes a compound described in JP-A-56-24347 as a silver stain preventive agent, and a compound described in JP-A-62-21 as an uneven development inhibitor.
No. 2,651) and compounds described in JP-A-61-267759 can be used as dissolution aids.

【0059】定着液は定着剤の他に必要に応じて硬膜剤
(例えば水溶性アルミニウム化合物)、酢酸及び二塩基
酸(例えば酒石酸、クエン酸又はこれらの塩)を含む水
溶液であり、好ましくは、pH3.8以上、より好まし
くは4.0〜6.5を有する。定着剤としてはチオ硫酸
ナトリウム、チオ硫酸アンモニウムなどであり、本発明
の効果は、どちらでも変わりなく発現する。定着剤の使
用量は適宜変えることができ、一般には約0.1〜約5
モル/リットルである。定着液中で主として硬膜剤とし
て使用する水溶性アルミニウム塩は一般に酸性硬膜定着
液の硬膜剤として知られている化合物であり、例えば塩
化アルミニウム、硫酸アルミニウム、カリ明ばんなどが
ある。本発明の効果は硬膜剤の有無にかかわらず発現す
る。前述の二塩基酸として、酒石酸あるいはその誘導
体、クエン酸あるいはその誘導体が単独で、あるいは二
種以上を併用することができる。これらの化合物は定着
液1リットルにつき、0.005モル以上含むものが有
効で、特に0.01モル/リットル〜0.03モル/リ
ットルが特に有効である。具体的には、酒石酸、酒石酸
カリウム、酒石酸ナトリウム、酒石酸カリウムナトリウ
ム、酒石酸アンモニウム、酒石酸アンモニウムカリウ
ム、などがある。本発明において有効なクエン酸あるい
はその誘導体の例としてクエン酸、クエン酸ナトリウ
ム、クエン酸カリウム、などがある。定着液にはさらに
所望により保恒剤(例えば、亜硫酸塩、重亜硫酸塩)、
pH緩衝剤(例えば、酢酸、硼酸)、pH調整剤(例え
ば、アンモニア、硫酸)、画像保存良化剤(例えば沃化
カリ)、キレート剤を含むことができる。ここでpH緩
衝剤は、現像剤のpHが高いので10〜40g/リット
ル、より好ましくは18〜25g/リットル程度用い
る。本発明の感光材料は前処理時間が15秒〜60秒で
ある自動現像機による迅速現像処理にすぐれた性能を示
す。本発明の迅速現像処理において、現像、定着の温度
および時間は約25℃〜50℃で各々25秒以下である
が、好ましくは30℃〜40℃で4秒〜15秒である。
The fixing solution is an aqueous solution containing, if necessary, a hardening agent (for example, a water-soluble aluminum compound), acetic acid and a dibasic acid (for example, tartaric acid, citric acid or a salt thereof). , PH 3.8 or more, more preferably 4.0 to 6.5. Examples of the fixing agent include sodium thiosulfate, ammonium thiosulfate, and the like, and the effects of the present invention can be exhibited in any case. The amount of the fixing agent to be used can be appropriately changed, and is generally about 0.1 to about 5
Mol / l. The water-soluble aluminum salt mainly used as a hardening agent in the fixing solution is a compound generally known as a hardening agent for an acidic hardening fixing solution, and examples thereof include aluminum chloride, aluminum sulfate and potassium alum. The effects of the present invention are exhibited regardless of the presence or absence of a hardener. As the above-mentioned dibasic acid, tartaric acid or a derivative thereof, citric acid or a derivative thereof can be used alone or in combination of two or more. It is effective that these compounds contain 0.005 mol or more per liter of the fixing solution, and particularly 0.01 to 0.03 mol / l is particularly effective. Specifically, there are tartaric acid, potassium tartrate, sodium tartrate, potassium sodium tartrate, ammonium tartrate, potassium ammonium tartrate, and the like. Examples of citric acid or a derivative thereof effective in the present invention include citric acid, sodium citrate, potassium citrate, and the like. The fixing solution may further contain a preservative (for example, sulfite or bisulfite), if desired.
It may contain a pH buffer (eg, acetic acid, boric acid), a pH adjuster (eg, ammonia, sulfuric acid), an image preserving agent (eg, potassium iodide), and a chelating agent. Here, the pH buffer is used in an amount of 10 to 40 g / liter, more preferably about 18 to 25 g / liter, because the pH of the developer is high. The light-sensitive material of the present invention exhibits excellent performance in rapid development processing by an automatic developing machine having a preprocessing time of 15 seconds to 60 seconds. In the rapid development processing of the present invention, the temperature and time for development and fixing are each about 25 ° C. to 50 ° C. for 25 seconds or less, preferably 30 ° C. to 40 ° C. for 4 seconds to 15 seconds.

【0060】本発明においては感光材料は現像、定着さ
れた後水洗または安定化処理に施される。ここで、水洗
工程は、2〜3段の向流水洗方式を用いることによって
節水処理することができる。また少量の水洗水で水洗す
るときにはスクイズローラー洗浄槽を設けることが好ま
しい。更に、水洗浴または安定浴からのオーバーフロー
液の一部または全部は特開昭60−235133号に記
載されているように定着液に利用することも出来る。こ
うすることによって廃液量も減少しより好ましい。ま
た、水洗水には、カビ防止剤(例えば堀口著、防菌防黴
の化学」、特開昭62−115154号公報に記載の化
合物)、水洗促進剤(亜硫酸塩など)、キレート剤など
を含有していてもよい。上記の方法による水洗または安
定浴の温度及び時間は0℃〜50℃で5秒〜30秒であ
るが、15℃〜40℃で4秒〜20秒が好ましい。本発
明では現像、定着、水洗された感光材料はスクイズロー
ラーを経て乾燥される。乾燥は40℃〜80℃で4秒〜
30秒で行われる。本発明における全処理時間とは自動
現像機の挿入口にフィルムの先端を挿入してから、現像
槽、渡り部分、定着槽、渡り部分、水洗槽、渡り部分、
乾燥部分を通過して、フィルムの先端から乾燥出口から
でてくるまでの全時間である。本発明に用いられる減力
液に関しては特に制限はなく、例えば前記のミーズ著
「ザ・セオリー・オヴ・ザ・フォトグラフィッツ・プロ
セス」に記載されたものが有効に用いられる。即ち、過
マンガン酸塩、過硫酸塩、第二鉄塩、第二銅塩、第二セ
リウム塩、赤血塩、重クロム酸塩等の減力成分を単独又
は併用し、さらに必要により硫酸等の無機酸、アルコー
ル類を含有せしめた減力液、あるいは、赤血塩、エチレ
ンジアミンテトラ酢酸第二鉄塩等の減力成分とチオ硫酸
塩、ロダン塩、チオ尿素あるいはその誘導体等のハロゲ
ン化銀溶剤、さらに必要により硫酸等の無機酸を含有せ
しめた減力液が用いられる。本発明に用いられる減力液
には、さらに必要により特開昭52−68419号公報
に記されたようなメルカプト基を有する化合物を含有せ
しめることが出来る。本発明の減力処理に用いる減力液
の組成、処理条件(温度、時間等)には特に制限はな
く、等業者が適宜、決定することが出来る。減力液及び
減力方法に関しては下記特許の記載を参考にすることが
出来る。特開昭51−140733号、同52−684
19号、同53−14901号、同54−119236
号、同54−119237号、同55−2245号、同
55−2244号、同55−17123号、同55−7
9444号、同55−81344号 以下に実施例を挙げて本発明をさらに具体的に説明す
る。
In the present invention, the light-sensitive material is subjected to washing or stabilization after development and fixing. Here, in the rinsing step, water can be saved by using a two- or three-stage countercurrent rinsing method. When washing with a small amount of washing water, a squeeze roller washing tank is preferably provided. Further, part or all of the overflow solution from the washing bath or the stabilizing bath can be used as a fixing solution as described in JP-A-60-235133. By doing so, the amount of waste liquid is reduced, which is more preferable. The washing water may contain a fungicide (for example, a compound described in Horiguchi, Chemistry of Bacterial and Mold Prevention, JP-A-62-115154), a washing accelerator (such as a sulfite), a chelating agent and the like. It may be contained. The temperature and time of the water washing or stabilizing bath according to the above method are 0 ° C to 50 ° C for 5 seconds to 30 seconds, preferably 15 ° C to 40 ° C for 4 seconds to 20 seconds. In the present invention, the photosensitive material that has been developed, fixed and washed with water is dried through a squeeze roller. Drying at 40 ° C ~ 80 ° C for 4 seconds ~
It takes 30 seconds. The total processing time in the present invention means that after inserting the leading end of the film into the insertion opening of the automatic developing machine, a developing tank, a transfer section, a fixing tank, a transfer section, a washing tank, a transfer section,
This is the total time from passing through the drying section to exiting the drying outlet from the leading edge of the film. There is no particular limitation on the reducer used in the present invention, and for example, those described in the above-mentioned "Theory of the Photography Process" by Mees are effectively used. That is, a permanganate, a persulfate, a ferric salt, a cupric salt, a ceric salt, an erythrocyte salt, a dichromate and other reducing components are used alone or in combination. Or a reducing solution containing an inorganic acid or alcohol, or a reducing agent such as red blood salt or ferric ethylenediaminetetraacetate, and a silver halide such as thiosulfate, rodane salt, thiourea or a derivative thereof. A reducer containing a solvent and, if necessary, an inorganic acid such as sulfuric acid is used. The reducer used in the present invention may further contain a compound having a mercapto group as described in JP-A-52-68419, if necessary. There are no particular restrictions on the composition of the reducer used in the reduction treatment of the present invention and on the treatment conditions (temperature, time, etc.), and those skilled in the art can appropriately determine the composition. The description of the following patent can be referred to for the reducing fluid and the reducing method. JP-A-51-140733 and JP-A-52-684.
No. 19, No. 53-14901, No. 54-119236
No. 54-119237, No. 55-2245, No. 55-2244, No. 55-17123, No. 55-7
Nos. 9444 and 55-81344 Hereinafter, the present invention will be described more specifically with reference to Examples.

【0061】[0061]

【実施例】【Example】

実施例1 乳剤Aの調製 1液 水 1.0リットル ゼラチン 20g 塩化ナトリウム 20g 1,3−ジメチルイミダゾリジン−2−チオン 20mg ベンゼンチオスルホン酸ナトリウム 6mg 2液 水 400ミリリットル 硝酸銀 100g 3液 水 400ミリリットル 塩化ナトリウム 30.5g 臭化カリウム 14.0g ヘキサクロロイリジウム(III)酸カリウム 15ml (0.001%水溶液) ヘキサブロモロジウム(III)酸アンモニウム 1.5ml (0.001%水溶液) 38℃、pH4.5に保たれた1液に2液と3液を攪拌
しながら同時に10分間にわたって加え、0.16μm
の核粒子を形成した。続いて下記4液、5液を10分間
にわたって加えた。さらにヨウ化カリウム0.15gを
加え粒子形成を終了した。 4液 水 400ミリリットル 硝酸銀 100g 5液 水 400ミリリットル 塩化ナトリウム 30.5g 臭化カリウム 14.0g K4 Fe(CN)6 (表1の量) その後常法にしたがってフロキュレーション法によって
水洗し、ゼラチン30gを加えた。
Example 1 Preparation of Emulsion A 1 solution water 1.0 liter gelatin 20 g sodium chloride 20 g 1,3-dimethylimidazolidin-2-thione 20 mg sodium benzenethiosulfonate 6 mg 2 solutions water 400 ml silver nitrate 100 g 3 solutions water 400 ml chloride Sodium 30.5 g Potassium bromide 14.0 g Potassium hexachloroiridate (III) 15 ml (0.001% aqueous solution) Ammonium hexabromorhodate (III) 1.5 ml (0.001% aqueous solution) 38 ° C, pH 4.5 Solution 2 and solution 3 are added simultaneously to solution 1 while stirring over 10 minutes.
Core particles were formed. Subsequently, the following liquids 4 and 5 were added over 10 minutes. Further, 0.15 g of potassium iodide was added to terminate the particle formation. 4 liquid 400 ml of water 100 g of silver nitrate 5 liquid 400 ml of water 30.5 g of sodium chloride 14.0 g of potassium bromide K 4 Fe (CN) 6 (amount in Table 1) Thereafter, water was washed by flocculation according to a conventional method, and gelatin was washed. 30 g were added.

【0062】これを2等分し、pHを5.5、pAgを
7.5に調整し、チオ硫酸ナトリウム3.7mgと塩化
金酸6.2mgを加え、65℃で最適感度になるように
化学増感した。一方の乳剤は、pHを5.3、pAgを
7.5に調整し、チオ硫酸ナトリウム2.6mgとN,N
−ジメチルセレノ尿素を1.0mgと塩化金酸6.2mgを
加え、ベンゼンチオスルホン酸ソーダを4mg、ベンゼン
スルフィン酸ソーダを1mg添加して55℃で最適感度に
なるように化学増感した。
This was divided into two equal parts, the pH was adjusted to 5.5, the pAg was adjusted to 7.5, 3.7 mg of sodium thiosulfate and 6.2 mg of chloroauric acid were added, and the optimum sensitivity was obtained at 65 ° C. Chemical sensitization. One emulsion was adjusted to pH 5.3, pAg to 7.5, 2.6 mg sodium thiosulfate and N, N
1.0 mg of dimethylselenourea and 6.2 mg of chloroauric acid were added, 4 mg of sodium benzenethiosulfonate and 1 mg of sodium benzenesulfinate were added, and the mixture was chemically sensitized at 55 ° C. so as to obtain an optimum sensitivity.

【0063】比較乳剤Bの調整 3液と5液の塩化ナトリウムと臭化カリウムをそれぞれ
9.9gと56gにした以外は乳剤Aと全く同様にして
最終的に塩化銀を20モル%含む平均粒子径0.18μ
mのヨウ塩臭化銀立方体粒子乳剤を得た。 塗布試料の作成 上記乳剤にオルソ増感色素(VI−1)を5×10-4モル
/モルAg加えてオルソ増感を施した。さらにカブリ防
止剤としてハイドロキノン、1−フェニル−5−メルカ
プトテトラゾールをAg1モルあたりそれぞれ2.5
g、50mg、可塑剤としてポリエチルアクリレートラ
テックスをゼラチンバインダー比25%、硬膜剤として
2−ビス(ビニルスルホニルアセトアミド)エタンを加
えて、ポリエステル支持体上にAg3.0g/m2、ゼラ
チン1.0g/m2になるように塗布した。この上に保護
層を同時塗布した。この時、非感光性上部層としてマッ
ト剤(ポリメチルメタアクリレートで平均粒子サイズ
3.4μmのもの)を0.10g/m2及び塗布ゼラチン
量を1.0g/m2になる様に添加し塗布助剤としてP−
ドデシルベンゼンスルホン酸ソーダと構造式(VI−2)
のフッソ界面活性剤を添加し乳剤層と同時に塗布した。
Preparation of Comparative Emulsion B An average grain finally containing 20 mol% of silver chloride was prepared in exactly the same manner as in Emulsion A except that 9.9 g and 56 g of sodium chloride and potassium bromide were used in the third and fifth solutions, respectively. 0.18μ diameter
Thus, a silver iodochlorobromide cubic grain emulsion was obtained. Preparation of Coated Sample Orthosensitizing dye (VI-1) was added to the above emulsion at 5 × 10 −4 mol / mol Ag to perform orthosensitization. Further, hydroquinone and 1-phenyl-5-mercaptotetrazole were used as antifoggants in an amount of 2.5
g, 50 mg, polyethyl acrylate latex gelatin binder ratio of 25% as a plasticizer, in addition to 2-bis (vinylsulfonyl acetamide) ethane as a hardening agent, Ag3.0g / m 2 on a polyester support, gelatin 1. The coating was performed so as to be 0 g / m 2 . A protective layer was simultaneously applied thereon. At this time, a matting agent (polymethyl methacrylate having an average particle size of 3.4 μm) was added as a non-photosensitive upper layer so that the amount became 0.10 g / m 2 and the amount of coated gelatin became 1.0 g / m 2. P- as coating aid
Sodium dodecylbenzenesulfonate and structural formula (VI-2)
Was added at the same time as the emulsion layer.

【0064】[0064]

【化26】 Embedded image

【0065】なお本実施例で使用したサンプルの支持体
は下記組成のバック層及びバック保護層を有する。 バック層 ゼラチン 2.0g/m2 ドデシルベンゼンスルホン酸ナトリウム 80mg/m2 染料(VI−3) 70mg/m2 染料(VI−4) 70mg/m2 染料(VI−5) 90mg/m2 1,3−ジビニルスルホニル−2−プロパノール 60mg/m2
The support of the sample used in this example has a back layer and a back protective layer having the following composition. Back layer Gelatin 2.0 g / m 2 Sodium dodecylbenzenesulfonate 80 mg / m 2 Dye (VI-3) 70 mg / m 2 Dye (VI-4) 70 mg / m 2 Dye (VI-5) 90 mg / m 2 1, 3-divinylsulfonyl-2-propanol 60 mg / m 2

【0066】[0066]

【化27】 Embedded image

【0067】 バック保護層 ゼラチン 0.5g/m2 ポリメチルメタクリレート(粒子サイズ4.7μm) 30mg/m2 ドデシルベンゼンスルホン酸ナトリウム 20mg/m2 含フッソ界面活性剤(VI−2) 2mg/m2 シリコーンオイル 100mg/m2 試料の評価 得られた試料を、488nmにピークをもつ干渉フィルタ
ーを介入し、発光時間10-5sec のキセノンフラッシュ
光で露光し、富士写真フイルム (株) 製自動現像機FG
−710NHを用いて下記に示した温度及び時間でセン
シトメトリーを行った。但し、現像液及び定着液はそれ
ぞれ富士写真フイルム (株) 製LD835とLF308
を用いた。 現像 38℃ 14秒 定着 37℃ 9.7秒 水洗 26℃ 9秒 スクイズ 2.4秒 乾燥 55℃ 8.3秒 合計 43.4秒 濃度3.0を与える露光量の逆数を感度とし、相対感度
で表1に示した。また、特性曲線で濃度0.1と3.0
の点を結ぶ直線の傾きを階調として同じく第1表に示し
た。
[0067] Back protective layer Gelatin 0.5 g / m 2 Polymethyl methacrylate (particle size 4.7 [mu] m) 30 mg / m 2 sodium dodecylbenzenesulfonate 20 mg / m 2 containing fluorine surfactant (VI-2) 2mg / m 2 Evaluation of Silicone Oil 100 mg / m 2 Sample The obtained sample was exposed to xenon flash light having an emission time of 10 −5 sec through an interference filter having a peak at 488 nm, and an automatic developing machine manufactured by Fuji Photo Film Co., Ltd. FG
Sensitometry was performed using -710NH at the temperature and time indicated below. However, the developer and the fixer are LD835 and LF308 manufactured by Fuji Photo Film Co., Ltd., respectively.
Was used. Developing 38 ° C 14 seconds Fixing 37 ° C 9.7 seconds Washing 26 ° C 9 seconds Squeeze 2.4 seconds Drying 55 ° C 8.3 seconds Total 43.4 seconds The sensitivity is defined as the reciprocal of the exposure that gives a density of 3.0. Are shown in Table 1. Further, the characteristic curves show that the concentrations are 0.1 and 3.0.
Table 1 also shows the gradient of the straight line connecting the points (1) and (2) as gradation.

【0068】[0068]

【表1】 [Table 1]

【0069】表1からわかるように本発明は高感硬調で
迅速処理適性を持つ。
As can be seen from Table 1, the present invention has a high sensitivity and a high processing speed.

【0070】実施例2 乳剤Aにおいて、5液のK4 Fe(CN)6 の代わりに
表2に示す化合物を3×10-5モル/Agモル用いた場
合の結果を表2に示す。
Example 2 Table 2 shows the results when 3 × 10 −5 mol / Ag mol of the compound shown in Table 2 was used instead of K 4 Fe (CN) 6 in Emulsion A.

【0071】[0071]

【表2】 [Table 2]

【0072】表2からわかるように本発明は高感硬調で
迅速処理適性を持つ。
As can be seen from Table 2, the present invention has high sensitivity and rapid processing suitability.

【0073】 実施例3 自動現像機FG710NHに下記現像液、定着液を入
れ、塗布銀量3.6g/m、ハロゲン組成クロル70
モル%の塩臭化銀フィルムを黒化率50%の条件で下記
現像液、定着液を180cc/mで補充しながら15
0m処理した。その液に実施例1のNo.1〜6と同
様のサンプルを通して評価した。結果を表3に示す。 現像液 ジエチレントリアミン−五酢酸 2.0g 炭酸ナトリウム 5.0g ホウ酸 10.0g 亜硫酸カリウム 85.0g 臭化ナトリウム 6.0g ジエチレングリコール 40.0g 5−メチルベンゾトリアゾール 0.2g ハイドロキノン 30.0g 4−ヒドロキシメチル−4−メチル−1−フェニ ル−3−ピラゾリドン 1.6g 化合物(イ)2,3,5,6,7,8−ヘキサヒド ロ−2−チオキソ−4−(1H)−キナゾリノン 0.09g 2−メルカプトベンツイミダゾール−5−スルホン 酸ナトリウム 0.3g 水酸化カリウムを加え、水を加えて1リットルとし pHを10.7に合わせる。 1リットル 定着液 チオ硫酸ナトリウム・5水塩 300g 亜硫酸ナトリウム 7g メタ重亜硫酸ナトリウム 20g EDTA 0.025g 化合物(ロ) 0.25モル 水を加えて1リットルとしpHを5.7に合わせる
Example 3 The following developing solution and fixing solution were placed in an automatic developing machine FG710NH, the coated silver amount was 3.6 g / m 2 , and the halogen composition was 70%.
The following developing solution and fixing solution were replenished with a mol% silver chlorobromide film at a blackening ratio of 50% at a rate of 180 cc / m 2.
Was 0m 2 processing. No. 1 of Example 1 was added to the solution. Evaluation was made through samples similar to 1 to 6. Table 3 shows the results. Developer Diethylenetriamine-pentaacetic acid 2.0 g Sodium carbonate 5.0 g Boric acid 10.0 g Potassium sulfite 85.0 g Sodium bromide 6.0 g Diethylene glycol 40.0 g 5-methylbenzotriazole 0.2 g Hydroquinone 30.0 g 4-hydroxymethyl -4-methyl-1-phenyl-3-pyrazolidone 1.6 g Compound (a) 2,3,5,6,7,8-hexahydro-2-thioxo-4- (1H) -quinazolinone 0.09 g 2 -0.3 g of sodium mercaptobenzimidazole-5-sulfonate Add potassium hydroxide, add water to make 1 liter and adjust the pH to 10.7. 1 liter Fixing solution Sodium thiosulfate pentahydrate 300 g Sodium sulfite 7 g Sodium metabisulfite 20 g EDTA 0.025 g Compound (b) 0.25 mol Add water to 1 liter to adjust pH to 5.7.

【0074】[0074]

【化28】 Embedded image

【0075】[0075]

【表3】 [Table 3]

【0076】表3からわかるように本発明は現像液、定
着液の補充量を200cc/m2以下に下げても、高感硬調
で迅速処理適性を持つ。
As can be seen from Table 3, even if the replenishment amounts of the developing solution and the fixing solution are reduced to 200 cc / m 2 or less, the present invention has high sensitivity and rapid processing suitability.

【0077】[0077]

【発明の効果】本発明は請求項に記載した構成をとるこ
とにより高照度短時間露光時に高感度であり、迅速処理
で低補充量処理しても良好な画質を与えるハロゲン化銀
感材が得られた。
According to the present invention, there is provided a silver halide light-sensitive material which has a high sensitivity at the time of high illuminance short time exposure and which provides a good image quality even when a low replenishing amount is processed by a rapid processing. Obtained.

Claims (4)

(57)【特許請求の範囲】(57) [Claims] 【請求項1】 支持体上にハロゲン化銀粒子を含有する
感光性乳剤層を少なくとも1層有するハロゲン化銀写真
感光材料において、該ハロゲン化銀粒子は塩化銀が30
モル%以上であるハロゲン化銀であり、銀に対して10
−8 モル以上10−6モル以下のイリジウム化合物を含
有し、かつ銀に対して10 −6 モル以上10−3モル以
下の鉄、レニウム、ルテニウム、オスミウム化合物の少
なくとも1種を含有し、かつ該感光性乳剤がセレン増感
剤で増感されていることを特徴とするハロゲン化銀写真
感光材料(但し、該感光材料が色素画像形成カプラーを
含有する場合を除く)。
1. A silver halide photographic material having at least one light-sensitive emulsion layer containing silver halide grains on a support, wherein the silver halide grains contain 30 silver chloride.
Silver halide is at least 10 mol%,
Contain -8 mol to 10 -6 mol of an iridium compound, containing at least one 10 -6 mol to 10 -3 mol of iron against Katsugin, rhenium, ruthenium, osmium compound, and wherein A silver halide photographic material , wherein the light-sensitive emulsion is sensitized with a selenium sensitizer, provided that the light-sensitive material is a dye image-forming coupler.
Except when it contains).
【請求項2】 全処理時間が15秒〜60秒である自動
現像機で処理することを特徴とする請求項1に記載のハ
ロゲン化銀写真感光材料の現像処理方法。
2. The method for developing a silver halide photographic material according to claim 1, wherein the processing is performed by an automatic developing machine having a total processing time of 15 to 60 seconds.
【請求項3】 ラインスピードが1000mm/min
以上の自動現像機を用いて処理することを特徴とする請
求項1又は2に記載のハロゲン化銀写真感光材料の現像
処理方法。
3. The line speed is 1000 mm / min.
3. The method for developing a silver halide photographic light-sensitive material according to claim 1, wherein the processing is performed using the above automatic developing machine.
【請求項4】 現像液、定着液補充量が各々200cc
/m以下である自動現像機を用いて処理することを特
徴とする請求項1、2又は3に記載のハロゲン化銀写真
感光材料の現像処理方法。
4. A replenishing amount of a developing solution and a fixing solution is 200 cc each.
Developing method for processing a silver halide photographic material as claimed in claim 1, 2 or 3, characterized in that the processing / m 2 or less is using an automatic developing machine.
JP3116611A 1991-04-22 1991-04-22 Silver halide photographic material and processing method thereof Expired - Fee Related JP2873886B2 (en)