JP2023106722A - Application agent for forming anti-fogging coating, method for producing anti-fogging article, and anti-fogging article - Google Patents

Application agent for forming anti-fogging coating, method for producing anti-fogging article, and anti-fogging article Download PDF

Info

Publication number
JP2023106722A
JP2023106722A JP2022007614A JP2022007614A JP2023106722A JP 2023106722 A JP2023106722 A JP 2023106722A JP 2022007614 A JP2022007614 A JP 2022007614A JP 2022007614 A JP2022007614 A JP 2022007614A JP 2023106722 A JP2023106722 A JP 2023106722A
Authority
JP
Japan
Prior art keywords
coating
antifogging
forming
agent
film
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP2022007614A
Other languages
Japanese (ja)
Inventor
りさ子 楠木
Risako Kusuki
拓史 野村
Takushi Nomura
勇貴 中村
Yuki Nakamura
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Central Glass Co Ltd
Original Assignee
Central Glass Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Central Glass Co Ltd filed Critical Central Glass Co Ltd
Priority to JP2022007614A priority Critical patent/JP2023106722A/en
Publication of JP2023106722A publication Critical patent/JP2023106722A/en
Pending legal-status Critical Current

Abstract

To provide a one-pack application agent for forming anti-fogging coating capable of effectively removing hair dyes and gargles and preventing the occurrence of swelling when water scale is removed, a method for producing an anti-fogging article using the application agent for forming anti-fogging coating, and an anti-fogging article.SOLUTION: An application agent for forming an anti-fogging coating contains (A) a polyisocyanate having two or more isocyanate groups, (B) a polyol having an oxyethylene unit as a repeat unit and having three or more hydroxy groups in each molecule, and (C) a solvent. There are also provided a method for producing an anti-fogging article using the application agent for forming anti-fogging coating, and an anti-fogging article.SELECTED DRAWING: None

Description

本開示は、防曇性被膜形成用塗布剤、防曇性物品の製造方法、及び防曇性物品に関する。 TECHNICAL FIELD The present disclosure relates to an antifogging film-forming coating agent, a method for producing an antifogging article, and an antifogging article.

浴室用・洗面化粧台用の鏡、自動車の窓ガラスやカメラのレンズ等の透明基材の視認性を確保するために、これらの基材の表面に曇り防止機能を付与することが強く求められている。 In order to ensure the visibility of transparent substrates such as mirrors for bathrooms and washstands, window glass of automobiles and lenses of cameras, it is strongly desired to impart anti-fogging function to the surface of these substrates. ing.

鏡やガラスなどのガラス基材の主面に生じる曇りは、無数の微小な水滴が基材表面上に生じる結露現象によって生じる。この曇りを防ぐために、基材表面上に生じた無数の微小な水滴を一様な水膜とする親水性被膜、水蒸気や水滴を被膜中に取り込むことで防曇性を発揮する吸水性被膜等を基材上に形成する技術が検討されている。 Fogging that occurs on the main surface of a glass substrate such as a mirror or glass is caused by a dew condensation phenomenon in which countless minute water droplets are formed on the surface of the substrate. In order to prevent this fogging, there are hydrophilic coatings that form a uniform water film with countless minute water droplets on the substrate surface, and water-absorbing coatings that exhibit anti-fogging properties by incorporating water vapor and water droplets into the coating. is being investigated on a substrate.

昨今、防曇性だけでなく、基材表面に汚れが付きにくい防汚性を兼ね備えることが求められることがある。特許文献1には、防曇性に加えて、防汚性を付与するために、基材上にポリウレタン被膜と、防汚剤を含む組成物の硬化物からなる被膜とを積層した構造を有する防曇性物品が記載されている。 In recent years, not only anti-fogging properties but also anti-fouling properties that make it difficult for dirt to adhere to the surface of substrates are sometimes required. Patent Document 1 discloses a structure in which a polyurethane film and a film made of a cured product of a composition containing an antifouling agent are laminated on a substrate in order to impart antifouling properties in addition to antifogging properties. An anti-fogging article is described.

また、特許文献2には、イソシアネート化合物、共重合ポリオール、アクリルポリオール、及び特定の構造の界面活性剤を含み、イソシアネート化合物とアクリルポリオールの含有量が特定の範囲内である防曇性被膜形成用塗布剤が記載されている。 Further, Patent Document 2 discloses an anti-fogging film-forming composition containing an isocyanate compound, a copolymer polyol, an acrylic polyol, and a surfactant with a specific structure, wherein the contents of the isocyanate compound and the acrylic polyol are within a specific range. A coating is described.

特開2021-4350号公報Japanese Patent Application Laid-Open No. 2021-4350 特許第6578479号公報Japanese Patent No. 6578479

特許文献1では、基材上にポリウレタン被膜を設け、さらにその上に防汚剤を含む組成物からなる被膜を積層することにより、防曇性と防汚性に優れる防曇性物品としている。 In Patent Document 1, an antifogging article having excellent antifogging properties and antifouling properties is obtained by providing a polyurethane coating on a substrate and further laminating a coating comprising a composition containing an antifouling agent thereon.

特許文献1では、少なくとも、ポリウレタン被膜形成用の塗布剤と、防汚剤を含む塗布剤という2種の塗布剤が必要であり、かつ塗布工程を少なくとも2回行う必要がある。 In Patent Document 1, at least two kinds of coating agents, namely, a coating agent for forming a polyurethane film and a coating agent containing an antifouling agent, are required, and the coating process must be performed at least twice.

また、特許文献2では親水性及び耐傷付き性を両立する防曇性被膜形成用塗布剤が記載されているが、鏡やガラスなどの防曇性被膜を設けた防曇性物品の表面には、毛染剤やうがい薬が付着することがあり、これらの除去性に優れる防曇性物品が求められている。さらに、表面に付着した水垢を除去した際に膨潤が発生しにくい防曇性物品が求められている。 In addition, Patent Document 2 describes a coating agent for forming an anti-fogging film that achieves both hydrophilicity and scratch resistance. , hair dyes and gargles may adhere, and an anti-fogging article excellent in removability of these is required. Further, there is a demand for an anti-fogging article that is less likely to swell when water scale adhering to its surface is removed.

本開示は、1液で、毛染剤除去性及びうがい薬除去性に優れ、かつ水垢を除去した際に膨潤が発生しにくい防曇性被膜形成用塗布剤を提供することを目的とする。 An object of the present disclosure is to provide a coating agent for forming an anti-fogging film that is a one-liquid material, has excellent hair dye and mouthwash removability, and is less likely to swell when water scale is removed.

また、本開示は、1回の塗布工程により毛染剤除去性及びうがい薬除去性に優れ、かつ水垢を除去した際に膨潤が発生しにくい防曇性物品を製造できる防曇性物品の製造方法を提供することを目的とする。 In addition, the present disclosure provides an anti-fogging article capable of producing an anti-fogging article that is excellent in hair dye removability and mouthwash removability by a single application step and that does not easily swell when water scale is removed. The purpose is to provide a method.

さらに、本開示は、毛染剤除去性及びうがい薬除去性に優れ、かつ水垢を除去した際に膨潤が発生しにくい、単層の防曇性被膜を有する防曇性物品を提供することを目的とする。 Furthermore, the present disclosure provides an anti-fogging article having a single-layer anti-fogging coating that is excellent in hair dye and mouthwash removability, and is less likely to swell when water scale is removed. aim.

本開示の課題は、下記構成により解決される。
<1>
(A)イソシアネート基を2つ以上有するポリイソシアネートと、
(B)オキシエチレンユニットを繰り返し単位として備え、ヒドロキシ基を分子内に3つ以上有するポリオールと、
(C)溶媒と、
を含む、防曇性被膜形成用塗布剤。
<2>
前記ポリオール(B)が、分岐型ポリオールである、<1>に記載の防曇性被膜形成用塗布剤。
<3>
前記ポリオール(B)が、環状ポリオールである、<1>に記載の防曇性被膜形成用塗布剤。
<4>
さらに、(D)撥水剤または(E)親水剤を含む、<1>~<3>のいずれか1つに記載の防曇性被膜形成用塗布剤。
<5>
ウレタン形成成分中のイソシアネート基の数n(NCO)と、ウレタン形成成分中の水酸基の数n(OH)との比であるn(NCO)/n(OH)が1.0~3.0である、<1>~<4>のいずれか1つに記載の防曇性被膜形成用塗布剤。
<6>
前記ポリイソシアネート(A)の含有量が、ウレタン形成成分100質量%に対して、25~75質量%である、<1>~<5>のいずれか1つに記載の防曇性被膜形成用塗布剤。
<7>
前記ポリオール(B)の含有量が、ウレタン形成成分100質量%に対して、25~75質量%である、<1>~<6>のいずれか1つに記載の防曇性被膜形成用塗布剤。
<8>
前記撥水剤(D)または親水剤(E)の含有量が、ウレタン形成成分100質量%に対して、0.001~10.0質量%である、<4>に記載の防曇性被膜形成用塗布剤。
<9>
基材と防曇性被膜とを有する防曇性物品の製造方法であって、
基材の表面に、<1>~<8>のいずれか1つに記載の防曇性被膜形成用塗布剤を塗布し、塗膜を形成する工程(1)と、
前記塗膜から前記溶媒(C)を蒸散させ、前記塗膜を硬化して防曇性被膜を形成する工程(2)と、
を備える、防曇性物品の製造方法。
<10>
前記基材はガラス基材である<9>に記載の防曇性物品の製造方法。
<11>
前記ガラス基材の表面には、シランカップリング剤が塗布されている、<10>に記載の防曇性物品の製造方法。
<12>
前記工程(2)において、前記ポリイソシアネート(A)のイソシアネート基と、前記ポリオール(B)のヒドロキシ基が反応し、ポリウレタンを形成する、<9>~<11>のいずれか1つに記載の防曇性物品の製造方法。
<13>
前記工程(2)において、前記塗膜を80~170℃で加熱する、<9>~<12>のいずれか1つに記載の防曇性物品の製造方法。
<14>
基材と防曇性被膜とを有する防曇性物品であって、
前記防曇性被膜は、<1>~<8>のいずれか1つに記載の防曇性被膜形成用塗布剤の硬化物であるポリウレタン樹脂を含む被膜であり、
前記防曇性被膜の膜厚は5μm~50μmである、
防曇性物品。
<15>
前記基材はガラス基材である<14>に記載の防曇性物品。
<16>
前記ガラス基材の表面には、シランカップリング剤が塗布されている、<15>に記載の防曇性物品。
<17>
水平に置いた前記防曇性被膜の表面に水を滴下し、60℃で1時間乾燥させた後に水垢を除去し、水垢が付着していた部分の膨潤部の段差が200nm以下である、<14>~<16>のいずれか1つに記載の防曇性物品。
The problem of the present disclosure is solved by the following configuration.
<1>
(A) a polyisocyanate having two or more isocyanate groups;
(B) a polyol comprising an oxyethylene unit as a repeating unit and having three or more hydroxy groups in the molecule;
(C) a solvent;
A coating agent for forming an antifogging film, comprising:
<2>
The coating agent for forming an antifogging film according to <1>, wherein the polyol (B) is a branched polyol.
<3>
The coating agent for forming an antifogging film according to <1>, wherein the polyol (B) is a cyclic polyol.
<4>
The coating agent for forming an antifogging film according to any one of <1> to <3>, further comprising (D) a water repellent agent or (E) a hydrophilic agent.
<5>
n ( NCO) /n (OH), which is the ratio of the number n (NCO) of isocyanate groups in the urethane-forming component to the number n (OH) of hydroxyl groups in the urethane-forming component, is 1.0 to 3.0; The coating agent for forming an antifogging film according to any one of <1> to <4>.
<6>
For forming an antifogging film according to any one of <1> to <5>, wherein the content of the polyisocyanate (A) is 25 to 75% by mass with respect to 100% by mass of the urethane-forming component. Coating agent.
<7>
The coating for forming an antifogging film according to any one of <1> to <6>, wherein the content of the polyol (B) is 25 to 75% by mass with respect to 100% by mass of the urethane-forming component. agent.
<8>
The antifogging coating according to <4>, wherein the content of the water repellent agent (D) or hydrophilic agent (E) is 0.001 to 10.0% by mass with respect to 100% by mass of the urethane-forming component. Forming coating.
<9>
A method for producing an antifogging article having a substrate and an antifogging coating, comprising:
A step (1) of applying the coating agent for forming an antifogging film according to any one of <1> to <8> to the surface of a substrate to form a coating film;
Step (2) of evaporating the solvent (C) from the coating film and curing the coating film to form an antifogging coating;
A method for manufacturing an anti-fogging article.
<10>
The method for producing an antifogging article according to <9>, wherein the substrate is a glass substrate.
<11>
The method for producing an antifogging article according to <10>, wherein the surface of the glass substrate is coated with a silane coupling agent.
<12>
According to any one of <9> to <11>, in the step (2), the isocyanate groups of the polyisocyanate (A) react with the hydroxy groups of the polyol (B) to form a polyurethane. A method for producing an antifogging article.
<13>
The method for producing an antifogging article according to any one of <9> to <12>, wherein in the step (2), the coating film is heated at 80 to 170°C.
<14>
An antifogging article having a substrate and an antifogging coating,
The anti-fogging coating is a coating containing a polyurethane resin, which is a cured product of the coating agent for forming an anti-fogging coating according to any one of <1> to <8>,
The film thickness of the antifogging coating is 5 μm to 50 μm,
Anti-fogging article.
<15>
The antifogging article according to <14>, wherein the substrate is a glass substrate.
<16>
The antifogging article according to <15>, wherein the surface of the glass substrate is coated with a silane coupling agent.
<17>
Water is dropped on the surface of the anti-fogging coating placed horizontally, dried at 60° C. for 1 hour, and then water scale is removed. 14> to <16>, the antifogging article according to any one of the above items.

本開示によれば、1液で、毛染剤除去性及びうがい薬除去性に優れ、かつ水垢を除去した際に膨潤が発生しにくい防曇性被膜形成用塗布剤を提供することができる。 According to the present disclosure, it is possible to provide an anti-fogging film-forming coating agent that is a one-liquid, excellent in hair dye removability and mouthwash removability, and less likely to swell when water scale is removed.

また、本開示によれば、1回の塗布工程により毛染剤除去性及びうがい薬除去性に優れ、かつ水垢を除去した際に膨潤が発生しにくい防曇性物品を製造できる防曇性物品の製造方法を提供することができる。 In addition, according to the present disclosure, an anti-fogging article can be manufactured that is excellent in hair dye removability and mouthwash removability in a single application step and that is less likely to swell when water scale is removed. can provide a manufacturing method of

さらに、本開示によれば、毛染剤除去性及びうがい薬除去性に優れ、かつ水垢を除去した際に膨潤が発生しにくい、単層の防曇性被膜を有する防曇性物品を提供することができる。 Furthermore, according to the present disclosure, there is provided an anti-fogging article having a single-layer anti-fogging coating that is excellent in hair dye and mouthwash removability, and is less likely to swell when water scale is removed. be able to.

[防曇性被膜形成用塗布剤]
本開示の防曇性被膜形成用塗布剤は、
(A)イソシアネート基を2つ以上有するポリイソシアネートと、
(B)オキシエチレンユニットを繰り返し単位として備え、ヒドロキシ基を分子内に3つ以上有するポリオールと、
(C)溶媒と、
を含む、防曇性被膜形成用塗布剤である。
<(A)イソシアネート基を2つ以上有するポリイソシアネート>
(A)イソシアネート基を2つ以上有するポリイソシアネート(「ポリイソシアネート(A)」とも呼ぶ。)について説明する。
[Coating agent for forming anti-fogging film]
The coating agent for forming an antifogging film of the present disclosure is
(A) a polyisocyanate having two or more isocyanate groups;
(B) a polyol comprising an oxyethylene unit as a repeating unit and having three or more hydroxy groups in the molecule;
(C) a solvent;
It is a coating agent for forming an antifogging film containing.
<(A) Polyisocyanate Having Two or More Isocyanate Groups>
(A) A polyisocyanate having two or more isocyanate groups (also referred to as “polyisocyanate (A)”) will be described.

ポリイソシアネート(A)は、防曇性被膜(単に「被膜」とも呼ぶ。)の骨格成分を担い、被膜に吸水性と硬度を付与することができる。 The polyisocyanate (A) serves as a skeleton component of the antifogging coating (also simply referred to as "coating"), and can impart water absorbency and hardness to the coating.

ポリイソシアネート(A)としては、特に限定されず、例えば、イソシアネート基を2つ以上5つ以下有する化合物が挙げられ、具体的には、ヘキサメチレンジイソシアネート、イソホロンジイソシアネート、ジフェニルメタンジイソシアネート、ビス(メチルシクロヘキシル)ジイソシアネート、トルエンジイソシアネート等が挙げられる。 The polyisocyanate (A) is not particularly limited, and examples thereof include compounds having 2 to 5 isocyanate groups. Specific examples include hexamethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, and bis(methylcyclohexyl). diisocyanate, toluene diisocyanate, and the like.

また、ポリイソシアネート(A)は、多量体(例えば、二量体、三量体など)であってもよいし、アロファネート構造、アダクト構造、ビウレット構造及びイソシアヌレート構造からなる群より選ばれる少なくとも1種の構造を有していてもよい。例えば、ヘキサメチレンジイソシアネートを出発原料としたダイマー、ヘキサメチレンジイソシアネートを出発原料としたアロファネート構造を有する化合物、ヘキサメチレンジイソシアネートを出発原料としたビウレット構造を有する化合物等であってもよい。ポリイソシアネート(A)が多量体である場合、数平均分子量は100~20000であることが好ましく、150~5000であることがより好ましく、200~2000であることが特に好ましい。 Further, the polyisocyanate (A) may be a polymer (e.g., dimer, trimer, etc.), or at least one selected from the group consisting of an allophanate structure, an adduct structure, a biuret structure and an isocyanurate structure. It may have a seed structure. For example, it may be a dimer using hexamethylene diisocyanate as a starting material, a compound having an allophanate structure using hexamethylene diisocyanate as a starting material, or a compound having a biuret structure using hexamethylene diisocyanate as a starting material. When the polyisocyanate (A) is a polymer, the number average molecular weight is preferably 100-20,000, more preferably 150-5,000, and particularly preferably 200-2,000.

ポリイソシアネート(A)のイソシアネート基はブロックイソシアネート基であってもよい。ブロックイソシアネート基を有するポリイソシアネート(A)を「ブロックポリイソシアネート(AH)」とも呼ぶ。 The isocyanate groups of polyisocyanate (A) may be blocked isocyanate groups. The polyisocyanate (A) having blocked isocyanate groups is also called "blocked polyisocyanate (AH)".

ブロックイソシアネート基は、イソシアネート基をブロック剤で保護した基であり、熱処理によってブロック剤が解離し、イソシアネート基が再生するものである。 A blocked isocyanate group is a group in which an isocyanate group is protected with a blocking agent, and the blocking agent is dissociated by heat treatment to regenerate the isocyanate group.

ブロックポリイソシアネート(AH)は特に限定されず、例えば、前述のポリイソシアネートのイソシアネート基を公知のブロック剤で保護したものであってもよい。 The blocked polyisocyanate (AH) is not particularly limited, and may be, for example, one in which the isocyanate groups of the aforementioned polyisocyanate are protected with a known blocking agent.

また、ブロックポリイソシアネート(AH)は、分子内にウレタン結合(-NHCOO-)を有していることが好ましい。 Also, the blocked polyisocyanate (AH) preferably has a urethane bond (--NHCOO--) in its molecule.

ブロックポリイソシアネート(AH)の数平均分子量は100~20000であることが好ましく、150~5000であることがより好ましく、200~2000であることが特に好ましい。
<(B)オキシエチレンユニットを繰返し単位として備え、ヒドロキシ基を分子内に3つ以上有するポリオール>
(B)オキシエチレンユニットを繰返し単位として備え、ヒドロキシ基を分子内に3つ以上有するポリオール(「ポリオール(B)」とも呼ぶ。)について説明する。
The number average molecular weight of the blocked polyisocyanate (AH) is preferably 100-20,000, more preferably 150-5,000, and particularly preferably 200-2,000.
<(B) Polyol Having Oxyethylene Units as Repeating Units and Having 3 or More Hydroxy Groups in the Molecule>
(B) A polyol having oxyethylene units as repeating units and having three or more hydroxy groups in the molecule (also referred to as "polyol (B)") will be described.

ポリオール(B)はオキシエチレンユニットを繰返し単位として備えることで、防曇性被膜に吸水性を付与することができる。オキシエチレンユニットを繰返し単位として備えるとは、分子内に、「-(CHCHO)-」を含むことを示す。pは2以上の整数を表す。 The polyol (B) can impart water absorbency to the antifogging coating by having oxyethylene units as repeating units. Having an oxyethylene unit as a repeating unit means that "-(CH 2 CH 2 O) p -" is included in the molecule. p represents an integer of 2 or more.

ポリオール(B)としては、特に限定されないが、例えば、(B1)ポリエチレングリコール、(B2)オキシエチレンユニットとオキシプロピレンユニットとを繰り返し単位として備える共重合ポリオール等が挙げられ、上記(B1)と上記(B2)を両方含んでもよい。 The polyol (B) is not particularly limited. Both (B2) may be included.

上記(B2)の共重合ポリオールは、開始剤にフォスファゼン化合物、ルイス酸化合物またはアルカリ金属化合物触媒を用い、エチレンオキシドおよびプロピレンオキシドを開環重合させて、ブロック付加またはランダム付加して得られる、ポリエーテルポリオールを使用することができる。 The copolymerized polyol (B2) is a polyether obtained by ring-opening polymerization of ethylene oxide and propylene oxide using a phosphazene compound, a Lewis acid compound or an alkali metal compound catalyst as an initiator, followed by block addition or random addition. Polyols can be used.

上記(B2)の共重合ポリオールのオキシエチレンユニット/オキシプロピレンユニットのモル比は、45/55~90/10としてもよく、好ましくは70/30~80/20としてもよい。 The molar ratio of oxyethylene units/oxypropylene units in the copolymerized polyol (B2) may be from 45/55 to 90/10, preferably from 70/30 to 80/20.

ポリオール(B)の数平均分子量は、200~10000であることがより好ましく、300~5000であることが更に好ましく、400~2000であることが特に好ましい。 The number average molecular weight of the polyol (B) is more preferably 200-10,000, still more preferably 300-5,000, and particularly preferably 400-2,000.

ポリオール(B)は、分岐型ポリオール(分子内に分岐構造を有するポリオール)又は環状ポリオール(分子内に四員環、五員環、六員環などの環状構造を有するポリオール)であることが好ましい。分岐型ポリオールとしては、例えば、トリメチロールプロパンエトキシラート、ペンタエリスリトールエトキシラート、ポリオキシエチレン(13)ポリグリセリルエーテル等が挙げられる。六員環型ポリオールとしては、例えば、ポリオキシエチレンメチルグルコシド(メチルグルセス-10、メチルグルセス-20など)、モノラウリン酸ポリオキシエチレンソルビタン等が挙げられる。また、ポリオール(B)として分岐型ポリオールと環状ポリオールの両方を用いてもよい。 Polyol (B) is preferably a branched polyol (polyol having a branched structure in the molecule) or a cyclic polyol (polyol having a cyclic structure such as a four-, five-, or six-membered ring in the molecule). . Examples of branched polyols include trimethylolpropane ethoxylate, pentaerythritol ethoxylate, polyoxyethylene (13) polyglyceryl ether, and the like. Six-membered ring polyols include, for example, polyoxyethylene methyl glucoside (methyl gluceth-10, methyl gluceth-20, etc.), polyoxyethylene sorbitan monolaurate, and the like. Moreover, both a branched polyol and a cyclic polyol may be used as the polyol (B).

ポリオール(B)は市中より入手可能で、例えば、Sigma-Aldrich製のトリメチロールプロパンエトキシラート及びペンタエリスリトールエトキシラート、阪本薬品工業製のポリオキシエチレン(13)ポリグリセリルエーテル(商品名「SCE-750」)、日油製のメチルグルセス-10(商品名「マクビオブライドMG-10E」)、日油製のメチルグルセス-20(商品名「マクビオブライドMG-20E」)、三洋化成製のモノラウリン酸ポリオキシエチレンソルビタン(商品名「ポリソルベートT-20C」)などが挙げられる。
<(C)溶媒>
(C)溶媒(「溶媒(C)」とも呼ぶ。)について説明する。
Polyol (B) is commercially available, for example, trimethylolpropane ethoxylate and pentaerythritol ethoxylate manufactured by Sigma-Aldrich, polyoxyethylene (13) polyglyceryl ether manufactured by Sakamoto Yakuhin Kogyo (trade name "SCE-750 ”), NOF Methyl Gluceth-10 (trade name “Macbiobride MG-10E”), NOF Methyl Gluceth-20 (trade name “Macbiobride MG-20E”), Sanyo Kasei Polymonolaurate oxyethylene sorbitan (trade name “Polysorbate T-20C”) and the like.
<(C) Solvent>
(C) The solvent (also referred to as “solvent (C)”) will be described.

溶媒(C)として、酢酸エステル系溶媒又はケトン類を使用することが好ましい。具体的には、酢酸エステル系溶媒としては、酢酸アミル、酢酸アリル、酢酸イソアミル、酢酸イソブチル、酢酸イソプロピル、酢酸エチル、酢酸2-エチルへキシル、酢酸シクロへキシル、酢酸n-ブチル、酢酸s-ブチル、酢酸プロピル、酢酸ベンジル、酢酸メチル、酢酸メチルシクロへキシル等が挙げられる。ケトン類としては、アセチルアセトン、アセトン、イソホロン、エチル-n-ブチルケトン、ジイソブチルケトン、ジイソプロピルケトン、ジエチルケトン、シクロヘキサノン、ジ-n-プロピルケトン、メチルオキシド、メチル-n-アミルケトン、メチルイソブチルケトン、メチルエチルケトン、メチルシクロヘキサノン、メチル-n-ブチルケトン、メチル-n-プロピルケトン、メチル-n-ヘキシルケトン、メチル-n-ヘプチルケトン、ジアセトンアルコール、これらの混合物等が挙げられる。特に、酢酸イソブチル、酢酸n-ブチル、酢酸s-ブチル、メチルエチルケトン等が好ましい。
<(D)撥水剤>
本開示の防曇性被膜形成用塗布剤は、(D)撥水剤(「撥水剤(D)」とも呼ぶ。)を含んでいてもよい。
As the solvent (C), it is preferable to use an acetate solvent or ketones. Specifically, the acetate solvents include amyl acetate, allyl acetate, isoamyl acetate, isobutyl acetate, isopropyl acetate, ethyl acetate, 2-ethylhexyl acetate, cyclohexyl acetate, n-butyl acetate, s- butyl, propyl acetate, benzyl acetate, methyl acetate, methyl cyclohexyl acetate and the like. Ketones include acetylacetone, acetone, isophorone, ethyl-n-butyl ketone, diisobutyl ketone, diisopropyl ketone, diethyl ketone, cyclohexanone, di-n-propyl ketone, methyl oxide, methyl-n-amyl ketone, methyl isobutyl ketone, methyl ethyl ketone, Methylcyclohexanone, methyl-n-butyl ketone, methyl-n-propyl ketone, methyl-n-hexyl ketone, methyl-n-heptyl ketone, diacetone alcohol, mixtures thereof and the like. Particularly preferred are isobutyl acetate, n-butyl acetate, s-butyl acetate and methyl ethyl ketone.
<(D) water repellent>
The coating agent for forming an antifogging film of the present disclosure may contain (D) a water repellent agent (also referred to as “water repellent agent (D)”).

撥水剤(D)は、防曇性被膜に防汚性を付与する成分である。 The water repellent (D) is a component that imparts antifouling properties to the antifogging coating.

撥水剤(D)は特に限定されないが、下記(D1)、(D2)及び(D3)からなる群より選択される少なくとも1つの化合物を含むことが好ましい。 The water repellent (D) is not particularly limited, but preferably contains at least one compound selected from the group consisting of (D1), (D2) and (D3) below.

(D1)ヒドロキシ基、加水分解でヒドロキシ基を生じる官能基、カルボキシ基、アミノ基、及びイソシアネート基からなる群より選択される少なくとも1つの基を有し、ジアルキルシロキサン部位(SiRO、Rはそれぞれ独立して、炭素数が1以上10以下の直鎖又は分岐状のアルキル基を表す)の数の平均が5~400である直鎖状ポリジアルキルシロキサン(「化合物(D1)」とも呼ぶ。)
(D2)ヒドロキシ基、加水分解でヒドロキシ基を生じる官能基、カルボキシ基、アミノ基、及びイソシアネート基からなる群より選択される少なくとも1つの基を有し、フルオロカーボン部位を有するフルオロアルキルシラン(「化合物(D2)」とも呼ぶ。)
(D3)ヒドロキシ基、加水分解でヒドロキシ基を生じる官能基、カルボキシ基、アミノ基、及びイソシアネート基からなる群より選択される少なくとも1つの基を有し、フルオロカーボン部位を有するパーフルオロポリエーテル(「化合物(D3)」とも呼ぶ。)
上記化合物(D1)、(D2)及び(D3)における加水分解でヒドロキシ基を生じる官能基としては、アルコキシ基が挙げられ、炭素数1~6の直鎖又は分岐鎖のアルコキシ基が好ましく、具体的には、メトキシ基、エトキシ基、プロポキシ基、イソプロポキシ基、ブトキシ基等が挙げられる。
(化合物(D1))
化合物(D1)は、滑り性に優れるジアルキルシロキサン部位を有するので、被膜に防汚性を付与することができる。
(D1) has at least one group selected from the group consisting of a hydroxy group, a functional group that produces a hydroxy group by hydrolysis, a carboxy group, an amino group, and an isocyanate group, and a dialkylsiloxane moiety (SiR 2 O, R is Linear polydialkylsiloxane (also referred to as “compound (D1)”) having an average number of 5 to 400 linear or branched alkyl groups each independently representing a linear or branched alkyl group having 1 to 10 carbon atoms. )
(D2) a fluoroalkylsilane having at least one group selected from the group consisting of a hydroxy group, a functional group that produces a hydroxy group upon hydrolysis, a carboxy group, an amino group, and an isocyanate group, and having a fluorocarbon moiety (“Compound (D2)".)
(D3) a perfluoropolyether having at least one group selected from the group consisting of a hydroxy group, a functional group that produces a hydroxy group upon hydrolysis, a carboxy group, an amino group, and an isocyanate group, and having a fluorocarbon moiety (" Also referred to as "compound (D3)".)
Examples of the functional group that produces a hydroxy group upon hydrolysis in the compounds (D1), (D2) and (D3) include an alkoxy group, preferably a linear or branched alkoxy group having 1 to 6 carbon atoms, specifically Specific examples include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, and a butoxy group.
(Compound (D1))
Since compound (D1) has a dialkylsiloxane moiety with excellent lubricity, it can impart antifouling properties to the film.

化合物(D1)において、防汚性と耐久性とがさらに良好な被膜とするためには、ジアルキルシロキサン部位(SiRO)の数の平均が20~50であることが好ましい。 In the compound (D1), the average number of dialkylsiloxane moieties (SiR 2 O) is preferably 20 to 50 in order to obtain a film having better antifouling properties and durability.

SiROのRはメチル基又はエチル基であることが好ましく、メチル基であることがより好ましい。 R of SiR 2 O is preferably a methyl group or an ethyl group, more preferably a methyl group.

化合物(D1)としては、例えば、下記一般式[1]で表されるポリジメチルシロキサンが好適に用いられる。 As the compound (D1), for example, polydimethylsiloxane represented by the following general formula [1] is preferably used.

Figure 2023106722000001
Figure 2023106722000001

一般式[1]中、X及びXは、それぞれ独立に、一価もしくは二価の官能基を表す。a及びbは、それぞれ独立に、0~3の整数であり、nは10~400の整数である。ただし、a+bは1以上であり、X及びXの少なくとも1つは、ヒドロキシ基、加水分解でヒドロキシ基を生じる官能基、カルボキシ基、アミノ基、及びイソシアネート基からなる群より選択される少なくとも1つである。 In general formula [1], X 1 and X 2 each independently represent a monovalent or divalent functional group. a and b are each independently an integer of 0-3, and n is an integer of 10-400. However, a + b is 1 or more, and at least one of X 1 and X 2 is at least selected from the group consisting of a hydroxy group, a functional group that produces a hydroxy group by hydrolysis, a carboxy group, an amino group, and an isocyanate group. is one.

及びXが表す一価もしくは二価の官能基の具体例としては、ヒドロキシ基、アミノ基、エポキシ基、カルボキシ基、アクリロイル基、アリル基、メルカプト基、-C(=O)-OR基(Rは炭素数1~4の直鎖もしくは分岐鎖の飽和のアルキル基を表す)、-O-C(=O)R基(Rは-C(=O)-OR基のRと同じ)、-A-B基(Aは二価の有機基を表し、Bはヒドロキシ基、アミノ基、エポキシ基、-C(=O)-OR基(Rは炭素数1~4の直鎖もしくは分岐鎖の飽和のアルキル基を表す)または-O-C(=O)R基(Rは-C(=O)-OR基のRと同じ)を表す)、-A-C(A)(A)(A)基(Aは二価の有機基を表し、Aは水素原子または1価の有機基を表し、A及びAは、それぞれ独立に、二価の有機基を表す。BまたはBは、それぞれ独立に、ヒドロキシ基、アミノ基、エポキシ基、カルボキシ基、アクリロイル基、アリル基、メルカプト基、-C(=O)-OR基(Rは炭素数1~4の直鎖もしくは分岐鎖の飽和のアルキル基を表す)または-O-C(=O)R基(Rは-C(=O)-OR基のRと同じ)である。
(化合物(D2))
化合物(D2)におけるフルオロカーボン部位は、CF又はCFであることが好ましい。
Specific examples of monovalent or divalent functional groups represented by X 1 and X 2 include a hydroxy group, an amino group, an epoxy group, a carboxy group, an acryloyl group, an allyl group, a mercapto group, and -C(=O)-OR. 1 group (R 1 represents a linear or branched saturated alkyl group having 1 to 4 carbon atoms), -O-C(=O)R 1 group (R 1 is -C(=O)-OR 1 group R 1 ), -A 1 -B 1 group (A 1 represents a divalent organic group, B 1 is a hydroxy group, amino group, epoxy group, -C(=O)-OR 1 group ( R 1 represents a linear or branched saturated alkyl group having 1 to 4 carbon atoms) or -O-C(=O)R 1 group (R 1 is -C(=O)-OR 1 group of R 1 )), -A 1 -C (A 2 ) (A 3 B 2 ) (A 4 B 3 ) group (A 1 represents a divalent organic group, A 2 represents a hydrogen atom or a monovalent A 3 and A 4 each independently represent a divalent organic group, B 2 or B 3 each independently represents a hydroxy group, an amino group, an epoxy group, a carboxy group, an acryloyl group , allyl group, mercapto group, -C(=O)-OR 1 group (R 1 represents a linear or branched saturated alkyl group having 1 to 4 carbon atoms) or -OC(=O)R 1 group (R 1 is the same as R 1 of -C(=O)-OR 1 group).
(Compound (D2))
The fluorocarbon moiety in compound (D2) is preferably CF2 or CF3 .

化合物(D2)としては、下記一般式[2]で表される、片側末端に官能基を有するフルオロアルキルシランや、下記一般式[3]で表される、両側末端に官能基を有するフルオロアルキルシランが好適に用いられる。 As the compound (D2), a fluoroalkylsilane having a functional group at one end represented by the following general formula [2], or a fluoroalkyl having a functional group at both ends represented by the following general formula [3] Silane is preferably used.

Figure 2023106722000002
Figure 2023106722000002

一般式[2]中、Yは、それぞれ独立に、一価の官能基を表す。pは1~3の整数であり、官能基の数を表す。mは2~6の整数である。ただし、少なくとも1つのYは、ヒドロキシ基、加水分解でヒドロキシ基を生じる官能基、カルボキシ基、アミノ基、及びイソシアネート基からなる群より選択される少なくとも1つを表す。 In general formula [2], each Y 1 independently represents a monovalent functional group. p is an integer of 1 to 3 and represents the number of functional groups. m is an integer of 2-6. However, at least one Y1 represents at least one selected from the group consisting of a hydroxy group, a functional group that produces a hydroxy group upon hydrolysis, a carboxy group, an amino group, and an isocyanate group.

Figure 2023106722000003
Figure 2023106722000003

一般式[3]中、Y及びYは、それぞれ独立に、一価の官能基を表す。mは2~6の整数であり、フルオロカーボン部位の数を表す。q及びrは、それぞれ独立に、1~3の整数であり、一価の官能基の数を表す。ただし、Y及びYの少なくとも1つは、ヒドロキシ基、加水分解でヒドロキシ基を生じる官能基、カルボキシ基、アミノ基、及びイソシアネート基からなる群より選択される少なくとも1つを表す。 In general formula [3], Y 2 and Y 3 each independently represent a monovalent functional group. m is an integer from 2 to 6 and represents the number of fluorocarbon moieties. q and r are each independently an integer of 1 to 3 and represent the number of monovalent functional groups. However, at least one of Y2 and Y3 represents at least one selected from the group consisting of a hydroxy group, a functional group that produces a hydroxy group upon hydrolysis, a carboxy group, an amino group, and an isocyanate group.

化合物(D2)は、皮脂成分、指紋、水垢等の汚れ成分に対する防汚性および除去性、さらに耐久性に優れたフルオロカーボン部位を有するため、得られる被膜の防汚性及び耐久性の向上に効果を奏する。 Compound (D2) has a fluorocarbon moiety that has excellent antifouling properties and removability against fouling components such as sebum components, fingerprints, and water stains, as well as durability, so it is effective in improving the antifouling properties and durability of the obtained film. play.

また、化合物(D2)の分子中にフルオロカーボン部位の数が2~6であるパーフルオロアルキル基(CF(CFt-1-)またはパーフルオロアルキレン基(-(CF-)を有するものが好ましい。フルオロカーボン部位の数が増加すると、得られる防汚性被膜の耐久性が増加する。t及びuは整数を表し、前記「-」は結合手を示している。
(化合物(D3))
化合物(D3)におけるフルオロカーボン部位は、CF又はCFであることが好ましい。
In addition, a perfluoroalkyl group (CF 3 (CF 2 ) t-1 -) or a perfluoroalkylene group (-(CF 2 ) u -) having 2 to 6 fluorocarbon moieties in the molecule of the compound (D2) is preferred. Increasing the number of fluorocarbon moieties increases the durability of the resulting antifouling coating. t and u represent integers, and the "-" indicates a bond.
(Compound (D3))
The fluorocarbon moiety in compound (D3) is preferably CF2 or CF3 .

化合物(D3)としては、下記一般式[4]~[6]のいずれかで表されるものが好ましい。 As the compound (D3), one represented by any one of the following general formulas [4] to [6] is preferable.

Figure 2023106722000004
Figure 2023106722000004

一般式[4]中、Rf1は、式:-C2pO-(pは1~6の整数である。)で表される構造、または、-C2q-(qは1~8の整数である。)で表される構造である。Zは、それぞれ独立に、炭素数1~6の直鎖もしくは分岐鎖のアルコキシ基を表し、具体的な基は、メトキシ基、エトキシ基、プロポキシ基、イソプロポキシ基、ブトキシ基等である。Rは炭素数が1~10のアルキル基であり、aは1~3の整数である。n及びn’はそれぞれ1~5の整数、m及びm’はそれぞれ0~2の整数である。 In general formula [4], Rf1 is a structure represented by the formula: -C p F 2p O- (p is an integer of 1 to 6), or -C q F 2q - (q is 1 to is an integer of 8.). Each Z independently represents a linear or branched alkoxy group having 1 to 6 carbon atoms, and specific groups include methoxy, ethoxy, propoxy, isopropoxy and butoxy. R is an alkyl group having 1 to 10 carbon atoms, and a is an integer of 1 to 3. n and n' are each integers of 1 to 5; m and m' are each integers of 0 to 2;

Figure 2023106722000005
Figure 2023106722000005

一般式[5]中、rは1~200の整数を表す。Zは、それぞれ独立に、炭素数1~6の直鎖もしくは分岐鎖のアルコキシ基を表し、具体的な基は、メトキシ基、エトキシ基、プロポキシ基、イソプロポキシ基、ブトキシ基等である。 In general formula [5], r represents an integer of 1-200. Each Z independently represents a linear or branched alkoxy group having 1 to 6 carbon atoms, and specific groups include methoxy, ethoxy, propoxy, isopropoxy and butoxy.

Figure 2023106722000006
Figure 2023106722000006

一般式[6]中、sは1~100の整数を表し、tは1~10の整数を表す。Zは、それぞれ独立に、炭素数1~6の直鎖もしくは分岐鎖のアルコキシ基を表し、具体的な基は、メトキシ基、エトキシ基、プロポキシ基、イソプロポキシ基、ブトキシ基等である。 In general formula [6], s represents an integer of 1-100, and t represents an integer of 1-10. Each Z independently represents a linear or branched alkoxy group having 1 to 6 carbon atoms, and specific groups include methoxy, ethoxy, propoxy, isopropoxy and butoxy.

化合物(D3)についても、化合物(D2)と同様に、皮脂成分、指紋、水垢等の汚れ成分に対する防汚性および除去性、さらに耐久性に優れたフルオロカーボン部位を有するので、得られる被膜の防汚性及び耐久性の向上に効果を奏する。
<(E)親水剤>
本開示の防曇性被膜形成用塗布剤は、(E)親水剤(「親水剤(E)」とも呼ぶ。)を含んでいてもよい。
Similarly to compound (D2), compound (D3) has antifouling properties and removability against staining components such as sebum components, fingerprints, and water stains, and has a fluorocarbon moiety that is excellent in durability. Effective in improving stain resistance and durability.
<(E) hydrophilic agent>
The coating agent for forming an antifogging film of the present disclosure may contain (E) a hydrophilic agent (also referred to as “hydrophilic agent (E)”).

親水剤(E)は特に限定されないが、下記一般式[7]~[9]のいずれかで表される化合物が好ましい。 Although the hydrophilic agent (E) is not particularly limited, a compound represented by any one of the following general formulas [7] to [9] is preferred.

Figure 2023106722000007
Figure 2023106722000007

[一般式[7]中、Xは単結合、置換基を有していてもよい炭素数1~10のアルキレン基、または置換基を有していてもよい炭素数6~18のアリーレン基のいずれかを示し、Yは単結合、エステル結合、アミド結合、スルホン酸エステル結合、スルホン酸アミド結合、エーテル結合のいずれかを示す。ただし、Xが単結合の場合は、YもXと一緒になって単結合となる。また、nは2~22の自然数である。] [In general formula [7], X is a single bond, an alkylene group having 1 to 10 carbon atoms which may have a substituent, or an arylene group having 6 to 18 carbon atoms which may have a substituent. Y represents either a single bond, an ester bond, an amide bond, a sulfonate ester bond, a sulfonate amide bond, or an ether bond. However, when X is a single bond, Y also becomes a single bond together with X. Also, n is a natural number from 2 to 22. ]

Figure 2023106722000008
Figure 2023106722000008

[一般式[8]中、Xは単結合、置換基を有していてもよい炭素数1~10のアルキレン基、または置換基を有していてもよい炭素数6~18のアリーレン基のいずれかを示し、Yは単結合、エステル結合、アミド結合、スルホン酸エステル結合、スルホン酸アミド結合、エーテル結合のいずれかを示す。ただし、Xが単結合の場合は、YもXと一緒になって単結合となる。また、nは2~22の自然数である。] [In the general formula [8], X is a single bond, an alkylene group having 1 to 10 carbon atoms which may have a substituent, or an arylene group having 6 to 18 carbon atoms which may have a substituent. Y represents either a single bond, an ester bond, an amide bond, a sulfonate ester bond, a sulfonate amide bond, or an ether bond. However, when X is a single bond, Y also becomes a single bond together with X. Also, n is a natural number from 2 to 22. ]

Figure 2023106722000009
Figure 2023106722000009

[一般式[9]中、Rは炭素数10~22の直鎖、分岐鎖、または環状のアルキル基である。]
一般式[7]や一般式[8]の含フッ素化合物は本開示の防曇性物品に対して防汚性の機能を付与し、また、界面活性剤としても作用する。更に、これらの界面活性剤は、水酸基、メルカプト基、アミノ基等のイソシアネート反応性基を有しないものである。なお、防汚性とは、皮脂成分、指紋、水垢等の汚れ成分に対する耐汚染性および汚れ成分に対する除去性をいう。
[In general formula [9], R is a linear, branched or cyclic alkyl group having 10 to 22 carbon atoms. ]
The fluorine-containing compounds represented by general formula [7] and general formula [8] impart an antifouling function to the antifogging article of the present disclosure, and also act as a surfactant. Furthermore, these surfactants are free of isocyanate-reactive groups such as hydroxyl groups, mercapto groups and amino groups. Here, the antifouling property refers to the staining resistance to staining components such as sebum components, fingerprints and water stains, and the removability of the staining components.

本開示では、一般式[7]で表される含フッ素界面活性剤、及び一般式[9]で表される四級アンモニウム塩が、親水性の高さや硬度を低下させない点から好ましい。 In the present disclosure, the fluorine-containing surfactant represented by the general formula [7] and the quaternary ammonium salt represented by the general formula [9] are preferable from the viewpoint of not reducing the hydrophilicity and hardness.

一般式[9]で表される四級アンモニウム塩において、Rは炭素数15~22の直鎖、分岐鎖、または環状のアルキル基であることが好ましく、16~20の直鎖、分岐鎖、または環状のアルキル基であることがより好ましい。 In the quaternary ammonium salt represented by the general formula [9], R is preferably a linear, branched or cyclic alkyl group having 15 to 22 carbon atoms, and a linear, branched or cyclic alkyl group having 16 to 20 carbon atoms. or more preferably a cyclic alkyl group.

なお、常温で固体である界面活性剤(例えば前記四級アンモニウム塩)は膜表面に存在するわずかな界面活性剤が結晶化して、膜が白濁してしまう場合がある。そのため、常温で液体である界面活性剤(例えば一般式[7]で表される含フッ素界面活性剤)がより好ましい。また、一般式[7]で表される含フッ素界面活性剤においては、一般式[7]中、X、Yは単結合であることが好ましく、nは8~16の自然数であることが好ましく、9~13の自然数であることがより好ましい。
<(F)ポリテトラメチレンエーテルグリコール>
本開示の防曇性被膜形成用塗布剤は、さらに、(F)ポリテトラメチレンエーテルグリコール(「ポリテトラメチレンエーテルグリコール(F)」とも呼ぶ。)を含んでいてもよい。ポリテトラメチレンエーテルグリコール(F)の数平均分子量は100~4000であることが好ましく、500~2000であることがより好ましく、800~1200であることが特に好ましい。
<(G)数平均分子量が60~200の短鎖ポリオール>
本開示の防曇性被膜形成用塗布剤は、さらに、(G)数平均分子量が60~200の短鎖ポリオール(「短鎖ポリオール(G)」とも呼ぶ。)を含んでいてもよい。
A surfactant that is solid at room temperature (eg, the quaternary ammonium salt) may crystallize a small amount of the surfactant present on the surface of the film, making the film cloudy. Therefore, surfactants that are liquid at room temperature (for example, fluorine-containing surfactants represented by general formula [7]) are more preferable. Further, in the fluorine-containing surfactant represented by the general formula [7], in the general formula [7], X and Y are preferably single bonds, and n is preferably a natural number of 8 to 16. , 9 to 13 natural numbers.
<(F) Polytetramethylene ether glycol>
The coating agent for forming an antifogging film of the present disclosure may further contain (F) polytetramethylene ether glycol (also referred to as "polytetramethylene ether glycol (F)"). The number average molecular weight of the polytetramethylene ether glycol (F) is preferably 100-4000, more preferably 500-2000, particularly preferably 800-1200.
<(G) Short-chain polyol having a number average molecular weight of 60 to 200>
The coating agent for forming an antifogging film of the present disclosure may further contain (G) a short-chain polyol having a number average molecular weight of 60 to 200 (also referred to as “short-chain polyol (G)”).

短鎖ポリオール(G)は、数平均分子量が60~200の範囲にある、鎖長の短いポリオールのことである。 The short chain polyol (G) is a polyol having a short chain length and having a number average molecular weight in the range of 60-200.

短鎖ポリオール(G)を含むことで、被膜の硬度が改善されやすくなる。短鎖ポリオール(G)の1分子あたりの水酸基数は、2又は3としてもよい。 By containing the short-chain polyol (G), the hardness of the coating is likely to be improved. The number of hydroxyl groups per molecule of the short-chain polyol (G) may be 2 or 3.

短鎖ポリオール(G)の例としては、エチレングリコール、1,2-プロパンジオール、1,3-プロパンジオール、1,2-ブタンジオール、1,3-ブタンジオール、1,4-ブタンジオール、2,3-ブタンジオール、1,5-ペンタンジオール、2-ブテン-1,4-ジオール、2-メチル-2,4-ペンタンジオール、2-エチル-1,3-ヘキサンジオール、ジエチレングリコール、ジプロピレングリコール、トリエチレングリコール、グリセリン、2-エチル-2-(ヒドロキシメチル)-1,3-プロパンジオール、1,2,6-ヘキサントリオール、2,2’-チオジエタノール等のアルキルポリオール、ジエタノールアミン、トリエタノールアミン等のアルカノールアミンがあげられ、それらを単独、又は混合物、若しくはそれらの数平均分子量が60~200の範囲の共重合体等を使用することができる。 Examples of short-chain polyols (G) include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2 , 3-butanediol, 1,5-pentanediol, 2-butene-1,4-diol, 2-methyl-2,4-pentanediol, 2-ethyl-1,3-hexanediol, diethylene glycol, dipropylene glycol , triethylene glycol, glycerin, 2-ethyl-2-(hydroxymethyl)-1,3-propanediol, 1,2,6-hexanetriol, alkyl polyols such as 2,2′-thiodiethanol, diethanolamine, triethanol Examples include alkanolamines such as amines, and they can be used alone, as a mixture, or as a copolymer having a number average molecular weight in the range of 60-200.

これらの中では、エチレングリコール、トリエチレングリコールが、被膜の硬度改善の観点から好ましく、1,2-プロパンジオール、1,2-ブタンジオール、1,3-ブタンジオール、2,3-ブタンジオールのような1級水酸基よりも活性の低い2級や3級水酸基を有する短鎖ポリオールは、塗布液の安定性(ポットライフの長期化)の点から好ましい。
<ウレタン形成成分>
本明細書で、「ウレタン形成成分」とは、本開示の防曇性被膜形成用塗布剤に含まれる成分のうち、ポリウレタンを形成する際の原料となる成分から、撥水剤(D)及び親水剤(E)を除いた全ての成分である。
Among these, ethylene glycol and triethylene glycol are preferable from the viewpoint of improving the hardness of the film, and 1,2-propanediol, 1,2-butanediol, 1,3-butanediol and 2,3-butanediol are preferred. Such short-chain polyols having secondary or tertiary hydroxyl groups, which are less active than primary hydroxyl groups, are preferable from the viewpoint of the stability of the coating solution (prolonged pot life).
<Urethane-forming component>
As used herein, the term “urethane-forming component” refers to, among the components contained in the coating agent for forming an anti-fogging film of the present disclosure, components that are raw materials for forming polyurethane, water repellent (D) and All components except hydrophilic agent (E).

典型的には、「ウレタン形成成分」とは、本開示の防曇性被膜形成用塗布剤中のポリイソシアネート(A)、ポリオール(B)、ポリテトラメチレンエーテルグリコール(F)、及び短鎖ポリオール(G)のことを表す。 Typically, the "urethane-forming component" is polyisocyanate (A), polyol (B), polytetramethylene ether glycol (F), and short-chain polyol in the antifogging film-forming coating agent of the present disclosure. Represents (G).

本開示の防曇性被膜形成用塗布剤が、ポリイソシアネート(A)及びポリオール(B)を含有し、ポリテトラメチレンエーテルグリコール(F)、及び短鎖ポリオール(G)を含有しない場合は、「ウレタン形成成分」は、ポリイソシアネート(A)及びポリオール(B)である。 When the coating agent for forming an antifogging film of the present disclosure contains polyisocyanate (A) and polyol (B), and does not contain polytetramethylene ether glycol (F) and short-chain polyol (G), " "Urethane-forming components" are polyisocyanate (A) and polyol (B).

その他の場合についても、上記と同様に「ウレタン形成成分」を考えるものとする。
<各成分の含有量>
本開示の防曇性被膜形成用塗布剤中のポリイソシアネート(A)の含有量は、ウレタン形成成分100質量%に対して、25~75質量%であることが好ましく、30~70質量%であることがより好ましく、35~70質量%であることが更に好ましい。
In other cases as well, the "urethane-forming component" is considered in the same manner as above.
<Content of each component>
The content of the polyisocyanate (A) in the coating agent for forming an antifogging film of the present disclosure is preferably 25 to 75% by mass, more preferably 30 to 70% by mass, based on 100% by mass of the urethane-forming component. more preferably 35 to 70% by mass.

本開示の防曇性被膜形成用塗布剤中のポリオール(B)の含有量は、ウレタン形成成分100質量%に対して、25~75質量%であることが好ましく、30~70質量%であることがより好ましく、30~65質量%であることが更に好ましい。 The content of the polyol (B) in the coating agent for forming an antifogging film of the present disclosure is preferably 25 to 75% by mass, more preferably 30 to 70% by mass, based on 100% by mass of the urethane-forming component. is more preferable, and 30 to 65% by mass is even more preferable.

本開示の防曇性被膜形成用塗布剤中の溶媒(C)の含有量は、例えば、本開示の防曇性被膜形成用塗布剤中の固形分濃度が10~50質量%となるように、調整することができる。固形分とは、本開示の防曇性被膜形成用塗布剤中の全成分から溶媒(C)を除いた全ての成分のことであり、固形分濃度とは、固形分の濃度(含有量)である。 The content of the solvent (C) in the anti-fogging film-forming coating agent of the present disclosure is, for example, such that the solid content concentration in the anti-fogging film-forming coating agent of the present disclosure is 10 to 50% by mass. , can be adjusted. The solid content refers to all components excluding the solvent (C) from all components in the coating agent for forming an antifogging film of the present disclosure, and the solid content concentration is the concentration (content) of the solid content. is.

本開示の防曇性被膜形成用塗布剤が、撥水剤(D)または親水剤(E)を含有する場合、本開示の防曇性被膜形成用塗布剤中の撥水剤(D)または親水剤(E)の含有量は、ウレタン形成成分100質量%に対して、0.001~10.0質量%であることが好ましく、0.005~5.0質量%であることがより好ましく、0.01~2.0質量%であることが更に好ましい。 When the coating agent for forming an antifogging film of the present disclosure contains a water repellent agent (D) or a hydrophilic agent (E), the water repellent agent (D) in the coating agent for forming an antifogging film of the present disclosure or The content of the hydrophilic agent (E) is preferably 0.001 to 10.0% by mass, more preferably 0.005 to 5.0% by mass, relative to 100% by mass of the urethane-forming component. , more preferably 0.01 to 2.0% by mass.

本開示の防曇性被膜形成用塗布剤が、ポリテトラメチレンエーテルグリコール(F)を含有する場合、本開示の防曇性被膜形成用塗布剤中のポリテトラメチレンエーテルグリコール(F)の含有量は、ウレタン形成成分100質量%に対して、5~15質量%であることが好ましく、8~10質量%であることがより好ましい。 When the coating agent for forming an antifogging film of the present disclosure contains polytetramethylene ether glycol (F), the content of polytetramethylene ether glycol (F) in the coating agent for forming an antifogging film of the present disclosure is preferably 5 to 15% by mass, more preferably 8 to 10% by mass, based on 100% by mass of the urethane-forming component.

本開示の防曇性被膜形成用塗布剤が、短鎖ポリオール(G)を含有する場合、本開示の防曇性被膜形成用塗布剤中の短鎖ポリオール(G)の含有量は、ウレタン形成成分100質量%に対して、1~15質量%であることが好ましく、2~10質量%であることがより好ましく、3~8質量%であることが更に好ましい。
<n(NCO)/n(OH)
本開示の防曇性被膜形成用塗布剤におけるウレタン形成成分中のイソシアネート基の数n(NCO)と、ウレタン形成成分中の水酸基の数n(OH)との比であるn(NCO)/n(OH)は1.0~3.0であることが好ましく、1.1~2.5であることがより好ましく、1.2~2.0であることが更に好ましい。
When the coating agent for forming an antifogging film of the present disclosure contains a short-chain polyol (G), the content of the short-chain polyol (G) in the coating agent for forming an antifogging film of the present disclosure is It is preferably 1 to 15% by mass, more preferably 2 to 10% by mass, and even more preferably 3 to 8% by mass, based on 100% by mass of the component.
<n (NCO) /n (OH) >
n (NCO) /n, which is the ratio of the number n (NCO) of isocyanate groups in the urethane-forming component and the number n (OH) of hydroxyl groups in the urethane-forming component in the coating agent for forming an antifogging film of the present disclosure (OH) is preferably 1.0 to 3.0, more preferably 1.1 to 2.5, even more preferably 1.2 to 2.0.

なお、ブロックイソシアネート基の数も、イソシアネート基の数n(NCO)に含める。
<その他の成分とその含有量>
本開示の防曇性被膜形成用塗布剤は、防曇性被膜形成用塗布剤を塗布してなる塗膜を硬化して防曇性被膜を形成する際の硬化速度を速くするために、硬化触媒を含んでもよい。
The number of blocked isocyanate groups is also included in the number n of isocyanate groups (NCO).
<Other components and their content>
The coating agent for forming an anti-fogging film of the present disclosure is cured to increase the curing speed when forming an anti-fogging film by curing the coating film formed by applying the coating agent for forming an anti-fogging film. It may contain a catalyst.

本開示の防曇性被膜形成用塗布剤が、硬化触媒を含有する場合、本開示の防曇性被膜形成用塗布剤中の硬化触媒の含有量は、ウレタン形成成分100質量%に対して、0.001~0.5質量%であることが好ましい。 When the coating agent for forming an antifogging film of the present disclosure contains a curing catalyst, the content of the curing catalyst in the coating agent for forming an antifogging film of the present disclosure is It is preferably 0.001 to 0.5% by mass.

硬化触媒の例として、有機錫化合物、有機チタン化合物、有機ジルコニウム化合物、有機ビスマス化合物等の有機金属化合物や、アミン化合物等が挙げられる。 Examples of curing catalysts include organic metal compounds such as organic tin compounds, organic titanium compounds, organic zirconium compounds and organic bismuth compounds, and amine compounds.

本開示の防曇性被膜形成用塗布剤は、塗膜の基材上での平滑性を促進させるレベリング剤を含んでもよい。 The coating agent for forming an antifogging film of the present disclosure may contain a leveling agent that promotes the smoothness of the coating film on the substrate.

本開示の防曇性被膜形成用塗布剤が、レベリング剤を含有する場合、本開示の防曇性被膜形成用塗布剤中のレベリング剤の含有量は、ウレタン形成成分100質量%に対して、0.01~0.50質量%であることが好ましく、0.05~0.25質量%であることがより好ましい。 When the coating agent for forming an anti-fogging film of the present disclosure contains a leveling agent, the content of the leveling agent in the coating agent for forming an anti-fogging film of the present disclosure is It is preferably 0.01 to 0.50% by mass, more preferably 0.05 to 0.25% by mass.

本開示の防曇性被膜形成用塗布剤は、塗膜の耐熱性、耐候性、耐水性を改善させる添加剤を含んでもよい。 The coating agent for forming an antifogging film of the present disclosure may contain additives that improve the heat resistance, weather resistance, and water resistance of the coating film.

上記添加剤の例として、ヒンダードアミン系光安定剤、ベンゾトリアゾール系紫外線吸収剤、ヒンダードフェノール系酸化防止剤、カルボジイミド系加水分解防止剤等が挙げられる。なお、上記添加剤は単独でも、複数のものを混合して用いても良い。 Examples of the additives include hindered amine-based light stabilizers, benzotriazole-based ultraviolet absorbers, hindered phenol-based antioxidants, carbodiimide-based hydrolysis inhibitors, and the like. The above additives may be used singly or in combination.

本開示の防曇性被膜形成用塗布剤が、上記添加剤を含有する場合、本開示の防曇性被膜形成用塗布剤中の上記添加剤の含有量は、ウレタン形成成分100質量%に対して、0.2~10.0質量%であることが好ましく、0.5~2.0質量%であることがより好ましい。 When the coating agent for forming an anti-fogging film of the present disclosure contains the above additive, the content of the additive in the coating agent for forming an anti-fogging film of the present disclosure is 0.2 to 10.0% by mass, more preferably 0.5 to 2.0% by mass.

本開示の防曇性被膜形成用塗布剤の用途は、特に限定されないが、建築用には、浴室用、洗面化粧台用等の鏡、窓ガラス等、車両、船舶、航空機等には、窓ガラスあるいは鏡、具体的にはルームミラー、ドアミラー等があげられ、その他に眼鏡やカメラ等のレンズ、ゴーグル、ヘルメットシールド、冷蔵ショーケース、冷凍ショーケース、試験機、精密機器ケース等の開口部やのぞき窓、道路反射鏡、携帯電話等の移動通信体のディスプレー等が挙げられる。
[防曇性物品の製造方法]
本開示の防曇性物品の製造方法は、
基材と防曇性被膜とを有する防曇性物品の製造方法の製造方法であって、
基材の表面に、前述の本開示の防曇性被膜形成用塗布剤を塗布し、塗膜を形成する工程(1)と、
前記塗膜から前記溶媒(C)を蒸散させ、前記塗膜を硬化して防曇性被膜を形成する工程(2)と、
を備える、防曇性物品の製造方法である。
The application of the coating agent for forming an anti-fogging film of the present disclosure is not particularly limited. Glass or mirrors, specifically rearview mirrors, door mirrors, etc., and other openings such as glasses, camera lenses, goggles, helmet shields, refrigerated showcases, freezer showcases, testing machines, precision equipment cases, etc. Examples include observation windows, road reflectors, displays of mobile communication devices such as mobile phones, and the like.
[Method for producing antifogging article]
The manufacturing method of the anti-fogging article of the present disclosure comprises:
A method for manufacturing an antifogging article having a substrate and an antifogging coating, comprising:
a step (1) of applying the coating agent for forming an antifogging film of the present disclosure to the surface of a substrate to form a coating film;
Step (2) of evaporating the solvent (C) from the coating film and curing the coating film to form an antifogging coating;
A method for manufacturing an antifogging article, comprising:

上記工程(1)と上記工程(2)をこの順に行うことで、防曇性物品が得られる。
<基材>
基材としては、板状のものが好ましく使用され、代表的なものとしてはガラスが用いられる。そのガラスは自動車用ならびに建築用、産業用ガラス等に通常用いられているソーダライムガラス製の板ガラスであり、フロート法、デュープレックス法、ロールアウト法等による板ガラスであって、製法は特に問わない。
An antifogging article is obtained by performing the above step (1) and the above step (2) in this order.
<Base material>
As the base material, a plate-like one is preferably used, and glass is typically used. The glass is plate glass made of soda-lime glass, which is commonly used for automotive, architectural, and industrial glass, and is plate glass produced by the float method, duplex method, roll-out method, or the like, and the manufacturing method is not particularly limited.

ガラス種としては、クリアをはじめグリーン、ブロンズ等の各種着色ガラスやUV、IRカットガラス、電磁遮蔽ガラス等の各種機能性ガラス、網入りガラス、低膨張ガラス、ゼロ膨張ガラス等防火ガラスに供し得るガラス、強化ガラスやそれに類するガラス、合わせガラスのほか複層ガラス等、銀引き法あるいは真空成膜法により作製された鏡、さらには平板、曲げ板等各種ガラス製品を使用できる。 Glass types include various colored glasses such as clear, green, bronze, etc., various functional glasses such as UV, IR cut glass, electromagnetic shielding glass, and fireproof glass such as wired glass, low expansion glass, and zero expansion glass. Various glass products such as glass, tempered glass and similar glass, laminated glass and multi-layer glass, mirrors produced by the silver coating method or vacuum film forming method, and flat plates and bent plates can be used.

基材の板厚は特に制限されないが、1mm以上10mm以下が好ましく、特に1mm以上5mm以下が好ましい。 The plate thickness of the substrate is not particularly limited, but is preferably 1 mm or more and 10 mm or less, and particularly preferably 1 mm or more and 5 mm or less.

基材表面への防曇性被膜の形成は、基材の片面だけ、或いは用途によっては両面に行ってもよい。また、防曇性被膜の形成は、基材表面の全面でも一部分であってもよい。 The formation of the antifogging coating on the surface of the substrate may be carried out on only one side of the substrate, or on both sides depending on the application. Moreover, the formation of the antifogging coating may be performed on the entire surface of the base material or on a part of the base material surface.

ガラス基材の表面は、ガラス基材と防曇性被膜との密着性を向上させるために、シランカップリング剤等のプライマー成分が塗布されたものであることが好ましい。前記基材への前記シランカップリング剤の塗布にあたって、前記シランカップリング剤は、アルコール及び水等で、0.05~2.0質量%程度に希釈されていてもよい。前記シランカップリング剤の例として、アミノシラン、メルカプトシラン及びエポキシシラン等が挙げられる。特には、アミノ基を有するシランカップリング剤が好ましく、γ-グリシドオキシプロピルトリメトキシ、γ-アミノプロピルトリエトキシシラン、3-(2-アミノエチルアミノ)プロピルトリエトキシシラン等が特に好ましい。このように、基材上に上記カップリング剤を含む溶液を基材に塗布する工程は、前記基材と前記被膜との接着性が向上する、特に好ましい態様である。 The surface of the glass substrate is preferably coated with a primer component such as a silane coupling agent in order to improve the adhesion between the glass substrate and the antifogging coating. When applying the silane coupling agent to the substrate, the silane coupling agent may be diluted with alcohol, water, or the like to about 0.05 to 2.0% by mass. Examples of the silane coupling agent include aminosilane, mercaptosilane and epoxysilane. Silane coupling agents having an amino group are particularly preferred, and γ-glycidoxypropyltrimethoxy, γ-aminopropyltriethoxysilane, 3-(2-aminoethylamino)propyltriethoxysilane and the like are particularly preferred. Thus, the step of applying a solution containing the above coupling agent to the base material is a particularly preferable embodiment in which the adhesiveness between the base material and the coating is improved.

基材がガラス基材であり、かつガラス基材の表面には、アミノ基を有するシランカップリング剤が塗布されていることが好ましい。 It is preferable that the base material is a glass base material and that a silane coupling agent having an amino group is applied to the surface of the glass base material.

基材は、ガラス基材以外に、ポリエチレンテレフタレート等の樹脂フィルム、ポリカーボネート等の樹脂等であってもよい。これら樹脂透明基材表面に前記防曇性被膜を形成して防曇性物品とし、該物品をガラス基材に貼付してもよい。
<工程(1)>
工程(1)は、基材の表面に、前述の本開示の防曇性被膜形成用塗布剤を塗布し、塗膜を形成する工程である。
The substrate may be a resin film such as polyethylene terephthalate, a resin such as polycarbonate, or the like, in addition to the glass substrate. An anti-fogging article may be obtained by forming the anti-fogging film on the surface of these resinous transparent substrates, and the article may be attached to a glass substrate.
<Step (1)>
Step (1) is a step of applying the coating agent for forming an antifogging film of the present disclosure to the surface of a substrate to form a coating film.

工程(1)の前に、前述の基材と、前述の本開示の防曇性被膜形成用塗布剤を準備する。 Before the step (1), the base material described above and the coating agent for forming the antifogging film of the present disclosure described above are prepared.

本開示の防曇性被膜形成用塗布剤の基材への塗布は、例えば、ディップコート、フローコート、スピンコート、ロールコート、スプレーコート、スクリーン印刷、フレキソ印刷等の公知手段によって行うことができる。
<工程(2)>
工程(2)は、前記塗膜から前記溶媒(E)を蒸散させ、前記塗膜を硬化して防曇性被膜を形成する工程である。
The coating agent for forming an antifogging film of the present disclosure can be applied to a substrate by known means such as dip coating, flow coating, spin coating, roll coating, spray coating, screen printing, and flexographic printing. .
<Step (2)>
Step (2) is a step of evaporating the solvent (E) from the coating film and curing the coating film to form an antifogging coating.

塗膜を硬化するということは、具体的には、塗膜中の原料を反応させてポリウレタンを形成し、塗膜を固化することを指す。 Curing the coating specifically refers to reacting raw materials in the coating to form polyurethane and to solidify the coating.

工程(2)では、ポリイソシアネート(A)のイソシアネート基と、ポリオール(B)のヒドロキシ基が反応し、ポリウレタンを形成することが好ましい。 In step (2), it is preferred that the isocyanate groups of the polyisocyanate (A) react with the hydroxy groups of the polyol (B) to form a polyurethane.

工程(2)では、室温で放置又は170℃以下の熱処理で、前記塗膜の硬化と共に溶媒(C)の蒸散がなされ、塗膜が固化されて防曇性被膜となる。 In step (2), the film is left at room temperature or heat-treated at 170° C. or less to cure the coating film and evaporate the solvent (C), thereby solidifying the coating film to form an antifogging coating.

塗膜の硬化を促進させるためには、80~170℃で加熱を行うことが好ましく、100~165℃で加熱を行うことがより好ましく、120~160℃で加熱を行うことが更に好ましい。
[防曇性物品]
本開示の防曇性物品は、
基材と防曇性被膜とを有する防曇性物品であって、
前記防曇性被膜は、前述の本開示の防曇性被膜形成用塗布剤の硬化物であるポリウレタンを含む被膜であり、
前記防曇性被膜の膜厚は5μm~50μmである、
防曇性物品である。
In order to promote curing of the coating film, heating is preferably performed at 80 to 170°C, more preferably at 100 to 165°C, and even more preferably at 120 to 160°C.
[Anti-fogging article]
The anti-fogging article of the present disclosure is
An antifogging article having a substrate and an antifogging coating,
The antifogging coating is a coating containing polyurethane, which is a cured product of the coating agent for forming an antifogging coating of the present disclosure,
The film thickness of the antifogging coating is 5 μm to 50 μm,
It is an antifogging article.

防曇性物品の基材については、[防曇性物品の製造方法]で記載したとおりである。特に、基材がガラス基材であり、かつガラス基材の表面には、アミノ基を有するシランカップリング剤が塗布されていることが好ましい。 The base material of the antifogging article is as described in [Method for producing antifogging article]. In particular, it is preferable that the base material is a glass base material, and that the surface of the glass base material is coated with a silane coupling agent having an amino group.

防曇性被膜の膜厚は5μm~50μmであり、10μm~45μmであることが好ましく、15μm~40μmであることがより好ましく、20μm~30μmであることが特に好ましい。 The thickness of the antifogging coating is 5 μm to 50 μm, preferably 10 μm to 45 μm, more preferably 15 μm to 40 μm, particularly preferably 20 μm to 30 μm.

防曇性被膜の鉛筆硬度が2H以上であることが好ましく、3H以上であることがより好ましい。 The pencil hardness of the antifogging coating is preferably 2H or more, more preferably 3H or more.

防曇性物品の防曇性被膜は、水平に置いた防曇性被膜の表面に水を滴下し、60℃で1時間乾燥させた後に水垢を除去し、水垢が付着していた部分の膨潤部の段差が200nm以下であることが好ましい。 The anti-fogging coating of the anti-fogging article is prepared by dripping water on the surface of the anti-fogging coating placed horizontally, drying at 60 ° C. for 1 hour, removing water scale, and swelling the part where water scale was attached. It is preferable that the step of the portion is 200 nm or less.

以下、本開示の実施例について説明するが、本開示は以下の実施例に限定されない。 Examples of the present disclosure will be described below, but the present disclosure is not limited to the following examples.

本実施例及び比較例では、防曇性物品を製造するための防曇性被膜形成用塗布剤(塗布液)を調製し、基材上に塗布された塗布液からなる塗膜を熱処理し、硬化して防曇性被膜とすることで、防曇性物品を製造した。該塗布液の調製方法及び防曇性物品の製造方法は後述の通りである。次に、得られた防曇性物品について、以下に示す方法により品質評価を行った。 In the present examples and comparative examples, a coating agent (coating solution) for forming an antifogging film for producing an antifogging article was prepared, and the coating film made of the coating solution applied on the substrate was heat-treated, An antifog article was produced by curing to an antifog coating. The method for preparing the coating liquid and the method for producing the antifogging article are as described below. Next, the obtained antifogging article was subjected to quality evaluation by the method shown below.

〔防曇性被膜の膜厚〕:防曇性被膜の膜厚は、防曇性被膜表面にカッターで切り込みを入れ、防曇性被膜表面と基材表面の段差を表面粗さ計(小坂研究所社製 Surfcorder ET-4000A)で測定し、5点の平均値を防曇性被膜の膜厚とした。 [Thickness of anti-fogging coating]: The thickness of the anti-fogging coating is measured by making a cut in the surface of the anti-fogging coating with a cutter, and using a surface roughness meter (Kosaka research Measured with Surfcorder ET-4000A manufactured by Shosha Co., Ltd., and the average value of 5 points was taken as the film thickness of the antifogging coating.

〔防曇性〕:温度10℃、湿度30%の室内において、防曇性物品の防曇性被膜膜表面に対し、15℃の飽和水蒸気を暴露させる。防曇性被膜膜表面が曇り始めた時間を防曇性被膜膜の防曇時間とした。防曇時間を膜厚で除した値を防曇性として評価した。 [Anti-fogging property]: The surface of the anti-fogging coating film of the anti-fogging article is exposed to saturated steam at 15°C in a room with a temperature of 10°C and a humidity of 30%. The antifogging time of the antifogging coating film was defined as the time when the surface of the antifogging coating film began to cloud. A value obtained by dividing the antifogging time by the film thickness was evaluated as the antifogging property.

〔鉛筆硬度〕:JIS K 5600 塗料一般試験方法(1999)に準拠して、荷重750gが負荷された鉛筆で防曇性被膜膜表面を2回引っ掻き、2回とも防曇性被膜膜の破れが無かった鉛筆の硬度を防曇性被膜膜の鉛筆硬度とした。 [Pencil hardness]: In accordance with JIS K 5600 Paint general test method (1999), the surface of the anti-fogging coating film was scratched twice with a pencil loaded with a load of 750 g. The hardness of the pencil that was absent was taken as the pencil hardness of the antifogging coating film.

〔毛染剤除去性〕:パラフェニレンジアミンを含有する、2液混合型の白髪染め用ヘアカラー剤(黒茶色)を直径10mm程度の円状で防曇性被膜膜表面に付着させ、1時間常温常湿(5~35℃ 、相対湿度45~85%)で放置後、付着部分の水洗を行い、ヘアカラー剤を洗い落とす。その後、無色透明な食器用中性洗剤(5倍希釈)を含ませたコットンをヘアカラー剤の着色部分に貼付け、1時間後、濡れた綿布で払拭する。試験後は、CM-2600d(コニカミノルタ社製)を用いて、着色部分の試験前後の色差を測定する。色差の算出には、ΔE94(CIE1994)の色差式を使用した。色差の値が小さい方が毛染剤除去性に優れる。 [Removability of hair dye]: A two-liquid mixed type hair coloring agent for gray hair (black brown) containing paraphenylenediamine was applied in a circular shape with a diameter of about 10 mm to the surface of the anti-fogging coating film, and left at room temperature for 1 hour. After allowing to stand at normal humidity (5-35°C, relative humidity 45-85%), the adhered portion is washed with water to wash off the hair coloring agent. After that, cotton soaked with a colorless and transparent neutral dishwashing detergent (5-fold dilution) is applied to the colored portion of the hair coloring agent, and after 1 hour, wipe off with a wet cotton cloth. After the test, CM-2600d (manufactured by Konica Minolta) is used to measure the color difference of the colored portion before and after the test. A color difference formula of ΔE94 (CIE1994) was used to calculate the color difference. The smaller the color difference value, the better the hair dye removability.

〔うがい薬除去性〕:ポピドンヨード系のうがい薬を直径10mm程度の円状で防曇性被膜膜表面に付着させ、1時間常温常湿(5~35℃ 、相対湿度45~85%)で放置後、付着部分の水洗を行い、うがい薬を洗い落とす。その後、無色透明な食器用中性洗剤(5倍希釈)を含ませたコットンをうがい薬の着色部分に貼付け、1時間後、濡れた綿布で払拭する。試験後は、CM-2600d(コニカミノルタ社製)を用いて、着色部分の試験前後の色差を測定する。色差の算出には、ΔE94(CIE1994)の色差式を使用した。色差の値が小さい方がうがい薬除去性に優れる。 [Removability of mouthwash]: A povidone-iodine mouthwash is applied in a circular shape with a diameter of about 10 mm to the surface of the anti-fogging film and left for 1 hour at normal temperature and normal humidity (5-35°C, relative humidity 45-85%). After that, wash the attached part with water and wash off the gargle. Thereafter, a cotton pad soaked with a colorless and transparent neutral dishwashing detergent (diluted 5 times) is attached to the colored portion of the mouthwash, and after 1 hour, wipe off with a wet cotton cloth. After the test, CM-2600d (manufactured by Konica Minolta) is used to measure the color difference of the colored portion before and after the test. A color difference formula of ΔE94 (CIE1994) was used to calculate the color difference. The smaller the color difference value, the better the mouthwash removability.

〔耐水垢試験〕:水平に置いた防曇性被膜表面に水道水を滴下し、60℃で1時間乾燥させる。乾燥後に水垢を除去し、水垢が付着していた部分の膨潤部の段差を測定し、目視で膨潤が確認困難なもの(200nm以下)を合格(〇)とし、200nmを超えるものは不合格(×)とした。
[比較例1]
(防曇塗布液の調製)
イソシアネートとしてヘキサメチレンジイソシアネートのダイマータイプのポリイソシアネート(商品名「デスモジュールN3200」;住化コベストロウレタン製)23.70gを準備し、これを薬剤Aとする。
[Water stain resistance test]: Tap water is dropped on the surface of the antifogging film placed horizontally, and dried at 60°C for 1 hour. After drying, the water scale is removed, and the step of the swollen part where the water scale has adhered is measured, and those that are difficult to visually confirm swelling (200 nm or less) are accepted (○), and those exceeding 200 nm are rejected ( x).
[Comparative Example 1]
(Preparation of anti-fogging coating liquid)
As an isocyanate, 23.70 g of a dimer-type polyisocyanate of hexamethylene diisocyanate (trade name “Desmodur N3200”; manufactured by Sumika Covestrourethane) was prepared, and this was used as a chemical agent A.

また、以下にあげる各成分が、以下の指定量で混合され、総量78.12gの薬剤Bが得られた。
<溶媒>
酢酸イソブチルとジアセトンアルコールとの混合液;60.00g
アセチルアセトン;1.80g
<吸水性ポリオール>
数平均分子量4000のオキシエチレン/オキシプロピレン共重合2官能ポリオール(商品名「トーホーポリオールPB-4000」;東邦化学工業製);9.78g
<脂肪族ポリエステルジオール>
数平均分子量1250の脂肪族ポリエステルジオール(商品名「プラクセルL212AL」;ダイセル製;4.89g、
<短鎖ポリオール>
エチレングリコール;1.63g
<レベリング剤>
有機変性シリコーンの基材湿潤剤KL-400HF(共栄社化学製);0.02g
上記の薬剤Aと薬剤Bを混合し、硬化触媒としてジブチル錫ジラウレート(以下、DBTDL)0.04gを添加することで、101.86gの塗布液1を調製した。
In addition, each component listed below was mixed in the following specified amounts to obtain a total amount of drug B of 78.12 g.
<Solvent>
Mixture of isobutyl acetate and diacetone alcohol; 60.00 g
Acetylacetone; 1.80 g
<Water absorbing polyol>
Oxyethylene/oxypropylene copolymer bifunctional polyol having a number average molecular weight of 4000 (trade name “Toho Polyol PB-4000”; manufactured by Toho Chemical Industry Co., Ltd.); 9.78 g
<Aliphatic Polyester Diol>
Aliphatic polyester diol having a number average molecular weight of 1250 (trade name “PLAXEL L212AL”; manufactured by Daicel; 4.89 g,
<Short chain polyol>
Ethylene glycol; 1.63 g
<Leveling agent>
Organically modified silicone substrate wetting agent KL-400HF (manufactured by Kyoeisha Chemical Co., Ltd.); 0.02 g
101.86 g of coating liquid 1 was prepared by mixing the above agents A and B, and adding 0.04 g of dibutyltin dilaurate (hereinafter referred to as DBTDL) as a curing catalyst.

塗布液1の総量を100質量%としたとき、塗布液1中のウレタン形成成分は、39質量%であった。また、塗布液1の原料ベースで、イソシアネート基の数は、ポリオール中の水酸基の数に対して2.0倍量であった。塗布液1において、イソシアネート化合物は、ウレタン形成成分の総量100質量%に対して59.3質量%含まれている。
(基材の準備)
矩形状で、サイズが100mm×100mm×5mm(厚さ)のソーダライムガラス板の裏面に通常の方法で銀膜を形成して、鏡を準備した。89gのイオン交換水と、10gのプロパノールとの混合溶液と、アミノ系シランカップリング剤の、3-(2-アミノエチルアミノ)プロピルトリメトキシシラン(東京化成製)1gとの混合溶液を準備した。該混合溶液を染み込ませたセルロース繊維からなるワイパー(商品名「ベンコット」、型式M-1、50mm×50mm、小津産業製)で、前記鏡のガラス表面を払拭し、その後、水洗して、プライマー層が形成された鏡を基材として準備した。
(防曇性物品の形成)
該基材のプライマー層が形成された主面に、前記塗布液1をスピンコートにより塗布して塗膜を形成し、その後、約160℃で約10分間熱処理することにより、膜厚18μmの防曇性被膜が形成された防曇性物品を得た。
[実施例1]
(防曇塗布液の調製)
イソシアネートとしてヘキサメチレンジイソシアネートのイソシアヌレートタイプのポリイソシアネート(商品名「MHG-80B」;固形分濃度80質量%;旭化成製)32.98gを準備した。これを薬剤Aとする。
When the total amount of Coating Liquid 1 was 100% by mass, the urethane-forming component in Coating Liquid 1 was 39% by mass. Also, based on the raw material of coating liquid 1, the number of isocyanate groups was 2.0 times the number of hydroxyl groups in the polyol. In coating liquid 1, the isocyanate compound is contained in an amount of 59.3% by mass with respect to 100% by mass of the total amount of urethane-forming components.
(Preparation of base material)
A mirror was prepared by forming a silver film on the back surface of a soda-lime glass plate having a rectangular shape and a size of 100 mm×100 mm×5 mm (thickness) by a conventional method. A mixed solution of 89 g of ion-exchanged water, 10 g of propanol, and 1 g of 3-(2-aminoethylamino)propyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) as an amino-based silane coupling agent were prepared. . Wipe the glass surface of the mirror with a wiper made of cellulose fiber (trade name “BEMCOT”, model M-1, 50 mm × 50 mm, manufactured by Ozu Sangyo) soaked with the mixed solution, then wash with water and apply a primer. A layered mirror was provided as a substrate.
(Formation of anti-fogging article)
The coating liquid 1 is applied by spin coating to the main surface of the substrate on which the primer layer is formed to form a coating film, and then heat treated at about 160 ° C. for about 10 minutes to obtain a film thickness of 18 μm. An antifogging article having a fogging coating was obtained.
[Example 1]
(Preparation of anti-fogging coating liquid)
As an isocyanate, 32.98 g of an isocyanurate-type polyisocyanate of hexamethylene diisocyanate (trade name “MHG-80B”; solid content concentration 80% by mass; manufactured by Asahi Kasei Corporation) was prepared. Let this be drug A.

また、以下にあげる各成分が、以下の指定量で混合され、総量69.79gの薬剤Bが得られた。
<溶媒>
酢酸イソブチルとジアセトンアルコールとの混合液;43.40g
アセチルアセトン;2.25g、
<吸水性ポリオール>
以下の構造を持つ数平均分子量450の4官能ポリオールのペンタエリスリトールエトキシラート(15/4 EO/OH、分岐型ポリオール)(Sigma-Aldrich製);23.62g
In addition, each component listed below was mixed in the following specified amounts to obtain a total amount of drug B of 69.79 g.
<Solvent>
Mixture of isobutyl acetate and diacetone alcohol; 43.40 g
Acetylacetone; 2.25 g,
<Water absorbing polyol>
Pentaerythritol ethoxylate (15/4 EO/OH, branched polyol) of a tetrafunctional polyol with a number average molecular weight of 450 having the following structure (manufactured by Sigma-Aldrich); 23.62 g

Figure 2023106722000010

a、b、c、dは正の整数であり、a+b+c+d=15である
Figure 2023106722000010

a, b, c, d are positive integers and a+b+c+d=15

<レベリング剤>
有機変性シリコーンの基材湿潤剤KL-400HF(共栄社化学製);0.02g
<光安定剤>
ヒンダードアミン系光安定剤のアデカスタブLA-72(ADEKA製);0.50g
上記の薬剤Aと薬剤Bを混合し、硬化触媒としてジブチル錫ジラウレート(以下、DBTDL)0.05gを添加することで、102.82gの塗布液2を調製した。
<Leveling agent>
Organically modified silicone substrate wetting agent KL-400HF (manufactured by Kyoeisha Chemical Co., Ltd.); 0.02 g
<Light stabilizer>
Hindered amine light stabilizer ADEKA STAB LA-72 (manufactured by ADEKA); 0.50 g
102.82 g of coating liquid 2 was prepared by mixing the above agents A and B and adding 0.05 g of dibutyltin dilaurate (hereinafter referred to as DBTDL) as a curing catalyst.

塗布液2の総量を100質量%としたとき、塗布液2中のウレタン形成成分は、49質量%であった。また、塗布液2の原料ベースで、イソシアネート基の数は、ポリオール中の水酸基の数に対して1.0倍量であった。塗布液2において、イソシアネート化合物は、ウレタン形成成分の総量100質量%に対して52.8質量%含まれている。
(基材の準備)
矩形状で、サイズが100mm×100mm×5mm(厚さ)のソーダライムガラス板の裏面に通常の方法で銀膜を形成して、鏡を準備した。89gのイオン交換水と、10gのプロパノールとの混合溶液と、アミノ系シランカップリング剤の、X-12-972F(信越化学製)1gとの混合溶液を準備した。該混合溶液を染み込ませたセルロース繊維からなるワイパー(商品名「ベンコット」、型式M-1、50mm×50mm、小津産業製)で、前記鏡のガラス表面を払拭し、その後、水洗して、プライマー層が形成された鏡を基材として準備した。
(防曇性物品の形成)
該基材のプライマー層が形成された主面に、前記塗布液2をスピンコートにより塗布して塗膜を形成し、その後、約160℃で約10分間熱処理することにより、膜厚23μmの防曇性被膜が形成された防曇性物品を得た。
[実施例2]
実施例1の薬剤Bにおいて、吸水性ポリオールのペンタエリスリトールエトキシラートを、以下の構造を持つ数平均分子量450の3官能ポリオールのトリメチロールプロパンエトキシラート(分岐型ポリオール)(Sigma-Aldrich製)に変えた以外は、実施例1と同様の操作を行い、防曇性物品を得た。
When the total amount of Coating Liquid 2 was 100% by mass, the urethane-forming component in Coating Liquid 2 was 49% by mass. Also, based on the raw material of coating liquid 2, the number of isocyanate groups was 1.0 times the number of hydroxyl groups in the polyol. In the coating liquid 2, the isocyanate compound is contained in an amount of 52.8% by mass with respect to 100% by mass of the total amount of the urethane-forming components.
(Preparation of base material)
A mirror was prepared by forming a silver film on the back surface of a soda-lime glass plate having a rectangular shape and a size of 100 mm×100 mm×5 mm (thickness) by a conventional method. A mixed solution of 89 g of ion-exchanged water, 10 g of propanol, and 1 g of amino-based silane coupling agent X-12-972F (manufactured by Shin-Etsu Chemical Co., Ltd.) were prepared. Wipe the glass surface of the mirror with a wiper made of cellulose fiber (trade name “BEMCOT”, model M-1, 50 mm × 50 mm, manufactured by Ozu Sangyo) soaked with the mixed solution, then wash with water and apply a primer. A layered mirror was provided as a substrate.
(Formation of anti-fogging article)
The coating liquid 2 is applied by spin coating to the main surface of the substrate on which the primer layer is formed to form a coating film, and then heat treatment is performed at about 160 ° C. for about 10 minutes to obtain a film thickness of 23 μm. An antifogging article having a fogging coating was obtained.
[Example 2]
In the agent B of Example 1, the water-absorbent polyol pentaerythritol ethoxylate was replaced with a trifunctional polyol trimethylolpropane ethoxylate (branched polyol) (manufactured by Sigma-Aldrich) having a number average molecular weight of 450 and having the following structure. Except for this, the same operation as in Example 1 was performed to obtain an antifogging article.

Figure 2023106722000011

e、f、gは正の整数であり、e+f+g=20
Figure 2023106722000011

e, f, g are positive integers, e+f+g=20

[実施例3]
(防曇塗布液の調製)
ブロックイソシアネート(商品名「デュラネートSBB70P」;固形分濃度70質量%;旭化成製)45.05gを準備した。これを薬剤Aとする。
[Example 3]
(Preparation of anti-fogging coating liquid)
45.05 g of blocked isocyanate (trade name “Duranate SBB70P”; solid content concentration 70% by mass; manufactured by Asahi Kasei Corporation) was prepared. Let this be drug A.

また、以下にあげる各成分が、以下の指定量で混合され、総量57.71gの薬剤Bが得られた。
<溶媒>
酢酸イソブチルとジアセトンアルコールとの混合液;36.49g
アセチルアセトン;2.25g
<吸水性ポリオール>
以下の構造を持つ数平均分子量738の4官能ポリオールのポリオキシエチレン(13)ポリグリセリルエーテル(商品名「SCE-750」阪本薬品工業製);18.47g
In addition, each component listed below was mixed in the following specified amounts to obtain a total amount of drug B of 57.71 g.
<Solvent>
Mixture of isobutyl acetate and diacetone alcohol; 36.49 g
Acetylacetone; 2.25g
<Water absorbing polyol>
Polyoxyethylene (13) polyglyceryl ether of a tetrafunctional polyol having a number average molecular weight of 738 and having the following structure (trade name “SCE-750” manufactured by Sakamoto Yakuhin Kogyo Co., Ltd.); 18.47 g

Figure 2023106722000012

Rはエチレンオキサイド(CHCHO)である。また、m、n、o、pは正の整数であり、m+n+o+p=13である。
Figure 2023106722000012

R is ethylene oxide ( CH2CH2O ). Also, m, n, o, and p are positive integers, and m+n+o+p=13.

<撥水剤(防汚剤)>
両末端ポリエーテル変性ポリジメチルシロキサン化合物のKF-6123(信越化学工業製):0.005g
<光安定剤>
ヒンダードアミン系光安定剤のアデカスタブLA-72(ADEKA製);0.50g
上記の薬剤Aと薬剤Bを混合し、硬化触媒としてジブチル錫ジラウレート(以下、DBTDL)0.025gを添加することで、102.78gの塗布液3を調製した。
<Water repellent agent (antifouling agent)>
KF-6123 (manufactured by Shin-Etsu Chemical Co., Ltd.) of polydimethylsiloxane compound modified with polyether at both ends: 0.005 g
<Light stabilizer>
Hindered amine light stabilizer ADEKA STAB LA-72 (manufactured by ADEKA); 0.50 g
102.78 g of coating liquid 3 was prepared by mixing the above agents A and B and adding 0.025 g of dibutyltin dilaurate (hereinafter referred to as DBTDL) as a curing catalyst.

塗布液3の総量を100質量%としたとき、塗布液3中のウレタン形成成分は、49質量%であった。また、塗布液3の原料ベースで、イソシアネート基の数は、ポリオール中の水酸基の数に対して1.1倍量であった。塗布液3において、イソシアネート化合物は、ウレタン形成成分の総量100質量%に対して63.1質量%含まれている。 When the total amount of Coating Liquid 3 was 100% by mass, the urethane-forming component in Coating Liquid 3 was 49% by mass. In addition, based on the raw material of coating liquid 3, the number of isocyanate groups was 1.1 times the number of hydroxyl groups in the polyol. In coating liquid 3, the isocyanate compound is contained in an amount of 63.1% by mass with respect to 100% by mass of the total amount of urethane-forming components.

塗布液2に代えて塗布液3を用いた以外は、実施例1と同様の操作を行い、防曇性物品を得た。
[実施例4]
(防曇塗布液の調製)
ブロックイソシアネート(商品名「デュラネートSBB70P」;固形分濃度70質量%;旭化成製)43.00gを準備した。これを薬剤Aとする。
An antifogging article was obtained in the same manner as in Example 1 except that Coating Liquid 3 was used instead of Coating Liquid 2.
[Example 4]
(Preparation of anti-fogging coating liquid)
43.00 g of blocked isocyanate (trade name “Duranate SBB70P”; solid content concentration 70% by mass; manufactured by Asahi Kasei Corporation) was prepared. Let this be drug A.

また、以下にあげる各成分が、以下の指定量で混合され、総量59.48gの薬剤Bが得られた。
<溶媒>
酢酸イソブチルとジアセトンアルコールとの混合液;42.10g
アセチルアセトン;2.03g
<吸水性ポリオール>
以下の構造を持つ数平均分子量634の4官能ポリオールのメチルグルセス-10(商品名「マクビオブライドMG-10E」;日油製、六員環型ポリオール);14.90g
In addition, each component listed below was mixed in the following specified amounts to obtain a total amount of drug B of 59.48 g.
<Solvent>
Mixture of isobutyl acetate and diacetone alcohol; 42.10 g
Acetylacetone; 2.03g
<Water absorbing polyol>
Methyl gluceth-10, a tetrafunctional polyol having a number average molecular weight of 634 and having the following structure (trade name “Macbiobride MG-10E”; manufactured by NOF Corporation, six-membered ring polyol); 14.90 g

Figure 2023106722000013

a、b、c、dは正の整数であり、a+b+c+d=10である。
Figure 2023106722000013

a, b, c, and d are positive integers, and a+b+c+d=10.

<光安定剤>
ヒンダードアミン系光安定剤のアデカスタブLA-72(ADEKA製);0.45g
上記の薬剤Aと薬剤Bを混合し、硬化触媒としてジブチル錫ジラウレート(以下、DBTDL)0.023gを添加することで、102.50gの塗布液4を調製した。
<Light stabilizer>
Hindered amine light stabilizer ADEKA STAB LA-72 (manufactured by ADEKA); 0.45 g
102.50 g of coating liquid 4 was prepared by mixing the above agents A and B and adding 0.023 g of dibutyltin dilaurate (hereinafter referred to as DBTDL) as a curing catalyst.

塗布液4の総量を100質量%としたとき、塗布液4中のウレタン形成成分は、44質量%であった。また、塗布液4の原料ベースで、イソシアネート基の数は、ポリオール中の水酸基の数に対して1.1倍量であった。塗布液4において、イソシアネート化合物は、ウレタン形成成分の総量100質量%に対して66.9質量%含まれている。 The urethane-forming component in the coating liquid 4 was 44% by mass when the total amount of the coating liquid 4 was 100% by mass. Also, based on the raw material of coating liquid 4, the number of isocyanate groups was 1.1 times the number of hydroxyl groups in the polyol. In coating liquid 4, the isocyanate compound is contained in an amount of 66.9% by mass with respect to 100% by mass of the total amount of urethane-forming components.

塗布液2に代えて塗布液4を用いた以外は、実施例1と同様の操作を行い、防曇性物品を得た。
[実施例5]
実施例4の薬剤Bにおいて、撥水剤としてX-22-4952(信越化学工業製):0.005gを更に加えた以外は実施例4と同様の操作を行い、防曇性物品を得た。
[実施例6]
実施例5の薬剤Bにおいて吸水性ポリオールの「マクビオブライドMG-10E」を、構造は同じであるがa+b+c+d=20である数平均分子量1074の4官能ポリオールの「メチルグルセス-20(商品名「マクビオブライドMG-20E」;日油製、六員環型ポリオール)に変え、撥水剤を「X-22-4952」から両末端ポリエーテル変性ポリジメチルシロキサン化合物のKF-6123(信越化学工業製)に変えた以外は実施例5と同様の操作を行い、防曇性物品を得た。
[実施例7]
実施例5の薬剤Bにおいて、吸水性ポリオールとしてトリメチロールプロパンエトキシラート(以下、TEEと記載)(Sigma-Aldrich製)を更に加え、固形分質量比を「マクビオブライドMG-10E:TEE=50:50」と変えた以外は実施例5と同様の操作を行い、防曇性物品を得た。
[実施例8]
実施例5の撥水剤である「X-22-4952」から、親水剤の片末端ヘキサフルオロプロペン変性ポリオキシエチレン化合物のフタージェント212M(ネオス社製);0.45gに変えた以外は実施例5と同様の操作を行い、防曇性物品を得た。
An antifogging article was obtained in the same manner as in Example 1, except that Coating Liquid 4 was used instead of Coating Liquid 2.
[Example 5]
An antifogging article was obtained in the same manner as in Example 4, except that 0.005 g of X-22-4952 (manufactured by Shin-Etsu Chemical Co., Ltd.) was added as a water repellent to the agent B of Example 4. .
[Example 6]
In the agent B of Example 5, the water-absorbing polyol "Macbiobride MG-10E" was replaced with "Methyl Gluceth-20" (trade name "Mac Biobride MG-20E"; made by NOF, six-membered ring polyol), and changed the water repellent agent from "X-22-4952" to KF-6123 (manufactured by Shin-Etsu Chemical Co., Ltd.), a polydimethylsiloxane compound modified with polyether at both ends ) was performed in the same manner as in Example 5 to obtain an antifogging article.
[Example 7]
In the drug B of Example 5, trimethylolpropane ethoxylate (hereinafter referred to as TEE) (manufactured by Sigma-Aldrich) was further added as a water-absorbing polyol, and the solid content mass ratio was changed to "Macbiobride MG-10E: TEE = 50. An antifogging article was obtained in the same manner as in Example 5, except that the content was changed to: 50.
[Example 8]
The water repellent agent "X-22-4952" of Example 5 was changed to one-end hexafluoropropene-modified polyoxyethylene compound Ftergent 212M (manufactured by Neos) as a hydrophilic agent; The same operation as in Example 5 was performed to obtain an antifogging article.

結果を下記表1に示す。 The results are shown in Table 1 below.

Figure 2023106722000014
Figure 2023106722000014

表1の結果より、実施例1~8の防曇性被膜形成用塗布剤は、1液で、毛染剤除去性及びうがい薬除去性に優れ、かつ水垢を除去した際に膨潤が発生しにくい防曇性被膜形成用塗布剤であることがわかった。 From the results in Table 1, the coating agents for forming an anti-fogging film of Examples 1 to 8 are one-liquid, excellent in hair dye removability and mouthwash removability, and swelling occurs when water scale is removed. It was found to be a coating agent for forming an anti-fogging film that is difficult to apply.

また、実施例1~8ではポリオール成分として吸水性ポリオールだけを使用し、従来技術や比較例1で使用した吸水性ポリオール以外のポリオール成分である脂肪族ポリエステルジオール、短鎖ポリオール、アクリルポリオールなどを含まなかったが、十分な膜硬度の防曇性被膜を得ることができた。 In Examples 1 to 8, only water-absorbent polyol was used as the polyol component, and aliphatic polyester diol, short-chain polyol, acrylic polyol, etc., which are polyol components other than the water-absorbent polyol used in the conventional technology and Comparative Example 1, were used. Although not included, an antifogging coating with sufficient film hardness could be obtained.

本開示の防曇性物品は、建築用には、浴室用、洗面化粧台用等の鏡、窓ガラス等、車両、船舶、航空機等には、窓ガラスあるいは鏡、具体的にはルームミラー、ドアミラー等に利用できる。その他、眼鏡やカメラ等のレンズ、ゴーグル、ヘルメットシールド、冷蔵ショーケース、冷凍ショーケース、試験機、精密機器ケース等の開口部やのぞき窓、道路反射鏡、携帯電話等の移動通信体のディスプレー等にも利用可能である。
The anti-fogging article of the present disclosure is used for construction such as mirrors and window glass for bathrooms and bathroom vanities, and for vehicles, ships, aircraft, etc., such as window glass or mirrors, specifically room mirrors, Can be used for door mirrors, etc. Other lenses such as eyeglasses and cameras, goggles, helmet shields, refrigerated showcases, freezer showcases, testing machines, openings and peepholes of precision equipment cases, road reflectors, displays of mobile communication devices such as mobile phones, etc. is also available.

Claims (17)

(A)イソシアネート基を2つ以上有するポリイソシアネートと、
(B)オキシエチレンユニットを繰り返し単位として備え、ヒドロキシ基を分子内に3つ以上有するポリオールと、
(C)溶媒と、
を含む、防曇性被膜形成用塗布剤。
(A) a polyisocyanate having two or more isocyanate groups;
(B) a polyol comprising an oxyethylene unit as a repeating unit and having three or more hydroxy groups in the molecule;
(C) a solvent;
A coating agent for forming an antifogging film, comprising:
前記ポリオール(B)が、分岐型ポリオールである、請求項1に記載の防曇性被膜形成用塗布剤。 The coating agent for forming an antifogging film according to claim 1, wherein the polyol (B) is a branched polyol. 前記ポリオール(B)が、環状ポリオールである、請求項1に記載の防曇性被膜形成用塗布剤。 The coating agent for forming an antifogging film according to claim 1, wherein the polyol (B) is a cyclic polyol. さらに、(D)撥水剤または(E)親水剤を含む、請求項1~3のいずれか1項に記載の防曇性被膜形成用塗布剤。 4. The coating agent for forming an antifogging film according to any one of claims 1 to 3, further comprising (D) a water repellent agent or (E) a hydrophilic agent. ウレタン形成成分中のイソシアネート基の数n(NCO)と、ウレタン形成成分中の水酸基の数n(OH)との比であるn(NCO)/n(OH)が1.0~3.0である、請求項1~4のいずれか1項に記載の防曇性被膜形成用塗布剤。 n ( NCO) /n (OH), which is the ratio of the number n (NCO) of isocyanate groups in the urethane-forming component to the number n (OH) of hydroxyl groups in the urethane-forming component, is 1.0 to 3.0; The coating agent for forming an antifogging film according to any one of claims 1 to 4. 前記ポリイソシアネート(A)の含有量が、ウレタン形成成分100質量%に対して、25~75質量%である、請求項1~5のいずれか1項に記載の防曇性被膜形成用塗布剤。 The coating agent for forming an antifogging film according to any one of claims 1 to 5, wherein the content of the polyisocyanate (A) is 25 to 75% by mass with respect to 100% by mass of the urethane-forming component. . 前記ポリオール(B)の含有量が、ウレタン形成成分100質量%に対して、25~75質量%である、請求項1~6のいずれか1項に記載の防曇性被膜形成用塗布剤。 The coating agent for forming an antifogging film according to any one of claims 1 to 6, wherein the content of the polyol (B) is 25 to 75% by mass with respect to 100% by mass of the urethane-forming component. 前記撥水剤(D)または親水剤(E)の含有量が、ウレタン形成成分100質量%に対して、0.001~10.0質量%である、請求項4に記載の防曇性被膜形成用塗布剤。 The antifogging coating according to claim 4, wherein the content of the water repellent agent (D) or hydrophilic agent (E) is 0.001 to 10.0% by mass with respect to 100% by mass of the urethane-forming component. Forming coating. 基材と防曇性被膜とを有する防曇性物品の製造方法であって、
基材の表面に、請求項1~8のいずれか1項に記載の防曇性被膜形成用塗布剤を塗布し、塗膜を形成する工程(1)と、
前記塗膜から前記溶媒(C)を蒸散させ、前記塗膜を硬化して防曇性被膜を形成する工程(2)と、
を備える、防曇性物品の製造方法。
A method for producing an antifogging article having a substrate and an antifogging coating, comprising:
A step (1) of applying the coating agent for forming an antifogging film according to any one of claims 1 to 8 to the surface of a substrate to form a coating film;
Step (2) of evaporating the solvent (C) from the coating film and curing the coating film to form an antifogging coating;
A method for manufacturing an anti-fogging article.
前記基材はガラス基材である請求項9に記載の防曇性物品の製造方法。 10. The method for producing an antifogging article according to claim 9, wherein said substrate is a glass substrate. 前記ガラス基材の表面には、シランカップリング剤が塗布されている、請求項10に記載の防曇性物品の製造方法。 The method for producing an antifogging article according to claim 10, wherein the surface of the glass substrate is coated with a silane coupling agent. 前記工程(2)において、前記ポリイソシアネート(A)のイソシアネート基と、前記ポリオール(B)のヒドロキシ基が反応し、ポリウレタンを形成する、請求項9~11のいずれか1項に記載の防曇性物品の製造方法。 The antifogging according to any one of claims 9 to 11, wherein in the step (2), the isocyanate groups of the polyisocyanate (A) react with the hydroxy groups of the polyol (B) to form polyurethane. method of manufacturing a sexual product. 前記工程(2)において、前記塗膜を80~170℃で加熱する、請求項9~12のいずれか1項に記載の防曇性物品の製造方法。 The method for producing an antifogging article according to any one of claims 9 to 12, wherein in the step (2), the coating film is heated at 80 to 170°C. 基材と防曇性被膜とを有する防曇性物品であって、
前記防曇性被膜は、請求項1~8のいずれか1項に記載の防曇性被膜形成用塗布剤の硬化物であるポリウレタン樹脂を含む被膜であり、
前記防曇性被膜の膜厚は5μm~50μmである、
防曇性物品。
An antifogging article having a substrate and an antifogging coating,
The antifogging coating is a coating containing a polyurethane resin, which is a cured product of the coating agent for forming an antifogging coating according to any one of claims 1 to 8,
The film thickness of the antifogging coating is 5 μm to 50 μm,
Anti-fogging article.
前記基材はガラス基材である請求項14に記載の防曇性物品。 15. The antifogging article according to claim 14, wherein said substrate is a glass substrate. 前記ガラス基材の表面には、シランカップリング剤が塗布されている、請求項15に記載の防曇性物品。 16. The antifogging article according to claim 15, wherein the surface of said glass substrate is coated with a silane coupling agent. 水平に置いた前記防曇性被膜の表面に水を滴下し、60℃で1時間乾燥させた後に水垢を除去し、水垢が付着していた部分の膨潤部の段差が200nm以下である、請求項14~16のいずれか1項に記載の防曇性物品。

Water is dropped on the surface of the antifogging coating placed horizontally, dried at 60° C. for 1 hour, and then water scale is removed. Item 17. The antifogging article according to any one of items 14 to 16.

JP2022007614A 2022-01-21 2022-01-21 Application agent for forming anti-fogging coating, method for producing anti-fogging article, and anti-fogging article Pending JP2023106722A (en)